Glass sheet production method

By optimizing the HF concentration and temperature in the etching solution based on the etching solution temperature, the method enhances the taper angle of through holes in glass plates, addressing the challenges of density and definition in existing glass plate manufacturing processes.

WO2024219376A1PCT designated stage expired Publication Date: 2024-10-24NIPPON ELECTRIC GLASS CO LTD

Patent Information

Application Number
PCT/JP2024/015073
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2024-04-16
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The existing methods for manufacturing glass plates with through holes result in tapered inner walls due to preferential etching near the surface, leading to issues with high-density hole formation and high-definition patterns, as the taper angle of the through holes is not adequately controlled.

Method used

A method involving laser modification followed by etching with a controlled HF concentration and temperature in the etching solution, where the HF concentration is optimized based on the etching solution temperature to increase the taper angle of the through holes, ensuring preferential removal of the modified portion and maintaining consistent etching conditions throughout the process.

Benefits of technology

This approach allows for the formation of glass plates with through holes having a large taper angle, enabling high-density and high-definition patterns on the glass surface, suitable for applications like displays and semiconductor packages.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015073_24102024_PF_FP_ABST
    Figure JP2024015073_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a glass sheet production method comprising: a modification step S1 for modifying a part 3, in which a through hole 10 is to be formed, by irradiating with laser beam L; and an etching step S2 for, after the modification step S1, immersing the glass sheet 2 in an etching solution 6 containing HF and thus forming the through hole 10 in the part 3 for the formation. The etching step S2 includes: a first etching step S2a for forming an initial through hole 9 in the part 3 for the formation; and a second etching step S2b for enlarging the initial through hole 9 to form the through hole 10. In the first etching step S2a, when the temperature of the etching solution 6 is x [°C] and the HF concentration of the etching solution 6 is y [mol / L], a relational expression of -0.04x+2.4≤y≤-0.04x+3.2 is established.
Need to check novelty before this filing date? Find Prior Art

Description

Glass plate manufacturing method

[0001] The present invention relates to a method for manufacturing a glass plate having a through hole.

[0002] For example, glass plates having minute through-holes for wiring (through electrodes, etc.) are used as substrates for tiling displays (micro LEDs, etc.), bezel-less displays, glass interposers, and the like.

[0003] A method for manufacturing a glass plate having this type of through hole includes, for example, a modification step in which the portion of the glass plate where the through hole is to be formed is modified by irradiating it with laser light, and an etching step in which, after the modification step, a through hole is formed in the portion by etching (see, for example, Patent Document 1).

[0004] The modified portion modified in the modification step has a higher etching rate than the unmodified portion not modified in the modification step. Therefore, the modified portion is preferentially removed in the etching step. Therefore, if the modified portion is formed in the portion where the through hole is to be formed, the through hole can be formed in the portion by etching.

[0005] JP 2020-196665 A

[0006] When forming through holes as described above, the portions closer to the main surface of the glass plate are more likely to be etched because they are in contact with the etching solution for a longer period of time. Therefore, the diameter of the through holes near the main surface is larger than that of the central portion in the thickness direction, and the inner wall surface of the through holes is tapered. If the taper angle of the through holes is small, the diameter of the through holes on the main surface of the glass plate becomes too large, which can cause problems such as the inability to form high-density through holes and the inability to form high-resolution patterns on the main surface of the glass plate. Here, the taper angle of the through holes refers to the angle between the direction perpendicular to the thickness direction and the inner wall surface of the through holes (see θ2 in FIG. 6 described later).

[0007] An object of the present invention is to increase the taper angle of a through hole formed in a glass plate.

