Joint structure
Laser welding technology is used to set up penetrations between metal materials of the same type, clamp and melt the dissimilar materials together, solving the problems of one-sided welding constraints and low productivity in spot welding technology, achieving efficient joining of dissimilar materials and improving productivity .
Patent Information
- Application Number
- CN202111237435.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2016-03-30
- Filing Date
- 2017-03-22
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2037-03-22
AI Technical Summary
Existing spot welding technology has the problem of restricting the shape of the product when welding on one side. The welding gun is heavy, slow to move, and takes a long time to pressurize, making it difficult to achieve efficient joining of lightweight materials. The complex rivet shape increases processing difficulty and cost.
Using laser welding technology, dissimilar materials are clamped between metal materials of the same type through a joint structure with penetration parts between metal materials of the same type, and laser fusion bonding is used to compress and fix the dissimilar materials, simplifying the joint structure. Reduce job time and increase productivity.
Efficient joining of dissimilar materials is achieved, production time is shortened, productivity is improved, manufacturing costs are reduced, and the rigidity and design freedom of the joint parts are increased.
Smart Images

Figure CN113828920B_ABST
Abstract
Description
[0001] This application is a divisional application of the invention patent application with application number 201780020691.3, application date March 22, 2017, and invention name “Joining Structure”. Technical Field
[0002] The present disclosure relates to a joining structure in which one or more different types of materials are clamped by the same type of metal materials using laser as a heat source. Background Art
[0003] In recent years, the globalization of transportation equipment, represented by automobiles, has led to an increase in production volume, and as a result, there has been a growing desire to reduce the total cost per product, particularly to improve productivity by shortening production time.
[0004] In addition, in order to prevent global warming, there is a strong demand for limiting CO2 emissions worldwide. In order to meet this demand, the transportation industry, represented by the automobile industry, is accelerating its efforts to improve fuel efficiency. As a specific effort to improve fuel efficiency, the pursuit of lightweight vehicles is being promoted, and research on increasing the proportion of lightweight raw materials is being promoted.
[0005] In the process of pursuing such a desire, spot welding has been widely used as a welding method used for transportation equipment such as automobiles. However, spot welding, which is resistance welding, requires the use of a spot welding gun for spot welding, that is, upper and lower electrodes to pressurize the material, and energize the upper and lower electrodes in a state where the gap between the welding materials is eliminated, thereby performing welding. Therefore, spot welding is not suitable for single-sided welding, and the welding part needs to be clamped from the top and bottom by the spot welding gun, which restricts the product shape. In addition, in order to pressurize the welding part, a space is required for the spot welding gun to enter the upper and lower parts of the welding material. In addition, the spot welding gun itself is heavy, so the moving speed of the spot welding gun is slow, and even if it reaches the welding position, it still needs time to pressurize, and it must also ensure cooling time after welding, which requires more time in addition to welding.
[0006] In order to reduce the weight of materials used in automobiles, research has been conducted to replace some parts from steel to light metal materials such as aluminum, and to develop a technology and structure for joining light metal materials to steel.
[0007] In the past, as a member for joining dissimilar materials, spot welding using rivets, joining using adhesives, etc. can be cited. For example, Patent Document 1 discloses a rivet shape, riveting, and spot welding method that absorbs the plastic flow of dissimilar materials caused by pressurization of dissimilar materials clamped by rivets and joining materials of the same material type as the rivet and welding heat during spot welding. It is possible to ensure space for a part of the dissimilar material to deform and move during riveting and spot welding, and prevent the dissimilar material from sinking due to the position deviation of the electrode during spot welding, thereby suppressing the reduction of the fastening force.
[0008] Prior Art Literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2015-42417 Summary of the invention
[0011] The joint structure disclosed in the present invention comprises: a first homogeneous metal material; a second homogeneous metal material, which can be welded to the first homogeneous metal material; and a dissimilar material, which is provided with a through-portion, sandwiched between the first homogeneous metal material and the second homogeneous metal material, and is difficult to weld to the first homogeneous metal material and the second homogeneous metal material. In the plate thickness direction in the irradiation area where the laser is irradiated toward the through-portion, the plate thickness in the irradiation area of the first homogeneous metal material located on the side irradiated with the laser is a prescribed thickness corresponding to the gap in the plate thickness direction in the irradiation area that exists in the state before welding, that is, the first gap. The first homogeneous metal material and the second homogeneous metal material are melted and bonded to each other via the through-portion to compress and fix the dissimilar materials, thereby fixing the dissimilar materials to the first homogeneous metal material and the second homogeneous metal material. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 It is a figure for demonstrating the joining structure of Embodiment 1 of this disclosure.
[0013] Figure 2A It is a diagram for explaining a joining state during laser welding according to the first embodiment of the present disclosure.
[0014] Figure 2B It is a diagram for explaining a joining state during laser welding according to the first embodiment of the present disclosure.
[0015] Figure 2C It is a diagram for explaining a joining state during laser welding according to the first embodiment of the present disclosure.
[0016] Figure 3This is a diagram showing a graph obtained by measuring the relationship between the plate thickness of the first material 1 and the plate thickness of the second material 2 (corresponding to the first gap 11) in the irradiated area of the irradiated laser 7 in the first embodiment of the present disclosure, and the gap in the plate thickness direction, namely, the first gap 11.
