Carbonaceous material and method for producing the same, water purification filter and water purifier

By optimizing the amount of benzene adsorption, vitamin B12 adsorption and mesoporous volume in carbonaceous materials, and using a fluidized bed furnace manufacturing method, combined with the introduction of oxygen-containing gas, it is solved that it is difficult to remove trihalomethane and 2- in the prior art in the art. The problem of MIB achieves efficient removal of these two harmful substances and improves the removal ability of the water purifier.

CN113727943BActive Publication Date: 2024-11-19KURARAY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202080030843.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-04-26
Filing Date
2020-04-22
Publication Date
2024-11-19
Estimated Expiration
2040-04-22

AI Technical Summary

Technical Problem

It is difficult to effectively remove two harmful substances in tap water with a single species, such as trihalomethane with small molecular size and 2-MIB with large molecular size, and the removal ability of the water purifier is insufficient.

Method used

Carbonaceous material with a benzene adsorption amount of 25-40%, vitamin B12 adsorption amount of 13.0-50.0 mg/g and a mesoporous volume of 0.070-0.150 cm3/g was used, and the material was manufactured through a fluidized bed furnace, combined with oxygen-containing gas The body is introduced to optimize the structure and achieve efficient adsorption of trihalomethane and 2-MIB.

Benefits of technology

It realizes efficient removal of trihalomethane and 2-MIB using a single species, improves the removal performance of the water purifier and meets the standards of the household goods quality identification method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003316747430000171
    Figure BDA0003316747430000171
  • Figure BDA0003316747430000191
    Figure BDA0003316747430000191
  • Figure HDA0003316747440000011
    Figure HDA0003316747440000011
Patent Text Reader

Abstract

One aspect of the present invention relates to a carbonaceous material having a benzene adsorption capacity of 25 to 40%, a vitamin B12 adsorption capacity of 13.0 to 50.0 mg / g, and a mesopore volume of 0.070 to 0.150 cm-1 obtained by a BJH method based on a nitrogen adsorption isotherm. 3 / g.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a carbonaceous material and also to a method for producing the carbonaceous material, a water purification filter and a water purifier using the carbonaceous material. Background Art

[0002] In recent years, there has been an increasing focus on the safety and hygiene of tap water quality, and there is a desire to remove harmful substances contained in tap water, such as free residual chlorine, VOCs (volatile organic compounds) such as trihalomethanes, pesticides represented by 2-chloro-4,6-diethylamino-1,3,5-triazine (CAT), and moldy odors represented by 2-methylisoborneol (2-MIB).

[0003] The Household Products Quality Labeling Act stipulates 13 substances that must be removed by water purifiers, namely: free residual chlorine, turbidity, chloroform, bromodichloromethane, dibromochloromethane, bromoform, tetrachloroethylene, trichloroethylene, 1,1,1-trichloroethane, total trihalomethanes (THM), CAT, 2-MIB (2-methylisoborneol) and soluble lead.

[0004] Various technologies for removing these removal target substances using carbonaceous materials have been proposed. For example, Patent Document 1 discloses a technology for removing moldy and smelly substances using a combination of granular activated carbon and fibrous activated carbon. Patent Document 2 discloses a technology for removing each removal target substance using a combination of fibrous activated carbon and an inorganic adsorbent. Patent Documents 3 to 5 also propose technologies for removing removal target substances using activated carbon having a specific surface structure.

[0005] Among the substances to be removed, activated carbon can be used to remove all substances except turbidity and soluble lead, but it is difficult to effectively remove VOCs such as trihalomethanes with small molecular sizes and 2-MIB with large molecular sizes using a single species of activated carbon. As the ability to remove harmful substances required of water purifiers increases, activated carbon that can remove both trihalomethanes and 2-MIB with a single species is required.

[0006] An object of the present invention is to provide a carbonaceous material capable of removing both trihalomethanes and 2-MIB with a single species.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Publication No. 8-52347

[0010] Patent Document 2: Japanese Patent Publication No. 2003-334543

[0011] Patent Document 3: Japanese Patent Publication No. 2003-290654

[0012] Patent Document 4: Japanese Patent Publication No. 2013-220413

[0013] Patent Document 5: Japanese Patent Publication No. 2006-282441 Summary of the invention

[0014] The present inventors have conducted intensive studies to solve the above problems. As a result, they have found that the above problems can be solved by a carbonaceous material having the following structure. Based on this finding, the inventors have further conducted studies and have completed the present invention.

[0015] That is, one aspect of the present invention relates to a carbonaceous material having a benzene adsorption capacity of 25 to 40%, a vitamin B12 adsorption capacity of 13.0 to 50.0 mg / g, and a mesopore volume of 0.070 to 0.150 cm-1 obtained from a nitrogen adsorption isotherm by the BJH method. 3 / g.

[0016] In addition, another aspect of the present invention relates to a method for manufacturing carbonaceous materials, which is a method for manufacturing carbonaceous materials using a fluidized bed furnace, wherein, in addition to introducing fluidizing gas from the furnace bed, an oxygen-containing gas is also introduced into the fluidized bed furnace so that the oxygen concentration in the combined gas of the fluidizing gas and the oxygen-containing gas becomes 0.004 to 1% by volume. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a schematic diagram for explaining a method for producing a carbonaceous material using a fluidized bed furnace according to one embodiment of the present invention.

[0018] Figure 2 This is a schematic diagram for explaining a method for producing a carbonaceous material using a fluidized bed furnace according to one embodiment of the present invention. DETAILED DESCRIPTION

[0019] Hereinafter, embodiments of the present invention will be described in detail, but the present invention is not limited to these descriptions.

[0020] [Carbonaceous materials]

[0021] The carbonaceous material according to one embodiment of the present invention has a benzene adsorption capacity of 25-40%, a vitamin B12 adsorption capacity of 13.0-50.0 mg / g, and a mesopore volume of 0.070-0.150 cm-1 obtained from a nitrogen adsorption isotherm by the BJH method. 3 / g.

[0022] According to the above configuration, it is possible to provide a carbonaceous material capable of removing both trihalomethanes and 2-MIB using a single species.

[0023] As described above, among the 13 removal target substances specified in the Household Products Quality Labeling Law, except for turbidity and soluble lead, carbonaceous materials such as activated carbon can be used for removal. However, it is difficult to effectively remove VOCs such as trihalomethanes with small molecular size and 2-MIB with large molecular size using a single species of carbonaceous material. In contrast, the carbonaceous material involved in one embodiment of the present invention having a benzene adsorption amount, a vitamin B12 adsorption amount, and a mesopore volume within the above-mentioned specific range can effectively remove VOCs such as trihalomethanes with small molecular size and 2-MIB with large molecular size using a single species.

[0024] (Benzene adsorption)

[0025] The amount of benzene adsorption is an indicator of the degree of activation of the carbonaceous material. Generally speaking, there is a tendency that carbonaceous materials with well-developed micropores are suitable for adsorbing trihalomethanes with small molecular sizes. The amount of benzene adsorption of the carbonaceous material involved in this embodiment is in the range of 25 to 40%, and has excellent trihalomethane adsorption performance.

[0026] From the perspective of achieving excellent trihalomethane adsorption performance, the benzene adsorption capacity of the carbonaceous material is in the range of 25 to 40%, with the upper limit preferably being less than 39%, less than 38%, less than 37%, less than 36% or less than 35%, and the lower limit being preferably more than 26%, more than 27%, more than 28%, more than 29% or more than 30%.

