Liquid ejection head and liquid ejection device
By using a multi-layer structure vibration plate design in a piezoelectric inkjet printer, using chromium or titanium oxide as an intermediate layer to reduce the reduction of silicon oxide, the layer caused by the reduction of silicon oxide in the prior art is solved. The problem of separation improves the stability and life of the equipment.
Patent Information
- Application Number
- CN202110533928.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-05-20
- Filing Date
- 2021-05-17
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-05-17
AI Technical Summary
In the existing piezoelectric inkjet printers, the heat treatment between the elastic film composed of silicon dioxide and the insulator film composed of zirconium oxide causes the silicon oxide to be reduced by zirconium, forming a void, resulting in separation or cracks between the layers of the vibrating plate, affecting Equipment stability.
Design of a multi-layer structure of diaphragm, in which the first layer is silicon, the second layer is oxide of metal elements that are more difficult to oxidize, such as chromium or titanium, and the third layer is zirconium oxide, which is formed by lamination technology to reduce silicon Reduction of oxides and interlayer separation.
It effectively reduces the reduction of silicon oxide and interlayer separation, improves the clinging force and stability of the vibration plate, reduces the risk of cracks, and extends the service life of the equipment.
Smart Images

Figure CN113696624B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a liquid ejection head, a liquid ejection device, a piezoelectric device and a method for manufacturing the piezoelectric device. Background Art
[0002] Liquid ejection devices represented by piezoelectric inkjet printers include a piezoelectric element and a vibration plate that vibrates by driving the piezoelectric element. For example, Patent Document 1 discloses a vibration plate having an elastic film composed of silicon dioxide and an insulating film composed of zirconium oxide. Here, the elastic film is formed by thermally oxidizing one side of a single crystal silicon substrate. The insulating film is formed by thermally oxidizing a layer of zirconium monomer formed on the elastic film by sputtering or the like.
[0003] Zirconium is more easily oxidized than silicon. Therefore, in a structure in which an elastic film composed of silicon dioxide and an insulating film composed of zirconium oxide are in contact as described in Patent Document 1, silicon dioxide in the elastic film is reduced by zirconium due to heat treatment when the insulating film is formed. As a result, there is a possibility that silicon monomer generated by the reduction diffuses from the elastic film to the insulating film, and a void is formed between the elastic film and the insulating film with the diffusion. The void becomes a major cause of damage such as interlayer separation or cracks on the vibration plate with the vibration.
[0004] Patent Document 1: Japanese Patent Application Publication No. 2008-78407 Summary of the invention
[0005] In order to solve the above problems, one method of the liquid ejection head involved in the present invention comprises: a piezoelectric body; a vibration plate, which vibrates by being driven by the piezoelectric body; a pressure chamber substrate, which is provided with a pressure chamber for applying pressure to the liquid by the vibration of the vibration plate, and the pressure chamber substrate, the vibration plate and the piezoelectric body are laminated in this order, and the vibration plate comprises: a first layer, which contains silicon as a constituent element; a second layer, which is arranged between the first layer and the piezoelectric body and includes any one metal element of chromium, titanium and aluminum as a constituent element; and a third layer, which is arranged between the second layer and the piezoelectric body and includes zirconium as a constituent element.
[0006] Another embodiment of the liquid ejection head involved in the present invention comprises: a piezoelectric body; a vibration plate, which vibrates by being driven by the piezoelectric body; a pressure chamber substrate, which is provided with a pressure chamber for applying pressure to the liquid by the vibration of the vibration plate, and the pressure chamber substrate, the vibration plate and the piezoelectric body are laminated in this order, and the vibration plate comprises: a first layer, which contains silicon as a constituent element; a second layer, which is arranged between the first layer and the piezoelectric body and contains a metal element that is more difficult to be oxidized than zirconium as a constituent element; and a third layer, which is arranged between the second layer and the piezoelectric body and contains zirconium as a constituent element.
[0007] Another embodiment of the liquid ejection head involved in the present invention comprises: a piezoelectric body; a vibration plate, which vibrates by being driven by the piezoelectric body; a pressure chamber substrate, which is provided with a pressure chamber for applying pressure to the liquid by the vibration of the vibration plate, and the pressure chamber substrate, the vibration plate and the piezoelectric body are laminated in this order, and the vibration plate comprises: a first layer, which contains silicon as a constituent element; a second layer, which is arranged between the first layer and the piezoelectric body and contains a metal element with a larger oxide formation free energy than zirconium as a constituent element; and a third layer, which is arranged between the second layer and the piezoelectric body and contains zirconium as a constituent element.
[0008] One aspect of a liquid ejection device according to the present invention includes: the liquid ejection head according to any one of the above aspects; and a control unit that controls the driving of the piezoelectric body.
[0009] One embodiment of the piezoelectric device involved in the present invention comprises: a piezoelectric body; a vibration plate on which the piezoelectric body is laminated, and the vibration plate comprises: a first layer, which contains silicon as a constituent element; a second layer, which is arranged between the first layer and the piezoelectric body and contains any one metal element of chromium, titanium and aluminum as a constituent element; and a third layer, which is arranged between the second layer and the piezoelectric body and contains zirconium as a constituent element.
[0010] One form of the manufacturing method of the piezoelectric device involved in the present invention is a manufacturing method for a piezoelectric device having a piezoelectric body and a vibration plate laminated with the piezoelectric body, the manufacturing method comprising: a process of forming the vibration plate and a process of forming the piezoelectric body, in the process of forming the vibration plate, a first layer containing silicon as a constituent element is formed, after the first layer is formed, a second layer containing a metal element that is more difficult to oxidize than zirconium as a constituent element is formed, and after the second layer is formed, a third layer containing zirconium as a constituent element is formed. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1It is a diagram schematically showing the structure of the liquid ejecting device according to the first embodiment.
[0012] Figure 2 It is an exploded perspective view of the liquid ejecting head according to the first embodiment.
[0013] Figure 3 for Figure 2 Sectional view along line III-III.
[0014] Figure 4 It is a plan view showing a vibration plate of the liquid ejecting head in the first embodiment.
[0015] Figure 5 for Figure 4 The Ⅴ-Ⅴ line cross-sectional view.
[0016] Figure 6 A diagram for explaining a method for manufacturing a piezoelectric device.
[0017] Figure 7 It is a cross-sectional view of a liquid ejecting head according to a second embodiment.
[0018] Figure 8 It is a cross-sectional view of a liquid ejecting head according to a third embodiment.
[0019] Fig. 9 This is a diagram showing the analysis results of the vibration plate in Example A7 by SIMS.
[0020] Fig.10 This is a diagram showing the analysis results of the vibration plate in Example B1 by SIMS.
[0021] Fig.11 It is a figure which shows the analysis result of the vibration plate in the comparative example by SIMS.
[0022] Fig.12 It is a figure which shows the analysis result of the vibration plate in Example C3, Example C4, and a comparative example by SIMS. DETAILED DESCRIPTION
[0023] Hereinafter, preferred embodiments of the present invention will be described with reference to the accompanying drawings. In addition, in the accompanying drawings, the size or scale of each part may be appropriately different from the actual situation, and there are also parts schematically shown for easy understanding. In addition, as long as the meaning of limiting the present invention is not particularly recorded in the following description, the scope of the present invention is not limited to these modes.
[0024] In addition, the following description is appropriately performed using the mutually intersecting X-axis, Y-axis, and Z-axis. In addition, a direction along the X-axis is referred to as the X1 direction, and the direction opposite to the X1 direction is referred to as the X2 direction. Similarly, the directions opposite to each other along the Y-axis are referred to as the Y1 direction and the Y2 direction. In addition, the directions opposite to each other along the Z-axis are referred to as the Z1 direction and the Z2 direction. In addition, the situation of observing along the Z-axis direction is referred to as "planar observation".
[0025] Here, the Z axis is typically a vertical axis, and the Z2 direction is equivalent to the downward direction in the vertical direction. However, the Z axis may also be a non-vertical axis. In addition, although the X axis, the Y axis, and the Z axis are typically orthogonal to each other, they are not limited to this, and for example, they only need to intersect at an angle within a range of 80° or more and 100° or less.
[0026] 1. First Implementation
[0027] 1-1. Overall structure of liquid ejection device
[0028] Figure 1 1 is a schematic structural diagram of a liquid ejection device 100 according to the first embodiment. The liquid ejection device 100 is an inkjet printing device that ejects ink, which is an example of a liquid, in the form of droplets onto a medium 12. The medium 12 is typically a printing paper. In addition, the medium 12 is not limited to the printing paper, and may be a printing object of any material such as a resin film or cloth.
