Optoelectronic devices

By cleaning the mesa structure of the optoelectronic device and forming a Group III oxide termination oxide layer, the non-radiative recombination and leakage current problems caused by the natural oxide layer are solved, and the efficiency and life of the optoelectronic device are improved.

CN113826220BActive Publication Date: 2024-11-19COMPTEK SOLUTIONS OY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080029334.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-05
Filing Date
2020-05-29
Publication Date
2024-11-19
Estimated Expiration
2040-05-29

AI Technical Summary

Technical Problem

During the manufacturing process, existing optoelectronic devices have problems with non-radiative recombination and leakage current caused by natural oxide layers, which affects the efficiency and life of the device.

Method used

By cleaning the mesa structure surface of the optoelectronic device, at least 75% of the natural oxide is removed and a group III oxide-based termination oxide layer is formed thereon to improve interface quality and passivation performance.

Benefits of technology

It effectively suppresses non-radiative recombination, improves the internal quantum efficiency and carrier life of optoelectronic devices, and extends the operating life of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113826220B_ABST
    Figure CN113826220B_ABST
Patent Text Reader

Abstract

The present invention relates to an optoelectronic device (100, 200, 250, 260, 300), which comprises a substrate layer (110, 210, 310, 107) having a first surface plane (112, 212, 105) and a second plane (214) opposite to and parallel to the first surface plane. The device also comprises a mesa structure (120, 220, 320, 820, 103, 123, 133) arranged on the first surface plane of the substrate layer. The mesa structure comprises at least one layer of III-V semiconductor material; the first surface (101, 131) forms an angle α with the first surface plane of the substrate layer, wherein the angle α is between 0° and 180°. The device also comprises a first type of first termination oxide layer (130, 230, 330) arranged on the first surface of the mesa structure, and before the first type of first termination oxide layer is arranged, the first surface of the mesa structure has been cleaned and at least 75% of the native oxide on the first surface has been removed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an optoelectronic device and a method for manufacturing the optoelectronic device. The optoelectronic device comprises a mesa structure.

[0002] background

[0003] Optoelectronic devices such as lasers, light-emitting diodes, detectors and photovoltaic devices are usually composed of epitaxially grown semiconductor heterostructures, including quantum well structures and structures based more precisely on compound semiconductor materials. Group III-V compound semiconductors are a typical example of compound semiconductor materials, which are obtained by combining group III elements (mainly Al, Ga, In) with group V elements (mainly N, P, As, Sb). In optoelectronic devices, heterostructures are obtained by epitaxially growing a given semiconductor material on top of another given semiconductor material. In addition, by using epitaxial growth manufacturing technology, group III-V semiconductors can manufacture quantum wells and stacked structures similar to them, such as diode (LED) structures for realizing light emission. Specifically, in semiconductors, quantum wells are formed by sandwiching materials such as indium gallium nitride (InGaN) between two layers of materials with a wider bandgap, such as gallium nitride (GaN). There are other possible material combinations that can form quantum wells, including indium gallium aluminum phosphide (InGaAlP) layers sandwiched between two layers of indium gallium aluminum phosphide with a higher aluminum concentration. These structures can be generated by processes such as molecular beam epitaxy (MBE) or metal organic chemical vapor deposition (MOCVD). In addition, epitaxially grown III-V compound semiconductor structures can be formed into mesa structures by vertically etching semiconductor layers using photolithography techniques known in the art. A mesa structure is a multilayer semiconductor structure with surface planes and inclined sides formed on top of a substrate layer.

[0004] As an example of an optoelectronic device, in a light emitting device, photon generation occurs during the recombination of carriers that are confined between potential energy barriers caused by energy band discontinuities. The wavelength of the photon depends on the energy difference between the conduction band minimum and the valence band maximum corresponding to the quantum well; i.e., the band gap energy. Similarly, in a photon detector, photon detection occurs when a photon (with energy above the band gap energy of the active region) is absorbed to generate an electron-hole pair, which is then collected by a voltage difference applied across the device.

[0005] Generally, in optoelectronic devices, especially light-emitting devices, it is necessary to efficiently inject current into the active quantum well region of the optoelectronic device. Micro-LED devices are a typical example, and driving micro-LED-based displays at low injection current levels will result in poor device efficiency. In general, it is desirable to transfer as high a percentage of the injected current as possible to the light generation in the active region of the device, so that the injected electrons recombine with holes and generate photons as much as possible. This is defined as the internal quantum efficiency (IQE) of the LED.

[0006] The reasons for the low efficiency are mainly due to the following factors: (i) Shockley-Read-Hall (SRH) recombination of electrons / holes; (ii) Auger recombination; (iii) electron overflow from the quantum well. It is worth noting that when the device is operated at low current density, the main reason for the decrease in IQE is the non-radiative Shockley-Read-Hall recombination in defect states, which in turn reduces the generation and output of light. In addition, this recombination process generates excessive heat, which reduces the operating life of the optoelectronic device.

[0007] In micro-LED devices, the specific surface area of ​​the LED increases as the size decreases, so the surface quality of the material will determine the final performance of the device. That is, due to the micro-LED mesa structure processed using etching and lithography techniques, the mesa sidewalls will produce a high density of atomic-level defects and disordered structures, which are the source of defect states, non-radiative Shockley-Read-Hall (SRH) recombination and leakage current. It is worth noting that in the example of micro-LED-based display devices, since the charge carrier diffusion length can be comparable to the micro-LED size and pixel pitch, the impact of defective sidewalls can extend to a long distance and affect the performance of the entire chip.

[0008] For typical compound semiconductor optoelectronic devices, the inherent source of high-density defects is the uncontrolled oxidation of III-V materials. Compound semiconductor oxides are characterized by atomic bond disorder, bond breaks (dangling bonds), and mixed III and V oxides. This nanometer-thick oxide layer is prone to produce a high density of electrically active defect states in the band gap of semiconductor materials. In particular, group V oxides are more prone to high-density defect states. This harmful oxide is easily formed during the processing of optoelectronic devices. In particular, during the manufacturing process of Micro-LED device mesas, the mesa surface will be oxidized after the mesa structure is formed using photolithography and etching techniques.

[0009] Currently known semiconductor production equipment solves the above problems when manufacturing optoelectronic devices by adopting some known technologies. One of the technologies is to chemically clean and passivate the mesa sidewall surface when manufacturing optoelectronic devices. This chemical passivation can be based on ammonium sulfide passivation or SU-8 passivation. However, the problem with this passivation is that it is unstable and easily oxidized. Another technology is to use atomic layer deposition (ALD), sputtering or plasma enhanced chemical vapor deposition (PECVD) and other technologies to deposit a metal oxide outer coating (such as Al 2 O 3 、SiO 2 ) is deposited onto the mesa sidewalls. These methods for fabricating optoelectronic devices produce a poor quality interfacial oxide layer and associated defects because the overcoat material contains oxygen and chemical cleaning is often insufficient to remove the oxide, especially in aluminum-containing compound semiconductor materials.

[0010] Therefore, in light of the foregoing discussion, there exists a need to address the shortcomings associated with conventional semiconductor devices and conventional manufacturing techniques.

[0011] Therefore, the present invention aims to provide a solution to the existing poor quality optoelectronic device mesas with native oxide layers and the associated non-radiative recombination and leakage current problems. The purpose of the present invention is to provide a solution that at least partially solves the problems encountered in the prior art and provides an economical, easy to implement and sophisticated optoelectronic device. Summary of the invention

[0012] The present invention is directed to a photovoltaic device and a method for manufacturing the photovoltaic device.

[0013] The present disclosure provides a photoelectric device, which includes a substrate layer having a first surface plane and a second surface plane opposite to and parallel to the first surface plane. The photoelectric device also includes a mesa structure arranged on the first surface plane of the substrate layer. The mesa structure includes at least one layer of group III-V material and a first surface arranged at an angle α relative to the first surface plane of the substrate layer, and the angle is between 0° and 180°. The device also includes a first termination oxide layer of a first type arranged on the first surface of the mesa structure, and before the first termination oxide layer of the first type is arranged, the first surface of the mesa structure has been cleaned and at least 75% of the native oxide on the first surface of the mesa structure has been removed.