[0027] The amount of benzene adsorption of the carbonaceous material can be measured by the method described in [Measurement of Benzene Adsorption] described later.

[0028] (Vitamin B12 adsorption)

[0029] Vitamin B12 (cyanocobalamin) has a large molecular weight of about 1355, and the amount of vitamin B12 adsorbed is an indicator of the adsorption characteristics of substances with large molecular sizes. The amount of vitamin B12 adsorbed by the carbonaceous material involved in this embodiment is 13.0 mg / g or more, and exhibits excellent adsorption performance for 2-MIB with large molecular size.

[0030] From the viewpoint of achieving excellent 2-MIB adsorption performance, the vitamin B12 adsorption of the carbonaceous material is 13.0 mg / g or more, preferably 15.0 mg / g or more, more preferably 16.0 mg / g or more, 17.0 mg / g or more, 18.0 mg / g or more, 19.0 mg / g or more or 20.0 mg / g or more. The upper limit of the vitamin B12 adsorption is not particularly limited, but from the viewpoint of the balance of other physical properties such as benzene adsorption, it is usually 50.0 mg / g or less, preferably 48.0 mg / g or less, 46.0 mg / g or less, 45.0 mg / g or less, 44.0 mg / g or less, 43.0 mg / g or less, 42.0 mg / g or less, 41.0 mg / g or less or 40.0 mg / g or less.

[0031] The amount of vitamin B12 adsorbed by the carbonaceous material can be measured by the method described in [Measurement of Vitamin B12 Adsorption Amount] described later.

[0032] (Mesopore volume)

[0033] The pores of carbonaceous materials can be classified into micropores (diameter less than 2 nm), mesopores (diameter 2 to 50 nm) and macropores (diameter greater than 50 nm) according to their diameters (the IUPAC classification standard is indicated in brackets). Mesopores are larger than micropores, and the volume of such mesopores can be mainly used as an indicator of the adsorption characteristics of 2-MIB with large molecular size. The mesopore volume of the carbonaceous material involved in this embodiment is between 0.070 and 0.150 cm a / g range, and has excellent adsorption performance for 2-MIB with large molecular size.

[0034] From the perspective of maintaining the adsorption characteristics of trihalomethanes and achieving excellent 2-MIB adsorption performance, the mesopore volume of carbonaceous materials is between 0.070 and 0.150 cm 3 / g, and the lower limit is preferably 0.072 cm 3 / g or more, 0.074cm3 / g or more, 0.075cm 3 / g or more, 0.076cm a / g or more, 0.077cm 3 / g or more, 0.078cm 3 / g or more, 0.079cm 3 / g or more, 0.080cm 3 / g or more. In addition, the upper limit is preferably 0.148 cm 3 / g or less, 0.146cm 3 / g or less, 0.145cm a / g or less, 0.144cm 3 / g or less, 0.143cm3 / g or less, 0.142cm 3 / g or less, 0.141cm 3 / g or less or 0.140cm 3 / g or less.

[0035] The mesopore volume of the carbonaceous material can be calculated using the BJH (Barrett-Joyner-Halenda) method and based on the nitrogen adsorption isotherm. The determination of the nitrogen adsorption isotherm and the calculation of the mesopore volume can be implemented by the method described in [Determination of nitrogen adsorption isotherm] and [Determination of mesopore pore volume by BJH method] described later.

[0036] The above attempts to explain the technical significance of the benzene adsorption, vitamin B12 adsorption and mesopore volume in the present invention, but the relationship between the structure of the carbonaceous material (adsorption medium) and the adsorption characteristics of the adsorbate is complex, and sometimes the benzene adsorption, vitamin B12 adsorption and mesopore volume are not immediately correlated with the adsorption characteristics of the adsorbate independently. In order to realize a carbonaceous material that can effectively remove trihalomethanes and 2-MIB with a single species, it should be noted that the balance of these benzene adsorption, vitamin B12 adsorption and mesopore volume is important. As described later, in the present embodiment, a carbonaceous material having the above characteristics is successfully manufactured by a specific manufacturing method using a fluidized bed furnace.

[0037] (Specific surface area)

[0038] From the viewpoint of achieving a high level of adsorption and removal performance required for a water purifier, the specific surface area of ​​the carbonaceous material is preferably 900 to 1500 m 2 The lower limit of the specific surface area is preferably 950 m 2 / g or above or 1000m 2 / g or more, and the upper limit is preferably 1400m 2 / g or below or 1300m 2 / g or less.

[0039] The specific surface area of ​​the carbonaceous material can be calculated from the nitrogen adsorption isotherm using the BET method. The measurement of the nitrogen adsorption isotherm and the calculation of the specific surface area can be carried out by the methods described in [Measurement of nitrogen adsorption isotherm] and [Measurement of specific surface area] described below.

[0040] (Average pore size)

[0041] From the viewpoint of being able to more effectively remove trihalomethanes and 2-MIB with a single species, the average pore size of the carbonaceous material is preferably in the range of 1.79 to 1.88 nm. The lower limit of the average pore size is preferably 1.80 nm or more, and the upper limit is preferably 1.87 nm or less or 1.86 nm or less.

[0042] The average pore diameter of the carbonaceous material can be calculated from the nitrogen adsorption isotherm. The measurement of the nitrogen adsorption isotherm and the calculation of the average pore diameter can be carried out by the methods described in [Measurement of nitrogen adsorption isotherm] and [Measurement of total pore volume and average pore diameter] described below.

[0043] (Pore volume ratio of micropores to total pore volume (micropore ratio))

[0044] From the viewpoint that trihalomethanes and 2-MIB can be further effectively removed with a single species, the carbonaceous material preferably has a pore volume ratio (micropore ratio) of micropores relative to the total pore volume of 96% or less. More preferably, it is 95% or less. The lower limit of the micropore ratio is not particularly limited, but from the viewpoint of achieving excellent trihalomethane adsorption performance, it is generally preferably 90% or more, preferably 92% or more.

[0045] The total pore volume of the carbonaceous material can be calculated based on the nitrogen adsorption amount at the relative pressure P / P0=0.99 in the nitrogen adsorption isotherm. In addition, the pore volume of the micropores can be calculated using the MP (Micropore) method and based on the nitrogen adsorption isotherm. The measurement of the nitrogen adsorption isotherm and the calculation of the total pore volume and the pore volume of the micropores can be implemented by the methods described in [Measurement of nitrogen adsorption isotherm], [Measurement of total pore volume and average pore diameter] and [Measurement of micropore pore volume by MP method] described later.

[0046] (Conductivity)

[0047] The carbonaceous material involved in this embodiment preferably has a conductivity in the range of 5 to 12 S / cm obtained by measuring the powder resistance under a load of 12 kN. If the conductivity is within this range, in more detail, if the carbonaceous material has a structure with a conductivity within the range, the high level of adsorption and removal performance required for the water purifier can be achieved. The upper limit of the conductivity is preferably less than 11 S / cm, less than 10 S / cm, or less than 9 S / cm, and the lower limit is preferably more than 5.5 S / cm, more than 6 S / cm, or more than 6.5 S / cm.

[0048] The electrical conductivity of the carbonaceous material can be measured by the method described in [Measurement of Electrical Conductivity] described later.

