A method for preparing high-cost-effective fine slices and fine slices

By adopting the three-layer blank structure fine slice preparation method, combined with cold pressing and hot pressing sintering technology, the existing fine slices have been solved in terms of edge cutting quality, cutting speed, service life and cost, and achieved cost-effective precision Slicing meets market demand.

CN113681004BActive Publication Date: 2024-11-19QUANZHOU ZHONGZHI NEW MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110911700.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-10
Publication Date
2024-11-19
Estimated Expiration
2041-08-10

AI Technical Summary

Technical Problem

The existing fine slices have shortcomings in taking into account the quality of edge cutting and cutting speed, and have short service life, high cost and low cost performance, making it difficult to meet market demand.

Method used

The cutting head is prepared by using the three-layer blank structure, including edge laminate, intermediate laminate and edge laminate. The cutting head is prepared by cold pressing and hot pressing sintering technology, and welded to the substrate to combine specific Raw materials and proportion design, optimize the thickness ratio of the cutter head to improve cutting performance and reduce costs.

Benefits of technology

It achieves cost-effective fine slicing, taking into account the quality of edge cutting and cutting speed, extends service life, and reduces production costs, and has a broad market prospect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113681004B_ABST
    Figure CN113681004B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and a fine slice with high cost performance ratio. The fine slice prepared can take into account both the edge cutting quality and the cutting speed, has a long service life, a low overall production cost, a high cost performance ratio and a broad market prospect. The fine slice of the invention abandons the single-layer structure of the existing fine slice and innovatively adopts a three-layer blank structure, which is composed of an edge layer pressed blank + an intermediate layer pressed blank + an edge layer pressed blank mode. The diamond grain size in the edge layer pressed blank is finer, which ensures that the edge cutting is neat during cutting and improves the edge cutting quality. The diamond in the intermediate layer pressed blank is coarser, which ensures that the edge cutting is sharp and the speed is fast during cutting. The fine grain size and low concentration can also greatly reduce the cost, so that both the sharpness and the good edge cutting quality can be maintained. Moreover, based on the specific raw materials and specific ratios of the two pressed blanks, the three-layer blank structure is prepared, which solves the problems of the slicing quality, cutting performance, service life and cost of the cutter head.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of diamond tool preparation, in particular to a preparation method and a fine slice with high cost performance. Background Art

[0002] At present, diamond slices have been widely used in the cutting of marble, concrete, granite, ceramics, glass and other hard and brittle non-metallic materials in the market; fine slices are a kind of diamond saw blade, which is mainly composed of a diamond bit and a matrix; during use, the diamond bit is mainly used to cut materials, and the matrix mainly supports the cutting work of the diamond bit; there are many objects that can be processed by diamond saw blades, and fine slices are mainly used to process some materials with high requirements on cutting edge quality, such as artificial stone, marble, ceramic tile, etc.; many fine slices are difficult to take into account good cutting edge quality, fast cutting speed, service life and cost issues, and the saw blades have low cost performance.

[0003] In view of this, the inventor has made in-depth considerations and actively researched, improved and tried to develop and design the present invention in order to solve the many deficiencies and inconveniences caused by the imperfections in the above-mentioned fine slice preparation method and structural design. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing a high-cost-effective fine-slice and a fine-slice. The fine-slice produced can take into account both the trimming quality and the cutting speed, has a long service life, has a low overall production cost, has a high cost-effectiveness, and has a broad market prospect.

[0005] In order to achieve the above object, the solution of the present invention is:

[0006] A method for preparing a high-cost-effective fine section comprises the following steps:

[0007] S1. Prepare a matrix material: weigh 15%-30% Fe-Cu-Sn-Co pre-alloy powder, 25%-40% Cu-Sn pre-alloy powder and 30%-50% Fe-Cu-Sn-Ni pre-alloy powder respectively by weight and mix them evenly to obtain a matrix material;

[0008] S2. Prepare diamond materials: a. Diamond material for the side layer: a uniform mixture of diamonds with a particle size of 70 / 80-100 / 120; b. Diamond material for the middle layer: a uniform mixture of diamonds with a particle size of 45 / 50-70 / 80;

