A processing technology for horizontal centrifuge spiral
The hardness and corrosion resistance of the horizontal spiral centrifuge spiral blades are improved through nickel-based alloy spray welding and fine processing technology, which solves the problem of incomplete separation of the screw conveyor at high speeds, extends the service life of the equipment and reduces jamming. Condition.
Patent Information
- Application Number
- CN202111023239.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-02
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-09-02
AI Technical Summary
When the screw conveyor of the horizontal screw centrifuge rotates at high speeds, due to the low hardness of the spiral blades and the small gap between the spiral blades and the inner wall of the drum, the material squeezes the spiral blades, resulting in incomplete or difficult separation.
Nickel-based alloy spray welding technology is used to improve the hardness and corrosion resistance of the spiral blades, and the gap between the spiral blades and the inner wall of the drum is reduced through fine machining and balancing, including shaping, grinding, spraying nickel-based alloy, and strengthening of the spiral blades. Rib welding and balancing.
It improves the hardness and corrosion resistance of the spiral blades, reduces material extrusion and incomplete separation, extends the service life of the equipment, and reduces the jamming of the screw conveyor during high-speed rotation.
Smart Images

Figure CN113751975B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of horizontal centrifuges, and in particular to a processing technology for a spiral of a horizontal centrifuge. Background Art
[0002] The horizontal spiral centrifuge is a spiral unloading sedimentation centrifuge. Its main function is to separate certain mixtures with different characteristics through centrifugal force, such as solid or liquid mixtures with large specific gravity differences or particle diameter differences. The spiral blades on the spiral pusher push the separated material A to the slag discharge port at the small end of the drum for discharge, and the separated material B overflows through the overflow hole at the large end of the drum.
[0003] See related technology Figure 1 A screw conveyor of a horizontal centrifuge includes a cylinder 1, which includes a large cylinder 11, a conical cylinder 12, and a small cylinder 13. The large cylinder 11, the conical cylinder 12, and the small cylinder 13 are coaxially arranged, one end of the large cylinder 11 is welded and fixed to the large end of the conical cylinder 12, and one end of the small cylinder 13 is welded and fixed to the small end of the conical cylinder 12. A spiral blade 2 is installed on the outside of the cylinder 1. The screw conveyor of the horizontal spiral centrifuge is mainly made of stainless steel and is directly used in normal production after annealing or solid solution treatment.
[0004] Regarding the above-mentioned related technologies, in recent years, with the expansion of product segmentation functions, the screw conveyor speed of the horizontal spiral centrifuge is relatively high, and the gap between the spiral blade and the inner wall of the drum is relatively small, and the spiral blade made of stainless steel has a relatively low hardness. During the separation process, there is a defect that material A squeezes the spiral blade, causing the spiral blade to deform, resulting in incomplete separation or difficulty in separating material A from material B. Summary of the invention
[0005] In order to improve the hardness and corrosion resistance of the spiral blades of the screw conveyor, the present application provides a processing technology for the spiral of a horizontal centrifuge.
[0006] The present application provides a horizontal centrifuge spiral processing technology using the following technical solutions:
[0007] A processing technology for a horizontal centrifuge spiral comprises the following steps:
[0008] S1. Cutting: Cutting the spiral blades and the cylinder;
[0009] S2. Pretreatment: Rough and fine turning of the cylinder, and calibration of the circumferential runout of the cylinder, repairing the center holes at both ends of the cylinder to make them coaxial; using a spiral blade forming fixture that matches the width of the spiral blade to bend the spiral blade;
[0010] S3, Line drawing: The staff draws the spiral blade position line on the cylinder according to the design drawing;
[0011] S4. Spiral blade welding: fix the spiral blade on the corresponding spiral blade position line, and weld the spiral blade to the cylinder by spot welding;
[0012] S5. Correction of spiral blades: Shape the spiral blades according to the designed dimensions, adjust the spacing and angle between two adjacent spiral blades along the length direction of the spiral conveyor; rough and fine turn the external dimensions of the spiral blades; grind the spiral blades with a grinder;
[0013] S6. Spray alloy on spiral blades: Spray nickel-based alloy on spiral blades. The thickness of the alloy within 10 mm close to the edge of the spiral blade can only be increased but not decreased.