[0017] Figure 4 It is a diagram for explaining an example of the joining structure according to the first embodiment of the present disclosure.
[0018] Figure 5A It is a diagram for explaining an example of the joining structure according to the first embodiment of the present disclosure.
[0019] Figure 5B It is a diagram for explaining an example of the joining structure according to the first embodiment of the present disclosure.
[0020] Figure 6 This is a diagram showing a graph obtained by measuring the relationship between the material of the second material 2 as a different material and the second gap 5 in the second embodiment of the present disclosure.
[0021] Figure 7 It is a diagram for explaining the bonding structure according to the third embodiment of the present disclosure.
[0022] Figure 8 It is a diagram for explaining a conventional method of joining dissimilar materials.
[0023] Description of Reference Numerals
[0024] 1. First material (first metal material of the same type)
[0025] 2. Second material (different material)
[0026] 3. The third material (the second metal material of the same type)
[0027] 4 Through hole (through part)
[0028] 5 Second gap
[0029] 6 Compression force
[0030] 7 Laser
[0031] 8.8a Welding section
[0032] 9 Spacers
[0033] 10 Fourth material (different materials)
[0034] 11 First Gap DETAILED DESCRIPTION
[0035] (Origin of this disclosure)
[0036] Before describing the embodiments, the origin of the present disclosure will be briefly described.
[0037] use Figure 8 To illustrate the conventional joining components of dissimilar materials. In order to ensure space for a part of the dissimilar material 200 to deform and move during riveting and spot welding, and to prevent the sinking of the dissimilar material 200 caused by the position deviation of the electrode 400 during spot welding, etc., so as to suppress the decrease in the fastening force, a complex rivet shape such as a radius chamfer 30 and an annular groove 31 is required. In this case, the shape of the rivet 51 requires precision and becomes a complex shape. Therefore, the processing of the rivet 51 requires precision processing and the manufacturing cost is also increased. Moreover, since it is spot welding as resistance welding, it takes time to pressurize, energize, cool, move, etc., so the operation time becomes longer. Moreover, during spot welding, it is necessary to use a welding gun (not shown) for spot welding to clamp the joining component 100 from both sides, so the design freedom of the joining component 100 is limited.
[0038] In addition, when the adjacent rivets are too close, the spot welding current is split, resulting in insufficient nugget formation in the welded portion where the resistance welding is performed. Therefore, a joint spacing greater than the minimum separation spacing that allows for desired nugget formation without splitting the current is required. As a result, there is a problem that rivets cannot be arranged at a joint spacing less than the minimum separation spacing, and the rigidity of the joint at the necessary position cannot be increased.
[0039] The present disclosure provides a simple joining structure for laser welding that can join dissimilar materials and improve productivity.
[0040] (Implementation Method 1)
[0041] In this embodiment, use Figure 1 to Figure 5B Provide explanation.
[0042] Figure 1 This is a diagram for explaining the bonding structure of the first embodiment. Figure 2A to Figure 2C It is a diagram showing a joining condition during laser welding according to the first embodiment.
[0043] Here, Figure 2A This is a diagram for explaining a case where the first material 1 as the upper plate has a circular structure. Figure 2B This is a diagram for explaining a case where the first material 1 as the upper plate has a circular shape such as an elliptical shape. Figure 2C 1 is a diagram for explaining a case where the first material 1 as the upper plate is in a square shape. Figure 2A to Figure 2C The II section shown corresponds to Figure 1 The cross-sectional position.
[0044] Figure 1The figure shows a configuration in which the second material 2 is sandwiched between the third material 3 and the first material 1 when the first material 1 and the third material 3, which are made of metal, are joined to the second material 2, which is a different material. The first material 1 and the third material 3 are metal materials of the same type. The first material 1, the second material 2, and the third material 3 are plate-shaped materials with approximately uniform thickness.
[0045] Here, the second material 2 is preliminarily processed with a through hole 4 as an example of a through portion of the present disclosure. Therefore, there is a gap between the first material 1 and the third material 3 at the position of the through hole 4. On the first material 1 and the third material 3, no special processing such as holes, protrusions, steps, etc. is performed at the position corresponding to the through hole 4 in the state where the second material 2 is sandwiched. Therefore, the plate thickness of the second material 2 is approximately equal to the gap in the plate thickness direction between the first material 1 and the third material 3, that is, the first gap 11. It should be noted that in this embodiment, the through portion is set as the through hole 4, but it can also be, for example, a through groove.
[0046] Here, the plate thickness direction refers to the direction perpendicular to the main surfaces of the first material 1, the second material 2, and the third material 3 before welding. Figure 1 The arrows in the middle indicate the direction.
[0047] In addition, it should be noted that the same type of metal materials are metals that can be welded to each other, not only the same material, but also iron-based metal materials, non-iron-based metal materials, etc., which have good welding properties (in other words, welding compatibility). Specifically, as a combination of materials for welding, for example, with respect to the first material 1 and the third material 3, it is iron-based metal materials such as mild steel and mild steel, mild steel and stainless steel, stainless steel and stainless steel, mild steel and high-strength steel (high-tensile steel), high-strength steel and stainless steel, high-strength steel and high-strength steel. Or, for example, non-ferrous metal materials such as aluminum and aluminum, aluminum and aluminum alloy, aluminum alloy and aluminum alloy.