[0009] S3, preparing edge layer blanks and middle layer blanks: a, edge layer blanks, weighing 75%-95% of matrix material and 5%-25% of edge layer diamond material by weight percentage and evenly mixing; b, middle layer blanks, weighing 75%-95% of matrix material and 5%-25% of middle layer diamond material by weight percentage and evenly mixing;

[0010] S4, preparing a cutter head: a, cold pressing the edge layer blank and the middle layer blank into an edge layer blank and an middle layer blank respectively; b, sequentially loading the blanks into a graphite mold in the order of a three-layer structure of "edge layer blank + middle layer blank + edge layer blank", and hot pressing and sintering to obtain a fine-slicing cutter head;

[0011] S5, welding the fine-slice cutter head obtained in step S4 to the substrate, and obtaining a fine-slice cutter head through shaping, polishing and sharpening.

[0012] In step S3, when mixing the side layer blanks, add 5-10 ml / kg of liquid paraffin and mix them in a mixer for 2-3 hours; when mixing the middle layer blanks, add 5-10 ml / kg of liquid paraffin and mix them in a mixer for 2-3 hours.

[0013] In step S4, the pressure used for cold pressing is 2.5-3.0 t / cm 2 .

[0014] In step S4, the graphite mold is hot-pressed and sintered in a hot-pressing sintering machine at a sintering temperature of 700-800°C and a sintering pressure of 350-400 kg / cm 2 , the sintering holding time is 1.5-2.5 minutes.

[0015] The thickness of the side layer blank: the thickness of the middle layer blank = 1:1.5-2.5.

[0016] The thickness of the side layer blank: the thickness of the middle layer blank = 1:1.8.

[0017] The components and weight percentages of the Fe-Cu-Sn-Co pre-alloyed powder are as follows: Fe 55%-65%, Cu 10%-20%, Sn 2%-10%, Co 10%-25%.

[0018] The components and weight percentages of the Cu-Sn pre-alloyed powder are as follows: Cu 80%-90% Sn 10%-20%.

[0019] The components and weight percentages of the Fe-Cu-Sn-Ni pre-alloyed powder are as follows: Fe 40%-50%, Cu 35%-45%, Sn 2%-8%, Ni 2%-10%.

[0020] The powder particle size of the Fe-Cu-Sn-Co pre-alloyed powder, the Cu-Sn pre-alloyed powder and the Fe-Cu-Sn-Ni pre-alloyed powder is 200-400 meshes.

[0021] In step S5, the substrate is selected to have a diameter of 350 mm, a material of 65Mn and 25 teeth.

[0022] In step S5, the fine slicing cutter head and the substrate are welded together using silver solder sheets and high-frequency induction.

[0023] A fine slice is prepared by the above-mentioned method for preparing the fine slice with high cost performance.

[0024] After adopting the above structure, the invention provides a method for preparing a high-cost-effective fine slice and a fine slice, and the fine slice prepared can take into account both the cutting quality and the cutting speed, has a long service life, a low overall production cost, a high cost-effectiveness, and a broad market prospect; and the beneficial effect relative to the prior art is that: the fine slice prepared by the invention abandons the single-layer structure of the existing fine slice, and innovatively adopts a three-layer blank structure, which is composed of an edge layer pressed blank + an intermediate layer pressed blank + an edge layer pressed blank mode; and the diamond grain size in the edge layer pressed blank is finer, which ensures that the cutting edge is neat during cutting and improves the cutting edge quality; the diamond in the intermediate layer pressed blank is coarser, which ensures that the cutting edge is sharp and the speed is fast; due to the fine grain size and low concentration, the cost can also be greatly reduced, so that both the sharpness and the good cutting quality can be maintained; and, based on the specific raw materials and specific ratios of the two pressed blanks, a three-layer blank structure is prepared, which solves the problems of the slicing quality, cutting performance, service life and cost of the cutter head. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a cross-sectional schematic diagram of the fine slicing cutter head of the present invention.