[0014] S7, spiral blade grinding: grinding the spiral blade after alloy spraying according to the preset size;
[0015] S8. Balance calibration: Using the center holes at both ends as reference, use a balancing machine to perform rough and fine machining on the spiral blades respectively, so that the counterweights at both ends of the screw conveyor are within the design accuracy.
[0016] By adopting the above technical solution, the nickel-based alloy spray-welded deposit layer has good corrosion resistance, wear resistance, and sliding wear resistance. By spray-welding the nickel-based alloy, it is helpful to improve the hardness of the spiral blades, which helps to reduce the possibility of material A squeezing the spiral blades, causing the spiral blades to deform or damage. At the same time, it helps to improve the corrosion resistance of the spiral blades, which helps to increase the service life of the screw conveyor, and helps to reduce the possibility of incomplete separation of the separated materials A and B. At the same time, first calibrating the circular runout of the cylinder, then installing and fixing the spiral blades, and finally balancing the spiral conveyor, it helps to reduce the inconsistent gap between the spiral blades and the inner wall of the drum, which causes the screw conveyor to get stuck with the drum during high-speed rotation.
[0017] Preferably, S6-1: using Ni45 nickel-based alloy powder for spraying until the alloy thickness is 0.45 to 0.5 mm; S6-2: using Ni55 nickel-based alloy powder for covering the surface.
[0018] By adopting the above technical solution, the Ni45 nickel-based alloy powder spray welding has a lower melting point and is easier to adhere to the surface of the spiral blades, which helps to reduce the oxidation damage of the internal spiral blades caused by long-term use. The use of Ni55 nickel-based alloy powder helps to improve the structural strength of the spiral blades and the surface hardness of the spiral blades, thereby helping to reduce the high-speed rotating materials squeezing the spiral blades and causing the spiral blades to deform.
[0019] Preferably, in S6, the thickness of the Ni45 nickel-based alloy powder is 0.5 mm, and the overall thickness of the alloy layer is 2 mm.
[0020] By adopting the above technical solution, the spray welding thickness can be controlled, which helps to ensure the quality of the spray welding layer and reduce the situation where some areas are not covered with Ni55 nickel-based alloy after subsequent vehicle repairs. It also helps to reduce the uneven thickness of the spray welding layer in various parts of the spiral blade, which leads to a large range of circular run-out in various parts of the spiral blade, affecting the structural strength of various parts of the spiral blade after correction.
[0021] Preferably, in S4, a plurality of reinforcing ribs are welded between the spiral blades on the conical cylinder.
[0022] By adopting the above technical scheme, the reinforcing ribs help to improve the structural strength of the spiral blades on the small cylinder body and the conical cylinder, and at the same time help to reduce the possibility of the spiral blades on the small cylinder body bending and deviating toward the side being welded during the overall welding process, thereby helping to improve the positioning accuracy of the spiral blades on the cylinder body.
[0023] Preferably, the processing technology also includes: S8-1: rough balancing: using a balancing machine to perform rough balancing processing on the spiral blades until the counterweights at both ends of the entire screw conveyor are between 60 grams and 80 grams; S8-2: polishing: surface polishing treatment is performed on the semi-finished screw conveyor obtained by S8-1; S8-3: cleaning treatment: cleaning treatment is performed on the semi-finished screw conveyor obtained by S8-2; S8-4: fine balancing: using a balancing machine to perform fine balancing processing on the spiral blades until the counterweights at both ends of the entire screw conveyor are less than 10 grams.
[0024] By adopting the above technical solution, balancing the spiral blades with a balancing machine can help reduce the circular runout of the spiral blades at various locations, and help reduce the occurrence of the outer edge of the spiral blade getting stuck with the inner wall of the drum during the rotation of the screw conveyor in the drum.
[0025] Preferably, in S1, the spiral blade is cut by a plasma profiling cutter according to the edge shape of the spiral blade in a flattened state in the design.
[0026] By adopting the above technical solution and using a plasma profiling cutting machine to cut the spiral blades, it is helpful to improve the smoothness of the cutting surface of the spiral blades, improve the dimensional accuracy of the spiral blades, reduce the thermal deformation of the spiral blades, and help reduce the stress generated by cutting the spiral blades.
[0027] Preferably, in S5, the runout of each part of the cylinder is detected, and the cylinder is corrected by a lathe.