[0029] like Figure 1 As shown, a liquid container 14 for storing ink is mounted on the liquid ejection device 100. As specific forms of the liquid container 14, for example, a cartridge that can be attached to and detached from the liquid ejection device 100, a bag-shaped ink bag formed of a flexible film, and an ink tank that can replenish ink can be cited. In addition, the type of ink stored in the liquid container 14 is arbitrary.
[0030] The liquid ejection device 100 includes a control unit 20, a conveying mechanism 22, a moving mechanism 24, and a liquid ejection head 26. The control unit 20 includes, for example, a processing circuit such as a CPU (Central Processing Unit) or an FPGA (Field Programmable Gate Array) and a storage circuit such as a semiconductor memory, and controls the operation of each element of the liquid ejection device 100. Here, the control unit 20 is an example of a "control unit" and controls the driving of the piezoelectric body 443 described later.
[0031] The transport mechanism 22 transports the medium 12 in the Y2 direction under the control of the control unit 20. The moving mechanism 24 reciprocates the liquid ejection head 26 in the X1 direction and the X2 direction under the control of the control unit 20. Figure 1 In the example shown, the moving mechanism 24 includes a substantially box-shaped conveying body 242 called a carriage that accommodates the liquid ejecting head 26, and a conveying belt 244 that fixes the conveying body 242. In addition, the number of liquid ejecting heads 26 carried on the conveying body 242 is not limited to one, and may be multiple. In addition, on the conveying body 242, in addition to the liquid ejecting head 26, the above-mentioned liquid container 14 may also be carried.
[0032] The liquid ejection head 26 ejects the ink supplied from the liquid container 14 from a plurality of nozzles toward the Z2 direction onto the medium 12 under the control of the control unit 20. This ejection is performed in parallel with the conveyance of the medium 12 by the conveyance mechanism 22 and the reciprocating movement of the liquid ejection head 26 by the moving mechanism 24, thereby forming an image formed by the ink on the surface of the medium 12. Here, the liquid ejection head 26 is an example of a "piezoelectric device". In addition, the structure and manufacturing method of the liquid ejection head 26 will be described in detail below.
[0033] 1-2. Overall structure of the liquid ejection head
[0034] Figure 2 It is an exploded perspective view of the liquid ejection head 26 according to the first embodiment. Figure 3 for Figure 2 The Ⅲ-Ⅲ line section view in the figure. Figure 2 As shown in FIG. 1 , the liquid ejection head 26 has a plurality of nozzles N arranged in a direction along the Y axis. Figure 2 In the example shown, the plurality of nozzles N are divided into a first column L1 and a second column L2 arranged at intervals in the direction along the X-axis. The first column L1 and the second column L2 are respectively a set of a plurality of nozzles N arranged in a straight line in the direction along the Y-axis. Here, the elements associated with each nozzle N in the first column L1 and the elements associated with each nozzle N in the second column L2 in the liquid ejection head 26 are substantially symmetrical structures with each other in the direction along the X-axis.
[0035] The positions of the plurality of nozzles N in the first column L1 and the plurality of nozzles N in the second column L2 in the direction along the Y axis may be consistent with each other or different from each other. In the following, a structure in which the positions of the plurality of nozzles N in the first column L1 and the plurality of nozzles N in the second column L2 in the direction along the Y axis are consistent with each other is illustrated.
[0036] like Figure 2 as well as Figure 3As shown, the liquid ejection head 26 includes a flow path structure 30 , a nozzle plate 62 , a vibration absorber 64 , a vibration plate 36 , a wiring substrate 46 , a frame portion 48 , and a drive circuit 50 .
[0037] The flow channel structure 30 is a structure that forms a flow channel for supplying ink to a plurality of nozzles N. The flow channel structure 30 of this embodiment includes a flow channel substrate 32 and a pressure chamber substrate 34, and these are laminated in this order in the Z1 direction. The flow channel substrate 32 and the pressure chamber substrate 34 are respectively plate-shaped members that are elongated in the direction along the Y axis. The flow channel substrate 32 and the pressure chamber substrate 34 are bonded to each other, for example, by an adhesive.
[0038] The vibration plate 36, the wiring substrate 46, the frame portion 48, and the drive circuit 50 are provided in the region located closer to the Z1 direction than the flow path structure 30. On the other hand, the nozzle plate 62 and the vibration absorber 64 are provided in the region located closer to the Z2 direction than the flow path structure 30. The elements of the liquid ejection head 26 are plate-like members elongated in the Y direction, similarly to the flow path substrate 32 and the pressure chamber substrate 34, and are bonded to each other, for example, by an adhesive.
[0039] The nozzle plate 62 is a plate-shaped member on which a plurality of nozzles N are formed. Each of the plurality of nozzles N is a circular through hole through which ink passes. The nozzle plate 62 is manufactured, for example, by a method of processing a single crystal silicon substrate by a semiconductor manufacturing technology using a processing technology such as dry etching or wet etching. However, in the manufacture of the nozzle plate 62, other known methods and materials may be appropriately used.
[0040] On the flow channel substrate 32, a space Ra, a plurality of supply flow channels 322, a plurality of connecting flow channels 324, and a supply liquid chamber 326 are formed for the first column L1 and the second column L2, respectively. The space Ra is an elongated opening extending in the direction of the Y axis when viewed in a plane along the direction of the Z axis. The supply flow channel 322 and the connecting flow channel 324 are through holes formed for each nozzle N, respectively. The supply liquid chamber 326 is an elongated space extending in the direction of the Y axis across the plurality of nozzles N, and connects the space Ra and the plurality of supply flow channels 322 to each other. The plurality of connecting flow channels 324 overlap with one nozzle N corresponding to the connecting flow channel 324 when viewed in a plane.
[0041] The pressure chamber substrate 34 is a plate-like member in which a plurality of pressure chambers C, called cavities, are formed for the first column L1 and the second column L2, respectively. The plurality of pressure chambers C are arranged in the direction along the Y axis. Each pressure chamber C is a strip-shaped space formed for each nozzle N and extending in the direction along the X axis when viewed in a plan view. Like the nozzle plate 62 described above, the flow channel substrate 32 and the pressure chamber substrate 34 are respectively manufactured by the following method, which is, for example, a method of processing a single crystal silicon substrate using semiconductor manufacturing technology. However, other well-known methods and materials may be appropriately used in the manufacture of each of the flow channel substrate 32 and the pressure chamber substrate 34.
[0042] The pressure chamber C is a space located between the flow channel substrate 32 and the vibration plate 36. For the first column L1 and the second column L2, a plurality of pressure chambers C are arranged in the direction along the Y axis. In addition, the pressure chambers C are respectively connected to the communication flow channel 324 and the supply flow channel 322. Therefore, the pressure chamber C is connected to the nozzle N via the communication flow channel 324, and is connected to the space Ra via the supply flow channel 322 and the supply liquid chamber 326.
[0043] A vibration plate 36 is disposed on the surface of the pressure chamber substrate 34 that faces the Z2 direction. The vibration plate 36 is a plate-shaped member that can vibrate elastically. The vibration plate 36 will be described in detail below.
[0044] On the surface of the vibration plate 36 facing the Z1 direction, a plurality of piezoelectric elements 44 corresponding to the nozzles N are respectively arranged for the first column L1 and the second column L2. Each piezoelectric element 44 is a passive element that is deformed by the supply of a driving signal. Each piezoelectric element 44 is in the shape of a long strip extending in the direction along the X-axis when viewed in a plane. The plurality of piezoelectric elements 44 are arranged in the direction along the Y-axis in a manner corresponding to the plurality of pressure chambers C. When the vibration plate 36 vibrates in conjunction with the deformation of the piezoelectric element 44, the pressure in the pressure chamber C changes, thereby ejecting ink from the nozzle N. The piezoelectric element 44 will be described in detail below.
[0045] The frame portion 48 is a housing for storing ink supplied to the plurality of pressure chambers C. Figure 3As shown, in the frame portion 48 of the present embodiment, a space Rb is formed for each of the first column L1 and the second column L2. The space Rb of the frame portion 48 and the space Ra of the flow channel substrate 32 are connected to each other. The space formed by the space Ra and the space Rb functions as a liquid storage chamber (liquid reservoir) R for storing the ink supplied to the plurality of pressure chambers C. The ink is supplied to the liquid storage chamber R through the inlet 482 formed in the frame portion 48. The ink in the liquid storage chamber R is supplied to the pressure chamber C through the supply liquid chamber 326 and each supply flow channel 322. The vibration absorber 64 is a flexible film (plastic substrate) constituting the wall surface of the liquid storage chamber R, and absorbs the pressure fluctuation of the ink in the liquid storage chamber R.