[0008] As a result of extensive research, the inventors have discovered the following. Specifically, by reducing the etching rate during the etching process, the selectivity ratio (etching rate of modified portion / etching rate of unmodified portion) of the etching rate of the modified portion, which is in a diffusion-limited state, to the etching rate of the unmodified portion, which is in a reaction-limited state, can be increased. Increasing the selectivity ratio promotes preferential removal of the modified portion, allowing for a larger taper angle of the through-hole. However, the selectivity does not always increase monotonically as the etching reaction rate decreases. In other words, if the etching reaction rate is reduced too much, the etching reaction rate of the modified portion also becomes reaction-limited at some point, and the selectivity changes from an increasing trend to a decreasing trend. Furthermore, because the diffusion rate and the reaction rate have different temperature dependencies, the concentration of the etching solution at which the diffusion-limited state transitions to a reaction-limited state also varies depending on the temperature of the etching solution. Therefore, it is necessary to select an optimal etching solution concentration that matches the temperature of the etching solution.

[0009] (1) The present invention, which has been invented to solve the above-mentioned problems, is based on the above-mentioned findings and is a method for manufacturing a glass plate having a first main surface, a second main surface, and a through hole penetrating between the first and second main surfaces, the method comprising: a modification step of modifying a portion where the through hole is to be formed by irradiating the portion by laser light; and an etching step of, after the modification step, immersing the glass plate in an etching solution containing HF to form a through hole in the portion where the through hole is to be formed; the etching step includes a first etching step of forming an initial through hole in the portion where the through hole is to be formed, and a second etching step of enlarging the initial through hole to form a through hole; and the first etching step is characterized in that, when the temperature of the etching solution is x [°C] and the HF concentration of the etching solution is y [mol / L], the relational expression -0.04x + 2.4 ≦ y ≦ -0.04x + 3.2 holds.

[0010] In this way, by performing etching in the first etching step so that the above relationship holds, it is possible to select an optimal HF concentration of the etching solution that matches the temperature of the etching solution, which results in the formation of an initial through hole with a large taper angle, and also allows the formation of a through hole with a larger taper angle.

[0011] (2) In the above configuration (1), the relational expression −0.04x+2.4≦y≦−0.04x+3.2 holds true in both the first etching step and the second etching step.

[0012] In this way, it is not necessary to change the temperature and HF concentration of the etching solution between the first etching step and the second etching step, and therefore the etching steps can be performed with a simple device configuration and control method.

[0013] (3) In the above configuration (1) or (2), the temperature of the etching solution is preferably 5° C. or higher and 30° C. or lower.

[0014] If the temperature of the etching solution is too low, the etching solution may freeze, making it impossible to carry out the etching process. On the other hand, if the temperature of the etching solution is too high, the etching solution may evaporate, making it difficult to maintain a constant concentration of the etching solution. In contrast, by keeping the temperature of the etching solution within the above numerical range, the occurrence of these problems can be suppressed. In other words, the concentration of the etching solution can be stabilized while preventing the etching solution from freezing.

[0015] (4) In any of the above (1) to (3), the etching solution preferably further contains HCl.

[0016] In etching using an etching solution containing HF, fluorides containing glass components are generated as insoluble by-products. Fluorides can be a factor in reducing productivity, such as reducing the etching rate and generating defects. However, by using a mixed acid of HF and HCl as the etching solution as described above, fluorides can be replaced with soluble chlorides and efficiently removed, thereby suppressing a decrease in productivity.

[0017] (5) In any of the configurations (1) to (4) above, in the first etching step, when the etching rate in the thickness direction of the modified portion modified in the modification step is V1 [μm / min] and the etching rate in the thickness direction of the unmodified portion not modified in the modification step is V2 [μm / min], it is preferable that the selectivity ratio (V1 / V2) between V1 and V2 is 3.0 or more.

[0018] This promotes preferential removal of the modified portion, making it possible to form a through-hole with a good taper angle.

[0019] (6) In any one of the above (1) to (5), the glass plate is preferably alkali-free glass.

[0020] In this way, a glass plate having through holes that are optimal for display applications can be produced.