[0049] The shape of the carbonaceous material is not particularly limited, and can be any shape such as a particle, a fiber (filament, a woven (cloth) shape, a felt shape), etc., and can be appropriately selected according to the specific use mode, but due to the high adsorption performance per unit volume, it is preferably a particle. In the case of a particle-shaped carbonaceous material, its size is not particularly limited, and the particle size can be appropriately adjusted according to the specific use mode.

[0050] The raw material (carbonaceous precursor) of the carbonaceous material is not particularly limited. For example, plant-based carbonaceous precursors (such as wood, wood shavings, charcoal, fruit shells such as coconut shells and walnut shells, fruit seeds, byproducts of pulp manufacturing, lignin, waste molasses and other plant-based materials); mineral-based carbonaceous precursors (such as peat, lignite (sub-charcoal), wood coal (brown coal), bituminous coal, anthracite, coke, coal tar, coal tar, petroleum distillation residues, petroleum asphalt and other mineral-based materials); synthetic resin-based carbonaceous precursors (such as phenolic resins, polyvinylidene chloride, acrylic resins and other synthetic resin-based materials); natural fiber-based carbonaceous precursors (such as natural fibers such as cellulose, natural fiber-based materials such as regenerated fibers such as rayon), etc. Among them, plant-based carbonaceous precursors are easy to use as carbonaceous materials with excellent adsorption properties for removal targets specified in the Household Products Quality Labeling Act, and are therefore preferred. Therefore, in a preferred embodiment, the carbonaceous material is derived from a plant-based carbonaceous precursor. From the viewpoint of realizing a carbonaceous material that can more effectively remove trihalomethanes and 2-MIB, coconut shell is preferably used as a raw material. Therefore, in a particularly preferred embodiment, coconut shell is used as a plant-based carbonaceous precursor.

[0051] The carbonaceous material involved in this embodiment can effectively remove VOCs such as trihalomethanes with small molecular size and 2-MIB with large molecular size with a single species. Therefore, the carbonaceous material of this embodiment can be suitable for use as a carbonaceous material for water purification (carbonaceous material for water purification), and is more suitable for use as a carbonaceous material for purifying tap water (carbonaceous material for tap water purification).

[0052] [Method for producing carbonaceous material]

[0053] The carbonaceous material according to one embodiment of the present invention is manufactured by activating the above-mentioned carbonaceous precursor. In addition, when carbonization is required before activation, it is usually isolated from oxygen or air and carbonized at, for example, 400 to 800° C. (preferably 500 to 800° C., more preferably 550 to 750° C.). At this time, the raw carbon obtained by carbonization of the carbonaceous precursor is activated to manufacture the carbonaceous material.

[0054] When achieving a carbonaceous material with a benzene adsorption amount, a vitamin B12 adsorption amount, and a mesopore volume within a specific range, an activation method is important. The method for manufacturing a carbonaceous material according to the present embodiment (hereinafter, also referred to as the "manufacturing method of the present embodiment") uses a fluidized bed furnace (fluidized bed activation furnace) as an activation furnace, and in addition to the fluidizing gas introduced from the furnace bed, an oxygen-containing gas is introduced into the fluidized bed furnace. Accordingly, a benzene adsorption amount of 25 to 40%, a vitamin B12 adsorption amount of 13.0 to 50.0 mg / g, and a mesopore volume of 0.070 to 0.150 cm-1 obtained from the nitrogen adsorption isotherm by the BJH method can be achieved. 3 / g of carbonaceous material, which is difficult to achieve in the conventional method of using a rotary kiln as an activation furnace and the conventional method of introducing only fluidizing gas from the furnace bed into the fluidized bed furnace.

[0055] The fluidizing gas is not particularly limited as long as it has the function of fluidizing and activating the raw coal, and any conventionally known substance can be used. In industry, since it contains water vapor and carbon dioxide in moderation, it is preferred to use a combustion gas of hydrocarbons (e.g., light gases such as methane, propane, and butane; liquid fuels such as light oil, kerosene, and heavy oil).

[0056] From the viewpoint of effectively activating the raw carbon, the water vapor concentration in the fluidizing gas is preferably 10 to 40% by volume. The upper limit is more preferably 35% by volume or less or 30% by volume or less, and the lower limit is more preferably 12% by volume or more, 14% by volume or more, or 15% by volume or more.

[0057] In the manufacturing method of the present embodiment, in addition to the fluidizing gas introduced from the furnace bed, an oxygen-containing gas is also introduced into the fluidized bed furnace. The oxygen-containing gas is introduced into the fluidized bed furnace in such a way that the oxygen concentration in the combined gas of the fluidizing gas and the oxygen-containing gas becomes 0.004 to 1% by volume. From the viewpoint of being able to obtain a further effective removal of trihalomethanes and 2-MIB with a single species, the oxygen concentration in the combined gas of the fluidizing gas and the oxygen-containing gas is preferably 0.005% by volume or more, 0.01% by volume or more, 0.02% by volume or more, 0.03% by volume or more, 0.04% by volume or more, or 0.05% by volume or more. The upper limit of the oxygen concentration is preferably 0.95% by volume or less, 0.9% by volume or less, 0.85% by volume or less, or 0.8% by volume or less. In the present embodiment, the oxygen concentration in the combined gas of the fluidizing gas and the oxygen-containing gas is a charge-converted concentration calculated based on the composition and introduction amount of the fluidizing gas, and the composition and introduction amount of the oxygen-containing gas.

[0058] The oxygen-containing gas is not particularly limited as long as it contains oxygen. For example, air and a gas diluted with other gases (such as inert gases such as nitrogen) can be used. The oxygen concentration in the oxygen-containing gas is not particularly limited as long as the oxygen concentration in the combined gas of the fluidizing gas and the oxygen-containing gas is in the range of 0.004 to 1% by volume, but is preferably 20% by volume or less, more preferably 15% by volume or less, 10% by volume or less, 8% by volume or less, 6% by volume or less, 5% by volume or less, 4% by volume or less, 3% by volume or less or 2% by volume or less. The lower limit of the oxygen concentration in the oxygen-containing gas can usually be set to 0.1% by volume or more, 0.2% by volume or more, etc. In addition, the fluidizing gas introduced from the furnace bed can contain oxygen, but when a combustion gas is used as the fluidizing gas, it is generally difficult to control the trace oxygen concentration in the combustion gas, so it is preferred to control the oxygen concentration by oxygen derived from the oxygen-containing gas.

[0059] Hereinafter, the manufacturing method of the present embodiment will be described with reference to the accompanying drawings. The main reference numerals in the respective drawings are as follows: 1 fluidizing gas inlet, 2 oxygen-containing gas inlet, 3 gas outlet, 4 gas dispersion layer, 5 raw charcoal, 6 raw charcoal (during fluidization activation), 7 fluidizing gas, 8 oxygen-containing gas, 9 exhaust gas, 10 gas dispersion section, 20 fluidized bed section, 100 fluidized bed furnace (fluidized bed activation furnace).