[0028] By adopting the above technical solution, the runout of various parts of the cylinder is reduced before installing the spiral blades, which helps to reduce the runout of the outer edge of the spiral blades after welding the spiral blades, helps to reduce the impact of the previous steps on the spiral blades, facilitates subsequent processing, and helps to improve the overall quality of the screw conveyor.
[0029] Preferably, in S5, the coaxiality of the center holes at both ends of the cylinder is less than or equal to 0.02 mm.
[0030] By adopting the above technical solution, the center holes at both ends of the cylinder are used as the positioning reference for subsequent detection and adjustment of the spiral blades. The higher the coaxiality of the center holes at both ends of the cylinder, the more convenient it is to perform balancing processing on the spiral blades, which helps to improve the overall quality of the screw conveyor.
[0031] In summary, the present application includes at least one of the following beneficial technical effects:
[0032] 1. By spraying a double layer of nickel-based alloy on the surface of the spiral blade, it helps to improve the hardness and corrosion resistance of the spiral blade, helps to increase the service life of the spiral blade, and helps to reduce the possibility of incomplete separation of the separated materials A and B;
[0033] 2. By controlling the thickness of the Ni45 nickel-based alloy layer and the Ni55 nickel-based alloy layer, it helps to reduce the oxidation damage of the internal spiral blades caused by long-term use of the spiral blades. At the same time, ensuring the surface hardness of the spiral blades helps to reduce the possibility of materials squeezing the spiral blades and causing the spiral blades to deform;
[0034] 3. Cutting the spiral blades by a plasma profiling cutting machine helps to improve the smoothness of the cutting surface of the spiral blades, improve the dimensional accuracy of the spiral blades, reduce the thermal deformation of the spiral blades, and help reduce the stress generated by cutting the spiral blades. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a cross-sectional view of the screw conveyor structure of the horizontal centrifuge mainly embodied in the embodiment of the present application.
[0036] Figure 2 This is a processing diagram of a horizontal centrifuge spiral according to an embodiment of the present application.
[0037] Figure numerals: 1, cylinder body; 11, large cylinder body; 12, conical cylinder; 13, small cylinder body; 2, spiral blades; 3, center hole. DETAILED DESCRIPTION
[0038] The following is combined with Figure 1-2 This application is described in further detail.
[0039] The embodiment of the present application discloses a processing technology for a horizontal centrifuge spiral, but the embodiments of the present invention are not limited thereto.
[0040] See also Figure 1 , Figure 2 The processing technology of the horizontal centrifuge spiral includes the following steps:
[0041] S1. Cutting:
[0042] S1-1: according to the edge shape of the spiral blade 2 in the flattened state in the design, a plasma profiling cutting machine is used to cut the spiral blade 2 blank;
[0043] S1-2: Cut the large barrel 11, the tapered barrel 12 and the small barrel 13 using a lathe, and the large barrel 11, the tapered barrel 12 and the small barrel 13 after cutting have machining allowances in the length and radial direction;
[0044] S2. Preprocessing:
[0045] S2-1: Rough and fine turning of the large barrel 11, the conical barrel 12 and the small barrel 13: In the process of rough and fine turning of the large barrel 11, due to the large mass of the large barrel 11, when turning the center hole 3 and the end surface of the large barrel 11, Figure 1 A center frame for supporting the large cylinder body 11 and the cylinder body 1 is respectively installed at the A point and the B point;
[0046] S2-2: Remove the center frame, repair the outer side surfaces of the supported positions at points A and B on the large cylinder body 11, and finish-turn the large cylinder body 11;
[0047] S2-3: Use an electric welder to weld and fix the large cylinder body 11, the conical cylinder 12 and the small cylinder body 13 respectively to form the cylinder body 1;
[0048] S2-4: Measuring cylinder 1 Figure 1 The circular runouts at the five positions of A, B, C, D, and E in the welding process are measured and marked with steel stamps as the calibration reference for the spiral blade 2 after welding; the cylinder 1 is repaired to make the circular runout of point A less than or equal to 0.05 mm, the circular runout of point B less than or equal to 0.05 mm, the circular runout of point C less than or equal to 0.3 mm, the circular runout of point D less than or equal to 0.4 mm, and the circular runout of point E less than or equal to 0.25 mm; the outer side surfaces of the supported positions of points A and B on the large cylinder 11 are re-machined;
[0049] S2-5: Repair the center holes 3 at both ends of the cylinder 1, so that the coaxiality of the center holes 3 at both ends is less than or equal to 0.02 mm, which serves as a processing reference for the spiral blades 2 after welding;
[0050] S2-6: Use a grinder to remove burrs on the opening edge of the spiral blade 2;
[0051] S2-7: using a spiral blade 2 forming fixture that matches the width of the spiral blade 2 to bend the spiral blade 2 until the spiral blade 2 is formed into a desired shape of the product;
[0052] S3, drawing lines: the staff draws the position lines of the spiral blades 2 on the cylinder 1 according to the design drawings;
[0053] S4. Blade welding:
[0054] S4-1: According to the drawn line position, the spiral blade 2 and the cylinder 1 are fixedly connected by argon arc spot welding using an electric welder. The spiral angle of the spiral blade 2 refers to the design drawing;
[0055] S4-2: Weld 3 to 4 reinforcing ribs between the spiral blades 2 adjacent to each other along the length direction of the cylinder body 1 on the conical cylinder 12;
[0056] S4-3: Weld all the welds between the spiral blade 2 and the cylinder 1 with an electric welder;
[0057] S4-4: Clean the welding slag on the weld and grind the weld.