[0014] The present invention also provides a method for manufacturing an optoelectronic device, the method comprising:

[0015] - obtaining a mesa structure arranged on a first surface plane of the substrate layer, the mesa structure comprising at least one layer of group III-V material and a first surface at an angle α relative to the surface plane of the substrate layer, wherein the angle α is between 0° and 180°,

[0016] - cleaning the first surface of the mesa structure by removing at least 75% of the native oxide on the first surface of the mesa structure,

[0017] - forming a first termination oxide layer of a first type on the first surface of the mesa structure.

[0018] BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The above summary and the detailed description of the following illustrative embodiments can be better understood in conjunction with the accompanying drawings. In order to demonstrate the present invention, exemplary configurations of the present invention are provided in the accompanying drawings. However, the present invention also discloses specific methods and devices. In addition, those skilled in the art will recognize that the drawings are not drawn to scale. Where possible, the same elements are represented by the same numbers.

[0020] Embodiments of the present invention will now be described, by way of example only, with reference to the following drawings, in which:

[0021] Figure 1A and 1B Schematic diagram of a photovoltaic device according to a first embodiment of the present invention.

[0022] Figure 2A , 2B 2C is a schematic diagram of a photovoltaic device according to a second embodiment of the present invention.

[0023] Figure 3A Schematic diagram of an optoelectronic device with native oxide on the surface of a mesa structure.

[0024] Figure 3B Schematic diagram of an optoelectronic device with an overcoat on top of a native oxide.

[0025] Figure 3C Schematic diagram of a photovoltaic device with a termination oxide layer according to a third embodiment of the present invention.

[0026] Figure 3D FIG. 4 is a schematic diagram of a photovoltaic device having a termination oxide layer and a dielectric cap layer according to a fourth embodiment of the present invention.

[0027] Figure 4 Schematic diagram of the process flow of the fifth embodiment of the present invention.

[0028] Figure 5 Schematic diagram of processing equipment according to the sixth embodiment of the present invention.

[0029] Figure 6 The carrier lifetime decay curves of the micro LED device with native oxide and the micro LED device processed by the seventh embodiment of the present invention are measured by time-correlated single photon counting.

[0030] Figure 7 1 and 2 are the photoluminescence spectra of a typical micro LED device with a natural oxide layer that has not been passivated, a micro LED device passivated using the prior art, and a micro LED device processed according to the eighth embodiment of the present invention.

[0031] Figure 8 FIG. 4 is a schematic diagram of a vertical cavity surface emitting laser diode according to a ninth embodiment of the present invention.

[0032] Fig. 9A This is the reflection high-energy electron diffraction pattern of the cleaned InGaAlP material surface.

[0033] Fig. 9B This is a reflection high energy electron diffraction pattern of the surface of the passivated InGaAlP material according to the tenth embodiment of the present invention.

[0034] Fig. 10A X-ray photoelectron spectrum of Ga2p on a micro-LED device with a native oxide layer on a mesa surface.

[0035] Fig. 10B This is the X-ray photoelectron spectrum of Ga2p on the micro LED device with a termination oxide layer according to the eleventh embodiment of the present invention.

[0036] Fig. 10C X-ray photoelectron spectrum of P2P on a micro-LED device with a native oxide layer on a mesa surface.

[0037] Fig. 10D FIG. 1 is an X-ray photoelectron spectrum of P2P on a micro LED device with a termination oxide layer according to the twelfth embodiment of the present invention.

[0038] Fig.11 FIG. 1 is a schematic diagram of a photoelectric device according to a thirteenth embodiment of the present invention.

[0039] Fig.12 Schematic diagram of a photoelectric device according to a fourteenth embodiment of the present invention.

[0040] Fig.13 Schematic diagram of a photoelectric device according to a fifteenth embodiment of the present invention.

[0041] In the drawings, underlined numbers are used to indicate the item in which the underlined number is located or the item adjacent to the underlined number. Non-underlined numbers are associated with the item identified by the row, linking the non-underlined number to the item. DETAILED DESCRIPTION

[0042] The following describes in detail the embodiments of the present invention and their implementation. Although some specific embodiments of the present invention have been disclosed, it will be appreciated by those skilled in the art that other embodiments for practicing the present invention are also feasible.

[0043] The present invention provides a photovoltaic device, which includes a substrate layer having a first surface plane and a second surface plane opposite to and parallel to the first surface plane. The photovoltaic device also includes a mesa structure arranged on the first surface plane of the substrate layer. The mesa structure includes at least one layer of III-V group material and a first surface arranged at an angle α relative to the first surface plane of the substrate layer, and the angle is between 0° and 180°. The device also includes a first termination oxide layer of a first type arranged on the first surface of the mesa structure, and before the first termination oxide layer of the first type is arranged, the first surface of the mesa structure has been cleaned and at least 75% of the native oxide on the first surface of the mesa structure has been removed.

[0044] The present invention also provides a method for manufacturing an optoelectronic device, the method comprising:

[0045] - obtaining a mesa structure arranged on a first surface plane of the substrate layer, the mesa structure comprising at least one layer of a III-V material and a first surface at an angle α relative to the surface plane of the substrate layer, wherein the angle α is between 0° and 180°;

[0046] - cleaning the first surface of the mesa structure by removing at least 75% of the native oxide on the first surface of the mesa structure;

[0047] - forming a first termination oxide layer of a first type on the first surface of the mesa structure.

[0048] Therefore, the present invention provides a new method for passivating optoelectronic semiconductor devices by generating a termination oxide layer on the surface of an optoelectronic device mesa structure. Compared with a native oxide layer or an oxide layer formed or deposited by other methods known to date, this termination oxide layer can well improve the physical and electrical properties of the optoelectronic device. Because this termination oxide layer provides beneficial passivation properties, it suppresses non-radiative recombination at the surface of the mesa structure and improves the interface quality for subsequent dielectric overcoat deposition. Therefore, this termination oxide layer improves carrier confinement within the mesa structure formed by the stacking of multiple semiconductor layers by increasing the energy barrier of the optoelectronic device.

[0049] In the optoelectronic device, before arranging the first termination oxide layer of the first type, the first surface of the mesa structure has been cleaned and at least 75% of the native oxide on the first surface of the mesa structure has been removed. The electrical properties of the native oxide are very low, so their presence will reduce the performance of the optoelectronic device. In addition, in the final product, at least the main native oxide has been removed before the termination oxide layer is formed. In fact, the structure of the termination oxide layer is ordered, so the ordered arrangement of the oxide of the termination oxide layer at the interface between the first surface of the mesa structure and the first termination oxide layer can prove that the mesa structure has been cleaned before it forms the first termination oxide layer. For example, the structure can be analyzed by using a transmission electron microscope (TEM) or an X-ray photoelectron spectroscopy (XPS). The difference between the uncleaned and cleaned mesa structure surfaces on the final product is also given in Figure 3, which will be described in more detail below.

[0050] It should also be noted that the conversion or formation rate of the first stop oxide layer is generally not 100%, even if at least 75% of the native oxide has been removed, and not all of the removed native oxide locations need to be covered by the stop oxide layer. For example, the conversion rate of the stop oxide can be 50%. In addition, the conversion rate of the stop oxide can be affected intentionally or unintentionally. An example of intentionally reducing the conversion rate is masking or covering certain areas after removing the native oxide and before forming the stop oxide layer to prevent further changes to the underlying areas. An example of unintentionally reducing the conversion rate is the presence of contamination, which prevents the formation of the stop oxide layer.

[0051] In this specification, the term "type" has been used in connection with the termination oxide layer. The term "type" refers to the nature of the termination oxide layer, i.e. its composition. The various termination oxide layers used may be the same or different from each other, as explained in more detail below. The type of the termination oxide layer is determined by the semiconductor layer in which it is located.

[0052] Optoelectronic devices may refer to devices that emit photons or are capable of detecting photons. Such optoelectronic devices may be light emitting diodes (LEDs), micro-LEDs, laser diodes, photovoltaic solar cells, and photodetectors. In the present invention, optoelectronic devices may also be part of an LED matrix, a photodetector matrix, or a multi-junction solar cell. Optoelectronic devices are therefore semiconductor devices.