[0026] Explanation of symbols

[0027] Side laminated blank 1 Middle laminated blank 2

[0028] Diamond 10, 20. DETAILED DESCRIPTION

[0029] In order to further explain the technical solution of the present invention, the present invention is described in detail below through specific embodiments.

[0030] The present invention discloses a method for preparing a high-cost-effective fine-section, which comprises the following steps:

[0031] S1. Prepare a matrix material: weigh 15%-30% Fe-Cu-Sn-Co pre-alloy powder, 25%-40% Cu-Sn pre-alloy powder and 30%-50% Fe-Cu-Sn-Ni pre-alloy powder respectively by weight and mix them evenly to obtain a matrix material;

[0032] S2. Prepare diamond materials: a. The side layer diamond material 10 is made of a uniform mixture of diamonds with a particle size of 70 / 80-100 / 120; b. The middle layer diamond material 20 is made of a uniform mixture of diamonds with a particle size of 45 / 50-70 / 80;

[0033] S3, preparing edge layer blanks and middle layer blanks: a, edge layer blanks, weighing 75%-95% of matrix material and 5%-25% of edge layer diamond material by weight percentage and evenly mixing; b, middle layer blanks, weighing 75%-95% of matrix material and 5%-25% of middle layer diamond material by weight percentage and evenly mixing;

[0034] S4, preparing the cutter head: a, cold pressing the edge layer blank and the middle layer blank into edge layer blank 1 and middle layer blank 2 respectively; b, sequentially loading the blanks into a graphite mold in the order of "edge layer blank + middle layer blank + edge layer blank", and hot pressing and sintering to obtain a fine-cutting cutter head (see Figure 1 );

[0035] S5, welding the fine-slice cutter head obtained in step S4 to the substrate, and obtaining a fine-slice cutter head through shaping, polishing and sharpening.

[0036] The invention discloses a method for preparing a high-cost-effective fine slice and a fine slice. The fine slice prepared by the invention can take into account both the cutting quality and the cutting speed, has a long service life, a low overall production cost, a high cost-effectiveness and a broad market prospect. The beneficial effects compared with the prior art are as follows: the fine slice prepared by the invention abandons the single-layer structure of the existing fine slice and innovatively adopts a three-layer blank structure, which is composed of an edge layer pressed blank + an intermediate layer pressed blank + an edge layer pressed blank mode; the diamond grain size in the edge layer pressed blank is finer, which ensures that the cutting edge is neat during cutting and improves the cutting edge quality; the diamond in the intermediate layer pressed blank is coarser, which ensures that the cutting edge is sharp and the cutting speed is fast; the fine grain size and low concentration can also greatly reduce the cost, so that both the sharpness and the good cutting edge quality can be maintained; and the three-layer blank structure is prepared on the basis of specific raw materials and specific ratios of the two pressed blanks, which solves the problems of the slicing quality, cutting performance, service life and cost of the cutter head.

[0037] In step S3 of the present invention, when mixing the edge layer blanks, 5-10 ml / kg of liquid paraffin is added and mixed in a mixer for 2-3 hours; when mixing the middle layer blanks, 5-10 ml / kg of liquid paraffin is added and mixed in a mixer for 2-3 hours.

[0038] In step S4 of the present invention, the pressure used for cold pressing is 2.5-3.0 t / cm 2 .

[0039] In step S4 of the present invention, the graphite mold is hot-pressed and sintered in a hot-pressing sintering machine at a sintering temperature of 700-800°C and a sintering pressure of 350-400kg / cm 2 , the sintering holding time is 1.5-2.5 minutes.

[0040] The thickness of the side layer blank 1 of the present invention: the thickness of the middle layer blank 2 = 1: 1.5-2.5.

[0041] The thickness of the side layer blank 1 of the present invention: the thickness of the middle layer blank 2 = 1:1.8.