[0058] S5. Blade correction:
[0059] S5-1: Use a hammer to shape the blade pitch and angle between the spiral blades 2 according to the design dimensions to eliminate welding stress;
[0060] S5-2: Using the center holes 3 at both ends as reference, use a lathe to detect and correct the circular runout of the spiral blade 2 at five points A, B, C, D, and E along the length direction of the screw conveyor, so that the circular runout of point A is less than or equal to 0.2 mm, the circular runout of point B is less than or equal to 0.4 mm, the circular runout of point C is less than or equal to 0.2 mm, the circular runout of point D is less than or equal to 0.6 mm, and the circular runout of point E is less than or equal to 0.6 mm, record the detection data, and correct the excess part of the spiral blade 2;
[0061] S5-3: Rough and fine turning of spiral blade 2, leaving a single-side grinding allowance of 0.08 mm;
[0062] S5-4; using a grinder to remove the burrs generated by turning the spiral blade 2;
[0063] S6. Blade alloy spraying: preheat the screw conveyor to between 300 degrees Celsius and 350 degrees Celsius;
[0064] S6-1: Use a metal powder spray welding gun to spray Ni45 nickel-based alloy powder to an alloy thickness of 0.45 to 0.5 mm;
[0065] S6-2: Use a metal powder spray welding gun to cover the Ni55 nickel-based alloy powder to a total alloy thickness of 2 mm;
[0066] The alloy thickness within 10 mm near the edge of spiral blade 2 can only be increased but not decreased;
[0067] S6-3: After spray welding, place the screw conveyor in an insulation box for more than 24 hours;
[0068] S7, blade grinding: grinding the spiral blade 2 after the alloy is sprayed according to the preset size;
[0069] S8, balance check: recheck and correct the circular runout of the spiral blade 2 at five points A, B, C, D, and E along the length direction of the spiral conveyor, ensuring that the circular runout of point A is less than or equal to 0.2 mm, the circular runout of point B is less than or equal to 0.4 mm, the circular runout of point C is less than or equal to 0.2 mm, the circular runout of point D is less than or equal to 0.6 mm, and the circular runout of point E is less than or equal to 0.6 mm;
[0070] S8-1: Rough balancing: Use a balancing machine to perform rough balancing on the screw conveyor until the weight at both ends of the entire screw conveyor is between 60 grams and 80 grams;
[0071] S8-2: Grinding: Grinding the surface of the semi-finished screw conveyor obtained in S8-1;
[0072] S8-3: Cleaning: Cleaning the semi-finished screw conveyor obtained in S8-2;
[0073] S8-4: Fine balancing: Use a balancing machine to finely balance the screw conveyor until the weight at both ends of the entire screw conveyor is less than 10 grams, and record the specific value;
[0074] S9. Completion inspection.