[0053] The optoelectronic device includes a mesa structure arranged on top of a substrate layer having a surface plane. The mesa structure refers to an isolated semiconductor stack and contains at least one layer of III-V material. Each isolated semiconductor stack is used as an optoelectronic component of the optoelectronic device. For example, optoelectronic devices such as lasers, light-emitting diodes, detectors and photovoltaic devices can be composed of semiconductor heterostructures including active layers such as quantum well structures, more precisely, structures based on compound semiconductor materials. The semiconductor heterostructure is generally grown on top of the substrate layer by epitaxial growth. Among them, GaAs wafer is an example of a substrate layer. Another example of a substrate layer is a III-V layer epitaxially grown on a wafer. The surface plane of the substrate layer refers to, for example, the (001) plane (in the case of GaAs or a III-V layer epitaxially grown on a wafer) or the (0001) plane (in the case of GaN).

[0054] The mesa structure (i.e., an isolated semiconductor stack) includes a first surface arranged at an angle α relative to a first surface plane of a substrate layer. The angle between the surface plane and the first surface can be 30-90 degrees. The first surface is a surface surrounding the side of the mesa structure, i.e., an inclined portion. According to an embodiment, the mesa structure also includes a second surface parallel to the first surface plane of the substrate layer. The second surface is the surface layer of the mesa structure farthest from the substrate. The surface layer refers to at least the first atomic layer of the structure.

[0055] The first surface is arranged at an angle α relative to the substrate layer first surface plane, wherein the angle is between 0° and 180°. According to an embodiment, the angle α is 30-90 degrees. Thus, the angle α can be from 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 105, 110, 115, 120, 125, 130, 135, 140, 145, 150, 155, 160, 165 or 170 degrees to 15, 20, 25, 30, 35, 40, 45, 50, 60, 65, 70, 75, 80, 85, 90, 95, 100, 105, 110, 115, 120, 125, 130, 135, 140, 145, 150, 155, 160, 165 or 175 degrees.

[0056] According to one embodiment, the optoelectronic device further comprises an outer coating on the outermost termination oxide layer. The function of such an outer coating may be to protect the termination oxide layer and the rest of the device. The outer coating may also be used to change the refractive index of the outer surface or to act as an anti-reflective coating or a high-reflective coating. Thus, the outer coating may have different thicknesses at different locations and may include spikes.

[0057] Furthermore, the overcoat layer may be disposed on only a portion of the surface of the optoelectronic device. In practice, when used, it is most often used to protect the termination oxide layer, but it may also be used to protect the remainder of the optoelectronic device. The overcoat layer may thus be discontinuous, and it may be made along a certain pattern.

[0058] The optoelectronic device further comprises a first termination oxide layer of a first type disposed on the first surface of the mesa structure. In another embodiment, a second termination oxide layer of a second type is disposed on the second surface of the mesa structure.

[0059] The first termination oxide layer surrounds the mesa structure, i.e., the side of the mesa structure. The first termination oxide layer is of the first type. The first type is preferably a termination oxide layer in which group III oxides account for the majority. Group III oxides account for the majority means that at least or more than 50% of the total oxides at the surface are group III oxides. It is worth noting that group V oxides and their associated atomic bonds tend to produce high-density defect states in the band gap of the semiconductor, so the surface oxide is intentionally arranged as group III oxides. In addition, the first termination oxide layer formed by the method of the present invention preferably exhibits a thickness of less than 10 nm. According to an embodiment, the composition (e.g., the percentage level) and thickness of the first termination oxide layer depend on the material present on the sidewall of the mesa (i.e., the first surface).

[0060] When the second termination oxide layer is present, it is disposed on the second surface of the mesa structure. The second termination oxide layer is of a second type. In one embodiment, the second type is different from the first type. In another embodiment, the second type may be the same as the first type. The second termination oxide layer is preferably homogeneous in composition and thickness. In an alternative embodiment, the second termination oxide layer is a crystalline termination oxide layer.

[0061] Thus, according to one embodiment, at least 50% of the total oxides of the first termination oxide layer are group III oxides. According to another embodiment, at least 50% of the total oxides of the second termination oxide layer are group III oxides. Thus, both the first and second termination oxide layers or either of the first and second termination oxide layers may be formed primarily of group III oxides.

[0062] The mesa structure may be in any form, i.e., when viewed from above (perpendicular to the first surface of the substrate layer), the mesa structure may be square, rectangular, circular or elliptical, or any other suitable form. When viewed from the side, the mesa structure may have a linear form, a nonlinear form, a combination of linear forms with different angles relative to the first substrate plane, a combination of nonlinear forms, or a combination of linear and nonlinear forms.

[0063] In embodiments where the optoelectronic device includes a plurality of mesa structures (e.g., 2-10 or 10-50 or 50-100 mesa structures), it is preferred to arrange the mesa structures regularly, or according to a regular pattern (e.g., in a circle, the mesa structures closer to the center of the circle are closer to each other than the mesa structures in the outer circle). The distance between adjacent mesa structures is expressed as the distance between adjacent centers of the mesa structures. The distance between the centers of two adjacent mesa structures may be, for example, 2-500 μm. The distance may be 2, 4, 6, 10, 15, 20, 25, 30, 35, 40, 45, 50, 60, 70, 80, 90, 100, 120, 150, 200, 250, 300 or 350 μm to 10, 15, 20, 25, 30, 35, 40, 45, 50, 60, 70, 80, 90, 100, 120, 150, 200, 250, 300, 350, 400, 450, 500 μm. In one embodiment, the optoelectronic device includes a plurality of mesa structures, wherein the angle α is greater than 0° and less than 180°, and the center distance between two adjacent mesa structures is 2-500 μm.

[0064] According to another embodiment, when the optoelectronic device includes a plurality of mesa structures, a third termination oxide layer of the third type is arranged on the surface between two adjacent mesa structures. The third type of termination oxide layer may be the same as one of the first or optional second termination oxide layer, or it may be the same as both the first and optional second termination oxide layers, or it may be different from both the first and optional second termination oxide layers. And it is also possible that only the first and third termination oxide layers exist without the second termination oxide layer. The third type of termination oxide layer may also be a group III oxide of at least 50% of the total oxide. In this case, it is best to clean the surface before forming the third termination oxide layer, by removing at least 75% of the native oxide on its surface to form the third termination oxide layer.

[0065] Therefore, the first, optional second and optional third termination oxide layers should contain at least 50% of group III oxide, and when there are multiple termination oxide layers, the content of group III oxide can be independently selected according to the needs of each termination oxide layer. According to one embodiment, the content of group III oxide is at least 50, 55, 60, 65, 70, 75, 80, 85, 90 or 95%.

[0066] According to another embodiment, the first, optional second and optional third termination oxide layers may further independently contain a certain amount of group V oxide, such as 20% of the total oxide. Alternatively, the amount of group V oxide is greater than 0% but below its detection limit (typically 0.1% or 1%). Therefore, the amount of group V oxide may be 0.1, 0.5, 1, 1.5, 2, 5, 10, 15 or 20%. The amount of group V oxide may also be as high as 50%.

[0067] Thus, according to one embodiment, the first, optional second and optional third termination oxide layers independently of each other contain at least 50% of Group III oxides and more than 0% of Group V oxides.

[0068] In one embodiment, the optoelectronic device can be a micro LED device. In fact, the optoelectronic device can also be a micro light emitting diode, where the mesa footprint on the substrate layer is 1-250000 μm 2 The area can be 1, 10, 100, 500, 1000, 1500, 2000, 5000, 10000, 10500, 15000, 20000, 50000, 100000 or 150000 μm 2 to 500, 1000, 1500, 2000, 5000, 10000, 10500, 15000, 20000, 50000, 100000, 150000, 200000 or 250000 μm 2 .

[0069] The mesa coverage area on the base layer is defined as the parallel projection of the mesa structure (ie, a single mesa structure) on the first surface plane of the base layer. The base layer in this specification represents the device portion not covered by the mesa structure.

[0070] The term "micro" as used herein refers to the descriptive size of the device, and in some embodiments may refer to the lateral dimensions of individual components ranging from 1 μm to 500 μm. Defects and associated non-radiative recombination centers are characteristic of the mesa structure of typical micro-LED devices, which allow injected charge carriers to create optical dead zones around the micro-LED device, reducing overall efficiency. The present application avoids this problem due to the characteristics of the termination oxide layer.