[0042] The precision slicing cutter head of the present invention is based on the specific raw materials and specific ratio of the edge layer blank 1 and the middle layer blank 2, and the thickness ratio of the two directly affects the quality, cutting performance, life and cost of the produced cutter head; the existing precision slicing cutter head adopts a single-layer structure, so the thickness ratio problem is not involved. Even if there are multi-layer structure designs in the field of cutter heads, they are usually the same multi-layer diamond layer structure. Even if there are different layer structures, the design of different layer thicknesses is not involved to achieve the overall performance optimization of the cutter head; the saw blade and cutter head designed for precision cutting of the present invention, the cutter head specially adopts a three-layer structure of specific blanks, and the thickness of the specific three-layer structure is optimized in a targeted manner. The effect brought about can take into account the cutting quality, cutting speed, service life and saw blade cost and other issues.

[0043] The components and weight percentages of the Fe-Cu-Sn-Co prealloyed powder of the present invention are as follows: Fe 55%-65%, Cu 10%-20%, Sn 2%-10%, Co 10%-25%; the Fe-Cu-Sn-Co prealloyed powder has good self-sharpening property, good diamond holding force, and can improve the sharpness of the saw blade.

[0044] The components and weight percentages of the Cu-Sn pre-alloyed powder of the present invention are as follows: Cu 80%-90%, Sn 10%-20%; the Cu-Sn pre-alloyed powder has a low sintering temperature and has a connection effect between various metals.

[0045] The components and weight percentages of the Fe-Cu-Sn-Ni pre-alloyed powder of the present invention are as follows: Fe 40%-50%, Cu 35%-45%, Sn 2%-8%, Ni 2%-10%; the Fe-Cu-Sn-Ni pre-alloyed powder has good impact resistance, and combined with the above two alloy powders, it can resist harder materials during cutting and enhance the cutting life of the product.

[0046] The powder particle size of the Fe-Cu-Sn-Co prealloyed powder, Cu-Sn prealloyed powder and Fe-Cu-Sn-Ni prealloyed powder of the present invention is 200-400 meshes.

[0047] In step S5 of the present invention, the substrate is a substrate with a diameter of 350 mm, a material of 65Mn and 25 teeth.

[0048] In step S5 of the present invention, the fine slicing cutter head and the substrate are welded together using silver solder sheets through high-frequency induction.

[0049] First embodiment

[0050] S1. Prepare carcass materials:

[0051] 1. Prepare Fe-Cu-Sn-Co pre-alloyed powder, weighing 55% Fe, 20% Cu, 5% Sn, and 20% Co by weight percentage;

[0052] 2. Prepare Cu-Sn pre-alloyed powder, weighing 80% Cu and 20% Sn by weight percentage;

[0053] 3. Prepare Fe-Cu-Sn-Ni pre-alloy powder, weighing 40% Fe, 45% Cu, 5% Sn, and 10% Ni by weight percentage;

[0054] 4. Weigh 15% Fe-Cu-Sn-Co prealloy powder, 35% Cu-Sn prealloy powder, and 50% Fe-Cu-Sn-Ni prealloy powder by weight and mix them evenly to form a matrix material; the powder particle size of the Fe-Cu-Sn-Co prealloy powder, the Cu-Sn prealloy powder, and the Fe-Cu-Sn-Ni prealloy powder is 200-400 mesh;

[0055] S2. Prepare diamond materials: a. Diamond material for the side layer: a uniform mixture of diamonds with a particle size of 70 / 80-100 / 120; b. Diamond material for the middle layer: a uniform mixture of diamonds with a particle size of 45 / 50-70 / 80;

[0056] S3, prepare the edge layer blank and the middle layer blank: a, edge layer blank, weigh 75%-95% of the matrix material and 5%-25% of the edge layer diamond material by weight percentage, add 5-10ml / kg of liquid paraffin, mix in a mixer for 2-3 hours; b, middle layer blank, weigh 75%-95% of the matrix material and 5%-25% of the middle layer diamond material by weight percentage, add 5-10ml / kg of liquid paraffin, mix in a mixer for 2-3 hours;

[0057] S4. Prepare the cutter head: a. Press the edge layer blank and the middle layer blank into edge layer blank and middle layer blank respectively by cold pressing, and the pressure used for cold pressing is 2.5-3.0t / cm 2b. The green sheets are sequentially loaded into a graphite mold in the order of "edge layer green sheet + middle layer green sheet + edge layer green sheet", and hot pressed and sintered to obtain a fine-cutting blade; the graphite mold is hot pressed and sintered in a hot pressing and sintering machine at a sintering temperature of 700-800°C and a sintering pressure of 350-400kg / cm 2 , sintering holding time is 1.5-2.5 minutes;

[0058] S5. The fine-slice cutter head obtained in step S4 is welded to the substrate by high-frequency induction using a silver solder sheet, and is shaped, polished, and sharpened to obtain a fine-slice cutter head.