[0046] The wiring substrate 46 is a plate-shaped member formed with wiring for electrically connecting the drive circuit 50 and the plurality of piezoelectric elements 44. The surface of the wiring substrate 46 facing the Z2 direction is bonded to the vibration plate 36 via a plurality of conductive bumps B. On the other hand, the drive circuit 50 is mounted on the surface of the wiring substrate 46 facing the Z1 direction. The drive circuit 50 is an IC (Integrated Circuit) chip that outputs a drive signal and a reference voltage for driving each piezoelectric element 44.
[0047] The end of the external wiring 52 is bonded to the surface of the wiring substrate 46 facing the Z1 direction. The external wiring 52 is composed of a connection component such as FPC (Flexible Printed Circuits) or FFC (Flexible Flat Cable). Figure 2 As shown, a plurality of wirings 461 and a plurality of wirings 462 are formed on the wiring substrate 46. The plurality of wirings 461 electrically connect the external wiring 52 and the driving circuit 50 together, and the plurality of wirings 462 are supplied with the driving signal output from the driving circuit 50 and the reference voltage.
[0048] 1-3. Details of the vibration plate and piezoelectric element
[0049] Figure 4 It is a plan view showing the vibration plate 36 of the liquid ejecting head 26 in the first embodiment. Figure 5 for Figure 4 The V-V line section view in the figure. Figure 4 as well as Figure 5 As shown, in the liquid ejection head 26, the pressure chamber substrate 34, the vibration plate 36, and the plurality of piezoelectric elements 44 are laminated in this order in the Z1 direction.
[0050] like Figure 5As shown in FIG. 1 , a hole 341 constituting the pressure chamber C is provided on the pressure chamber substrate 34. Accordingly, a wall-like partition portion 342 extending in the direction along the X-axis is provided between two adjacent holes 341 on the pressure chamber substrate 34. Figure 4 In FIG. 1 , the dotted line indicates the plan view shape of the hole 341 formed on the single crystal silicon substrate with a plane orientation (110) by anisotropic etching. In addition, the plan view shape of the hole 341 is not limited to Figure 4 The examples shown are rather arbitrary.
[0051] like Figure 4 As shown, the piezoelectric element 44 overlaps the pressure chamber C when viewed in a plan view. Figure 5 As shown in FIG. 1 , the piezoelectric element 44 includes a first electrode 441, a piezoelectric body 443, and a second electrode 442, and these are laminated in this order in the Z1 direction. In addition, the piezoelectric element 44 may also adopt a structure in which the electrodes and the piezoelectric body layers are alternately laminated into multiple layers, and the piezoelectric element 44 is expanded and contracted toward the vibration plate 36. In addition, other layers such as a layer for improving adhesion may be appropriately provided between the layers of the piezoelectric element 44 or between the piezoelectric element 44 and the vibration plate 36.
[0052] The first electrode 441 is an independent electrode that is disposed in a manner separated from each other for each piezoelectric element 44. Specifically, a plurality of first electrodes 441 extending in the direction along the X-axis are arranged in a manner spaced apart from each other in the direction along the Y-axis. A drive signal for ejecting ink from the nozzle N corresponding to the piezoelectric element 44 is applied to the first electrode 441 of each piezoelectric element 44 via the drive circuit 50.
[0053] The first electrode 441, for example, has a layer composed of iridium (Ir) and a layer composed of titanium (Ti), and they are laminated in the Z1 direction in this order. Here, iridium is an electrode material with excellent conductivity. Therefore, by using iridium in the constituent material of the first electrode 441, it is possible to achieve low resistance of the first electrode 441. In addition, when the layer composed of titanium forms the piezoelectric body 443, the island-shaped Ti becomes a crystallization nucleus and controls the orientation of the piezoelectric body 443, thereby improving the crystallinity or orientation of the piezoelectric body 443. In addition, a layer composed of other metal materials can be provided instead of the layer composed of iridium, or in addition to the layer. As the other metal materials, for example, metal materials such as platinum (Pt), aluminum (Al), nickel (Ni), gold (Au), and copper (Cu) can be listed, and one of these metal materials can be used alone or two or more of these metal materials can be combined for use. Alternatively, oxides of these metal elements can also be used.
[0054] The piezoelectric body 443 is in the shape of a band extending in the direction along the Y axis in a continuous manner across the plurality of piezoelectric elements 44. Although not shown in the figure, a through hole extending through the piezoelectric body 443 in the direction along the X axis is provided in the region corresponding to the gap between the pressure chambers C adjacent to each other when viewed in a plan view.
[0055] The piezoelectric body 443 has a general formula ABO 3 The piezoelectric material is composed of a piezoelectric material having a perovskite crystal structure represented by . As the piezoelectric material, for example, lead titanate (PbTiO 3 ), lead zirconate titanate (Pb(Zr,Ti)O 3 ), lead zirconate (PbZrO 3 )、lead lanthanum titanate ((Pb, La, TiO 3 ), lead lanthanum zirconate titanate ((Pb, La)(Zr, Ti)O 3 ), lead zirconate titanate niobium (Pb(Zr, Ti, Nb)O 3 ), lead zirconate magnesium niobate titanate (Pb(Zr,Ti)(Mg,Nb)O 3 ) etc. Among them, lead zirconate titanate is preferably used as the constituent material of the piezoelectric body 443.
[0056] The second electrode 442 is a belt-shaped common electrode extending in the direction along the Y axis so as to continuously extend across the plurality of piezoelectric elements 44. A predetermined reference voltage is applied to the second electrode 442.
[0057] The second electrode 442 is, for example, made of iridium (Ir). In addition, the constituent material of the second electrode 442 is not limited to iridium, and may be, for example, a metal material such as platinum (Pt), aluminum (Al), nickel (Ni), gold (Au), or copper (Cu). In addition, the second electrode 442 may use one of these metal materials alone, or may use a combination of two or more in a laminated manner. Alternatively, oxides of these metal elements may also be used.
[0058] exist Figure 4In the example shown, a first conductor 55 and a second conductor 56 are provided on the surface of the second electrode 442. The first conductor 55 is a strip-shaped conductive film extending in the direction along the Y axis along the edge in the X1 direction of the second electrode 442. The second conductor 56 is a strip-shaped conductive film extending in the direction along the Y axis along the edge in the X2 direction of the second electrode 442. The first conductor 55 and the second conductor 56 are made of a low-resistance conductive material such as gold, for example, and are formed together as the same layer. By means of the above-mentioned first conductor 55 and second conductor 56, the voltage drop of the reference voltage in the second electrode 442 can be suppressed. In addition, the first conductor 55 and the second conductor 56 also function as a counterweight to limit the vibration area of the vibration plate 36. In addition, the first conductor 55 and the second conductor 56 only need to be provided as needed, and can also be omitted.
[0059] As described above, the liquid ejection head 26 includes: the piezoelectric body 443; the vibration plate 36 that vibrates by driving the piezoelectric body 443; and the pressure chamber substrate 34 that is provided with the pressure chamber C that applies pressure to ink as an example of liquid by vibration of the vibration plate 36. The pressure chamber substrate 34, the vibration plate 36, and the piezoelectric body 443 are stacked in this order.
[0060] like Figure 5 As shown, the vibration plate 36 has a first layer 361, a second layer 362, and a third layer 363, and they are laminated in this order in the Z1 direction. That is, the vibration plate 36 has: a first layer 361; a second layer 362, which is arranged between the first layer 361 and the piezoelectric body 443; and a third layer 363, which is arranged between the second layer 362 and the piezoelectric body 443. Here, the first layer 361 is bonded to the pressure chamber substrate 34. The third layer 363 is bonded to a plurality of piezoelectric elements 44. The second layer 362 is interposed between the first layer 361 and the third layer 363. In addition, although in Figure 5 In the figure, for the sake of convenience, the interface between the layers constituting the vibration plate 36 is clearly shown, but the interface may be unclear, and for example, the constituent materials of the two layers may be mixed and exist near the interface between the two adjacent layers.
[0061] The first layer 361 is a layer containing silicon (Si) as a constituent element. More specifically, the first layer 361 is made of, for example, silicon oxide (SiO 2 Here, in addition to silicon oxide and its constituent elements, the first layer 361 may also contain a small amount of zirconium (Zr), titanium (Ti), iron (Fe), chromium (Cr) or hafnium (Hf) as an impurity. Such an impurity softens the silicon oxide (SiO 2 ) effect.