[0060] Figure 1 A schematic diagram of a fluidized bed furnace (fluidized bed activation furnace) 100 used in the manufacturing method of the present embodiment is shown. The fluidized bed furnace 100 includes a fluidizing gas inlet 1, an oxygen-containing gas inlet 2, a gas outlet 3, and a gas dispersion layer 4. The fluidizing gas inlet 1 is usually arranged on the furnace bed, and the fluidizing gas (not shown) introduced into the fluidized bed furnace 100 passes through the gas dispersion layer 4 and contacts the raw coal 5 to provide fluidization activation for the raw coal. Then, the fluidizing gas is discharged to the outside of the furnace from the gas outlet 3 usually arranged on the furnace top. Figure 1 In FIG. 5 , the main flow direction of the fluidizing gas (ie, the flow direction from the furnace bed to the furnace top) is represented as direction Z.

[0061] The gas dispersion layer 4 is not particularly limited as long as it has the function of dispersing the flow of the fluidizing gas introduced from the fluidizing gas inlet 1 and making the fluidizing gas and the raw coal 5 contact uniformly, and a conventionally known gas dispersion layer can be used. For example, when a perforated plate is used to disperse the fluidizing gas, the buffer area from the furnace bed to the perforated plate is included and is called the gas dispersion layer 4. Figure 1 As shown in FIG. 1 , the gas distribution layer 4 is arranged on the upstream side in the fluidized bed furnace when viewed from the main flow direction Z of the fluidizing gas. In the present embodiment, the region formed by the gas distribution layer 4 is referred to as a gas distribution section 10. Therefore, when viewed from the main flow direction Z of the fluidizing gas, the fluidized bed furnace 100 includes the gas distribution section 10 on the upstream side in the fluidized bed furnace.

[0062] The fluidized bed furnace 100 further includes a fluidized bed section 20 on the downstream side in the fluidized bed furnace when viewed from the main flow direction Z of the fluidizing gas. In the fluidized bed section 20 , the raw coal 5 contacts the fluidizing gas, and fluidization activation of the raw coal 5 is performed.

[0063] As described above, in addition to introducing the fluidizing gas from the furnace bed, the manufacturing method of the present embodiment also introduces an oxygen-containing gas into the fluidized bed furnace. Furthermore, when realizing a carbonaceous material having a benzene adsorption amount, a vitamin B12 adsorption amount, and a mesopore volume within a specific range, the position where the oxygen-containing gas is introduced is important. That is, when the upstream end position of the gas dispersion section in the main flow direction Z of the fluidizing gas is set to 0 (m), the downstream end position is set to t1 (m) (t1>0), and the oxygen-containing gas introduction position is set to t2 (m), it is preferred to satisfy the relationship of 0.5t1 and t2. When 0.5t1>t2, it is difficult to realize the carbonaceous material involved in the present embodiment having a benzene adsorption amount, a vitamin B12 adsorption amount, and a mesopore volume within a specific range. Preferably, 0.7t1≤t2, more preferably 0.8t1≤t2, 0.gt1≤t2, or t1≤t2, particularly preferably t1<t2, 1.2t1≤t2, 1.4t1≤t2, or 1.5t1≤t2. The upper limit of t2 is not particularly limited as long as the oxygen-containing gas can contact the raw coal in the fluidized activation process, and can be any position up to the furnace top, but preferably, when the height (thickness) of the fluidized bed 20 is T (m) (i.e., T = (height of the furnace top - t1)) when viewed from the direction Z, t2 ≤ 0.8T, t2 ≤ 0.7T, t2 ≤ 0.6T or t2 ≤ 0.5T. In addition, when the oxygen-containing gas inlet 2 has a width (thickness) when viewed from the direction Z, the oxygen-containing gas introduction position t2 refers to the center position of its width (thickness).

[0064] Figure 2 It means use Figure 1 Schematic diagram of the fluidized bed furnace fluidizing and activating raw carbon. Figure 2 In, use Figure 1 Components and parts denoted by the same reference numerals represent the same Figure 1 Same components and parts.

[0065] exist Figure 2In the fluidized bed furnace 100, a fluidizing gas 7 is introduced from the furnace bed into the fluidized bed furnace 100, and an oxygen-containing gas 8 is introduced from the side of the furnace into the fluidized bed furnace 100. The fluidizing gas 7 passes through the gas dispersion section 10 formed by the gas dispersion layer 4, and contacts the raw charcoal in the fluidized bed section 20 to provide fluidization activation of the raw charcoal. In addition, the oxygen-containing gas 8 (more specifically, the oxygen in the gas) contacts the raw charcoal 6 during fluidization activation to provide local activation of the raw charcoal. It can be inferred that by locally activating the raw charcoal with such an oxygen-containing gas, mesopores can be locally developed while maintaining micropores, and as a result, a carbonaceous material having a benzene adsorption amount, a vitamin B12 adsorption amount and a mesopore volume within a specific range can be advantageously produced.

[0066] The raw carbon activation conditions may adopt conventionally known conditions except for introducing the oxygen-containing gas and the fluidizing gas separately. For example, the activation temperature may be 700 to 1000°C (preferably 800 to 1000°C, 850 to 950°C), and the activation time may be any time that achieves the desired amount of benzene adsorption (the desired degree of activation progress).

[0067] As described above, in the manufacturing method of the present embodiment, the desired carbonaceous material having a benzene adsorption amount, a vitamin B12 adsorption amount, and a mesopore volume within a specific range can be manufactured by the action of the oxygen-containing gas introduced separately from the fluidizing gas. Here, the activation of the raw carbon using water vapor and carbon dioxide in the fluidizing gas is an endothermic reaction, whereas the activation of the raw carbon using oxygen in the oxygen-containing gas is a rapid exothermic reaction. Therefore, in the manufacturing method of the present embodiment in which the oxygen-containing gas is brought into contact with the raw carbon during fluidization activation, the heat supply from the outside required to maintain the activation of the raw carbon can be reduced, which is also extremely advantageous from the perspective of energy balance.

[0068] The fluidizing gas 7 and the oxygen-containing gas 8 are supplied to activate the raw coal and then discharged to the outside of the furnace from the gas outlet ( Figure 2 9) By circulating part or all of the exhaust gas or performing heat exchange, the thermal energy of the exhaust gas can be reused.

[0069] Figure 1 and Figure 2 The fluidized bed furnace is shown with one fluidizing gas inlet 1, one oxygen-containing gas inlet 2, and one gas outlet 3. Figure 1 and Figure 2 It is just a schematic diagram, and the fluidized bed furnace may have multiple fluidizing gas inlets 1, oxygen-containing gas inlets 2, and gas outlets 3. When there are multiple oxygen-containing gas inlets 2, they may be arranged at the same position (height) or at different positions (heights) when viewed from the main flow direction Z of the fluidizing gas.

[0070] When using a plant-based carbonaceous precursor or a mineral-based carbonaceous precursor such as a coconut shell containing impurities such as an alkali metal, an alkaline earth metal, and a transition metal, the activated carbonaceous material is washed in order to remove ash or chemical reagents. Therefore, in one embodiment, the manufacturing method of the present invention may also include a step of washing the activated carbonaceous material. At this time, an inorganic acid or water is used in the washing, and preferably hydrochloric acid with high washing efficiency is used as the inorganic acid. In the case of washing (pickling) the carbonaceous material with an inorganic acid such as hydrochloric acid, it is preferably washed with water after pickling, etc., and deacidification is performed.

[0071] After washing, the obtained carbonaceous material is dried, and if necessary, pulverized and sieved to obtain a carbonaceous material product.