[0059] Second embodiment

[0060] S1. Prepare carcass materials:

[0061] 1. Prepare Fe-Cu-Sn-Co pre-alloyed powder, weighing 65% Fe, 15% Cu, 5% Sn, and 15% Co by weight percentage;

[0062] 2. Prepare Cu-Sn pre-alloyed powder, weighing 90% Cu and 10% Sn by weight percentage;

[0063] 3. Prepare Fe-Cu-Sn-Ni pre-alloy powder, weighing 50% Fe, 40% Cu, 5% Sn, and 5% Ni by weight percentage;

[0064] 4. Weigh 30% Fe-Cu-Sn-Co prealloy powder, 30% Cu-Sn prealloy powder, and 40% Fe-Cu-Sn-Ni prealloy powder by weight and mix them evenly to form a matrix material; the powder particle size of the Fe-Cu-Sn-Co prealloy powder, the Cu-Sn prealloy powder, and the Fe-Cu-Sn-Ni prealloy powder is 200-400 mesh;

[0065] S2. Prepare diamond materials: a. Diamond material for the side layer: a uniform mixture of diamonds with a particle size of 70 / 80-100 / 120; b. Diamond material for the middle layer: a uniform mixture of diamonds with a particle size of 45 / 50-70 / 80;

[0066] S3, prepare the edge layer blank and the middle layer blank: a, edge layer blank, weigh 75%-95% of the matrix material and 5%-25% of the edge layer diamond material by weight percentage, add 5-10ml / kg of liquid paraffin, mix in a mixer for 2-3 hours; b, middle layer blank, weigh 75%-95% of the matrix material and 5%-25% of the middle layer diamond material by weight percentage, add 5-10ml / kg of liquid paraffin, mix in a mixer for 2-3 hours;

[0067] S4. Prepare the cutter head: a. Press the edge layer blank and the middle layer blank into edge layer blank and middle layer blank respectively by cold pressing, and the pressure used for cold pressing is 2.5-3.0t / cm 2 b. The green sheets are sequentially loaded into a graphite mold in the order of "edge layer green sheet + middle layer green sheet + edge layer green sheet", and hot pressed and sintered to obtain a fine-cutting blade; the graphite mold is hot pressed and sintered in a hot pressing and sintering machine at a sintering temperature of 700-800°C and a sintering pressure of 350-400kg / cm 2 , sintering holding time is 1.5-2.5 minutes;

[0068] S5. The fine-slice cutter head obtained in step S4 is welded to the substrate by high-frequency induction using a silver solder sheet, and is shaped, polished, and sharpened to obtain a fine-slice cutter head.

[0069] See also Figure 1 The present invention also discloses a fine slice, which is made by the above-mentioned method for preparing a high-cost-effective fine slice; the fine slice comprises a substrate and a fine slice cutter head welded on the substrate; the fine slice cutter head is a three-layer structure, having two edge layer blanks located at the upper and lower layers and an intermediate layer blank located at the intermediate layer; the fine slice made can take into account both the edge cutting quality and the cutting speed, has a long service life, a low overall production cost, a high cost-effectiveness, and a broad market prospect; the fine slice made by the present invention abandons the single-layer structure of the existing fine slice, and innovatively adopts a three-layer blank structure, the three The layer blank structure is composed of edge laminated blank + middle laminated blank + edge laminated blank mode; the diamond grain size in the edge laminated blank is finer, which ensures neat cutting edge and improves cutting edge quality; the diamond in the middle laminated blank is coarser, which ensures sharpness and fast cutting speed; the fine grain size and low concentration can also greatly reduce the cost, so that both sharpness and good cutting edge quality can be maintained; moreover, based on the specific raw materials and specific ratios of the two pressed blanks, a three-layer blank structure is made, which solves many problems such as slicing quality, cutting performance, service life and cost of the cutter head.