[0062] Thus, the first layer 361 includes, for example, silicon oxide. Such a first layer 361 is formed by thermal oxidation of a single crystal silicon substrate, and can be formed with higher productivity than when formed by a sputtering method.
[0063] In addition, the silicon in the first layer 361 may exist in the form of a monomer, a nitride, or a nitride oxide, in addition to being in the form of an oxide. In addition, the impurities in the first layer 361 may be elements that are inevitably mixed when the first layer 361 is formed, or may be elements that are intentionally mixed in the first layer 361.
[0064] The thickness T1 of the first layer 361 is determined by the thickness T and width W of the vibration plate 36 and is not particularly limited, but is preferably in the range of 100 nm to 2000 nm, and more preferably in the range of 500 nm to 1500 nm.
[0065] The third layer 363 is a layer containing zirconium (Zr) as a constituent element. More specifically, the third layer 363 is, for example, a layer made of zirconium oxide (ZrO 2 Here, in the third layer 363, in addition to zirconium oxide and its constituent elements, a small amount of titanium (Ti), iron (Fe), chromium (Cr) or hafnium (Hf) and other elements may be included as impurities. Such impurities soften the zirconium oxide (ZrO 2 ) effect.
[0066] Thus, the third layer 363 includes, for example, zirconium oxide. Such a third layer 363 is obtained, for example, by forming a zirconium monomer layer by sputtering or the like and then thermally oxidizing the layer. Therefore, when forming the third layer 363, the third layer 363 of a desired thickness can be easily obtained. In addition, since zirconium oxide has excellent electrical insulation, mechanical strength, and toughness, by making the third layer 363 include zirconium oxide, the characteristics of the vibration plate 36 can be improved. In addition, for example, in the case where the piezoelectric body 443 is composed of lead zirconate titanate, there is also the advantage that, by making the third layer 363 include zirconium oxide, when forming the piezoelectric body 443, it is easy to obtain a piezoelectric body 443 that is (100) oriented with a high orientation rate.
[0067] In addition, zirconium in the third layer 363 may exist in the form of a single substance, a nitride, or a nitride oxide, in addition to being present in the form of an oxide. Furthermore, the impurities in the third layer 363 may be elements that are inevitably mixed when the third layer 363 is formed, or may be elements that are intentionally mixed in the third layer 363. For example, the impurities are impurities contained in a zirconium target used when the third layer 363 is formed by a sputtering method.
[0068] The thickness T3 of the third layer 363 is determined by the thickness T and the width W of the vibration plate 36 and is not particularly limited, but is, for example, within a range of 100 nm to 2000 nm.
[0069] The second layer 362 is interposed between the first layer 361 and the third layer 363. Therefore, it is possible to prevent the first layer 361 and the third layer 363 from contacting each other. Therefore, compared with a structure in which the first layer 361 and the third layer 363 are in contact, it is possible to reduce the reduction of silicon oxide in the first layer 361 by zirconium in the third layer 363.
[0070] The second layer 362 is a layer containing a metal element that is less easily oxidized than zirconium as a constituent element. More specifically, the second layer 362 is composed of, for example, an oxide of the metal element. As described later, the metal element is aluminum, titanium, and chromium, but other examples include manganese, vanadium, tungsten, iron, and copper.
[0071] Thus, the second layer 362 contains a metal element that is more difficult to be oxidized than zirconium. In other words, the second layer 362 contains a metal element having a larger oxide formation free energy than zirconium. Preferably, the second layer 362 contains any one of chromium, titanium and aluminum as a constituent element. In addition, the magnitude relationship of the oxide formation free energy can be evaluated based on the well-known Ellingham diagram, for example.
[0072] The metal element contained in the second layer 362 is more difficult to be oxidized than zirconium. In other words, the oxide formation free energy of the metal element contained in the second layer is greater than the oxide formation free energy of zirconium. Therefore, compared with a structure in which the metal element contained in the second layer 362 is more easily oxidized than zirconium, that is, compared with a structure in which the oxide formation free energy of the metal element contained in the second layer is less than the oxide formation free energy of zirconium, the reduction of silicon oxide contained in the first layer 361 can be reduced. Therefore, since the diffusion of silicon monomer generated by the reduction from the first layer 361 to the second layer 362 is reduced, the gap generated by the diffusion between the first layer 361 and the third layer 363 can be reduced. As a result, the adhesion between the first layer 361 and the third layer 363 can be improved compared with a structure in which the second layer 362 is not used.
[0073] Chromium is more difficult to be oxidized than silicon. In other words, the free energy of oxide formation of chromium is greater than the free energy of oxide formation of silicon. Therefore, when chromium is included as a metal element in the second layer 362, the reduction of silicon oxide included in the first layer 361 can be reduced compared to the case where the second layer 362 does not include a metal element that is more difficult to be oxidized than silicon.
[0074] In addition, the oxides of titanium or aluminum are easily moved by heat. Therefore, when titanium or aluminum is included as a metal element in the second layer 362, the interlayer adhesion between the first layer 361 and the third layer 363 and the second layer 362 can be improved through the anchoring effect or chemical bonding formed by the oxides of the metal elements.
[0075] Moreover, titanium easily forms oxides with silicon or zirconium. Therefore, when titanium is contained as a metal element in the second layer 362, the adhesion between the first layer 361 and the second layer 362 can be improved by forming an oxide with titanium and silicon, or the adhesion between the second layer 362 and the third layer 363 can be improved by forming an oxide with titanium and zirconium.
[0076] In addition, when the second layer 362 contains chromium, for example, chromium forms an oxide and contains chromium oxide. Such a second layer 362 is obtained by forming a chromium monomer layer by sputtering or the like and then thermally oxidizing the layer. Therefore, when forming the second layer 362, the second layer 362 of a desired thickness can be easily obtained.
[0077] Here, the chromium oxide included in the second layer 362 may be in any state of polycrystalline, amorphous, or single crystal. However, when the chromium oxide included in the second layer 362 has an amorphous structure in an amorphous state, the compressive stress generated in the second layer 362 can be reduced compared to the case where the chromium oxide included in the second layer 362 is in a polycrystalline or single crystal state. As a result, the strain generated at the interface between the first layer 361 or the third layer 363 and the second layer 362 can be reduced.
[0078] In addition, when the second layer 362 includes titanium, for example, titanium forms an oxide, thereby including titanium oxide. Such a second layer 362 is obtained by forming a titanium monomer layer by sputtering or the like, and then thermally oxidizing the layer. Therefore, when the second layer 362 is formed, the second layer 362 of a desired thickness can be easily obtained.
[0079] Here, the titanium oxide contained in the second layer 362 may also be in any state of polycrystalline, amorphous or single crystal. However, it is preferred that the titanium oxide contained in the second layer 362 is in a polycrystalline or single crystal state, and it is particularly preferred that it has a rutile structure as a crystal structure. Among the crystal structures that titanium oxide can take, the rutile structure is the most stable, and even if it moves due to heat, it is difficult to change into various forms such as anatase or selenium copper nickel ore. Therefore, by making the titanium oxide contained in the second layer 362 have a rutile structure, the thermal stability of the second layer 362 can be improved compared to the case where the crystal structure of the titanium oxide contained in the second layer 362 is other crystal structures.
[0080] In addition, when the second layer 362 includes aluminum, for example, aluminum forms an oxide and includes aluminum oxide. Such a second layer 362 is obtained by forming an aluminum monomer layer by sputtering or the like and then thermally oxidizing the layer. Therefore, when the second layer 362 is formed, the second layer 362 of a desired thickness can be easily obtained.
[0081] Here, the aluminum oxide included in the second layer 362 may be in any state of polycrystalline, amorphous, or single crystal, and when in the polycrystalline or single crystal state, the aluminum oxide has a trigonal structure as a crystal structure.
[0082] In addition, in the second layer 362, in addition to the above-mentioned metal elements, a small amount of titanium (Ti), silicon (Si), iron (Fe), chromium (Cr) or hafnium (Hf) and other elements may be included as impurities. For example, the impurity is an element included in the first layer 361 or the third layer 363. The impurity exists in the second layer 362 together with the metal element in the form of an oxide. Such impurities bring about the following effects, namely, reducing the diffusion of silicon from the first layer 361 to the second layer 362, or, even if silicon diffuses from the first layer 361 to the second layer 362, reducing the diffusion of the silicon to the third layer 363.
[0083] From this point of view, it is preferable that the second layer 362 and the third layer 363 each contain a mixed substance. In this case, the second layer 362 and the third layer 363 are softened compared to a case where this is not the case, and the risk of cracks in the vibration plate 36 can be reduced.