[0071] Micro-LED devices can indeed transform the micro-LED mesa surface and its sidewall surface into a termination oxide layer with a smaller number of defects and fewer non-radiative recombination and carrier leakage characteristics through passivation.

[0072] In another embodiment, the optoelectronic device is a vertical cavity surface emitting laser (VCSEL), and its lateral size can be selected to be as small as 1 μm. The optoelectronic device can indeed be a vertical cavity surface emitting laser, wherein the area of ​​the terrace on the substrate layer is 1-250000 μm 2 For example, the area of ​​the terrace may be 1, 10, 100, 500, 1000, 1500, 2000, 5000, 10000, 10500, 15000, 20000, 50000, 100000 or 150000 μm. 2 , to 500, 1000, 1500, 2000, 5000, 10000, 15000, 20000, 50000, 100000, 150000, 200000 or 250000 μm 2 . The mesa structure of a vertical cavity surface emitting laser may have a plurality of aluminum-containing III-V group layers (such as AlGaAs and AlAs layers). The aluminum-containing layer may be protected from environmental influences in the vertical direction by arranging one or more surface passivation layers thereon, wherein the surface passivation layer and the termination oxide layer are provided. It is known that the aluminum-containing layer of a vertical cavity surface emitting laser is usually easily exposed to the environment on the side surfaces of the mesa structure, especially after the wafer has been cut into individual dies. The natural oxidation that occurs in the aluminum-containing oxide layer is uncontrolled, and the thickness of the natural oxide layer increases from the edge of the aluminum-containing layer inward, and eventually even reaches the active layer of the vertical cavity surface emitting laser, thereby reducing performance or even preventing operation. The vertical cavity surface emitting laser is usually installed in a sealed package, which is relatively expensive and may be relatively bulky. Due to the use of the first and optional second termination oxide layers, the present invention avoids the problem of packaging.

[0073] In another embodiment, the optoelectronic device is a photodetector. In fact, the optoelectronic device can be a photodetector in which a mesa has an area of ​​1 μm on the substrate. 2 To 100μm 2 For example, the area can be 1, 5, 50, 100, 250, 500, 700, 1000 μm 2 , 0.01, 0.1, 1, 10, 15, 20, 30, 35, 40, 45, 50, 55, 6, 65 or 70 mm 2 To 50, 100, 250, 500, 700, 1000 μm 2 , 0.01, 0.1, 1, 10, 15, 20, 30, 35, 40, 45, 50, 55, 65, 70, 75, 80, 85, 90, 95 or 100 mm 2 .

[0074] Photodetectors typically consist of multiple layers of semiconductor materials, such as InP, InGaAs, InGaAsP, and GaAs, stacked in any combination. Photodetectors typically have at least one pn junction that can convert photons into an electric current, which can be collected by applying a voltage across the pn junction or by generating a voltage difference across the pn junction after photon absorption. The absorbed photons form electron-hole pairs in the depletion region. Photodiodes and phototransistors are examples of photodetectors.

[0075] In addition, the present invention relates to a novel structure of a vertically etched optoelectronic device, wherein a termination oxide layer covers the surface of the mesa structure.

[0076] In another aspect, the present invention provides a method for manufacturing an optoelectronic device. A mesa structure is prefabricated (arranged) on top of a substrate layer. The mesa structure is further processed to form a first termination oxide layer of a first type on its first surface, and optionally a second termination oxide layer of a second type on its second surface.

[0077] The method can be divided into three main steps; step S1 (preparation), step S2 (formation of the first and optional second termination oxide layers) and optional step S3 (overcoating). These will be discussed in more detail below.

[0078] In the manufacturing method, the materials of the first surface and the optional second surface exposed to the air are prone to form a natural oxide layer, and those skilled in the art will understand that the natural oxide layer may cause the occurrence of dark current and leakage current. Therefore, it is best to prevent such oxidation to avoid the dark current and leakage current leakage current phenomenon caused by the natural oxide layer, which may lead to a decrease in the efficiency of the optoelectronic device.

[0079] The method further comprises cleaning the first surface of the mesa structure by removing at least 75% of the native oxide on the first surface of the mesa structure. This is usually performed in at least one cleaning step before forming the first termination oxide layer. A detailed description of various possible cleaning steps in step S1 is given below.

[0080] According to an embodiment, the mesa structure includes a second surface parallel to the plane of the first surface of the substrate layer, so the method further includes forming a second termination oxide layer of a second type on the second surface of the mesa structure. In this case, it is preferred to clean the second surface of the mesa structure by removing at least 75% of the native oxide on the second surface of the mesa structure before forming the second termination oxide layer.

[0081] The method may also include removing the substrate layer after forming the first termination oxide layer and the optional second termination oxide layer (and the optional third termination oxide layer). After processing, the obtained optoelectronic device no longer includes the substrate layer. It can be selectively placed on another substrate layer, and in the case where the angle α is different from 90°, the angle β between the new substrate layer and the first surface of the mesa structure (i.e., the first surface including the first termination oxide layer) is naturally 90°-α. The mesa can be transferred from one base layer to another base layer using methods known in the art. The new surface of the mesa structure may thus be exposed (by removing the substrate layer), and this new surface may also be provided with a termination oxide layer (which may be the same as or different from the other termination oxide layers).

[0082] In addition, the mesa structure can be formed (not ready-made). The formation of the mesa structure can be performed by methods known in the art, such as reactive ion etching (RIE). The etching depth of the isolated mesa is preselected. In one example, the material can be etched all the way to the substrate. In another example, a portion of the material can be left on the substrate between the mesas.

[0083] Step S1

[0084] In step S1, contaminants, carbon and native oxides are removed from the mesa structure. They must be removed because these substances are not conducive to the formation of the first and optional second termination oxide layers. The substrate may not have any contaminants and carbon, but if native oxides are present, at least 75% of the oxides should be removed. According to embodiments, at least 80%, 85%, 90%, 95%, 96%, 97%, 98%, 99% or more of the native oxides will be removed. Even a few thousandths of the native oxide may remain.

[0085] According to an embodiment, the process begins with obtaining or providing a substrate having a mesa structure. In step S1, a series of treatments are performed to remove contaminants, carbon, and native oxides from the substrate layer and the mesa structure surface. In one embodiment, contaminant removal includes wet chemical treatment, such as acetone-methanol-isopropanol treatment. In other embodiments, contaminant removal can be performed under ultrasonic agitation.

[0086] In one embodiment, a wet chemical treatment process is used to remove carbon-related atomic species from the surface of the mesa structure. This process can be an acetone-methanol-isopropanol treatment or an additional RCA cleaning. The details of RCA cleaning are well known in the art. And this wet chemical treatment process can be carried out under ultrasonic agitation. In another embodiment, the carbon removal step can be a dry cleaning process, such as using an oxygen plasma treatment. For example, the oxygen plasma generated in a downstream remote plasma configuration can effectively generate volatile carbon-related substances, which can be easily removed by a vacuum pump used in a plasma chamber configuration.

[0087] In one embodiment, after the carbon removal step, the native oxide will be removed. It is worth noting that the native oxides of III-V semiconductors exhibit poor properties and contain a high density of defects and associated electronic states in the semiconductor band gap. The native oxide consists of a mixture of Group III and Group V related oxides, dangling bonds and dimer bonds. Generally, Group V related oxides and their associated electronic states are believed to reduce the performance of optoelectronic devices. The effects of these oxides are given in Figure 10 below.

[0088] In one embodiment, wet chemical treatment can be used to remove native oxides. For example, different chemicals (e.g., hydrofluoric acid-based solutions, citric acid-based solutions, or sulfuric acid-based solutions) can be used to remove native oxides from different materials. For example, to clean a mesa structure containing materials such as InGaAlP, GaAs, AlGaAs, InP, GaP, GaN, InGaN, etc., a hydrochloric acid solution can be used. The molar concentration of the solution can vary between 0.1M and 12M, and the solvent can be deionized water, isopropanol, or methanol. The etching time can vary from 1 second to 5 minutes, depending on the selected solution molar concentration and the material composition of the mesa structure. In order to avoid reoxidation of the mesa surface after chemical treatment, the etching process can be carried out in an inert gas environment, wherein the oxygen content is at least less than 1000 parts per million (ppm). Other wet etching recipes that can also be used, such as hydrofluoric acid solutions. The hydrofluoric acid solution can be diluted with deionized water, and a buffer such as ammonium fluoride can also be used. It is worth noting that in wet chemical etching technology, the chemical formula can vary according to the material to be processed.