[0048] In addition, the second material 2 as a dissimilar material is a material of a different material from the first material 1 and the third material 3 as the same type of metal material, and is a material that is difficult to weld with respect to the same type of metal material. For example, when the first material 1 and the third material 3 as the same type of metal material are both iron-based metals, the second material 2 as a dissimilar material is a non-iron-based metal such as copper or aluminum. Moreover, when the first material 1 and the third material 3 are metal materials, the second material 2 as a dissimilar material is, for example, CFRP (Carbon Fiber Reinforced Plastics) or PET (Polyethylene terephthalate) as a resin material.
[0049] Welding conditions such as Figure 2AAs shown, the laser 7 is directed from the upper side of the first material 1 in the plate thickness direction toward the through hole 4 of the second material 2 (see Figure 1 ) is irradiated in a circular shape. As a result, the weld formed is Figure 1 The welded portion 8 is shown. In this way, when the laser beam 7 is irradiated to the first material 1, the first material 1 corresponds to the first homogeneous metal material of the present disclosure, and the third material 3 corresponds to the second homogeneous metal material of the present disclosure.
[0050] Next, regarding the joint conditions during and after welding, use Figure 1 As explained. If the laser 7 is irradiated in a circular shape to the irradiation area of the laser 7 located inside the through hole 4 of the first material 1 and the third material 3 to perform welding, when the welded portion 8 is formed, the molten metal solidifies and shrinks at the welded portion 8 when the first material 1 and the third material 3 are welded. In addition, for the second material 2 as a different material sandwiched between the first material 1 and the third material 3, a compressive force 6 is generated to reduce the gap in the plate thickness direction in the irradiation area of the laser 7 between the first material 1 and the third material 3 as the same type of metal materials, that is, the first gap 11 corresponding to the plate thickness of the second material 2.
[0051] When the thickness of the first gap 11, i.e., the second material 2, is set to be greater than 6% and less than 38% relative to the thickness of the first material 1 serving as the upper plate on the side irradiated with the laser 7 or the third material 3 serving as the lower plate on the side irradiated with the laser 7 in the irradiation area of the laser 7, the solidification shrinkage of the weld 8 becomes a compressive force 6 that clamps the second material 2 between the first material 1 and the third material 3, thereby crimping and fixing the second material 2.
[0052] The setting that the thickness of the second material 2 corresponding to the first gap 11 is set to be 6% or more and 38% or less relative to the thickness of the first material 1 or the third material 3 on the side irradiated with the laser beam 7 is derived from experimental data. Figure 3 shown. Figure 3 This is a graph obtained by measuring the relationship between the plate thickness of the first material 1 as the upper plate on the side irradiated with the laser 7 from the plate thickness direction, the second material 2 as a different material sandwiched between the first material 1 and the third material 3 of the same type of metal materials, and the plate thickness of the second material 2 as the first gap 11.
[0053] Figure 3 The graph is obtained by measuring the relationship between the plate thickness of the first material 1 and the plate thickness of the second material 2 (corresponding to the first gap 11 ) in the irradiated area of the laser beam 7 according to the embodiment of the present disclosure, and the gap in the plate thickness direction, that is, the first gap 11 .
[0054] In a combination in which the first material 1 and the third material 3, which are the same type of metal, are respectively made of mild steel materials, and the second material 2, which is a different type of material, is made of a resin material, i.e., PET material, the first material 1 is arranged on the upper side relative to the third material 3. And, in a state where the second material is sandwiched between them and overlapped in the vertical direction, the laser 7 is irradiated in a circular shape from the upper side in the plate thickness direction toward the inner side of the through hole 4 of the second material 2, i.e., the irradiation area of the irradiated laser 7, with a laser output of 3 kW to perform welding, Figure 3 An example of this case is shown.
[0055] For example, the through hole 4 of the second material 2 is φ12 mm, and welding is performed by setting the outer dimension of the weld of the welding portion 8, which is the irradiation area of the laser 7 irradiated from the plate thickness direction, to a circle of φ8 mm, which is smaller than the through hole 4 of the second material 2, in a manner that is smaller than the diameter or width of the through hole 4, which is the through portion of the second material 2, by a specified distance.
[0056] For example, when the plate thickness of the first material 1 is 0.8 mm, the compression fixation by the solidification shrinkage of the molten metal in the welded portion 8 can be performed until the plate thickness of the second material 2 corresponding to the gap 11 in the plate thickness direction between the first material 1 and the third material 3 is 0.1 to 0.3 mm. When the plate thickness of the second material 2 increases beyond 0.3 mm, a part of the weld line becomes an open hole (at least one open hole is formed in the welded portion due to insufficient filling of the weld metal during welding), causing welding failure. Therefore, 13% to 38% of the plate thickness of the first material 1 is an effective range.