[0084] Here, it is preferred that the content of the impurities in the second layer 362 is higher than the content of the impurities in the third layer 363. In other words, it is preferred that the concentration peak of the impurities in the thickness direction of the laminate composed of the second layer 362 and the third layer 363 is located in the second layer 362. In this case, it is possible to prevent or reduce the formation of gaps at the interface between the second layer 362 and the third layer 363 or in the third layer 363. In contrast, when the concentration peak is located in the third layer 363, the crystal structure in the third layer 363 is deformed by the impurities. Therefore, a gap is generated at the interface between the second layer 362 and the third layer 363 or in the third layer 363, and as a result, the risk of cracks in the vibration plate 36 is sometimes increased.
[0085] The metal elements in the second layer 362 may exist in the form of an oxide, a monomer, a nitride, or a nitride oxide, etc. In addition, the impurities in the second layer 362 may be elements that are inevitably mixed when the second layer 362 is formed, or may be elements that are intentionally mixed into the second layer 362.
[0086] The thickness T2 of the second layer 362 is determined by the thickness T and width W of the vibration plate 36 and is not particularly limited, but is preferably thinner than the thickness T1 of the first layer 361 and the thickness T3 of the third layer 363. In this case, there is an advantage that the characteristics of the vibration plate 36 can be easily optimized.
[0087] The specific thickness T2 of the second layer 362 is preferably within the range of 20 nm to 50 nm, and more preferably within the range of 25 nm to 40 nm, when the metal element contained in the second layer 362 is titanium. In addition, when the metal element contained in the second layer 362 is aluminum, it is preferably within the range of 20 nm to 50 nm, and more preferably within the range of 20 nm to 35 nm. In addition, when the metal element contained in the second layer 362 is chromium, it is preferably within the range of 1 nm to 50 nm, and more preferably within the range of 2 nm to 30 nm. It can be seen from this that when the metal element contained in the second layer 362 is any one of titanium, aluminum, and chromium, as long as the thickness T2 of the second layer 362 is within the range of 20 nm to 50 nm, the preferred condition is met. By making the thickness T2 within such a range, the effect of improving the adhesion between the first layer 361 and the third layer 363 through the second layer 362 can be appropriately exerted.
[0088] On the other hand, when the thickness T2 is too thin, the effect of reducing the diffusion of silicon monomers from the first layer 361 by the second layer 362 tends to decrease depending on the type of metal element contained in the second layer 362. For example, when the second layer 362 is made of titanium oxide, when the thickness T2 is too thin, silicon monomers diffused from the first layer 361 to the second layer 362 may reach the third layer 363 due to the conditions of the heat treatment during manufacturing. On the other hand, when the thickness T2 is too thick, the heat treatment during manufacturing of the second layer 362 may not be sufficiently performed, or the thermal oxidation may take a long time, resulting in adverse effects on other layers.
[0089] 1-4. Method for manufacturing piezoelectric device
[0090] Figure 6 FIG. 1 is a diagram for explaining a method for manufacturing a piezoelectric device. Figure 6 , the method for manufacturing a piezoelectric device is described by taking the case of manufacturing the above-mentioned liquid ejection head 26 as an example.
[0091] like Figure 6 As shown, the method for manufacturing the liquid ejection head 26 includes a substrate preparation step S10, a vibration plate forming step S20, a piezoelectric element forming step S30, and a pressure chamber forming step S40. Here, the vibration plate forming step S20 includes a first layer forming step S21, a second layer forming step S22, and a third layer forming step S23. Hereinafter, each step will be described in sequence.
[0092] The substrate preparation step S10 is a step of preparing a substrate to be the pressure chamber substrate 34. This substrate is, for example, a single crystal silicon substrate.
[0093] The vibration plate forming step S20 is a step of forming the vibration plate 36 and is performed after the substrate preparing step S10. In the vibration plate forming step S20, the first layer forming step S21, the second layer forming step S22, and the third layer forming step S23 are performed in sequence.
[0094] The first layer forming step S21 is a step of forming the first layer 361. In the first layer forming step S21, for example, one surface of the single crystal silicon substrate prepared in the substrate preparing step S10 is thermally oxidized to form a silicon oxide (SiO 2 ) constitutes the first layer 361.
[0095] The second layer forming step S22 is a step of forming the second layer 362. In the second layer forming step S22, for example, a layer of chromium, titanium or aluminum is formed on the first layer 361 by sputtering, and the layer is thermally oxidized, thereby forming the second layer 362 composed of chromium oxide, titanium oxide or aluminum oxide. In addition, the formation of the second layer 362 is not limited to the method using thermal oxidation, for example, CVD (Chemical Vapor Deposition) or atomic layer deposition (ALD) can also be used. In addition, the thermal oxidation in the second layer forming step S22 can also be performed together with the thermal oxidation in the third layer forming step S23 described later.
[0096] The third layer forming step S23 is a step of forming the third layer 363. In the third layer forming step S23, for example, a zirconium layer is formed on the second layer 362 by sputtering and the layer is thermally oxidized to form the third layer 363 made of zirconium oxide.
[0097] The piezoelectric element forming step S30 is a step of forming the plurality of piezoelectric elements 44 and is performed after the third layer forming step S23. In the piezoelectric element forming step S30, the first electrode 441, the piezoelectric body 443, and the second electrode 442 are sequentially formed on the third layer 363.
[0098] The first electrode 441 and the second electrode 442 are formed by known film forming techniques such as sputtering and known processing techniques such as photolithography and etching. The piezoelectric body 443 is formed by forming a precursor layer of the piezoelectric body by, for example, a sol-gel method and sintering the precursor layer to crystallize it.
[0099] After the piezoelectric element 44 is formed, one of the two surfaces of the substrate other than the surface on which the piezoelectric element 44 is formed is polished by CMP (chemical mechanical polishing) or the like as necessary to flatten the surface or adjust the thickness of the substrate.
[0100] The pressure chamber forming step S40 is a step of forming the pressure chamber C, and is performed after the piezoelectric element forming step S30. In the pressure chamber forming step S40, for example, the hole 341 constituting the pressure chamber C is formed by anisotropically etching the surface of the single crystal silicon substrate after the piezoelectric element 44 is formed, which is different from the surface on which the piezoelectric element 44 is formed. As a result of forming the hole 341, the pressure chamber substrate 34 can be obtained. At this time, as an etching liquid for the anisotropic etching, for example, a potassium hydroxide aqueous solution (KOH) or the like can be used. In addition, at this time, the first layer 361 functions as a stop layer for stopping the anisotropic etching.
[0101] After the pressure chamber forming step S40 , by appropriately performing a step of bonding the flow path substrate 32 and the like to the pressure chamber substrate 34 using an adhesive, the liquid ejection head 26 can be obtained.
[0102] 2. Second Implementation
[0103] In the following, the second embodiment of the present invention will be described. In the following exemplary embodiment, the same elements as those in the first embodiment are assigned the same reference numerals as those in the first embodiment, and detailed descriptions thereof will be omitted as appropriate.
[0104] Figure 7 2 is a cross-sectional view of a liquid ejection head 26A according to the second embodiment. The liquid ejection head 26A is the same as the liquid ejection head 26 according to the first embodiment except that the vibrating plate 36 is replaced with a vibrating plate 36A. The vibrating plate 36A is the same as the vibrating plate 36 except that the second layer 362 is replaced with a second layer 362A. Figure 7 In the figure, for the sake of convenience, the interface between the layers constituting the vibration plate 36B is clearly shown, but the interface may be unclear, and for example, the constituent materials of the two layers may be mixed and exist near the interface between the two adjacent layers.
[0105] The second layer 362A includes a layer 362a and a layer 362b which are stacked in this order in the Z1 direction. The layer 362a and the layer 362b are each a layer containing a metal element that is less susceptible to oxidation than zirconium, and are composed of, for example, an oxide containing the metal element.
[0106] The compositions of the materials constituting the layer 362a and the layer 362b are different from each other. Specifically, the types or contents of the impurities in the layer 362a and the layer 362b are different from each other. As in the first embodiment described above, the impurities are elements such as titanium (Ti), silicon (Si), iron (Fe), chromium (Cr) or hafnium (Hf). Such layers 362a and 362b are formed by, for example, forming a layer composed of a monomer of the metal element by sputtering, and adjusting the time or temperature of the heat treatment so that the distribution of the impurities in the thickness direction of the layer is different. In addition, the formation of these layers is not particularly limited, and for example, it can also be carried out by forming each layer independently by using a CVD (chemical vapor deposition) method.