[0021] (7) The present invention, which has been invented to solve the above-mentioned problems, is a method for manufacturing a glass plate having a first main surface, a second main surface, and a through hole penetrating between the first main surface and the second main surface, the method comprising: a modification step of modifying a portion where the through hole is to be formed by irradiating the portion with laser light; and an etching step of, after the modification step, immersing the glass plate in an etching solution containing HF to form a through hole in the portion where the through hole is to be formed, wherein, in the etching step, when the temperature of the etching solution is x [°C] and the HF concentration of the etching solution is y [mol / L], a relational expression of -0.04x + 2.4≦y≦-0.04x + 3.2 is established.

[0022] In this way, the same effect as that of the above configuration (1) can be achieved.

[0023] (8) A glass plate manufactured by the glass plate manufacturing method according to any one of (1) to (6) above, characterized in that the plate thickness is 25 μm or more and 2500 μm or less, the diameter of the through hole in the first main surface or the second main surface is 3 μm or more and 500 μm or less, and the angle between the direction perpendicular to the plate thickness direction and the inner wall surface of the through hole is 75° or more.

[0024] In such a glass plate, the large taper angle allows through holes to be formed at a high density.

[0025] (9) The present invention, which has been invented to solve the above-mentioned problems, is a glass plate having a first main surface, a second main surface, and a through hole penetrating between the first main surface and the second main surface, wherein the plate thickness is 25 μm or more and 2500 μm or less, the diameter of the through hole in the first main surface or the second main surface is 3 μm or more and 500 μm or less, and the angle between the direction perpendicular to the plate thickness direction and the inner wall surface of the through hole is 75° or more.

[0026] In such a glass plate, the large taper angle allows through holes to be formed at a high density.

[0027] According to the present invention, the taper angle of the through hole formed in the glass plate can be increased.

[0028] FIG. 1 is a flow diagram showing a method for manufacturing a glass plate according to an embodiment of the present invention. FIG. 2 is a cross-sectional view showing a modification step. FIG. 3 is a cross-sectional view showing an etching step. FIG. 4 is a cross-sectional view of a glass plate in a first etching step, showing a state before a planned formation portion of the glass plate is penetrated. FIG. 5 is a cross-sectional view of a glass plate in a first etching step, showing a state when a planned formation portion of the glass plate is penetrated and an initial through hole is formed. FIG. 6 is a cross-sectional view of a glass plate in a second etching step, showing a state in which an initial through hole is enlarged to form a glass plate having a through hole. FIG. 7 is a graph showing the relationship between the HF concentration of an etching solution and a selectivity. FIG. 8 is a graph showing the relationship between the HF concentration of an etching solution and a taper angle of a through hole. FIG. 9 is a graph showing the relationship between the temperature of the etching solution and an optimal HF concentration of the etching solution.

[0029] Hereinafter, embodiments of the present invention will be described with reference to the drawings.

[0030] As shown in FIG. 1, the method for manufacturing a glass plate according to this embodiment includes a modifying step S1 and an etching step S2.

[0031] (Modification Process) As shown in FIG. 2 , the modification process S1 is a process of modifying a through-hole formation planned portion 3 in the glass plate 2 by using laser light L irradiated from a laser device 1. The modification process S1 results in the planned formation portion 3 including a modified portion 4. The modified portion 4 extends along the plate thickness direction and has a property of being more susceptible to etching than the unmodified unmodified portion 5. The modified portion 4 is a portion different from the unmodified portion 5 in terms of density, refractive index, stress, etc. The diameter of the modified portion 4 is, for example, 2 μm or more and 10 μm or less. The modified portion 4 may also include a non-through hole or a minute crack. The modified portion 4 is preferably formed continuously along the plate thickness direction, but may also be formed intermittently along the plate thickness direction. When forming a plurality of through holes 10 (see FIG. 6 described later) in the glass plate 2, a plurality of planned formation portions 3 including the modified portion 4 are also formed.