[0057] In addition, when the plate thickness of the first material 1 is 1.6 mm, the compression fixation by the solidification shrinkage of the molten metal in the welded portion 8 can be performed until the plate thickness of the second material 2 is 0.1 to 0.5 mm. When the plate thickness of the second material 2 increases beyond 0.5 mm, a part of the weld line becomes an open hole state (at least one open hole is formed in the welded portion due to insufficient filling of the weld metal during welding), causing poor welding. Thus, the prescribed range of the plate thickness of the second material 2 as a different material corresponding to the plate thickness of the first material 1 as a metal material of the same type on the side irradiated with the laser 7 becomes the range that can be compressed and fixed by welding.
[0058] In other words, this means that the molten metal equivalent to 31% to 38% of the maximum plate thickness of the first material 1 falls into the inside of the through hole 4 and the bonding can be performed without opening the hole. When the molten metal exceeds 31% to 38% of the maximum plate thickness of the first material 1, the amount of molten metal required to fill the inside of the through hole 4 cannot be ensured, so a state in which a part of the hole is opened occurs.
[0059] On the contrary, when the thickness of the second material 2, which is the gap in the thickness direction, i.e., the first gap 11, is less than 0.1 mm, the gap between the first material 1 and the third material 3 irradiated with the laser 7 is too small, and the first material 1 and the third material 3, which are the same type of metal materials, are melted and bonded to each other, and the compression force 6 for compressing and fixing the second material 2, which is a different type of material, is insufficient.
[0060] In this way, the larger the gap in the direction of the plate thickness, i.e., the first gap 11, is within the range that can ensure the amount of molten metal during welding, in other words, within the range that does not produce openings, the greater the solidification shrinkage of the molten metal in the weld 8 during welding caused by the irradiation of the laser 7, and the greater the compression force 6 as a fixing force that clamps the second material 2 between the first material 1 and the third material 3.
[0061] In this embodiment, the laser irradiation direction is set to irradiate the laser 7 from the first material 1 side, but as long as the first gap 11, which is the plate thickness of the second material 2, is set to 6% to 38% of the plate thickness of the first material 1 or the third material 3 on the side irradiated with the laser 7, the amount of molten metal required for the first gap 11 can be ensured during welding, and the solidification shrinkage of the weld 8 can make the first material 1 and the third material 3 clamp the second material 2 and compress and fix it. It should be noted that there is no problem in irradiating the laser 7 from the third material 3 side by setting the laser irradiation direction to the lower side instead of the upper side. In this case, the first homogeneous metal material of the present disclosure is equivalent to the third material 3, and the second homogeneous metal material of the present disclosure is equivalent to the first material 1.
[0062] In addition, the materials of the first material 1 and the third material 3 are the same type of metal materials, and are respectively recorded as soft steel materials, but as long as they are the same type of metal materials that can be welded and can obtain bonding strength, there is no problem even if the materials are different. For example, the first material 1 and the third material 3, which are the same type of metal materials, are soft steel materials, stainless steel materials, high-strength steel materials, etc., which are iron-based metal materials, or a combination of soft steel and high-strength steel (high-tensile steel), high-strength steel and stainless steel, etc., or a combination of aluminum materials, aluminum alloys, aluminum and aluminum alloys, etc., which are non-ferrous metal materials, and are materials that can be laser-joined.
[0063] On the other hand, regarding the second material 2 as a dissimilar material, copper, various resin materials, or materials with poor compatibility with the first material 1 and the third material 3 in terms of welding bonding, which have low laser absorption and are difficult to perform laser joining (for example, a combination in which the first material 1 and the third material 3 are respectively soft steel materials and the second material 2 is aluminum. Or there is also the opposite combination (the first material 1 and the third material 3 are aluminum materials and the second material 2 is soft steel)) are suitable.
[0064] It should be noted that in the irradiated area of the laser beam 7, the thickness of the second material 2 sandwiched between the first material 1 and the third material 3 is 6% or more and 38% or less relative to the thickness of the first material 1 or the third material 3 as the same type of metal material on the side irradiated with the laser beam 7, which is a range in which compression and fixation can be performed by welding. On the other hand, if the thickness of the second material 2 as a different type of material is used as a reference, in other words, the thickness of the first material 1 or the third material 3 as the same type of metal material on the side irradiated with the laser beam 7 is a predetermined thickness corresponding to the thickness of the different type of material or the gap in the thickness direction, i.e., the first gap 11, which is a gap 250% or more and 1600% or less of the thickness of the second material 2 as the different type of material or the first gap 11, and if welding is performed within this thickness range, it is a range in which compression and fixation can be performed. As a result, the first material 1 and the third material as the same type of metal material can be melt-bonded to each other and the second material 2 as the different type of material can be compressed and fixed.
[0065] <Example>
[0066] Figure 4 An embodiment is shown in which a second material 2 as a dissimilar material and a fourth material 10 as a dissimilar material different from the second material 2 are sandwiched and joined between a first material 1 and a third material 3. When the first material 1 and the third material 3 are sandwiched by metal materials of the same type, and the total thickness of the second material 2 and the fourth material 10 sandwiched therebetween is set as a first gap 11, laser welding is performed in a state where the size of the first gap 11 is appropriate.