[0072] [Water purification filter]

[0073] A water purification filter can be manufactured using a carbonaceous material. A water purification filter according to a preferred embodiment will be described below.

[0074] In a preferred embodiment, a water purification filter includes the carbonaceous material according to the present embodiment described above and a fibrous binder.

[0075] The fibrous binder is not particularly limited as long as it can be shaped by entanglement with the carbonaceous material through fibrillation, and both synthetic and natural products can be widely used. Examples of such fibrous binders include acrylic fibers, polyethylene fibers, polypropylene fibers, polyacrylonitrile fibers, cellulose fibers, nylon fibers, aramid fibers, pulp, etc. The fiber length of the fibrous binder is preferably 4 mm or less.

[0076] The fibrous binder can be used in combination of two or more. It is particularly preferred to use polyacrylonitrile fiber or pulp as the binder. This can further increase the density and strength of the molded body and suppress performance degradation.

[0077] In a preferred embodiment, the water permeability of the fibrous binder is about 10 to 150 mL in terms of CSF value. In the present embodiment, the CSF value is a value measured in accordance with the Canadian Standard Freeness Method of JIS P8121 "Test Method for Water Filterability of Pulp". In addition, the CSF value can be adjusted, for example, by fibrillating the fibrous binder. If the CSF value of the fibrous binder is less than 10 mL, water permeability cannot be obtained, and there is a risk that the strength of the molded body will decrease and the pressure loss will also increase. On the other hand, when the CSF value exceeds 150 mL, the powdered activated carbon cannot be fully retained, the strength of the molded body will decrease, and there is a possibility that the adsorption performance will deteriorate.

[0078] From the perspective of the removal performance and formability of the object to be removed, the filter for water purification preferably contains 4 to 10 parts by mass of the fibrous binder relative to 100 parts by mass of the carbonaceous material, and more preferably contains 4.5 to 6 parts by mass. Therefore, in a preferred embodiment, the filter for water purification contains the carbonaceous material and the fibrous binder involved in the present embodiment, and the CSF value of the fibrous binder is 10 to 150 mL, and contains 4 to 10 parts by mass of the fibrous binder relative to 100 parts by mass of the carbonaceous material. In addition, in the case where the filter for water purification contains other functional components described later, the "relative to 100 parts by mass of the carbonaceous material" in the filter composition is rewritten as "relative to 100 parts by mass of the carbonaceous material and other functional components in total" is applicable.

[0079] The water purification filter may further contain other functional components as long as the effect of the present invention is not inhibited. Other functional components include lead adsorbing materials such as titanium silicate or zeolite powder that can adsorb and remove soluble lead, ion exchange resins or integrated resins, or various adsorbing materials containing silver ions and / or silver compounds to impart antibacterial properties.

[0080] The water purification filter involved in the present embodiment includes the carbonaceous material involved in the present embodiment, so it can effectively remove VOCs such as trihalomethanes with small molecular size and 2MIB with large molecular size. The water flow conditions are not particularly limited, for example, it is implemented at a space velocity (SV) of 300 to 6500 / hr so ​​that the pressure loss does not become extremely large. By plotting the relationship between each removal rate calculated based on the concentration of the removal target substance in the raw water and the permeated water, and the ratio of the amount of water (L) flowing from the start of water flow to the volume (mL) of the water purification filter element (cumulative permeated water volume L / mL), the performance of the water purification filter can be confirmed.

[0081] [Water Purifier]

[0082] A water purifier can be manufactured using the carbonaceous material or the water purification filter. In a preferred embodiment, the water purifier includes the carbonaceous material or the water purification filter according to the present embodiment as described above.

[0083] In a preferred embodiment, the water purifier includes a water purification filter element, which is formed using the carbonaceous material or water purification filter involved in the present embodiment. For example, the carbonaceous material involved in the present embodiment can be filled into a housing to form a water purification filter element, and further, the water purification filter involved in the present embodiment can also be filled into a housing to form a water purification filter element. In addition to the carbonaceous material or water purification filter involved in the present embodiment, the water purification filter element can also be combined to include a known non-woven filter, various adsorbents, mineral additives, ceramic filter materials, hollow fiber membranes, etc.

[0084] As described above, this specification discloses various aspects of technology, and its main technologies are summarized as follows.

[0085] The carbonaceous material according to one aspect of the present invention has a benzene adsorption capacity of 25-40%, a vitamin B12 adsorption capacity of 13.0-50.0 mg / g, and a mesopore volume of 0.070-0.150 cm-3 obtained from a nitrogen adsorption isotherm by the BJH method. 3 / g.

[0086] According to this configuration, it is possible to provide a carbonaceous material capable of removing both trihalomethanes and 2-MIB using a single species.

[0087] In addition, in the carbonaceous material, preferably, the specific surface area calculated from the nitrogen adsorption isotherm by the BET method is 900 to 1500 m 2 / g. It is considered that this can achieve a high level of adsorption removal performance required for a water purifier.

[0088] In addition, in the carbonaceous material, the average pore diameter calculated from the nitrogen adsorption isotherm is preferably 1.79 to 1.88 nm, which is considered to make it possible to more effectively remove trihalomethanes and 2-MIB with a single species.

[0089] In addition, in the carbonaceous material, preferably, the ratio of the pore volume of micropores calculated by the MP method based on the nitrogen adsorption isotherm to the total pore volume calculated based on the nitrogen adsorption amount at the relative pressure P / P0=0.99 in the nitrogen adsorption isotherm is 96% or less. It is believed that this can further effectively remove trihalomethanes and 2-MIB with a single species.

[0090] In addition, in the carbonaceous material, it is preferred that the electrical conductivity obtained by powder resistance measurement under a load of 12 kN is 5 to 12 S / cm. It is considered that this can achieve a high level of adsorption and degation performance required for a water purifier.

[0091] In addition, it is preferred that the carbonaceous material is derived from a plant-based carbonaceous precursor. It is believed that this makes it easy to use a carbonaceous material with excellent adsorption performance for the removal target substances specified in the Household Products Quality Labeling Law. It is further preferred that the plant-based carbonaceous precursor is coconut shell, which is believed to be able to achieve a carbonaceous material that can further effectively remove trihalomethanes and 2-MIB.

[0092] A method for producing a carbonaceous material according to another aspect of the present invention uses a fluidized bed furnace, and in addition to introducing a fluidizing gas from the furnace bed, introduces an oxygen-containing gas into the fluidized bed furnace so that the oxygen concentration in the combined gas of the fluidizing gas and the oxygen-containing gas is 0.004 to 1% by volume. With this configuration, an excellent carbonaceous material as described above can be obtained.

[0093] Furthermore, in the production method, it is preferred that the concentration of water vapor in the fluidizing gas introduced from the hearth is 10 to 40% by volume. This is considered to enable the raw carbon to be effectively activated.

[0094] In addition, in the production method, it is preferred that the fluidized bed furnace has a gas dispersion section on the upstream side of the fluidized bed furnace when viewed from the main flow direction Z of the fluidizing gas, and when the upstream end position of the gas dispersion section in the direction Z is set to 0 (m), the downstream end position is set to t1 (m), and the position for introducing the oxygen-containing gas is set to t2 (m), the oxygen-containing gas is introduced in a manner that satisfies the relationship of 0.5t1≤t2. It is believed that the excellent carbonaceous material as described above can be obtained more reliably according to this.