[0032] The type and irradiation conditions of the laser light L are not particularly limited as long as the modified portion 4 can be formed in the planned formation portion 3. In this embodiment, the laser light L is a short-pulse laser light (picosecond laser light, nanosecond laser light, or femtosecond laser light). The diameter W of the modified portion 4 can be adjusted by the spot diameter of the laser light L, for example. The spot diameter of the laser light L is, for example, 2 μm or more and 10 μm or less. The output of the laser light L is, for example, 1 W or more and 20 W or less. The focus of the laser light L is set, for example, at the middle part of the glass plate 2 in the plate thickness direction, but is not limited to this position.

[0033] The glass plate 2 may be, for example, an alkali-free glass plate, and the glass composition preferably contains, in mass %, 58 to 68% SiO, 15 to 23% (particularly 17 to 21%) AlO, 3 to 9% (particularly 5 to 7%) BO, 0 to less than 1% (particularly 0 to 0.5%) LiO + NaO + KO, 1 to 6% (particularly 1 to 4%) MgO, 3 to 13% (particularly 5 to 10%) CaO, 0 to 10% (particularly 0.1 to 3%) SrO, and 0 to 10% (particularly 2 to 7%) BaO. This allows the glass plate to be suitably used as a glass substrate for displays.

[0034] The lower limit of the thickness of the glass plate 2 before the etching step is preferably 30 μm or more, more preferably 200 μm or more, and even more preferably 400 μm or more. The upper limit of the thickness of the glass plate 2 before the etching step is preferably 3000 μm or less, more preferably 2400 μm or less, and even more preferably 1200 μm or less.

[0035] (Etching Step) The etching step S2 is a step of forming through holes 10 that penetrate the planned formation portion 3, including the modified portion 4, in the plate thickness direction between the first main surface 2a and the second main surface 2b of the glass plate 2. As shown in Fig. 1 , the etching step S2 includes a first etching step S2a of forming initial through holes 9 in the planned formation portion 3, and a second etching step S2b of enlarging the initial through holes 9 to form the through holes 10.

[0036] 3 , in the etching step S2, the glass plate 2 is immersed in an etching solution 6 containing HF. The etching solution 6 is stored in an etching tank 7. In this embodiment, etching proceeds simultaneously from both the first main surface 2 a and the second main surface 2 b of the glass plate 2.

[0037] The etchant 6 containing HF may be, for example, an aqueous solution containing only HF as an acid, or an aqueous solution containing HF and at least one acid selected from HCl, HNO3, and H2SO4. By using a mixed acid of HCl or the like and HF as the etchant 6, the poorly soluble fluoride produced as a by-product during etching can be replaced with soluble chloride and efficiently removed, thereby preventing a decrease in productivity. In particular, it is preferable to use a mixed acid of HCl and HF as the etchant 6.

[0038] When the etching step S2 is performed after the modifying step S1, the modified portions 4 are preferentially removed because the etching rate of the modified portions 4 is higher than that of the unmodified portions 5. As a result, the to-be-formed portions 3 including the modified portions 4 are gradually removed by etching, as shown in Figures 4 to 6. In Figures 4 to 6, the reference symbols 2ao and 2b indicate the positions of the main surfaces 2a and 2b before etching.

[0039] In detail, as shown in FIG. 4, in the early stage of the first etching step S2a, the portion 3 to be formed does not penetrate in the plate thickness direction, and a bottomed recess 8 having a tapered inner wall surface 8a whose opening area decreases toward the center in the plate thickness direction is formed in the portion 3 to be formed on each of the first main surface 2a side and the second main surface 2b side.

[0040] 5 , in the first etching step S2a, the intended formation portion 3 is penetrated in the plate thickness direction to form an initial through hole 9. The initial through hole 9 has a tapered first inner wall surface 9a whose opening area decreases from the first main surface 2a side toward the center in the plate thickness direction, and a tapered second inner wall surface 9b whose opening area decreases from the second main surface 2b side toward the center in the plate thickness direction, and both inner wall surfaces 9a, 9b are connected to each other at the center in the plate thickness direction.