[0067] For example, in the irradiated area of the irradiated laser 7, the distance of the first gap 11 is set to be not less than 6% and not more than 38% of the thickness of the first material 1 as the upper plate. Thus, the second material 2 and the fourth material 10 can be crimped and fixed by the first material 1 and the third material 3 using the compressive force 6 generated by the solidification shrinkage of the molten metal at the welding portion 8 of the first material 1 and the third material 3. In particular, when two different dissimilar materials, namely the second material 2 and the fourth material 10, are resin materials such as PET materials or non-metallic materials such as CFRP, the transmittance of the laser 7 is high in most cases, and it is difficult to directly join the dissimilar materials to each other, so this embodiment is effective.
[0068] In addition, as the shape of the first material 1, Figure 2B and Figure 2C Shown in Figure 2A Examples other than circular welding. Figure 2B When viewed from above, the scanning trajectory of the laser beam 7 (not shown) as the welding shape is elliptical. Figure 2B As shown, the width W2 of the second material 2 and the third material 3 is greater than Figure 2AThe width W1 shown is large, and when the strength required for the welded portion 8 during welding by irradiation with the laser 7 has directionality, it is sufficient to arrange the long side direction of the ellipse of the first material 1 in the direction of the width W2 of the second material 2 and the third material 3 along the direction of high strength. In this way, the area can be reduced without making the first material 1 into a large circular shape.
[0069] In addition, through Figure 2C By making the weld shape linear, for example, the first material 1 can be made rectangular instead of a large circle. Thus, the area of the first material 1 can be reduced. Furthermore, by making the scanning trajectory of the laser 7 one or more linear, the scanning of the laser 7 becomes simpler than welding at multiple locations in a circular or elliptical shape, and welding can be achieved in a short time.
[0070] In addition, embodiments for further improving strength or facilitating positioning may be implemented such as Figure 5A and Figure 5B shown.
[0071] exist Figure 5A In the embodiment, the first material 1 also has the function of positioning the second material 2 when the third material 3 is joined to the second material 2. Specifically, the second material 2 can be easily positioned by making the second material 2, which is a different material, abut against the step portion of the first material 1 bent into a step shape, and sandwiching the second material 2 between the first material 1 and the third material 3.
[0072] in addition, Figure 5A The joining structure shown is a joining structure that improves the tensile strength of the joining portion. Specifically, it is a joining structure (double support) in which the first material 1 is joined to the third material 3 via the second material 2 at the welding portion 8, and the first material 1 is directly joined to the third material without passing through the second material at the welding portion 8a different from the welding portion 8. Thus, when an external force caused by the pulling and twisting of the second material 2 is applied to the third material 3, the stress is dispersed to the welding portion 8 and the welding portion 8a. Therefore, it is possible to suppress the situation in which stress acts concentratedly on the welding portion 8 of the first material 1 and the third material 3 joined via the second material 2. Thus, as a whole, the strength of the joining of the same type of metal material and the different type of material can be improved.
[0073] In addition, you can Figure 5B In this way, the third material 3 is folded back, thereby eliminating the need for the first material 1, and the function of the upper plate of the first material 1 that clamps the second material 2 is included in the third material 3, thereby forming an integrated structure that does not require the first material 1. In addition, by setting the structure in which the second material 2 is pressed against the bent side of the third material 3 (folding back), the positioning of the second material 2 becomes easy.
[0074] Here, in Figure 5B In the embodiment, the first metal material of the same type disclosed in the present invention corresponds to the upper plate portion formed by folding back the third material 3, and the second metal material of the same type disclosed in the present invention corresponds to the lower plate portion formed by folding back the third material 3. That is, the first metal material of the same type disclosed in the present invention and the second metal material of the same type disclosed in the present invention may be integrated before welding.
[0075] As described above, the joining structure based on the laser 7 of the present embodiment for welding comprises: a first homogeneous metal material; a second homogeneous metal material that can be mutually welded with the first homogeneous metal material; and a through hole 4 as an example of a through portion, which is sandwiched between the first homogeneous metal material and the second homogeneous metal material, and is a dissimilar material that is difficult to weld with respect to the first homogeneous metal material and the second homogeneous metal material. In the plate thickness direction in the irradiation area where the laser 7 is irradiated toward the through portion, the plate thickness in the irradiation area of the first homogeneous metal material located on the side irradiated with the laser 7 is a prescribed thickness corresponding to the dissimilar material. The first homogeneous metal material and the second homogeneous metal material are mutually melted and bonded via the through hole 4 to compress and fix the dissimilar materials, thereby fixing the dissimilar materials to the first homogeneous metal material and the second homogeneous metal material.
[0076] Thus, the first material 1 and the third material, which are metal materials of the same type, are melt-bonded to each other, and the second material 2, which is a different type of material, can be compressed and fixed.
[0077] (Implementation Method 2)
[0078] Next, regarding the second embodiment, use Figure 1 and Figure 6 Provide explanation.
[0079] In this joining structure, the area irradiated by the laser 7 in the plate thickness direction has a specified distance relative to the end of the through hole 4 of the second material 2, and the joining structure has a second gap 5 which is the distance between the end of the through hole 4 of the second material 2 and the outer dimension of the welding part 8.