[0095] Another aspect of the present invention relates to a water purification filter comprising: the carbonaceous material as described above; and a fibrous binder, wherein the CSF value of the fibrous binder is 10 to 150 mL, and 4 to 10 parts by mass of the fibrous binder are included relative to 100 parts by mass of the carbonaceous material. In addition, the present invention also includes: a water purifier comprising the carbonaceous material as described above; and a water purifier comprising the water purification filter.

[0096] Example

[0097] Hereinafter, the present invention will be further specifically described by way of examples, however, the present invention is not limited to these examples.

[0098] <Evaluation method>

[0099] The physical property values ​​in the examples were measured by the methods shown below.

[0100] [Determination of benzene adsorption amount]

[0101] The carbonaceous materials prepared in the examples and comparative examples were dried in a constant temperature dryer at 115°C for 3 hours and then cooled to room temperature in a dryer using silica gel as a desiccant. Next, dry air containing benzene at a concentration of 1 / 10 of the saturated concentration was passed through the carbonaceous material in a constant temperature bath at 20°C. The benzene adsorption amount (mass %) was calculated according to the following formula (1) based on the mass of the carbonaceous material that reached adsorption equilibrium and the mass of the carbonaceous material before adsorption (i.e., the mass of the carbonaceous material after drying and cooling).

[0102] [Formula (1)]

[0103] Benzene adsorption amount (mass %) = [{(mass of sample after benzene adsorption) - (mass of sample before benzene adsorption)} / (mass of sample before benzene adsorption)] × 100

[0104] [Determination of vitamin B12 adsorption]

[0105] The carbonaceous material prepared in the examples and comparative examples was crushed into a volume-based cumulative distribution of the carbonaceous material with a 50% particle size (D50) of about 9 to 11 μm, and dried in a constant temperature dryer at 115°C for 3 hours, and then cooled to room temperature in a dryer using silica gel as a desiccant. In addition, the particle size of the crushed carbonaceous material was measured using a laser diffraction measurement method. That is, the carbonaceous material to be measured was added to ion exchange water together with a surfactant, ultrasonic vibration was applied to prepare a uniform dispersion, and the measurement was performed using Microtrac MT3200 manufactured by Microtrac BEL Co., Ltd. The surfactant used was "Polyoxyethylene (10) octylphenyl ether" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. The analysis conditions are shown below.

[0106] (Analysis conditions)

[0107] Number of measurements: 1

[0108] Measurement time: 30 seconds

[0109] Distribution Display: Volume

[0110] Particle size classification: Standard

[0111] Calculation mode: MT3000

[0112] Solvent name: Water

[0113] Upper limit of measurement: 1408μm, Lower limit of measurement: 0.265μm

[0114] Residual component ratio: 0.00

[0115] By composition ratio: 0.00

[0116] Residual component ratio setting: Invalid

[0117] Particle permeability:

[0118] Particle refractive index: 1.81

[0119] Particle shape: non-spherical

[0120] Solvent refractive index: 1.333

[0121] DV value: 0.0100~0.0500

[0122] Transmittance (TR): 0.750~0.920

[0123] Flow rate: 50%

[0124] To about 0.05 g to 0.30 g of the obtained carbonaceous material, vitamin B12 (C63 H 8s N 14 O 14 PCo: molecular weight 1355.4) aqueous solution 100mL, and oscillate at 160 times / min at 25°C for 2 hours to adsorb vitamin B12, and recover the filtrate after filtering the carbonaceous material. The absorbance at 330nm was measured for the vitamin B12 test water before adsorption of about 320ppm used in the adsorption test and the vitamin B12 filtrate after adsorption treatment, and the concentration of vitamin B12 was calculated based on the pre-made calibration curve. Based on the obtained vitamin B12 concentration, the adsorption amount of vitamin B12 per 1g of carbonaceous material was calculated by the following formula (2).

[0125] [Formula (2)]

[0126] Vitamin B12 adsorption amount (mg / g) = {Vitamin B12 concentration before adsorption (ppm) - Vitamin B12 concentration after adsorption treatment (ppm)} × 0.1 / mass of carbonaceous material (g)

[0127] The adsorption amount of vitamin B12 when the concentration of vitamin B12 after adsorption treatment exceeded 300 ppm and the adsorption amount of vitamin B12 when the concentration was less than 300 ppm were calculated. Furthermore, the adsorption amount of vitamin B12 after adsorption treatment when the concentration of vitamin B12 after adsorption treatment reached 300 ppm was calculated by power approximate expression and was taken as the adsorption amount of vitamin B12.

[0128] [Determination of nitrogen adsorption isotherm]

[0129] The carbonaceous material was heated at 300° C. for 3 hours under a nitrogen flow (nitrogen flow rate: 50 mL / min) using BELSORP-mini manufactured by Microchip BEL CORPORATION, and then the nitrogen desorption isotherm of the carbonaceous material at 77 K was measured.

[0130] [Measurement of specific surface area]

[0131] The nitrogen adsorption isotherm obtained by the above method was analyzed by a multipoint method using the BET equation, and the specific surface area was calculated from a straight line in the relative pressure region of P / P0=0.01 to 0.1 of the obtained curve.

[0132] [Measurement of total pore volume and average pore diameter]

[0133] The total pore volume was calculated by the Gurvish method from the nitrogen adsorption amount at the relative pressure P / P0=0.99 of the nitrogen adsorption isotherm obtained by the above method. The average pore diameter was calculated based on the total pore volume and the specific surface area obtained by the BET method described above according to the following formula (3).

[0134] [Formula (3)]

[0135] Average pore diameter (nm) = total pore volume (cm 3 / g) / Specific surface area (m 2 / g)×4000

[0136] [Measurement of micropore volume and micropore ratio by MP method]

[0137] The MP method was applied to the nitrogen adsorption isotherm obtained by the above method to calculate the pore volume of the micropores. The ratio of the pore volume of the micropores obtained by the MP method to the total pore volume calculated by the above method was taken as the micropore ratio. In addition, when analyzing by the MP method, the reference curve "NGCB-BEL.t" provided by Michik BEL Co., Ltd. was used.

[0138] [Measurement of mesopore volume by BJH method]

[0139] The BJH method was applied to the nitrogen adsorption isotherm obtained by the above method to calculate the pore volume of the mesopores. In addition, when performing the analysis by the BJH method, the reference curve "NGCB-BEL.t" provided by Microchip BEL Co., Ltd. was used.

[0140] [Determination of electrical conductivity]

[0141] The electrical conductivity of the carbonaceous material was measured using a powder resistivity test system (manufactured by Mitsubishi Chemical Analytical Tech Co., Ltd., MCP-PD51). Since the particle size of the test sample has a great influence on the measurement of the electrical conductivity, it was crushed so that the 50% particle size (D50) of the cumulative distribution of the carbonaceous material on a volume basis was about 5 to 8 μm, and the electrical conductivity of the carbonaceous material particles was measured when a load of 12 kN was applied. In addition, the particle size of the crushed carbonaceous material was measured using a laser diffraction measurement method. The measurement procedure and analysis conditions for the particle size of the carbonaceous material are as described above in [Measurement of Vitamin B12 Adsorption].