[0041] After the initial through hole 9 is formed, in the second etching process S2b, the diameter of the initial through hole 9 is enlarged, and finally, a through hole 10 having a tapered first inner wall surface 10a and a tapered second inner wall surface 10b as shown in Figure 6 is formed.

[0042] In the first etching step S2a, when the temperature of the etching solution 6 is x [°C] and the HF concentration of the etching solution 6 is y [mol / L], the following relationship holds: -0.04x + 2.4 ≦ y ≦ -0.04x + 3.2. This allows the optimal HF concentration of the etching solution 6 to be selected in accordance with the temperature of the etching solution 6. Therefore, the selectivity ratio (V1 / V2) between the etching rate V1 [μm / min] in the thickness direction of the modified portion 4 and the etching rate V2 [μm / min] in the thickness direction of the unmodified portion 5 can be increased. As a result, the taper angle θ1 of the initial through hole 9 when the planned formation portion 3 penetrates increases. The taper angle θ2 of the finally formed through hole 10 is largely dependent on the taper angle θ1 of the initial through hole 9. Therefore, as the taper angle θ1 of the initial through hole 9 increases, the taper angle θ2 of the through hole 10 also necessarily increases. In this embodiment, the relational expression -0.04x+2.4≦y≦-0.04x+3.2 is established in both the first etching step S2a and the second etching step S2b, but this relational expression may also be established in only the first etching step S2a.

[0043] In this embodiment, the first etching step S2a is performed, and then the second etching step S2b is performed consecutively. That is, after the first etching step S2a is performed, the second etching step S2b is performed without changing the etching conditions in the same etching tank 7. This allows the etching step S2 to be performed with a simple device configuration and control method, and also allows the etching step S2 to be performed without spending time transferring the glass plate 2 to another etching tank 7 or changing the etching conditions.

[0044] The taper angle θ1 of the initial through hole 9 is preferably 75° or more, more preferably 80° or more, and even more preferably 84° or more. The taper angle θ1 of the initial through hole 9 is ideally 90°, but when the productivity of the glass plate 2 is taken into consideration, it can be, for example, 85° or less.

[0045] The temperature of the etching solution 6 is preferably 5° C. or higher. The temperature of the etching solution 6 is preferably 30° C. or lower, more preferably 20° C. or lower, and even more preferably 15° C. or lower. This can prevent problems such as the etching solution 6 freezing due to an excessively low temperature or the etching solution 6 becoming too hot, resulting in a large change in HF concentration. Note that the change in HF concentration can occur due to evaporation of HF and moisture contained in the etching solution 6.

[0046] In the first etching step S2a, the selectivity (V1 / V2) is preferably 3.0 or more, more preferably 6.0 or more, and even more preferably 10.0 or more. This promotes preferential removal of the modified region 4, allowing the formation of an initial through hole 9 having a favorable taper angle θ1. As a result, it becomes easier to form a through hole 10 having a large taper angle θ2. Meanwhile, the upper limit of the selectivity can be set to, for example, 12 or less. Here, the selectivity (V1 / V2) can be calculated, for example, as shown in FIG. 5 , by the ratio (E1 / E2) of the etching amount E1 of the modified region 4 in the thickness direction when the initial through hole 9 is formed and penetrates the planned formation region 3 to the etching amount E2 of the unmodified region 5 in the thickness direction when the initial through hole 9 is formed and penetrates the planned formation region 3. The etching amounts E1 and E2 are calculated based on the position 2a0 on the main surface 2a and / or the position 2b on the main surface 2b of the glass plate 2 before etching. Specifically, for example, the etching amount E1 of the modified portion 4 can be calculated by (thickness of the glass plate 2 before etching) / 2, and the etching amount E2 of the non-modified portion 5 can be calculated by [(thickness of the glass plate 2 before etching) - (thickness of the glass plate 2 when the planned formation portion 3 penetrates)] / 2. When calculating the selectivity ratio (V1 / V2), the etching amounts E1 and E2 may be calculated from one glass plate 2, or, if the processing conditions are the same, the etching amounts E1 and E2 may be calculated from two glass plates 2, respectively. In this embodiment, the second etching step S2b also maintains substantially the same selectivity as the first etching step S2a.