[0089] In another embodiment, the native oxide can be removed using a dry etching process. For example, an atomic hydrogen flux can be used under vacuum conditions to remove dry native oxide from the surface of the mesa structure. The atomic hydrogen flux can be generated using a remote electron cyclotron resonance plasma source or by using a hydrogen thermal cracker. The thermal cracker can decompose molecular hydrogen into atomic hydrogen. Another dry cleaning process for native oxide is ion sputtering of an inert gas.

[0090] According to an alternative embodiment, a dry process for removing native oxide from the surface of the mesa structure is to use ion bombardment, for example, an inert gas species such as helium, argon, neon or xenon for sputtering. In such an example, the ion source can be an end-Hall type gridless ion source with sufficiently low ion energy (<200eV) but high current density, minimizing sputtering damage and ion implantation to the mesa structure, but allowing gentle removal of the native oxide. In another example, the substrate can be biased to a negative voltage during ion bombardment to increase the ion energy.

[0091] According to an embodiment, after cleaning as described above (to remove contaminants, native oxides and carbon), the tabletop is introduced into an ultra-high vacuum chamber condition for step S2. Ultra-high vacuum (UHV) herein refers to a condition whose base pressure is between 1x10 -7 Up to 1x10 -11 Vacuum in the mbar range.

[0092] Step S2

[0093] In the first sub-step of S2, the optoelectronic device is heated to a high temperature in a degassing step under ultra-high vacuum conditions to evaporate the volatile compounds left on the surface of the mesa structure in the previous cleaning step. In one embodiment of the degassing step, the degassing temperature may vary between 200°C and 600°C, depending on the material of the mesa structure. It should be noted that the correct temperature and degassing time are required to promote the removal of volatile substances from the cleaned mesa structure surface. In one embodiment, the temperature can be selected to achieve a slight removal of group V atoms such as arsenic and phosphorus, so that the first atomic layer of the first surface of the mesa structure becomes rich in group III elements.

[0094] After the degassing step, the mesa is treated to form a first stop oxide layer. The mesa is controllably oxidized to form one or more stop oxide layers on the surface of the mesa structure.

[0095] When the oxygen dose and surface temperature are chosen correctly, oxygen is absorbed into the surface and promotes the transformation of the surface structure into a high-quality terminated oxide layer.

[0096] In fact, in one embodiment, the oxidation conditions are selected so that the process promotes the production of volatile group V oxides (which are easily removed from the surface under high temperature conditions), thereby making the first atomic layer of the mesa surface lacking group V atoms and converting the surface to high-quality group III-related oxides. During the degassing process, the effect of removing group V species can be monitored using, for example, reflection high energy electron diffraction (RHEED), X-ray photoelectron spectroscopy (XPS), or mass spectrometry. Figure 9 gives a more detailed illustration of the effect of the treatment.

[0097] In one embodiment, before forming the termination oxide layer, metal deposition is performed by evaporating 0.2-10 monolayers of In, Ga or Sn metal on the surface of the mesa structure to produce a surface layer rich in group III or group IV. By performing such metal deposition, the resulting surface is more susceptible to forming a termination oxide layer lacking group V.

[0098] According to an embodiment, the first termination oxide layer is of a first type. The first type is a compound semiconductor oxide layer rich in group III oxides and having a thickness less than 10 nm. Figures 9 and 10 give more details.

[0099] The optional second termination oxide layer is of the second type. The second type depends on the processing conditions and geometry. The second type is a compound semiconductor oxide layer rich in group III oxides and having a thickness of less than 10 nm. In addition, if the flat surface of the structure has a crystal orientation of (001), the second termination oxide layer can be a crystalline termination oxide layer.

[0100] For example, the termination oxide layer can be produced by using an oxygen flux under vacuum conditions. The first and optional second termination oxide layers can be produced by introducing oxygen (in gaseous form, such as O 2 or 3 , or there is H 2 O 2 The oxidation conditions are selected so as to promote the production of a group V oxide that is highly volatile and easily removed from the surface under high temperature conditions, so that the topmost atomic layer of the surface of the mesa structure lacks group V atoms and the surface is converted into a high-quality group III related oxide. Generally, only oxygen is used as a reagent in the present process, compared with more traditional oxide layer formation processes, which generally involve the use of more than one element reaction and the growth of new oxide material on the surface rather than changing the existing surface.

[0101] In another example, the outer surface of the mesa structure is heated to at least 200°C and up to 750°C, depending on the material composition of the outer surface, to promote the oxidation process. The reaction is usually carried out under vacuum conditions, and the pressure of the chamber is usually 1x10 -11 to 1x10 -7 Subsequently, the outer surface of the mesa structure is exposed to oxygen atoms, molecules, ozone or other oxidants such as H at a selected temperature. 2 O 2The oxygen partial pressure during oxidation is usually 5x10 -8 to 5x10 -3 mbar range, depending on the material composition of the treated mesa structure. In addition, the oxidation time can be between 5 seconds and 60 minutes. In another embodiment, the termination oxide layer is formed under vacuum conditions under ultraviolet light irradiation. During the oxidation process, ultraviolet irradiation can promote oxygen molecules to form more reactive singlet oxygen quantum states. In addition, short-wavelength ultraviolet irradiation has the effect of destroying surface atomic bonds and promoting surface reactions. Among them, 172nm is an example of a wavelength that promotes surface reactions.

[0102] In an additional or alternative embodiment, indium atoms are deposited onto the mesa surface before the surface is converted into a termination oxide layer. Alternatively, tin atoms can be deposited onto the mesa surface before the surface is converted into a termination oxide layer. In another example, gallium atoms are deposited onto the mesa surface before the surface is converted into a termination oxide layer. The deposition of metal atoms onto the cleaned mesa surface has the effect of forming a thin group V defect layer on the surface of the mesa structure to promote the formation of group III or additional group IV (Sn) related oxides during the formation of the termination oxide layer. In such an embodiment, the amount of metal deposited is between 0.2 monolayers and 10 monolayers. The deposition of such a metal layer can be performed using a percolation cell or additionally a thermal evaporator such as electron beam evaporation.

[0103] The termination oxide layer can be formed under ultra-high vacuum conditions, whereby the process can occur in a free molecular flow regime where the mean free path of the molecules is greater than the dimensions of the chamber in which the process occurs. The molecules can easily collide with any surface in the chamber. This property allows the process to conform well to 3D surfaces.

[0104] After the formation of the oxide layer is terminated, the mesa structure is cooled to below 100° C. in a cooling step, preferably under ultra-high vacuum conditions.

[0105] Step S3

[0106] As an optional step, after forming the termination oxide layer, the optoelectronic device can deposit an outer coating. For example, the outer coating can be deposited using chemical vapor deposition (CVD), ALD or PECVD or by sputtering. The outer coating can be Al 2 O 3 , HfO 2 、SiN x or SiO 2 Transfers are preferably made via a vacuum transfer line to minimize contamination, although air transfer has also been shown to provide good results. Transfers can also be made under ultra-high vacuum or high vacuum conditions, or in an air or inert gas environment.

[0107] Cleaning also plays a role in the manufacturing process in that the capping layer can be formed without creating a disordered interface between the capping layer and the semiconductor because the terminating oxide layer is ordered.

[0108] In one embodiment, the vacuum transfer further comprises a degassing step. After the deposition of the outer coating, an annealing treatment such as rapid thermal annealing (RTA) may be performed to improve the layer quality.

[0109] Thus, according to an embodiment, the method further comprises depositing an overcoat layer on the termination oxide layer.The termination oxide layer refers herein to any termination oxide layer present on the mesa.