[0107] When silicon is included as an impurity in the layer 362a, the layer 362b can be regarded as the "second layer", and in this case, the layer 362a can be regarded as the "fourth layer". That is, the layer 362a is arranged between the first layer 361 and the layer 362b, and contains the metal element and silicon contained in the layer 362b. In this way, by including silicon in the layer 362a, the diffusion of silicon from the first layer 361 to the second layer 362A can be reduced, or even when silicon diffuses from the first layer 361 to the second layer 362A, the diffusion of the silicon to the third layer 363 can be reduced. In addition, there is an effect that a gap is not easily generated at the interface between the first layer 361 and the second layer 362A.
[0108] Here, although the layer 362b may also contain silicon, it is preferable that the content of silicon in the layer 362a is higher than the content of silicon in the layer 362b. In other words, it is preferable that the content of silicon in the layer 362b is lower than the content of silicon in the layer 362a. By setting the relationship between the content of silicon in the layer 362a and the layer 362b to be such, for example, when the second layer 362A contains titanium oxide, the crystal strain caused by silicon in the titanium oxide in the second layer 362A can be reduced. In addition, by reducing the content of silicon in the layer 362b, the adhesion between the layer 362b and the third layer 363 can be improved.
[0109] In addition, when zirconium is included as an impurity in the layer 362b, the layer 362a can be regarded as the "second layer", and in this case, the layer 362b can be regarded as the "fifth layer". That is, the layer 362b is arranged between the layer 362a and the third layer 363, and contains the metal element and zirconium contained in the layer 362a. In this way, by including zirconium in the layer 362b, the diffusion of zirconium from the third layer 363 to the second layer 362A can be reduced, or even when zirconium diffuses from the third layer 363 to the second layer 362A, the diffusion of the zirconium to the first layer 361 can be reduced. In addition, there is also an effect that a gap is not easily generated at the interface between the third layer 363 and the second layer 362A.
[0110] According to the second embodiment, as in the first embodiment, the occurrence of damage such as interlayer separation or cracks in the diaphragm can be reduced.
[0111] 3. Third Implementation
[0112] In the following exemplary embodiment, the elements having the same action or function as those in the first embodiment are assigned the same reference numerals as those in the first embodiment, and detailed descriptions thereof are appropriately omitted.
[0113] Figure 8 2 is a cross-sectional view of a liquid ejection head 26B according to the third embodiment. The liquid ejection head 26B is the same as the liquid ejection head 26 according to the first embodiment except that the vibrating plate 36 is replaced with a vibrating plate 36B. The vibrating plate 36B is the same as the vibrating plate 36 except that the second layer 362 is replaced with a second layer 362B. Figure 8 In the figure, for the sake of convenience, the interface between the layers constituting the vibration plate 36B is clearly shown, but the interface may be unclear, and for example, the constituent materials of the two layers may be mixed and exist near the interface between the two adjacent layers.
[0114] The second layer 362B includes a layer 362a, a layer 362b, and a layer 362c, which are stacked in this order in the Z1 direction. The layers 362a, 362b, and 362c are each a layer containing a metal element that is less easily oxidized than zirconium, and are composed of, for example, an oxide containing the metal element.
[0115] The compositions of the materials constituting the layer 362a, the layer 362b, and the layer 362c are different from each other. Specifically, the types or contents of the impurities in the layer 362a, the layer 362b, and the layer 362c are different from each other. As in the first embodiment described above, the impurities are elements such as titanium (Ti), silicon (Si), iron (Fe), chromium (Cr), or hafnium (Hf). The formation of the layer 362a, the layer 362b, and the layer 362c is performed by, for example, forming a layer composed of a monomer of the metal element by sputtering, and adjusting the time or temperature of the heat treatment so that the distribution of the impurities in the thickness direction of the layer is different. In addition, the formation of these layers is not particularly limited, and for example, it can also be performed by forming each layer independently by using a CVD (chemical vapor deposition) method.
[0116] As in the second embodiment described above, when silicon is contained as a mixed substance in the layer 362a, the layer 362b can be regarded as a "second layer", and in this case, the layer 362a can be regarded as a "fourth layer".
[0117] In addition, when zirconium is included as an impurity in the layer 362c, the layer 362b can be regarded as the "second layer", and in this case, the layer 362c can be regarded as the "fifth layer". That is, the layer 362c is arranged between the layer 362b and the third layer 363, and contains the metal element and zirconium contained in the layer 362b. In this way, by including zirconium in the layer 362c, the diffusion of zirconium from the third layer 363 to the second layer 362B can be reduced, or even when zirconium diffuses from the third layer 363 to the second layer 362B, the diffusion of the zirconium to the first layer 361 can be reduced. In addition, there is an effect that a gap is not easily generated at the interface between the third layer 363 and the second layer 362B.
[0118] According to the third embodiment, as in the first embodiment, the occurrence of damage such as interlayer separation or cracks in the diaphragm can be reduced.
[0119] 4. Modifications
[0120] The various methods in the above examples can be modified in many ways. The specific modified methods that can be applied to the above various methods are illustrated below. In addition, two or more methods that can be arbitrarily selected from the following examples can be appropriately combined within the scope of not contradicting each other.
[0121] 4-1. Modification 1
[0122] The liquid ejection head only needs to have a structure having a piezoelectric body and a vibration plate, and is not limited to the structure of the above-mentioned embodiment. In addition, although the liquid ejection head is described as an example of a piezoelectric device in the above-mentioned embodiment, it is not limited to this. In addition to the liquid ejection head, the piezoelectric device may be, for example, a driving device such as a piezoelectric actuator having a piezoelectric body and a vibration plate, or a detection device such as a pressure sensor having a piezoelectric body and a vibration plate.
[0123] 4-2. Modification 2
[0124] In each of the above-mentioned embodiments, the liquid ejection head 26, the liquid ejection head 26A, or the liquid ejection head 26B has a plurality of piezoelectric elements 44 including a piezoelectric body 443. Here, the plurality of piezoelectric elements 44 have a plurality of first electrodes 441 independently provided for the plurality of piezoelectric elements, and a second electrode 442 provided in common for the plurality of piezoelectric elements 44. The plurality of first electrodes 441 are arranged between the piezoelectric body 443 and the vibration plate 36.
[0125] Thus, although the above-mentioned embodiments illustrate a structure in which the first electrode 441 is an independent electrode and the second electrode 442 is a common electrode, the first electrode 441 may be a common electrode that is continuous across a plurality of piezoelectric elements 44, and the second electrode 442 may be an independent electrode that is independent for each piezoelectric element 44. In addition, both the first electrode 441 and the second electrode 442 may be independent electrodes.
[0126] 4-3. Modification 3
[0127] Although the above-mentioned embodiments illustrate a serial type liquid ejecting device 100 in which the transport body 242 carrying the liquid ejecting head 26 reciprocates, the present invention can also be applied to a line type liquid ejecting device in which a plurality of nozzles N are distributed across the entire width of the medium 12 .
[0128] 4-4. Modification 4
[0129] The liquid ejection device 100 illustrated in each of the above-mentioned modes can be used in various devices such as fax machines and copiers in addition to devices dedicated to printing. Originally, the use of the liquid ejection device of the present invention is not limited to printing. For example, a liquid ejection device that ejects a solution of a color material is used as a manufacturing device for forming a color filter of a liquid crystal display device. In addition, a liquid ejection device that ejects a solution of a conductive material is used as a manufacturing device for forming wiring and electrodes of a wiring substrate.
[0130] Example
[0131] Hereinafter, specific examples of the present invention will be described. In addition, the present invention is not limited to the following examples.
[0132] A. Manufacturing of a vibration plate using titanium oxide in the second layer
[0133] A-1. Example A1
[0134] First, a first layer having a thickness of 1460 nm and made of silicon oxide was formed by thermally oxidizing one surface of a single crystal silicon substrate having a surface orientation of (110).
[0135] Then, a film composed of titanium was deposited on the first layer by sputtering, and the film was thermally oxidized at 650° C., thereby forming a second layer having a thickness of 10 nm and mainly composed of titanium oxide.
[0136] Next, a film made of zirconium was deposited on the second layer by sputtering, and the film was thermally oxidized at 900° C., thereby forming a third layer made of zirconium oxide with a thickness of 400 nm.
[0137] Then, a potassium hydroxide aqueous solution (KOH) or the like is used as an etching solution to anisotropically etch the other surface of the single crystal silicon substrate, thereby forming a recessed portion having the first layer as the bottom surface.
[0138] Through the above steps, a vibration plate consisting of the first layer, the second layer, and the third layer is manufactured.
[0139] A-2. Example A2
[0140] A vibration plate was manufactured in the same manner as in Example A1 described above except that the thickness of the titanium film was changed to 15 nm.