[0047] The lower limit of the thickness of the glass plate 2 after the etching step is preferably 25 μm or more, more preferably 150 μm or more, and even more preferably 300 μm or more. The upper limit of the thickness of the glass plate 2 after the etching step is preferably 2500 μm or less, more preferably 2000 μm or less, and even more preferably 1000 μm or less.

[0048] The glass plate 2 can be used as a substrate for a tiling display (such as a micro LED), a bezel-less display, a glass interposer, or the like, or as a core substrate for a semiconductor package.

[0049] The lower limit of the diameter of the through hole 10 on the first main surface 2a and the second main surface 2b is preferably 3 μm or more, more preferably 20 μm or more, and even more preferably 40 μm or more. The upper limit of the diameter of the through hole 10 on the first main surface 2a and the second main surface 2b is preferably 500 μm or less, more preferably 400 μm or less, and even more preferably 200 μm or less. If the through hole 10 is within this range, it can be suitably used as a substrate for a tiling display (such as a micro LED), a bezel-less display, a glass interposer, or the like, or as a core substrate for a semiconductor package.

[0050] The present invention is not limited to the configuration of the above-described embodiment, nor is it limited to the above-described effects. The present invention can be modified in various ways without departing from the spirit of the present invention.

[0051] In the above embodiment, the etching step S2 may include a measurement step of measuring the temperature of the etching solution 6 and the HF concentration of the etching solution 6, and an adjustment step of adjusting at least one of the temperature and the HF concentration of the etching solution 6 based on the results of the measurement step. In this way, the HF concentration of the etching solution 6 can be reliably maintained at an optimum value in accordance with the temperature of the etching solution 6.

[0052] In the above embodiment, the etching step S2 may include a cleaning step of removing the glass plate 2 from the etching solution 6 and cleaning it. In this way, impurities such as fluorides formed in the etching step S2 can be efficiently removed.

[0053] In the above embodiment, when a plurality of through holes 10 are formed, the plurality of through holes 10 may be formed regularly at high density.

[0054] In the above embodiment, the etching solution 6 may be stirred during the etching step S2. Methods for stirring the etching solution 6 include vibrating the etching solution 6 with ultrasonic waves, or rotating or vibrating a stirring member to stir the etching solution 6. Furthermore, the output of the ultrasonic waves or the rotation speed or frequency of the stirring member may be changed during the etching step S2.

[0055] In the above embodiment, the first etching step S2a is performed followed by the second etching step S2b. However, this is not limiting. The etching conditions may be different between the first etching step S2a and the second etching step S2b. For example, in the first etching step S2a, the initial through-holes 9 are not formed, so the etching liquid in the recesses 8 cannot move in the thickness direction. Therefore, even if the stirring speed of the etching liquid 6 is increased in the first etching step S2a, the exchange efficiency of the etching liquid 6 in the recesses 8 is unlikely to be improved. On the other hand, in the second etching step S2b, the initial through-holes 9 are formed, so the etching liquid 6 in the initial through-holes 9 can move in the thickness direction. Therefore, by increasing the stirring speed of the etching liquid 6 in the second etching step S2b, the exchange efficiency of the etching liquid in the initial through-holes 9 can be improved. Alternatively, after the first etching step S2a is performed, the glass plate 2 may be transferred to another etching tank 7, and the second etching step S2b may be performed. This allows the change in etching conditions to be completed quickly when changing the etching conditions between the first etching step S2a and the second etching step S2b.