[0110] In such additional embodiments, the benefit of generating an oxygen-containing structure on a mesa surface (the inclined side surface of a mesa structure) is provided, the oxygen-containing structure of the surface can prevent the material from being further exposed to oxygen, and has a low amount of atomic-level defects. These embodiments are suitable for optoelectronic and photovoltaic applications including mesa structures formed by quantum well (QW) semiconductor material structures. Semiconductor devices generally include a stacked structure of multiple semiconductor layers so that the multiple semiconductor layers can accommodate charge carriers.

[0111] The gain effect of the termination oxide layer and its passivation effect can be measured by evaluating the minority carrier lifetime of the device. This measurement can be done using time-correlated single photon counting methods to resolve the time-resolved photoluminescence characteristics of the device. The carrier lifetime is defined as the average time required for minority carriers to recombine. In the case of typical material systems with high defect density, the minority carrier lifetime is short due to carrier losses due to non-radiative recombination. Figure 6 The effect of the termination oxide layer is given.

[0112] Furthermore, the effect of the termination oxide layer can also be characterized by photoluminescence (PL) spectroscopy. In this technique, the microLED surface is excited by an external laser with a wavelength corresponding to an energy greater than the energy of the band gap of the semiconductor material. After excitation, the generated charge carriers recombine and, in the case of radiative recombination, the semiconductor material emits light. The intensity of the photoluminescence is particularly affected by the amount of surface state defects generated by poor-quality oxides. In the case of high defect density, Shockley-Read-Hall recombination dominates and the photoluminescence intensity emitted by the material is generally lower compared to low defect density materials. Figure 7 Specific examples are given. The luminescence levels obtained using micro devices with a termination oxide layer are several times higher than the same devices passivated using known passivation techniques.

[0113] In the manufacturing process, steps S1, S2 and S3 are usually completed in separate chambers. These chambers and other chambers can be isolated from each other by gate valves, which can allow material transfer between different chambers when the gate valves are in the open position. In addition, the equipment will have different components to monitor and implement steps S1, S2 and S3, such as pressure gauges and thermometers, heaters, vacuum pumps, plasma sources, plasma guns, sputtering heads, gas pipelines, leak valves, etc.

[0114] The present invention provides a passivation method for a semiconductor device, which includes a stacked configuration of multiple semiconductor layers processed to form a mesa structure. The multiple semiconductor layers can accommodate charge carriers. The method includes first cleaning carbon and contaminants on the surface of the material exposed to the environment, then removing the native oxide (with poor electrical properties), and then generating the above-mentioned termination oxide layer in a process that conforms to the 3D shape through a process with controllable conditions such as UHV conditions, substrate temperature, time, gas partial pressure, etc.

[0115] In one embodiment, a substrate comprising a mesa structure is provided, and the first surface of the mesa structure comprises InAs. Contaminants and carbon on the mesa surface are removed by solvent. The solvents used are acetone, methanol and isopropanol. The sample is immersed in each solvent for 1 minute. The native oxide on the mesa structure is then removed by argon ion sputtering. The ion gun filament current is 15 mA, the voltage is 2 kV, and the argon partial pressure is 3*10 -6 mbar, the sputtering time is 15min. Then the table is introduced with a pressure of 1*10 -9 mbar ultra-high vacuum chamber. The table was degassed under ultra-high vacuum conditions and annealed at 450°C for 30 minutes. After low-energy electron diffraction measurements, the treated surface showed a (4x2) reconstruction. It was then oxidized with oxygen. The oxygen partial pressure was 3*10 -6 mbar, and the oxidation time was 15 minutes. The results showed that the first termination oxide layer contained an oxide layer of 90% group III oxide and 10% group V oxide.

[0116] Other aspects, advantages, features and objects of the invention will emerge from the enclosed declarations in conjunction with the drawings and detailed description of illustrative embodiments. It is noted that the invention is susceptible to being combined in various combinations without departing from the scope of the invention as defined in the appended claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0117] Figure 1A is a schematic diagram of an optoelectronic device 100 viewed from above in one embodiment. Figure 1B is a diagram of a cross section AA of the optoelectronic device 100 . Figure 1AThe optoelectronic device 100 includes nine mesa structures 120. Each mesa structure is arranged on top of the substrate layer 110, that is, on its first surface plane. The first surface plane 112 of the substrate layer 110 is Figure 1B The first type of first termination oxide layer 130 is arranged on the first surface of the mesa structure 120. Figure 1A , a first termination oxide layer 130 surrounds the mesa structure from all side directions. A second termination oxide layer 132 is arranged on the second surface of the mesa structure 120. The second termination oxide layer 132 is parallel to the surface plane 112 of the substrate layer 110. In addition, between the mesa structures, a third termination oxide 134 layer has been formed on top of the base layer.

[0118] Figure 2A , 2B 2C is a schematic diagram of a photovoltaic device of the second embodiment. Figure 2A In the embodiment, the optoelectronic device 200 includes a mesa structure 220 arranged on top of a substrate 210, i.e., on a first surface plane thereof. The first surface plane 212 is opposite and parallel to a second surface plane 214. The mesa structure 220 includes a first layer 202 (a buffer layer in the case where the optoelectronic device is an LED or a micro-LED) epitaxially grown on top of the substrate, a second layer 204 grown on top of the first layer, an active region 206 grown on top of the second layer, and a third layer 208 grown on top of the active region. A first type first termination oxide layer 230 is arranged on a first surface of the mesa structure 220. A second type second termination oxide layer 232 is arranged on a second surface of the mesa structure 220. Figure 2A is an explanatory enlarged view of the first surface. It can be seen that the thickness of the first termination oxide layer 230 varies depending on the material of the mesa structure layer. As can be seen in the explanatory enlarged view, layer 206 includes a portion 240 of the termination oxide layer on its side, whose thickness is different from the thickness of the portion 242 arranged on the epitaxial layer 204. While layer 208 includes a portion 244 of the termination oxide layer on its side, the thickness of which is similar to the thickness of portion 240. In addition, contact layer 222 is formed on top of third layer 208, and third termination oxide layer 234 is arranged on the surface of the substrate layer.

[0119] Figure 2B 2 is a photovoltaic device 250 in another embodiment. In this embodiment, the mesa structure 220 has been formed on the substrate 210, but only the first surface thereof has been processed and a termination oxide layer 230 has been formed. Figure 2C Another optoelectronic device 260 is shown, which includes a mesa structure 220, a first termination oxide layer 230, a second termination oxide layer 232, and a third termination oxide layer 234. In this embodiment, the mesa structure has been processed so that the first layer 202 is not completely etched and remains on the substrate layer 210.

[0120] Figure 3A 3 is a schematic diagram of an optoelectronic device 300 having a native oxide on the surface of a mesa structure. The mesa structure 320 is arranged on top of a substrate 310. The mesa structure 320 includes a contact layer 322 fabricated using photolithography techniques on top of the mesa structure 320 and a native oxide layer 370 on the surface of the crystalline semiconductor material 360 of the mesa structure 320. The native oxide layer 370 is also Figure 3A The local enlarged figure is given in the figure.

[0121] Figure 3B 3 is a schematic diagram of an optoelectronic device 300 having an outer coating on top of a native oxide. A mesa structure 320 is disposed on top of a substrate 310. The mesa structure 320 includes a native oxide layer 370 on the surface of a crystalline semiconductor material 360 of the mesa structure 320 and a dielectric layer 390 disposed on top of the native oxide layer, the dielectric layer 390 also being disposed on the surface of the native oxide layer. Figure 3B The local enlarged figure is given in the figure. Figure 3B An enlarged view of an optoelectronic device fabricated according to known methods is also shown. Figure 3B It can be seen that the oxide is disordered at the interface.

[0122] Figure 3C 3 is a schematic diagram of an optoelectronic device 300 with a termination oxide layer according to a third embodiment of the present invention. A mesa structure 320 is arranged on top of a substrate 310. The mesa structure 320 includes a contact layer 322 manufactured on top of the mesa structure 320 using a photolithography technique. In addition, a first termination oxide layer 330 of a first type, a second termination oxide layer 332 of a second type, and a third termination oxide layer 334 arranged on the surface of the substrate layer 310 are also included. The first termination oxide layer 330 is also disposed on the surface of the crystalline semiconductor material 360 of the mesa structure 320. Figure 3C The enlarged view shows the order of the oxide at the interface. This schematically illustrates the at least major removal of the native oxide before the formation of the final product termination oxide layer.