[0080] It should be noted that the outer dimensions of the welded portion 8 are of a size corresponding to the outer dimensions of the irradiation region of the laser beam 7 .
[0081] Here, when the second material 2 is welded by utilizing the welding heat input transferred from the weld portion 8 melted by the irradiation of the laser beam 7 , the positional relationship between the second material 2 and the second gap 5 is important.
[0082] If the distance of the second gap 5 relative to the through hole 4 is set within an appropriate range, the second material 2 as a different material is indirectly affected by the heat of welding input to the weld 8 of the first material 1 and the third material 3 as the same type of metal material due to the irradiation of the laser 7. Then, the second material 2 as a different material, which is softened and melted, stably flows into the gap between the through hole 4 of the second material 2 and the outer edge of the weld 8, that is, the second gap 5. That is, the second material 2 as a different material is indirectly input with heat and melted due to the welding heat input of the first material 1 as the first same type of metal material during the laser 7 welding. In addition, the second material 2 as a different material can flow to the outer edge of the weld 8 formed by the first material 1 as the first same type of metal material and the third material as the second same type of metal being melted and joined to each other, and is closely fixed to the outer edge. As a result, not only the compression and fixing effect caused by the solidification shrinkage of the weld 8, but also the close bonding of the surfaces of the first material 1 and the third material 3 and the second material 2 can be achieved.
[0083] If welding is performed in a state where the distance between the through hole 4 of the second material 2 and the outer edge of the weld 8 formed by irradiation of the laser 7 in the direction of the plate thickness, i.e., the second gap 5, is too close, the through hole 4 of the second material 2 will be directly or indirectly affected by the thermal input of the welding heat of the weld 8 generated by the irradiation of the laser 7.
[0084] Thus, the molten second material 2 flows into the gap of the welded portion 8 when welding between the first material 1 and the third material 3. When the second material 2 is a material with a low boiling point such as resin, the resin material of the second material 2, which is a different material, may be vaporized and ejected, causing welding failure. On the other hand, when the distance of the second gap 5 is too far away from the through hole 4, the second material 2 is not melted, so that only the compression fixing effect due to the solidification shrinkage effect exists.
[0085] Here, the relationship between the melting state of the first material 1 and the third material 3 due to the influence of heat and the second gap 5 changes depending on the material of the second material 2 .
[0086] As an example, Figure 6 An example of experimental data is shown. Figure 6 This is a measurement result obtained by measuring the relationship between the material of the second material 2 and the second gap 5 .
[0087] Figure 6 This is a graph obtained by measuring the relationship between the material of the second material 2 as a different material and the second gap 5 according to the embodiment of the present disclosure.
[0088] The data are experimental data when the second material 2 is a PET (polyethylene terephthalate) material and a CFRP (Carbon Fiber Reinforced Plastics) material, which are examples of a resin material, and an A5000-based aluminum alloy material, which is a non-ferrous metal.
[0089] This is an example of circular welding with a laser output of 3kW in which the first material 1 and the third material 3 are made of mild steel and have a plate thickness of 1.6 mm, and any of the various materials of the second material 2 as a different material with a plate thickness of 0.4 mm is overlapped in between. In addition, the through hole 4 of the second material 2 is φ12 mm, and circular laser welding is performed. At this time, the first gap 11 is 0.4 mm, which is equal to the plate thickness of the second material 2.
[0090] In the case where the second material 2 is a PET material as a resin material, as long as the second gap 5 is greater than 0.8 mm, that is, the second gap 5 is greater than 200% relative to the first gap 11, even if the second material 2 is thermally affected by the welding heat input generated by the laser 7 welding the first material 1 and the third material 3, there will be no situation in which the molten second material 2 flows into the gap of the welding portion 8 between the first material 1 and the third material 3 to cause poor joining, and compression fixing can be performed.
[0091] However, if the second gap 5 is less than 0.8 mm, that is, the second gap 5 is less than 200% relative to the first gap 11, the outer periphery of the welding portion 8 which is the irradiation range of the laser 7 is too close to the through hole 4 of the second material 2, and the heat generated by the welding of the first material 1 and the third material 3 will cause the molten second material 2 to flow into the welding portion 8 between the first material 1 and the third material 3 during welding, vaporize and spray out, causing poor welding.
[0092] In the case of a CFRP material which is an example of a fiber-reinforced resin among resin materials, as long as the second gap 5 is greater than 0.6 mm, that is, the second gap 5 is greater than 150% relative to the first gap 11, even if the first material 1 and the third material 3 are thermally affected by the laser 7 welding, the molten second material 2 will not flow into the welding portion 8 between the first material 1 and the third material 3 to cause poor joining, and the second material 2 can be compressed and fixed.
[0093] However, if the second gap 5 is less than 0.6 mm, that is, the second gap 5 is less than 150% relative to the first gap 11, the outer periphery of the welded portion 8 as the irradiation range of the laser 7 is too close to the through hole 4 of the second material 2, and the second material 2 is melted by the heat of the welding of the first material 1 and the third material 3 and flows into the welded portion 8 between the first material 1 and the third material 3 during welding, and is vaporized and ejected, which may cause welding failure. As described above, the size of the second gap 5 allowed during welding varies depending on the characteristics such as the melting point or boiling point of the resin material of the second material 2 as a different material sandwiched between the same type of metal materials.