[0070] The above embodiments and drawings do not limit the product form and style of the present invention. Any appropriate changes or modifications made thereto by ordinary technicians in the relevant technical field should be deemed to be within the patent scope of the present invention.

Claims

1. A method for preparing a high-cost-effective fine section, characterized in that: The following steps are involved: S1. Prepare the matrix material: weigh 15%-30% Fe-Cu-Sn-Co pre-alloy powder, 25%-40% Cu-Sn pre-alloy powder and 30%-50% Fe-Cu-Sn-Ni pre-alloy powder respectively by weight and mix them evenly to obtain the matrix material; The components and weight percentages of the Fe-Cu-Sn-Co pre-alloyed powder are as follows: Fe 55%-65%, Cu 10%-20%, Sn 2%-10%, Co 10%-25%; The components and weight percentages of the Cu-Sn pre-alloyed powder are as follows: Cu 80%-90% Sn 10%-20%; The components and weight percentages of the Fe-Cu-Sn-Ni pre-alloyed powder are as follows: Fe 40%-50%, Cu 35%-45%, Sn 2%-8%, Ni 2%-10%; S2. Prepare diamond materials: a. Diamond material for the side layer: a uniform mixture of diamonds with a particle size of 70 / 80-100 / 120; b. Diamond material for the middle layer: a uniform mixture of diamonds with a particle size of 45 / 50-70 / 80; S3, preparing edge layer blanks and middle layer blanks: a, edge layer blanks, weighing 75%-95% of matrix material and 5%-25% of edge layer diamond material by weight percentage and evenly mixing; b, middle layer blanks, weighing 75%-95% of matrix material and 5%-25% of middle layer diamond material by weight percentage and evenly mixing; S4, preparing a cutter head: a, cold pressing the edge layer blank and the middle layer blank into an edge layer blank and an middle layer blank respectively; b, sequentially loading the blanks into a graphite mold in the order of a three-layer structure of "edge layer blank + middle layer blank + edge layer blank", and hot pressing and sintering to obtain a fine-slicing cutter head; S5, the fine slice obtained in step S4 is welded to the substrate, and after shaping, polishing, and sharpening to obtain a fine slice; In step S3, when the edge layer of the billet is mixed, add liquid paraffin at a ratio of 5-10ml / kg, and mix on a mixer for 2-3 hours; when the intermediate layer of the billet is mixed, add liquid paraffin at a ratio of 5-10ml / kg, and mix on a mixer for 2-3 hours; In step S4, the pressure used for cold pressing is 2.5-3.0 t / cm 2 ;The graphite mold is hot pressed and sintered in a hot press sintering machine. The sintering temperature is 700-800℃ and the sintering pressure is 350-400kg / cm 2 , the sintering holding time is 1.5-2.5 minutes.

2. A method for preparing a high-cost-effective fine section as claimed in claim 1, characterized in that: The thickness of the side layer blank: the thickness of the middle layer blank = 1:1.5-2.

5.

3. A method for preparing a high-cost-effective fine section as claimed in claim 2, characterized in that: The thickness of the side layer blank: the thickness of the middle layer blank = 1:1.

8.

4. A method for preparing a high-cost-effective fine section as claimed in claim 1, characterized in that: The powder particle size of the Fe-Cu-Sn-Co pre-alloyed powder, the Cu-Sn pre-alloyed powder and the Fe-Cu-Sn-Ni pre-alloyed powder is 200-400 meshes.

5. A method for preparing a high-cost-effective fine section as claimed in claim 1, characterized in that: In step S5, the substrate is selected to have a diameter of 350 mm, a material of 65Mn and 25 teeth.

6. A method for preparing a high-cost-effective fine section as claimed in claim 1, characterized in that: In step S5, the fine slicing cutter head and the substrate are welded together using silver solder sheets and high-frequency induction.

7. A fine section, characterized in that: The fine slice is made by the method for preparing the cost-effective fine slice according to any one of claims 1 to 6.