[0123] Figure 3D 3 is a schematic diagram of an optoelectronic device 300 with a termination oxide layer and a dielectric cap layer according to a fourth embodiment of the present invention. A mesa structure 320 is arranged on top of a substrate 310. The mesa structure 320 includes a contact layer 322 fabricated on top of the mesa structure 320 using a photolithography technique and a first type first termination oxide layer 330 and a second type oxide layer 332 arranged on the surface of the crystalline semiconductor material 360 of the mesa structure 320. A third termination oxide layer 334 is arranged on the surface of the substrate layer 310. In this illustration, a dielectric cap layer 340 is arranged on top of the termination oxide layers 330, 332, and 334. These have also been described in detail in detail. Figure 3D The local enlarged figure is given in the figure.

[0124] Figure 4 is a process flow chart of an embodiment of the present invention. The process flow describes the main process steps S1 (preparation), S2 (forming a termination oxide layer) and S3 (external coating). The process begins with forming a substrate having a patterned mesa structure on a substrate 400. Step S1 performs a series of treatments, such as 402, 404 and 406, respectively, to remove pollutants, carbon and native oxides. In this embodiment, the pollutant removal step 402 includes a wet chemical treatment, such as an acetone-methanol-IPA treatment. In one embodiment, a wet chemical treatment, such as an acetone-methanol-isopropanol treatment or an additional RCA cleaning, is used when performing the carbon removal step 404. In another embodiment, a dry cleaning process can be used for the carbon removal step 404, such as using an oxygen plasma treatment. After the carbon removal step 404, the native oxide will be removed in step 406. In one embodiment of the native oxide removal 406, a wet chemical treatment 410 will be used, such as a natural oxide treatment based on hydrochloric acid or hydrofluoric acid. In another embodiment of native oxide removal 406, a dry cleaning process 408 is used, such as atomic hydrogen treatment or ion sputtering using an inert gas. After native oxide removal 406, in step 412 of S1, the cleaned substrate with a mesa structure is introduced into an ultra-high vacuum chamber for degassing. The degassing step is to clean the mesa structure by annealing the mesa structure between 200°C and 600°C in a controlled manner. After the degassing step 414, in one embodiment, a metal deposition step 416 is performed by evaporating 0.2-10 monolayers of In, Ga or Sn metal on the surface of the mesa structure, thereby producing a surface layer rich in group III or group IV. Step 418 is to arrange a termination oxide layer, which can be after the degassing step 414 or after the metal precipitation step 416. In one embodiment, in step 418, oxygen (in gaseous form, such as O 2 or 3 , or in H 2 O 2The terminating oxide layer is arranged by transferring the mesa structure to the hot mesa structure surface under the condition of the presence of a layer of at least one oxidizing agent. After step 418, the mesa structure can selectively undergo a post-oxidation high temperature annealing step 420. In addition, the mesa structure can undergo a UV activation step 422. Step 424 is to cool the mesa to below 100° C. under ultra-high vacuum conditions. After the mesa structure has undergone the cooling treatment of step 424, the mesa structure is transferred to the outer coating equipment in step 426 of S3. The transfer can be carried out under ultra-high vacuum conditions or under high vacuum conditions in step 428, or directly in air or in an inert gas environment. In one embodiment, the ultra-high vacuum transfer also includes a degassing step 428. Subsequently, step 430 is to deposit a dielectric outer coating, which can be deposited using atomic layer deposition, plasma enhanced chemical vapor deposition, or by sputtering deposition. After the dielectric coating is deposited, a post-annealing treatment can be performed in step 432.

[0125] Figure 5 Schematic diagram of the process equipment of the embodiment of the present invention. The process equipment includes a glove box 510, in which wet preparation can be performed. The preparation process can be inert (N 2 ) is carried out under a controlled atmosphere in which the oxygen concentration is less than 100 ppm. The glove box 510 is connected to a transfer chamber 520, in which a transfer mechanism for moving the device from the glove box to different parts of the equipment is installed, such as a robot, or in another example, a linear transfer rod system. The transfer chamber can realize the transfer of samples between chambers at the required vacuum level. The transfer chamber is connected to the buffer chamber 530, which is in turn connected to the oxidation chamber 540, which can realize the transfer of samples to the termination oxide layer formation chamber 540 at the required high vacuum level. The role of the buffer chamber is to compensate for the different pressure levels required for different steps. For example, the pressure in the oxidation chamber 540 can be between 10 -10 mbar, while the pressure in the transfer line 520 is 10 -6 The processing time is reduced by adjusting the pressure in the buffer chamber 530, which has a significantly smaller volume than other chambers. The transfer chamber 520 is also connected to an outer coating deposition chamber 550, which can perform deposition of dielectric materials. The outer coating chamber 550 can be an atomic layer deposition chamber or a plasma enhanced chemical vapor deposition chamber.

[0126] Figure 6The charge carrier lifetime decay curves of a standard micro LED device with a native oxide layer on the surface of a mesa structure and a charge carrier lifetime decay curve of a micro LED device with a terminated oxide layer on the surface of a mesa structure measured using the time-correlated single photon counting method are respectively shown. Both devices are InGaAlP-based micro LED arrays with a size of less than 5μm. The carrier lifetime is defined as the average time required for minority carriers to recombine. In the case of a material system with a high defect density, the minority carrier lifetime will be shortened due to carrier losses caused by non-radiative recombination. Figure 6 As shown, the carrier lifetime of the device with the termination oxide layer is significantly improved. In the figure, the lifetime (in nanoseconds) is shown on the abscissa and the counts (in absolute units) are shown on the ordinate. The triangles show the results of the standard micro-LED (<τ> about 2.8 nanoseconds), and the circles show the results of the micro-LED containing the termination oxide layer of the present invention (<τ> about 3.5 nanoseconds).

[0127] Figure 7 The photoluminescence spectra of a standard micro-LED device with a native oxide layer at the surface of the mesa structure (the bottom curve), the photoluminescence spectrum of a micro-LED device with a mesa structure surface passivated using the prior art (the middle curve), and the photoluminescence spectrum of a micro-LED device with a termination oxide layer on the surface of the mesa structure of an embodiment of the present invention (the top curve) are shown. The wavelength (in nm) is shown on the abscissa, and the photoluminescence intensity (in counts) is shown on the ordinate. These are all micro-LEDs with a size of 10 μm InGaAlP-based materials, and the middle of the figure is a reference for the three curves.

[0128] According to an embodiment, Figure 8 8 is a schematic diagram of a vertical cavity surface emitting laser (VCSEL) structure 800. Semiconductor layers 812 and 814 are arranged on top of substrate 810. In this example, semiconductor layer 812 is included in a bottom distributed Bragg reflector (DBR) and layer 814 is an n-contact layer. A mesa structure is arranged on top of the n-contact layer 814. In this example, the mesa structure includes multiple semiconductor layers constituting an n-type DBR 826, an optical microcavity 824, an oxide aperture layer 816, a p-type DBR 822, and a top p-type contact layer 818. In this example, the top dielectric DBR 828 is formed by multiple layers of dielectric material. A first type of first termination oxide layer 830 is arranged on a first surface of the mesa structure 820. A second type of second termination oxide layer 832 is arranged on a second surface of the mesa structure. A third termination oxide layer 840 is arranged on top of the n-contact layer 814.

[0129] This termination oxide layer increases the semiconductor device energy barrier and improves carrier confinement within the mesa structure formed by the stack of multiple semiconductor layers. The termination oxide layer provides a passivation effect, preventing uncontrolled oxidation of the surfaces of 822, 826, 816, 818 and 824. The need to encapsulate such devices in a sealed package is avoided.

[0130] Fig. 9A This is a reflection high-energy electron diffraction pattern of the InGaAlP (001) material surface cleaned by the above cleaning process. The diffraction pattern shows that the surface is long-range ordered and has a (2x4) surface symmetry (the other azimuth angle is not shown), which indicates that the surface has been successfully cleaned of native oxides and other contaminants, and the surface has been reconstructed to form a clean (2x4) surface symmetry as shown in the figure.