[0056] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples.

[0057] A glass plate made of alkali-free glass (OA-11 manufactured by Nippon Electric Glass Co., Ltd.) with a thickness of 500 μm before etching was prepared. Next, a modified portion was formed by irradiating a short-pulse laser beam to a planned formation portion of the prepared glass plate using a Vitrion 5510 device manufactured by LPKF. Thereafter, the glass plate on which the modified portion was formed was immersed in an etching solution containing HF and etched to form a through hole in the planned formation portion.

[0058] In the first evaluation test, when forming through holes as described above, the selectivity (etching rate V1 in the plate thickness direction of the modified portion / etching rate V2 in the plate thickness direction of the unmodified portion) was evaluated for changes in the HF concentration of the etching solution when the temperature of the etching solution was 5° C., 10° C., 20° C., and 30° C. The results of the first evaluation test are shown in FIG.

[0059] In addition, as a second evaluation test, when forming the through holes as described above, the change in the taper angle of the initial through holes was evaluated when the HF concentration of the etching solution was changed for each of the cases where the temperature of the etching solution was 5° C., 10° C., 20° C., and 30° C. The results of the second evaluation test are shown in FIG.

[0060] 7 also confirms that, regardless of whether the temperature of the etching solution is 5°C, 10°C, 20°C, or 30°C, a peak at which the selectivity is maximized is observed as the HF concentration of the etching solution decreases. This is because the etching reaction in the modified region transitions from a diffusion-limited to a reaction-limited state as the HF concentration of the etching solution decreases. In other words, the selectivity peaks at which the selectivity is maximized at the HF concentration at which the etching reaction in the modified region transitions from a diffusion-limited to a reaction-limited state.

[0061] 8 also confirms that the taper angle reaches a maximum peak as the HF concentration of the etching solution decreases, regardless of whether the etching solution temperature is 5° C., 10° C., 20° C., or 30° C. In addition, the change in the taper angle in FIG. 8 corresponds to the change in the selectivity in FIG. 7. In other words, it can be confirmed that the taper angle increases as the selectivity increases, regardless of whether the etching solution temperature is 5° C., 10° C., 20° C., or 30° C.

[0062] Then, in the results of Fig. 8, the data for etching solution temperatures of 5°C, 10°C, 20°C, and 30°C were fitted with a quadratic function to determine the HF concentration of the etching solution at which the taper angle was maximized (optimum HF concentration) for each temperature. Fig. 9 shows the relationship between the temperature (liquid temperature) of the etching solution and the optimal HF concentration of the etching solution.

[0063] When the temperature of the etching solution is x [°C] and the optimum HF concentration of the etching solution is y [mol / L], the relationship between the optimum HF concentration of the etching solution and the temperature of the etching solution shown in FIG. 9 can be approximated by the following formula (1): y = -0.04x + 2.8 (1)

[0064] 8, the decrease in the taper angle of the initial through hole was 0.1° or less if the optimum HF concentration of the etching solution was within ±0.4 [mol / L]. Therefore, it can be seen that if the relationship between the optimum HF concentration of the etching solution and the temperature of the etching solution satisfies the following formula (2), the taper angle of the initial through hole can be maintained at a large value. -0.04x + 2.4≦y≦-0.04x + 3.2 (2)

[0065] In FIG. 8 , when the temperature of the etching solution is 5° C., the four data points from the left are comparative examples that do not satisfy formula (2), and the two data points from the right are examples that satisfy formula (2). When the temperature of the etching solution is 10° C., the three data points from the left and the one data point from the right are comparative examples that do not satisfy formula (2), and the two data points between them are examples that satisfy formula (2). When the temperature of the etching solution is 20° C., the three data points from the left and the two data points from the right are comparative examples that do not satisfy formula (2), and the one data point between them is an example that satisfies formula (2). When the temperature of the etching solution is 30° C., the two data points from the left and the two data points from the right are comparative examples that do not satisfy formula (2), and the two data points between them are examples that satisfy formula (2).