[0141] A-3. Example A3
[0142] A vibration plate was manufactured in the same manner as in Example A1 described above except that the thickness of the film made of titanium was changed to 20 nm.
[0143] A-4. Example A4
[0144] A vibration plate was manufactured in the same manner as in Example A1 described above except that the thickness of the film made of titanium was changed to 25 nm.
[0145] A-5. Example A5
[0146] A vibration plate was manufactured in the same manner as in Example A1 described above except that the thickness of the titanium film was changed to 30 nm.
[0147] A-6. Example A6
[0148] A vibration plate was manufactured in the same manner as in Example A1 described above except that the thickness of the film made of titanium was changed to 35 nm.
[0149] A-7. Example A7
[0150] A vibration plate was manufactured in the same manner as in Example A1 described above except that the thickness of the film made of titanium was changed to 40 nm.
[0151] A-8. Example A8
[0152] A vibration plate was manufactured in the same manner as in Example A1 described above except that the thickness of the film made of titanium was changed to 50 nm.
[0153] A-9. Example A9
[0154] A vibration plate was manufactured in the same manner as in Example A1 described above except that the thickness of the titanium film was changed to 60 nm.
[0155] B. Manufacturing of a vibration plate using alumina in the second layer
[0156] B-1. Example B1
[0157] A vibration plate was manufactured in the same manner as in Example A1 except that the second layer mainly composed of aluminum oxide and having a thickness of 20 nm was formed. Here, the atomic layer deposition method was used to form the second layer.
[0158] B-2. Example B2
[0159] A vibration plate was manufactured in the same manner as in Example B1 except that the thickness of the second layer was set to 30 nm.
[0160] B-3. Example B3
[0161] A vibration plate was manufactured in the same manner as in Example B1 except that the thickness of the second layer was set to 35 nm.
[0162] B-4. Example B4
[0163] A vibration plate was manufactured in the same manner as in Example B1 except that the thickness of the second layer was set to 40 nm.
[0164] B-5. Example B5
[0165] A vibration plate was manufactured in the same manner as in Example B1 except that the thickness of the second layer was set to 45 nm.
[0166] B-6. Example B6
[0167] A vibration plate was manufactured in the same manner as in Example B1 except that the thickness of the second layer was set to 50 nm.
[0168] C. Manufacturing of a vibration plate using chromium oxide in the second layer
[0169] C-1. Example C1
[0170] A vibration plate was manufactured in the same manner as in Example A1 above, except that a second layer mainly composed of chromium oxide was formed with a thickness of 1 nm and the thickness of the third layer was set to 600 nm. Here, the second layer was formed by forming a film composed of chromium on the first layer by sputtering and thermally oxidizing the film at 650°C.
[0171] C-2. Example C2
[0172] A vibration plate was manufactured in the same manner as in Example C1 except that the thickness of the second layer was set to 2 nm.
[0173] C-3. Example C3
[0174] A vibration plate was manufactured in the same manner as in Example C1 except that the thickness of the second layer was set to 5 nm.
[0175] C-4. Example C4
[0176] A vibration plate was manufactured in the same manner as in Example C1 except that the thickness of the second layer was set to 15 nm.
[0177] C-5. Example C5
[0178] A vibration plate was manufactured in the same manner as in Example C1 except that the thickness of the second layer was set to 30 nm.
[0179] C-6. Example C6
[0180] A vibration plate was manufactured in the same manner as in Example C1 except that the thickness of the second layer was set to 50 nm.
[0181] D. Manufacturing of vibration plates without using the second layer
[0182] D-1. Comparative Example
[0183] A vibration plate was manufactured in the same manner as in the above-described Example A1 except that the formation of the second layer was omitted.
[0184] E. Evaluation
[0185] E-1. Impurity peak position, second layer structure, and Si diffusion
[0186] The vibration plates of each embodiment and comparative example were analyzed by SIMS (Secondary Ion Mass Spectrometry). A representative portion of the analysis results is shown in FIG. Figures 9 to 12 middle. Fig. 9 This is a diagram showing the analysis results of the vibration plate in Example A7 by SIMS. Fig.10 This is a diagram showing the analysis results of the vibration plate in Example B1 by SIMS. Fig.11 It is a figure which shows the analysis result of the vibration plate in the comparative example by SIMS. Fig.12 : is a graph showing the analysis results of the vibration plates in Example C3, Example C4 and Comparative Example by SIMS. Fig.12 Represents the distribution of silicon.
[0187] The results of this analysis show that in Examples A1-A7 and Examples B1-B6, the peak of the concentration of impurities such as iron (Fe) or chromium (Cr) in the thickness direction of the vibration plate is located in the second layer. It is known that in Examples A8, A9, C1-C6, the peak of the impurity concentration is located in the third layer. It is known that in the comparative example, the peak of the impurity concentration is located at the interface between the first layer and the third layer. These results are shown in Table 1.
[0188] Table 1
[0189]
[0190] In addition, it can be seen that in Examples A1-A3 and Examples C1-C4, the impurities diffuse across the entire area of the second layer in the thickness direction, and the second layer is composed of a single layer. It can be seen that in Examples B1-B6, Example C5 and Example C6, the impurities diffuse only to a portion of the third layer side in the second layer, and the second layer is composed of two layers such as a layer where the impurities diffuse and a layer where they are not diffused. It can be seen that in Examples A4-A9, the impurities diffuse to a portion of the third layer side in the second layer, and silicon diffuses to a portion of the first layer side in the layer where the impurities in the second layer are not diffused, and the second layer is composed of three layers. These results are also shown in Table 1.
[0191] In addition, the presence or absence of diffusion of silicon into the third layer was evaluated based on the following criteria. Table 1 shows the evaluation results.
[0192] A: There is no diffusion into the third layer of silicon.
[0193] B: Some diffusion of silicon into the third layer is observed.
[0194] C: Remarkable diffusion of silicon into the third layer is observed.
[0195] E-2. Moisture intrusion
[0196] For each example and each comparative example, the vibration plate was cut into small pieces, exposed to a heavy water atmosphere at a temperature of 45° C. and a humidity of 95% for 24 hours, and then analyzed by SIMS. The results of the analysis were evaluated based on the following criteria. The evaluation results are shown in Table 1.
[0197] A: There is no intrusion of moisture between the first layer and the third layer.
[0198] B: Some intrusion of moisture into between the first layer and the third layer was observed.
[0199] C: Significant intrusion of moisture into between the first layer and the third layer was observed.
[0200] E-3. Adhesion
[0201] As described below, the adhesion between the first layer and the third layer was evaluated for each of Examples C1 to C6 and Comparative Example.
[0202] First, the vibration plate is cut into small pieces, and dilute hydrofluoric acid (water: hydrofluoric acid = 50:1) is used as an etching solution. After the small pieces are immersed in the etching solution for 60 minutes, the width of the part that has changed color due to etching from the end face of the small piece is measured ten times, and the average etching amount is calculated.
[0203] As a result, in Example C1, the etching amount was 310 μm. In Example C2, the etching amount was 288 μm. In Example C3, the etching amount was 170 μm. In Example C4, the etching amount was 11 μm. In Examples C5 and C6, the etching amounts were each less than 10 μm. In the comparative example, the etching amount was 346 μm.
[0204] Based on the above results, the adhesion was evaluated according to the following criteria. The results are shown in Table 1.
[0205] A: The amount of etching is very small and the adhesion is good.
[0206] B: Although the etching amount is slightly large, improvement in adhesion is observed.
[0207] C: The etching amount is very large and the adhesion is poor.
[0208] E-4. Others
[0209] For each embodiment and comparative example, the cross section of the vibration plate was observed by STEM (scanning transmission electron microscope). The result was that in each embodiment, no gap was generated between the first layer and the third layer. In contrast, in the comparative example, a gap was generated between the first layer and the third layer. However, in embodiment A9, a gap was generated in the third layer. This is because Fe and Cr caused strain in the crystal structure of zirconium oxide in the third layer.
[0210] E-5. Comprehensive evaluation
[0211] Based on the above evaluation results, a comprehensive evaluation was performed. The results are shown in Table 1. In Table 1, A, B, C, and D, which represent the results of the comprehensive evaluation, are ranked in order of A, with A being the best. As described above, it can be seen that each embodiment can reduce the diffusion of silicon into the third layer compared to the comparative example and exhibits excellent durability.