[0094] It should be noted that, in the case where the second material 2 is an A5000 series aluminum alloy material as an example of a non-ferrous metal, as long as the second gap 5 is greater than 0.5 mm, that is, the second gap 5 is greater than 125% relative to the first gap 11, then even if it is affected by the heat of the welding of the first material 1 and the third material 3, the second material 2 will not melt and flow into the gap of the weld 8 between the first material 1 and the third material 3 during welding to cause poor joining, and compression fixing can be performed.
[0095] However, if the second gap 5 is less than 0.5 mm, that is, the second gap 5 is less than 125% of the first gap 11, the molten second material 2 flows into the gap of the welded portion 8 between the first material 1 and the third material 3 due to the heat of welding, resulting in poor fusion and poor joining. As described above, there are cases where poor joining occurs depending on the material properties.
[0096] The above content is experimental data showing an example of the difference caused by the material of the second material 2. However, if the second material 2 is a resin material, there is a tendency that the size of the second gap 5 is almost the same as that of the PET material. Moreover, among resin materials, as long as it is a fiber-reinforced resin such as a CFRP material, there is a tendency that the size of the second gap 5 is almost the same as that of the CFRP material. Moreover, if the second material 2 is a non-ferrous metal, when the size of the second gap 5 is less than 0.5 mm, that is, the second gap 5 is less than 125% of the first gap 11, even an A5000 series aluminum alloy material may cause poor bonding. There are almost similar tendencies in other non-ferrous metals.
[0097] (Implementation method 3)
[0098] Next, regarding the third embodiment, use Figure 7The description of the parts repeated so far is omitted. The difference from the first embodiment is that when the thickness of the second material 2 sandwiched between the first material 1 and the third material 3 is large, a spacer 9 made of the same type of metal material that can be welded with the first material 1 and the third material 3 is arranged inside the through hole 4 of the second material 2, and the first gap 11, which is the gap between the first material 1 and the third material 3 in the thickness direction of the plate, is reduced in the through hole 4 of the second material 2 when the laser 7 is irradiated and welded.
[0099] The plate thickness of the spacer 9 is set so that the size of the first gap 11 in the plate thickness direction when the spacer 9 is arranged between the first material 1 and the third material 3 in the through hole 4 of the second material 2 in the irradiated area of the laser 7 is 6% to 38% of the plate thickness of the first material 1 as the upper plate irradiated by the laser 7. It should be noted that the spacer 9 arranged between the first material 1 and the third material 3 may not only be arranged separately as another component, but may also be directly formed between the first material 1 and the third material 3 using a welding material such as a melting electrode or a filler.
[0100] In this case, as in the first and second embodiments, if the range of the first gap 11 is Figure 3 The range of the first gap 11 is specified to correspond to the plate thickness of the first material 1 or the third material 3 of the same type of metal material on the side irradiated with the laser 7 as shown. By setting the gap in the plate thickness direction of the through hole 4 of the first material 1 and the third material 3, i.e., the first gap 11, keyhole-type laser welding is performed so as to penetrate to the third material 3 as the lower plate. As a result, the solidification shrinkage of the weld 8 becomes a compressive force 6, which can compress and fix the second material 2.
[0101] It should be noted that when the first gap 11 exceeds 31% to 38% of the maximum thickness of the same type of metal material on the side irradiated with the laser 7, the amount of molten metal required for the first gap 11 cannot be ensured, so a state of partial opening occurs.
[0102] On the contrary, when the gap in the plate thickness direction, i.e., the first gap 11, is less than 0.1 mm, the gap is too small, and the compression fixing force for melting and bonding the first material 1 and the third material 3, which are the same type of metal materials, and compressing and fixing the second material 2, which is a different type of material, is insufficient.
[0103] It should be noted that in the present embodiment, regarding the laser irradiation direction, the laser 7 is irradiated from the first material 1 side as the upper plate, but there is no problem in irradiating from the third material 3 side as the lower plate. In this case, the first homogeneous metal material of the present disclosure corresponds to the third material 3, and the second homogeneous metal material of the present disclosure corresponds to the first material 1.
[0104] (Summarize)
[0105] Rivets, which are conventional components for joining dissimilar materials, require complex rivet shapes such as rounded chamfers and annular grooves in order to ensure space for a portion of the dissimilar material to deform and move during riveting and spot welding and to prevent the dissimilar material from sinking in due to electrode position deviation during spot welding, etc., in order to suppress a decrease in fastening force.
[0106] In this case, the rivet shape needs to be accurate and complex. Therefore, the processing of the rivet requires precision processing, etc., and the manufacturing cost is also increased. In addition, since it is spot welding, it takes time to pressurize, energize, cool, move, etc., so the productivity is low, and it needs to be clamped from both sides, so the design freedom of the joint component is limited. In addition, when the adjacent rivets are too close, the spot welding current will be shunted, resulting in insufficient formation of the weld nugget, that is, the weld solidified part produced in the weld part subjected to resistance welding. Therefore, a spacing of the joint spacing greater than the minimum limit that can form the desired weld nugget is required. As a result, there is a problem that the rigidity at the necessary position cannot be increased. Through the present disclosure, the previous problems can be solved.