[0131] Fig. 9B The figure is a reflection high energy electron diffraction pattern of the surface of the InGaAlP (001) material with a crystalline termination oxide layer of the present invention. The diffraction pattern shows a long range order of the surface with (3x1) surface symmetry in the plane (001) surface (the other orientation is not shown), that is, the termination oxide layer is crystalline.

[0132] Fig. 10A The Ga2X-ray photoelectron (XPS) spectrum emission spectrum of an InGaAlP-based material with a native oxide layer on the mesa structure. The deconvoluted emission spectrum shows the characteristic component 1010 of the Ga-O bond. In addition, 1012 is the characteristic component of the Ga bonding environment in the bulk semiconductor stack.

[0133] Fig. 10B This is a Ga2px-ray photoelectron emission spectrum of a mesa structure with a termination oxide layer and an InGaAlP-based material according to an embodiment of the present invention. The deconvoluted emission spectrum shows a characteristic component 1020 of the Ga-O bond, which is much smaller than the case with a native oxide layer. In addition, 1022 is a characteristic component of the Ga bonding environment in the bulk semiconductor stack.

[0134] Fig. 10C Figure 1 is a graph of the P2p x-ray photoelectron emission spectrum of an InGaAlP based material from a mesa structure with a native oxide layer. The deconvoluted emission spectrum shows a weaker P bond component 1030 within the bulk semiconductor material and a strong component 1032 representing phosphorus oxide.

[0135] Fig. 10D The P2p x-ray photoelectron emission spectrum of the mesa structure with the termination oxide layer of the InGaAlP-based material of the embodiment of the present invention is shown in the figure. The deconvoluted emission spectrum clearly shows the characteristic component 1040 of the P bond in the main semiconductor material. The characteristic component 1042 of the phosphorus oxide is below the detection range of the XPS instrument.

[0136] According to the embodiment Fig.11 is similar to Figure 1A and 1B A side view of an optoelectronic device is shown in . It shows the angle α between the first surface 101 of the mesa structure 103 and the first surface plane 105 of the substrate layer 107. The line with reference numeral 109 gives the distance between the centers of two adjacent mesa structures.

[0137] Fig.12 14 is a schematic diagram of an optoelectronic device according to the fourteenth embodiment of the present invention. In this embodiment, the first surface of the mesa structure 123 is divided into two parts, namely 121a and 121b, which are arranged at a certain angle to each other. As shown in the figure, the angle α has been measured by measuring along the active area 125 of the mesa structure.

[0138] Fig.13 15 is a schematic diagram of an optoelectronic device according to the fifteenth embodiment of the present invention. In this embodiment, the first surface 131 of the mesa structure 133 is a partial spherical surface. As shown in the figure, the angle α has been measured by measuring along the active area 135 of the mesa structure.

[0139] The embodiments of the present disclosure described above may be modified without departing from the scope of the claims appended hereto. Expressions such as "comprises," "comprising," "including," "having," "is," etc. used to describe and claim the present invention are intended to be interpreted in a non-exclusive manner, i.e., allowing for the presence of items, components, or elements that are not explicitly described. References to the singular should also be interpreted as relating to the plural.

Claims

1. An optoelectronic device (100, 200, 250, 260, 300), comprising - the substrate layer (110, 210, 310, 107) has a first surface plane (112, 212, 105) and a second surface plane (214) opposite to and parallel to the first surface plane; - a mesa structure (120, 220, 320, 820, 103, 123, 133) arranged on a first surface plane of the substrate layer, the mesa structure comprising - at least one layer of III-V material; and - a first surface (101, 131) arranged at an angle α relative to a first surface plane of the substrate layer, wherein the angle α is between 0° and 180°; - A first type of first termination oxide layer (130, 230, 330) arranged on the first surface of the mesa structure, wherein before forming the first type of first termination oxide layer by oxidation, the first surface of the mesa structure has been cleaned and at least 75% of the native oxide on the first surface has been removed, wherein the structure of the first termination oxide layer is ordered so that the surface of the first termination oxide layer has long-range order.

2. The optoelectronic device (100, 200, 250, 260, 300) according to claim 1, wherein the mesa structure (120, 220, 320, 820, 103, 123, 133) also includes a second surface (132) parallel to the first surface plane (112, 212, 105) of the substrate layer (110, 210, 310, 107) and a second type second termination oxide layer (132, 232, 332, 832) arranged on the second surface of the mesa structure.

3. The optoelectronic device (100, 200, 250, 260, 300) according to claim 1 or 2, wherein the optoelectronic device (100, 200, 250, 260, 300) is a micro light emitting diode, and the area of ​​the mesa structure (120, 220, 320, 820, 103, 123, 133) on the substrate is 1-250000 μm 2 .

4. The optoelectronic device (100, 200, 250, 260, 300) according to claim 1 or 2, wherein the optoelectronic device (100, 200, 250, 260, 300) is a photodetector, and the area of ​​the mesa structure (120, 220, 320, 820, 103, 123, 133) on the substrate is 1-100 μm 2 .

5. The optoelectronic device (100, 200, 250, 260, 300) according to claim 1 or 2, wherein the optoelectronic device (100, 200, 250, 260, 300) is a vertical cavity surface emitting laser, and the area of ​​the mesa structure (120, 220, 320, 820, 103, 123, 133) on the substrate is 1-250000 μm 2 .

6. The optoelectronic device (100, 200, 250, 260, 300) of any one of the preceding claims, wherein at least 50% of the total oxide of the first termination oxide layer (130, 230, 330, 840) is a Group III oxide.

7. The optoelectronic device (100, 200, 250, 260, 300) according to any one of claims 2 to 6, wherein at least 50% of the total oxide of the second termination oxide layer (132, 232, 332, 832) is a Group III oxide.

8. The optoelectronic device (100, 200, 250, 260, 300) according to any one of claims 2 to 7, wherein the second termination oxide layer (132, 232, 332, 832) is a crystalline termination oxide layer.

9. The optoelectronic device (100, 200, 250, 260, 300) according to any of the preceding claims, comprising a plurality of mesa structures (120, 220, 320, 820, 103, 123, 133), wherein the angle α is greater than 0° and less than 180°, and the center distance between two adjacent mesa structures is 2-500 μm.

10. The optoelectronic device (100, 200, 250, 260, 300) according to claim 9, wherein a third termination oxide layer (134, 234, 334, 840) of a third type is arranged on the surface (120, 220, 320, 820, 103, 123, 133) between two adjacent mesa structures.

11. An optoelectronic device according to any one of the preceding claims, further comprising an overcoat layer on the outermost termination oxide layer.

12. An optoelectronic device according to any one of the preceding claims, wherein the angle α is 30-90°.

13. An optoelectronic device according to any one of the preceding claims, wherein the first termination oxide layer has a thickness of less than 10 nm.

14. A method for manufacturing an optoelectronic device (100, 200, 250, 260, 300), the method comprising - obtaining a mesa structure (120, 220, 320, 820, 103, 123, 133) arranged on a first surface plane (112, 212, 105) of a substrate layer (110, 210, 310, 107), the mesa structure comprising - at least one layer of III-V material, and - the first surface (101, 131) is arranged at an angle α relative to the surface plane of the substrate layer, wherein the angle α is between 0° and 180°; - cleaning the first surface of the mesa structure by removing at least 75% of the native oxide on the first surface of the mesa structure; and - forming a first type of first termination oxide layer (130, 230, 330) on the first surface of the mesa structure by oxidation, wherein the structure of the first termination oxide layer is ordered so that the surface of the first termination oxide layer has a long-range order.

15. The method according to claim 14, wherein the mesa structure includes a second surface (132) parallel to the first surface plane (112, 212, 105) of the substrate layer (110, 210, 310, 107); and the method also includes forming a second type second termination oxide layer (132, 232, 332, 832) on the second surface of the mesa structure (120, 220, 320, 820, 103, 123, 133).

16. The method according to claim 14 or 15, which removes the substrate layer (110, 210, 310, 107) after forming the first termination oxide layer (130, 230, 330) and the optional second termination oxide layer (132, 232, 332, 832).