[0212] Explanation of symbols
[0213] 20…control unit (control unit); 26…liquid ejection head; 26A…liquid ejection head; 26B…liquid ejection head; 34…pressure chamber substrate; 36…vibration plate; 36A…vibration plate; 36B…vibration plate; 44…piezoelectric element; 100…liquid ejection device; 361…first layer; 362…second layer; 362A…second layer; 362B…second layer; 362a…layer (fourth layer); 362b…layer (second layer); 362c…layer (fifth layer); 363…third layer; 441…first electrode; 442…second electrode; 443…piezoelectric body; T1…thickness; T2…thickness; T3…thickness.
Claims
1. A liquid ejection head, characterized in that: have: Piezoelectric body; a vibration plate that is vibrated by being driven by the piezoelectric body; a pressure chamber substrate provided with a pressure chamber for applying pressure to the liquid by the vibration of the vibration plate, The pressure chamber substrate, the vibration plate, and the piezoelectric body are laminated in this order. The vibration plate has: a first layer containing silicon as a constituent element; a second layer disposed between the first layer and the piezoelectric body and containing, as a constituent element, a metal element that is less susceptible to oxidation than zirconium; The third layer is disposed between the second layer and the piezoelectric body and contains zirconium as a constituent element.
2. The liquid ejection head according to claim 1, wherein: The metal element included in the second layer is more difficult to be oxidized than silicon.
3. A liquid ejection head, characterized in that: have: Piezoelectric body; a vibration plate that is vibrated by being driven by the piezoelectric body; a pressure chamber substrate provided with a pressure chamber for applying pressure to the liquid by the vibration of the vibration plate, The pressure chamber substrate, the vibration plate, and the piezoelectric body are laminated in this order. The vibration plate has: a first layer containing silicon as a constituent element; a second layer disposed between the first layer and the piezoelectric body and containing, as a constituent element, a metal element having a larger oxide formation free energy than zirconium; The third layer is disposed between the second layer and the piezoelectric body and contains zirconium as a constituent element.
4. The liquid ejection head according to claim 3, wherein: The oxide formation free energy of the metal element contained in the second layer is greater than the oxide formation free energy of silicon.
5. The liquid ejection head according to claim 1 or 3, characterized in that: The second layer includes chromium oxide.
6. The liquid ejection head according to claim 5, wherein: The chromium oxide contained in the second layer has an amorphous structure.
7. The liquid ejection head according to claim 1 or 3, wherein: The second layer includes titanium oxide.
8. The liquid ejection head according to claim 7, wherein: The titanium oxide contained in the second layer has a rutile structure.
9. The liquid ejection head according to claim 1 or 3, characterized in that: The second layer includes aluminum oxide.
10. The liquid ejection head according to claim 9, wherein: Aluminum oxide included in the second layer has an amorphous structure or a trigonal structure.
11. The liquid ejection head according to claim 1 or 3, wherein: The second layer is thinner than the first layer and the third layer.
12. The liquid ejection head according to claim 1 or 3, wherein: The vibration plate further includes a fourth layer that is disposed between the first layer and the second layer and includes the metal element included in the second layer and silicon as constituent elements.
13. The liquid ejection head according to claim 12, wherein: The second layer further contains silicon as a constituent element, The silicon content in the fourth layer is higher than the silicon content in the second layer.
14. The liquid ejection head according to claim 1 or 3, wherein: The vibration plate further includes a fifth layer that is disposed between the second layer and the third layer and includes the metal element included in the second layer and zirconium as constituent elements.
15. The liquid ejection head according to claim 1 or 3, wherein: The second layer and the third layer each contain a mixture.
16. The liquid ejection head according to claim 15, wherein: The content rate of the impurity in the second layer is higher than the content rate of the impurity in the third layer.
17. A liquid ejection head, characterized in that: have: Piezoelectric body; a vibration plate that is vibrated by being driven by the piezoelectric body; a pressure chamber substrate provided with a pressure chamber for applying pressure to the liquid by the vibration of the vibration plate, The pressure chamber substrate, the vibration plate, and the piezoelectric body are laminated in this order. The vibration plate has: a first layer containing silicon as a constituent element; a second layer disposed between the first layer and the piezoelectric body and containing any one of chromium, titanium and aluminum as a constituent element; a third layer disposed between the second layer and the piezoelectric body and containing zirconium as a constituent element, The second layer comprises titanium oxide, The titanium oxide contained in the second layer has a rutile structure.
18. A liquid ejection head, characterized in that: have: Piezoelectric body; a vibration plate that is vibrated by being driven by the piezoelectric body; a pressure chamber substrate provided with a pressure chamber for applying pressure to the liquid by the vibration of the vibration plate, The pressure chamber substrate, the vibration plate, and the piezoelectric body are laminated in this order. The vibration plate has: a first layer containing silicon as a constituent element; a second layer disposed between the first layer and the piezoelectric body and containing any one of chromium, titanium and aluminum as a constituent element; a third layer disposed between the second layer and the piezoelectric body and containing zirconium as a constituent element, The second layer is thinner than the first layer and the third layer.
19. A liquid ejection head, characterized in that: have: Piezoelectric body; a vibration plate that is vibrated by being driven by the piezoelectric body; a pressure chamber substrate provided with a pressure chamber for applying pressure to the liquid by the vibration of the vibration plate, The pressure chamber substrate, the vibration plate, and the piezoelectric body are laminated in this order. The vibration plate has: a first layer containing silicon as a constituent element; a second layer disposed between the first layer and the piezoelectric body and containing any one of chromium, titanium and aluminum as a constituent element; a third layer disposed between the second layer and the piezoelectric body and containing zirconium as a constituent element, The vibration plate further includes a fourth layer that is disposed between the first layer and the second layer and includes the metal element included in the second layer and silicon as constituent elements.
20. A liquid ejection head, characterized in that: have: Piezoelectric body; a vibration plate that is vibrated by being driven by the piezoelectric body; a pressure chamber substrate provided with a pressure chamber for applying pressure to the liquid by the vibration of the vibration plate, The pressure chamber substrate, the vibration plate, and the piezoelectric body are laminated in this order. The vibration plate has: a first layer containing silicon as a constituent element; a second layer disposed between the first layer and the piezoelectric body and containing any one of chromium, titanium and aluminum as a constituent element; a third layer disposed between the second layer and the piezoelectric body and containing zirconium as a constituent element, The vibration plate further includes a fifth layer that is disposed between the second layer and the third layer and includes the metal element included in the second layer and zirconium as constituent elements.
21. A liquid ejection head, characterized in that: have: Piezoelectric body; a vibration plate that is vibrated by being driven by the piezoelectric body; a pressure chamber substrate provided with a pressure chamber for applying pressure to the liquid by the vibration of the vibration plate, The pressure chamber substrate, the vibration plate, and the piezoelectric body are laminated in this order. The vibration plate has: a first layer containing silicon as a constituent element; a second layer disposed between the first layer and the piezoelectric body and containing any one of chromium, titanium and aluminum as a constituent element; a third layer disposed between the second layer and the piezoelectric body and containing zirconium as a constituent element, The second layer and the third layer each contain a mixture.
22. The liquid ejection head according to any one of claims 1, 3, 17 to 21, characterized in that: The first layer comprises silicon oxide, The third layer includes zirconium oxide.
23. The liquid ejection head according to any one of claims 1, 3, 17 to 21, characterized in that: The thickness of the second layer is in the range of 20 nm to 50 nm.
24. The liquid ejection head according to any one of claims 1, 3, 17 to 21, characterized in that: It also has a plurality of piezoelectric elements including the piezoelectric body, The plurality of piezoelectric elements include a plurality of first electrodes independently provided for the plurality of piezoelectric elements and a second electrode commonly provided for the plurality of piezoelectric elements. The plurality of first electrodes are arranged between the piezoelectric body and the vibration plate.
25. The liquid ejection head according to any one of claims 1, 3, 17 to 21, characterized in that: It also has a plurality of piezoelectric elements including the piezoelectric body, The plurality of piezoelectric elements include a first electrode provided in common with respect to the plurality of piezoelectric elements and a plurality of second electrodes provided independently with respect to the plurality of piezoelectric elements. The first electrode is arranged between the piezoelectric body and the vibration plate.
26. A liquid ejection device, characterized in that: have: The liquid ejection head according to any one of claims 1 to 25; A control unit controls the driving of the piezoelectric body.
Citation Information
Patent Citations
Liquid spray head manufacturing method, liquid spray head, and printing equipment
CN104772988A
Piezoelectric device, liquid discharging head, and liquid discharging apparatus
CN108933191A
Liquid discharge head, liquid discharge apparatus, piezoelectric device, and ultrasonic sensor
CN109484029A
Liquid ejecting head, liquid ejecting apparatus, and piezoelectric device
CN109514998A
Ink-jet printer head and printer equipment
CN1258600A