[0066] REFERENCE SIGNS LIST 1 laser device 2 glass plate 3 formation target portion 4 modified portion 5 non-modified portion 6 etching solution 7 etching bath 8 recess 9 initial through hole 10 through hole L laser light S1 modification step S2 etching step S2a first etching step S2b second etching step θ1 taper angle of initial through hole θ2 taper angle of through hole

Claims

1. A method for manufacturing a glass plate having a first main surface, a second main surface, and a through hole penetrating between the first main surface and the second main surface, comprising: a modification step of modifying a portion where the through hole is to be formed by irradiating the glass plate with laser light; and an etching step of, after the modification step, immersing the glass plate in an etching solution containing HF to form the through hole in the portion where the through hole is to be formed, the etching step including a first etching step of forming an initial through hole in the portion where the through hole is to be formed, and a second etching step of enlarging the initial through hole to form the through hole, wherein in the first etching step, a relational expression of -0.04x + 2.4≦y≦-0.04x + 3.2 is satisfied, where x [°C] is the temperature of the etching solution and y [mol / L] is the HF concentration of the etching solution.

2. The method for producing a glass plate according to claim 1, wherein the relationship -0.04x+2.4≦y≦-0.04x+3.2 is satisfied in both the first etching step and the second etching step.

3. A method for manufacturing a glass plate according to claim 1 or 2, wherein the temperature of the etching solution is 5°C or higher and 30°C or lower.

4. The method for manufacturing a glass plate according to claim 1 or 2, wherein the etching solution further contains HCl.

5. A method for manufacturing a glass plate as described in claim 1 or 2, wherein in the first etching step, when an etching rate in the plate thickness direction of the modified portion modified in the modification step is V1 [μm / min] and an etching rate in the plate thickness direction of the non-modified portion not modified in the modification step is V2 [μm / min], the selectivity ratio (V1 / V2) between V1 and V2 is 3.0 or more.

6. The method for manufacturing a glass plate according to claim 1 or 2, wherein the glass plate is an alkali-free glass.

7. A method for manufacturing a glass plate having a first main surface, a second main surface, and a through hole penetrating between the first main surface and the second main surface, comprising: a modification step of modifying an area where the through hole is to be formed by irradiating the area with laser light; and an etching step of, after the modification step, immersing the glass plate in an etching solution containing HF to form the through hole in the area where the through hole is to be formed, wherein, in the etching step, when the temperature of the etching solution is x [°C] and the HF concentration of the etching solution is y [mol / L], a relational expression of -0.04x + 2.4≦y≦-0.04x + 3.2 is satisfied.

8. A glass plate manufactured by the manufacturing method according to claim 1 or 2, characterized in that the plate thickness is 25 μm or more and 2500 μm or less, the diameter of the through hole in the first main surface or the second main surface is 3 μm or more and 500 μm or less, and the angle between the direction perpendicular to the plate thickness direction and the inner wall surface of the through hole is 75° or more.

9. A glass plate having a first main surface, a second main surface, and a through hole penetrating between the first main surface and the second main surface, the plate thickness being 25 μm or more and 2500 μm or less, the diameter of the through hole in the first main surface or the second main surface being 3 μm or more and 500 μm or less, and the angle between the direction perpendicular to the plate thickness direction and the inner wall surface of the through hole being 75° or more.

Citation Information

Patent Citations

  • Method for producing glass articles by laser damage and etching

    JP2016506351A

  • Glass substrate having microstructure and production method for glass substrate having microstructure

    WO2020129553A1

  • Glass etching solution and glass substrate manufacturing method

    WO2020179312A1

  • Glass substrate having through hole

    WO2022075068A1

Cited By

  • Method for producing glass plate, glass plate, etching device, and device for producing glass plate

    WO2026105460A1