[0075] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A processing technology for a horizontal centrifuge spiral, characterized in that: The following steps are involved: S1, unloading: unloading the spiral blade (2) and the cylinder (1); S2, pretreatment: rough and fine turning of the cylinder (1), and checking the circumferential runout of the cylinder (1), repairing the center holes (3) at both ends of the cylinder (1), so that the center holes (3) at both ends are coaxial; using a spiral blade (2) forming fixture that matches the width of the spiral blade (2) to bend the spiral blade (2); S3, drawing lines: the staff draws the position lines of the spiral blades (2) on the cylinder (1) according to the design drawings; S4, blade welding: fixing the spiral blade (2) on the corresponding spiral blade (2) position line, and welding the spiral blade (2) to the cylinder (1) by spot welding; S5, blade correction: shaping the spiral blade (2) according to the designed size, adjusting the distance and angle between two adjacent spiral blades (2) along the length direction of the spiral conveyor; roughing and fine turning the outer dimensions of the spiral blade (2); grinding the spiral blade (2) using a grinder; S5-1: Using a hammer to shape the blade pitch and angle between the spiral blades (2) according to the designed dimensions to eliminate welding stress; S5-2: Using the center holes (3) at both ends as reference, use a lathe to detect and correct the circular runout of the spiral blade (2) at five points A, B, C, D, and E along the length direction of the spiral conveyor, so that the circular runout at point A is less than or equal to 0.2 mm, the circular runout at point B is less than or equal to 0.4 mm, the circular runout at point C is less than or equal to 0.2 mm, the circular runout at point D is less than or equal to 0.6 mm, and the circular runout at point E is less than or equal to 0.6 mm, record the detection data, and correct the excess part of the spiral blade (2); S5-3: Rough and fine turning of the spiral blade (2), leaving a single-side grinding allowance of 0.08 mm; S5-4; using a grinder to remove the burrs generated by turning the spiral blade (2); S6. Blade alloy spraying: Spray the nickel-based alloy onto the spiral blade (2). The thickness of the alloy within 10 mm close to the edge of the spiral blade (2) can only be increased but not decreased. S7, blade grinding: grinding the spiral blade (2) after the alloy is sprayed according to a preset size; S8, balancing: using the center holes (3) at both ends as reference, use a balancing machine to perform rough and fine processing on the spiral blades (2) respectively, so that the counterweights at both ends of the screw conveyor are within the design accuracy; S8-1: Rough balancing: Use a balancing machine to perform rough balancing on the spiral blade (2) until the weight at both ends of the entire spiral conveyor is between 60 grams and 80 grams; S8-2: Grinding: Grinding the surface of the semi-finished screw conveyor obtained in S8-1; S8-3: Cleaning: Cleaning the semi-finished screw conveyor obtained in S8-2; S8-4: Use a balancing machine to finely balance the screw conveyor until the weight at both ends of the entire screw conveyor is less than 10 grams, and record the specific value.
2. The processing technology of a horizontal centrifuge spiral according to claim 1, characterized in that: The process also includes: S6-1: Use Ni45 nickel-based alloy powder to spray until the alloy thickness is 0.45 to 0.5 mm; S6-2: Use Ni55 nickel-based alloy powder to cover the surface.
3. The processing technology of a horizontal centrifuge spiral according to claim 2, characterized in that: In S6, the thickness of Ni45 nickel-based alloy powder is 0.5 mm, and the overall thickness of the alloy layer is 2 mm.
4. The processing technology of a horizontal centrifuge spiral according to claim 1, characterized in that: In S4, a plurality of reinforcing ribs are welded between the spiral blades (2) on the conical cylinder (12).
5. The processing technology of a horizontal centrifuge spiral according to claim 1, characterized in that: In S1, according to the edge shape of the spiral blade (2) in the flattened state in the design, the spiral blade (2) is cut using a plasma profiling cutting machine.
6. The processing technology of a horizontal centrifuge spiral according to claim 1, characterized in that: In S5, the runout of the cylinder (1) at various locations is detected, and the cylinder (1) is corrected by a lathe.
7. The processing technology of a horizontal centrifuge spiral according to claim 6, characterized in that: In S5, the coaxiality of the center holes (3) at both ends of the cylinder (1) is less than or equal to 0.02 mm.
Citation Information
Patent Citations
Process for assembling and welding ultralong hollow shafting auger flight
CN101412156A
High-intensity wear-resistant and corrosion-resistant spiral discharging sedimentation centrifuge and manufacturing process therefore
CN102861677A
Large-sized circulating pump impeller forming method through swing welding
CN103394880A
Manufacturing process for centrifugal water extractor rotor body
CN104084772A
Processing and manufacturing method of high-speed blower impeller
CN106826140A