[0142] <Example 1>

[0143] The particle size of coconut shell charcoal obtained by carbonizing coconut shells produced in the Philippines was adjusted from 10 mesh (1.7 mm) to 30 mesh (0.5 mm). 1 kg of the coconut shell charcoal was put into a fluidized bed activation furnace heated to 900°C, and a fluidizing gas of 15% by volume of water vapor and 11% by volume of carbon dioxide was introduced from the furnace bed at 50 L / min, and an oxygen-containing gas of 0.5% by volume of oxygen and 99.5% by volume of nitrogen was introduced from the side of the furnace at 5 L / min, and an activation treatment was performed until the amount of benzene adsorption reached about 35% by weight (the oxygen concentration in the total gas introduced into the fluidized bed activation furnace was about 0.045% by volume). The fluidized bed activation furnace used a furnace with a gas dispersion layer on the upstream side of the furnace when viewed from the main flow direction Z of the fluidizing gas. In addition, the introduction position t2 of the oxygen-containing gas in the direction Z and the downstream end t1 of the gas dispersion layer satisfied the relationship t1<t2. That is, the oxygen-containing gas was introduced into the fluidized bed portion of the fluidized bed activation furnace.

[0144] The activated carbon obtained was washed with dilute hydrochloric acid, and then fully washed with ion exchange water to remove the residual hydrochloric acid, and then dried to obtain a carbonaceous material. Table 1 shows the treatment conditions and the physical properties of the obtained carbonaceous material.

[0145] <Example 2>

[0146] A carbonaceous material was obtained in the same manner as in Example 1 except that the particle size of the coconut shell charcoal before activation was adjusted from 30 mesh (0.5 mm) to 60 mesh (0.25 mm). Table 1 shows the treatment conditions and the physical properties of the obtained carbonaceous material.

[0147] <Example 3>

[0148] A carbonaceous material was obtained in the same manner as in Example 2 except that the concentration of the oxygen-containing gas introduced during the activation treatment was changed to 0.05% by volume of oxygen and 99.95% by volume of nitrogen. Table 1 shows the treatment conditions and the physical properties of the obtained carbonaceous material.

[0149] <Example 4>

[0150] A carbonaceous material was obtained in the same manner as in Example 2 except that the concentration of the oxygen-containing gas introduced during the activation treatment was changed to 1% by volume of oxygen and 99% by volume of nitrogen. Table 1 shows the treatment conditions and the physical properties of the obtained carbonaceous material.

[0151] <Example 5>

[0152] A carbonaceous material was obtained in the same manner as in Example 2 except that the concentration of the oxygen-containing gas introduced during the activation treatment was changed to 5% by volume of oxygen and 95% by volume of nitrogen. Table 1 shows the treatment conditions and the physical properties of the obtained carbonaceous material.

[0153] <Example 6>

[0154] A carbonaceous material was obtained in the same manner as in Example 2 except that the concentration of the oxygen-containing gas introduced during the activation treatment was changed to 10% by volume of oxygen and 90% by volume of nitrogen. Table 1 shows the treatment conditions and the physical properties of the obtained carbonaceous material.

[0155] <Example 7>

[0156] A carbonaceous material was obtained by the same method as in Example 4 except that the activation treatment was performed until the benzene adsorption amount of the activated carbon reached about 28% by weight. Table 1 shows the treatment conditions and the physical properties of the obtained carbonaceous material.

[0157] <Example 8>

[0158] A carbonaceous material was obtained in the same manner as in Example 1 except that the particle size of the coconut shell charcoal before activation was adjusted from 50 mesh (0.3 mm) to 100 mesh (0.15 mm). Table 1 shows the treatment conditions and the physical properties of the obtained carbonaceous material.

[0159] <Comparative Example 1>

[0160] The particle size of coconut shell charcoal obtained by carbonizing coconut shells produced in the Philippines was adjusted from 10 mesh (1.7 mm) to 30 mesh (0.5 mm). 1 kg of the coconut shell charcoal was put into a rotary kiln heated to 900°C, and an activation gas of 15% by volume of water vapor and 11% by volume of carbon dioxide was introduced at 10 L / min, and an additional gas of 0.5% by volume of oxygen and 99.5% by volume of nitrogen was introduced at 1 L / min, and an activation treatment was performed until the benzene adsorption reached about 35% by weight.

[0161] The activated carbon obtained was washed with dilute hydrochloric acid, and then fully washed with ion exchange water to remove the residual hydrochloric acid, and then dried to obtain a carbonaceous material. Table 1 shows the treatment conditions and the physical properties of the obtained carbonaceous material.

[0162] <Comparative Example 2>

[0163] A carbonaceous material was obtained in the same manner as in Comparative Example 1 except that the particle size of the coconut shell charcoal before activation was adjusted from 30 mesh (0.5 mm) to 60 mesh (0.25 mm). Table 1 shows the treatment conditions and the physical properties of the obtained carbonaceous material.

[0164] <Comparative Example 3 (Reference Example)>

[0165] A carbonaceous material was obtained by the same method as in Example 2 except that the activation treatment was performed until the benzene adsorption amount of the activated carbon reached about 45% by mass. The treatment conditions and the physical properties of the obtained carbonaceous material are shown in Table 1. It should be noted that in the method for producing a carbonaceous material using a fluidized bed furnace, an oxygen-containing gas is supplied in addition to the fluidizing gas, so this Comparative Example 3 is shown as a reference example rather than a method involved in the prior art. The same is true for Comparative Examples 4 and 6 described later.

[0166] <Comparative Example 4 (Reference Example)>

[0167] A carbonaceous material was obtained by the same method as in Example 2 except that the activation treatment was performed until the benzene adsorption amount of the activated carbon reached about 25 mass %. Table 1 shows the treatment conditions and the physical properties of the obtained carbonaceous material.

[0168] <Comparative Example 5>

[0169] A carbonaceous material was obtained by the same method as in Example 2 except that the oxygen-containing gas introduced during the activation treatment was changed to nitrogen gas not containing oxygen. Table 1 shows the treatment conditions and the physical properties of the obtained carbonaceous material.

[0170] <Comparative Example 6 (Reference Example)>

[0171] A carbonaceous material was obtained by the same method as in Example 2 except that the oxygen-containing gas introduced during the activation treatment was changed to air. Table 1 shows the treatment conditions and the physical properties of the obtained carbonaceous material.

[0172] <Comparative Example 7>

[0173] A carbonaceous material was obtained by the same method as in Comparative Example 2, except that the oxygen-containing gas introduced during the activation treatment was changed to nitrogen gas not containing oxygen. Table 1 shows the treatment conditions and the physical properties of the obtained carbonaceous material.

[0174] <Comparative Example 8>

[0175] A carbonaceous material was obtained in the same manner as in Comparative Example 2 except that the concentration of the oxygen-containing gas introduced during the activation treatment was changed to 1% by volume of oxygen and 99% by volume of nitrogen. Table 1 shows the treatment conditions and the physical properties of the obtained carbonaceous material.

[0176] <Comparative Example 9>

[0177] A carbonaceous material was obtained in the same manner as in Comparative Example 2 except that the concentration of the oxygen-containing gas introduced during the activation treatment was changed to 5% by volume of oxygen and 95% by volume of nitrogen. Table 1 shows the treatment conditions and the physical properties of the obtained carbonaceous material.