[0107] As described above, the joining structure of the embodiment includes: a first metal material of the same type; a second metal material of the same type that can be welded to the first metal material of the same type; and a through hole 4 as an example of a through portion, which is sandwiched between the first metal material of the same type and the second metal material of the same type and is a different material that is difficult to weld with respect to the first metal material of the same type and the second metal material of the same type. In the plate thickness direction in the irradiation area where the laser 7 is irradiated toward the through portion, the plate thickness in the irradiation area of the first metal material of the same type located on the side irradiated with the laser 7 is a predetermined thickness corresponding to the gap in the plate thickness direction in the irradiation area that exists in the state before welding, that is, the first gap 11.
[0108] Thus, in the irradiated area of the laser, the laser is irradiated while the first gap before welding exists, the first homogeneous metal material and the second homogeneous metal material are melted and bonded to each other through the through hole 4, and the dissimilar materials are compressed and fixed, thereby fixing the dissimilar materials to the first homogeneous metal material and the second homogeneous metal material.
[0109] When this joint structure is used, complex and precision-required structural parts are no longer required. Moreover, laser welding is used instead of spot welding, so the operation time including welding can be shortened to about 25% compared to spot welding, and productivity is significantly improved. In addition, the rigidity of the necessary parts can be increased, expanding the degree of freedom in design.
[0110] The first gap 11 may correspond to the length of the through hole 4 in the plate thickness direction in the irradiated region.
[0111] The first gap 11 in the irradiated region may be 6% or more and 38% or less relative to the thickness of the first metal material of the same type in the irradiated region.
[0112] The irradiation region of the laser beam 7 in the plate thickness direction may be smaller than the through hole 4 by a predetermined second gap 5 .
[0113] The different-type material 2 can flow toward the outer edge of the weld 8 where the first metal material of the same type and the second metal material of the same type are melt-joined to each other.
[0114] The different material may be a resin material, and the second gap 5 may be 200% or more of the first gap 11 .
[0115] The different material may be a fiber-reinforced resin material, and the second gap 5 may be 150% or more of the first gap 11 .
[0116] The different material may be a non-ferrous metal, and the second gap 5 may be 125% or more of the first gap 11 .
[0117] A spacer 9 made of a material weldable to the first metal material of the same type and the second metal material of the same type may be disposed in the through hole 4 of the different type material.
[0118] Industrial Applicability
[0119] The joint structure disclosed in the present invention can significantly shorten the production cycle time and increase the rigidity of necessary parts with a simple structure when joining dissimilar materials. In addition, it is industrially useful as a joint structure for laser welding that expands the design freedom of the joined member.
Claims
1. A joining structure, characterized in that: have: The first is metal material of the same type; a second metal material of the same type, which can be welded to the first metal material of the same type; and A dissimilar material having a through portion and sandwiched between the first metal material of the same type and the second metal material of the same type, wherein the dissimilar material is difficult to weld to the first metal material of the same type and the second metal material of the same type. In a state where there is a gap, i.e., a first gap before welding, between the first homogeneous metal material and the second homogeneous metal material in the plate thickness direction in the irradiation area of the first homogeneous metal material located on the side irradiated with the laser in the plate thickness direction in the irradiation area of the first homogeneous metal material on the side irradiated with the laser, the laser is irradiated from the first homogeneous metal material side, the first homogeneous metal material and the second homogeneous metal material are melted and bonded to each other via the through-portion, and the dissimilar materials are compressed and fixed, thereby the dissimilar materials are fixed to the first homogeneous metal material and the second homogeneous metal material, and the thickness of the first gap corresponds to the plate thickness of the first homogeneous metal material. The first gap in the irradiated region is equal to or greater than 6% and equal to or less than 38% of the thickness of the first homogeneous metal material in the irradiated region.
2. The joining structure according to claim 1, wherein: The first gap corresponding to the thickness of the dissimilar material in the plate thickness direction in the irradiated region is equal to the plate thickness of the first homogeneous metal material.
3. The joining structure according to claim 1 or 2, wherein: The irradiation area of the laser irradiation in the plate thickness direction is smaller than the through portion by a predetermined second gap, and the dissimilar material is a resin material. The dissimilar material flows and comes into close contact with the outer edge of the welded portion where the first metal material of the same type and the second metal material of the same type are melt-joined to each other.
4. The joining structure according to claim 1, wherein: A spacer made of a material weldable to the first homogeneous metal material and the second homogeneous metal material is disposed in the penetration portion of the heterogeneous material.
Citation Information
Patent Citations
Dissimilar material bonding rivet, dissimilar material bonding member, dissimilar material bonding element manufacturing method, and dissimilar material bonding element
JP2015042417A
Bonding method of dissimilar materials made from metals and bonding structure thereof
CN101274387A
Method for the manufacture of a joint between a metal structure and a plastic composite structure
EP2698224A1
Car body
JP1985001077A
Method for joining dissimilar metals
JP2008006465A