[0178] <Comparative Example 10>

[0179] A carbonaceous material was obtained in the same manner as in Comparative Example 2 except that the concentration of the oxygen-containing gas introduced during the activation treatment was changed to 10% by volume of oxygen and 90% by volume of nitrogen. Table 1 shows the treatment conditions and the physical properties of the obtained carbonaceous material.

[0180] <Comparative Example 11>

[0181] A carbonaceous material was obtained by the same method as in Comparative Example 3 except that the oxygen-containing gas introduced during the activation treatment was changed to nitrogen gas not containing oxygen. Table 1 shows the treatment conditions and the physical properties of the obtained carbonaceous material.

[0182] <Comparative Example 12>

[0183] Powdered activated carbon PGW-100MD manufactured by Kuraray Co., Ltd. was obtained before pulverization, and the particle size was adjusted from 30 mesh (0.5 mm) to 60 mesh (0.25 mm) to obtain a carbonaceous material for Comparative Example 12. The physical properties are shown in Table 1.

[0184]

[0185] [Evaluation of Filtration Capacity of Carbonaceous Materials]

[0186] The carbonaceous materials prepared in Examples 1 to 8 and Comparative Examples 1 to 12 were filled in a water purification filter element with a diameter of 34 mm, a height of 67 mm, and an internal volume of 60 mL, and the filtration capacity test of trihalomethane and 2-MIB was carried out according to the household water purifier test method specified in JIS S 3201 (2010) and the following steps. In addition, for the carbonaceous materials of Example 1 and Comparative Example 1, the particle size was adjusted to 30 mesh (0.5 mm) to 60 mesh (0.25 mm) and then the test was carried out.

[0187] [Total trihalomethane filtration capacity test]

[0188] The water adjusted to chloroform concentration of 45±9 ppb, bromodichloromethane concentration of 30±6 ppb, dibromochloromethane concentration of 20±4 ppb, and bromoform concentration of 5±1 ppb was used as the test water and the mixture was stirred at 1 L / min and space velocity (SV) = 1000 hr. -1 Under the conditions of , the filtration capacity test was carried out with the point where the removal rate was less than 80% as the break point. In this test, the filtration capacity of 7.0 (L / mL) or more was considered qualified. The water flow test conditions and results are shown in Table 2.

[0189] [2-MIB filtering capability test]

[0190] The 2-MIB concentration was adjusted to 50±10 ppt as test water, and the mixture was stirred at 1 L / min and space velocity (SV) = 1000 hr. -1 Under the conditions of , the filtration capacity test was conducted with the point where the removal rate was less than 80% as the breaking point. In this test, the filtration capacity of 30.0 (L / mL) or more was considered qualified. The water flow test conditions and results are shown in Table 2.

[0191] Table 2

[0192]

[0193] (Inspection)

[0194] It is clear from the results in Table 2 that the carbonaceous materials according to the embodiments of the present invention can remove both trihalomethanes with small molecular size and 2-MIB with large molecular size.

[0195] In contrast, in Comparative Examples 1 to 12 in which at least one of the benzene adsorption amount, vitamin B12 adsorption amount and / or mesopore volume does not meet the requirements of the present invention, only either trihalomethane or 2-MIB can be removed, and both cannot be removed like the carbonaceous materials of the examples.

[0196] This application is based on Japanese patent application No. 2019-085514 filed on April 26, 2019, the contents of which are incorporated herein by reference.

[0197] In order to express the present invention, the present invention has been appropriately and fully described above by referring to specific examples and drawings, but it should be recognized that those skilled in the art can easily change and / or improve the aforementioned embodiments. Therefore, as long as the modified embodiments or improved embodiments implemented by those skilled in the art do not deviate from the protection scope of the claims recorded in the claims, the modified embodiments or improved embodiments can be interpreted as being included in the protection scope of the claims.

[0198] Industrial Applicability

[0199] The carbonaceous material of the present invention is particularly useful for removing substances to be removed as specified in the Household Product Quality Labeling Act. Therefore, the present invention has wide industrial applicability in water purification technologies such as water purification filters and water purifiers.

Claims

1. A carbonaceous material, characterized in that: The benzene adsorption capacity is 25-40%, the vitamin B12 adsorption capacity is 13.0-50.0 mg / g, and the pore volume of the mesopores obtained from the nitrogen adsorption isotherm by the BJH method is 0.070-0.150 cm 3 / g.

2. The carbonaceous material according to claim 1, characterized in that The specific surface area calculated by the BET method based on the nitrogen adsorption isotherm is 900-1500m 2 / g.

3. The carbonaceous material according to claim 1 or 2, characterized in that: The average pore diameter calculated from the nitrogen adsorption isotherm was 1.79 to 1.88 nm.

4. The carbonaceous material according to claim 1 or 2, characterized in that: The ratio of the pore volume of micropores calculated from the nitrogen adsorption isotherm by the MP method to the total pore volume calculated from the nitrogen adsorption amount at a relative pressure of P / P0=0.99 in the nitrogen adsorption isotherm is 96% or less.

5. The carbonaceous material according to claim 1 or 2, characterized in that: The electrical conductivity obtained by measuring the powder resistance under a load of 12 kN is 5 to 12 S / cm.

6. The carbonaceous material according to claim 1 or 2, characterized in that: The carbonaceous material is derived from a plant-based carbonaceous precursor.

7. The carbonaceous material according to claim 6, characterized in that The plant-based carbonaceous precursor is coconut shell.

8. A method for producing a carbonaceous material according to any one of claims 1 to 7, characterized in that A method for producing a carbonaceous material using a fluidized bed furnace, wherein: In addition to the fluidizing gas introduced from the furnace bed, an oxygen-containing gas is introduced into the fluidized bed furnace so that the oxygen concentration in the total gas of the fluidizing gas and the oxygen-containing gas becomes 0.004 to 1% by volume.

9. The method for producing a carbonaceous material according to claim 8, characterized in that: The water vapor concentration in the fluidizing gas introduced from the hearth is 10 to 40% by volume.

10. The method for producing a carbonaceous material according to claim 8 or 9, characterized in that: The fluidized bed furnace includes a gas dispersion portion on the upstream side of the fluidized bed furnace when viewed from the main flow direction Z of the fluidizing gas. When the upstream end position of the gas dispersion section in the direction Z is set to 0 in meters, the downstream end position is set to t1 in meters, and the position for introducing the oxygen-containing gas is set to t2 in meters, the oxygen-containing gas is introduced in a manner that satisfies the relationship of 0.5t1≤t2.

11. A water purification filter, characterized in that Include: The carbonaceous material according to any one of claims 1 to 7; and a fibrous binder, wherein The CSF value of the fibrous binder is 10 to 150 mL. The fibrous binder is contained in an amount of 4 to 10 parts by mass based on 100 parts by mass of the carbonaceous material.

12. A water purifier, characterized in that Comprising: the carbonaceous material according to any one of claims 1 to 7.

13. A water purifier, characterized in that It comprises: the water purification filter according to claim 11.

Citation Information

Patent Citations

  • Water treating filter material

    JP1996052347A

  • Active carbon fiber, manufacture method therefor, for cartridge water-cleaning device and water-cleaning device

    JP2003290654A

  • Active carbon molding, manufacturing method therefor, and water purifier using the molding

    JP2003334543A

  • Powdered activated carbon for removing musty odor

    JP2006282441A

  • Activated carbon for water purifier, and activated carbon cartridge using the same

    JP2013220413A