Particle-based anisotropic composites for magnetic cores
By applying a magnetic field to the matrix material of the magnetic core, the ferromagnetic particles form a chain structure, the energy loss problem caused by eddy current is solved, efficient magnetic permeability and low-cost manufacturing are achieved, and it is suitable for a variety of magnetic equipment.
Patent Information
- Application Number
- CN202080038058.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-06-17
- Filing Date
- 2020-06-04
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-06-04
AI Technical Summary
In applications such as transformers and inductors, existing magnetic cores have frequency-related problems due to energy loss caused by eddy currents. The existing manufacturing methods rely on laminated thin film cores or thin film cores, which are costly and complex in manufacturing process.
Using anisotropic composite materials, the ferromagnetic particles form a chain structure by applying a magnetic field to form a magnetic conduction permeability, and suppressing eddy currents. The combination of microns and nanoparticles is used to increase the direction of the applied magnetic field. Magnetic permeability, reduce electrical conduction and eddy current in the vertical direction.
It realizes improving magnetic permeability in the direction of the magnetic field, reducing eddy currents in the vertical direction, reducing manufacturing costs, and providing a fast and low-cost manufacturing process. It is suitable for inductors, transformers, amplifiers and other equipment.
Smart Images

Figure CN113853661B_ABST
Abstract
Description
Background Art
[0001] The present disclosure relates generally to the field of magnetic cores, such as those used in inductors, amplifiers, transformers and power supply devices, and methods of making such devices and such magnetic cores. In particular, it relates to magnetic cores obtained by arranging ferromagnetic particles into chains by applying a magnetic field.
[0002] A magnetic core is an object made of a magnetic material with high magnetic permeability. Such materials are used to confine and guide magnetic fields in various devices. Typically, magnetic cores are used to significantly increase the magnetic field strength in electromagnetic coils. Nevertheless, side effects can be observed, for example in applications such as transformers and inductors, which are mainly caused by eddy currents (in AC devices). This leads to frequency-dependent energy losses. Different manufacturing methods have been proposed, which rely in particular on laminated thin-film cores, radial field-oriented sputtering of thin-film cores or uniformly distributed particles (forming the composite material of the inductor core). Summary of the invention
[0003] According to a first aspect, the present invention is embodied as a magnetic core. The core comprises an anisotropic composite material, which itself comprises a matrix material (e.g., a dielectric, a non-magnetic material or a paramagnetic material) and magnetically arranged ferromagnetic particles. The particles may, for example, comprise micrometers and / or nanometer particles. They form particle chains in the matrix material. Such chains form a permeation path for magnetic conduction. The path extends along a first direction, whereby each chain extends substantially along the first direction. However, these chains remain different and away from each other along a second direction perpendicular to the first direction and possibly along a third direction perpendicular to both the first and second directions. The composite material preferably comprises 10 to 50 volume percent of ferromagnetic particles. The chain may, for example, be arranged substantially according to a parallel line configuration, a concentric ring configuration or a racetrack configuration of a particle chain.
[0004] The solution relies on a magnetic assembly of ferromagnetic particles, where the penetration of the particles is applied in the direction of the applied magnetic field during fabrication, while being suppressed (or mitigated) in the perpendicular direction. This results in an increased effective magnetic permeability in the direction of the applied magnetic field, while suppressing (or at least mitigating) the electrical conduction and, thus, the eddy currents in the perpendicular direction. That is, the magnetic flux is enhanced along the direction of the chain, while the electrical conduction and eddy currents are reduced in the perpendicular direction. As one may appreciate, this approach advantageously allows for a fast and low-cost manufacturing process compared to, for example, thin film microfabrication.
[0005] Preferably, the particles include first particles (first type) and second particles (second type), wherein the second particles have an average diameter smaller than the first particles. For example, the first particles may include micron-sized particles, while the second particles may include nano-sized particles. The second particles may advantageously be used to form a necking bridge between the first particles, bridging the latter in a first direction.
[0006] The first and second particles will preferably have an average sintering temperature that is significantly lower than the melting temperature of the matrix material to allow a sintering process to enhance the mechanical stability and magnetic permeability of the chain.
[0007] According to another but related aspect, the invention is embodied in a magnetic device comprising a magnetic core as described above. The device may in particular be an inductor, a transformer, an amplifier or a power supply device.
[0008] According to another aspect, the present invention is embodied as a method for manufacturing a magnetic core as described above. According to the method: a matrix material is provided, comprising ferromagnetic particles, and a magnetic field is applied to magnetically align the ferromagnetic particles in the matrix material, thereby forming an anisotropic composite material for the magnetic core. Consistent with the first aspect of the invention mentioned above, this is performed to form particle chains (e.g., comprising micron-sized particles) within the matrix material, wherein the chains form a permeable path for magnetic conduction extending along a first direction. That is, the chains each extend along a first direction while being different and away from each other along a second direction perpendicular to the first direction, as described above. Also as described above, the ferromagnetic particles introduced into the matrix material can typically account for 10 to 50 volume percent of the composite material formed.
[0009] The applied magnetic field preferably has a strength of at least 20 mT. The magnetic field can be applied in particular using permanent magnets and / or electromagnets. In all cases, the magnetic field can be applied so that the chain is arranged according to a parallel line configuration, a concentric ring configuration or a racetrack configuration of the particle chain.
[0010] Preferably, the introduced particles include first particles (ie, particles of a first type), and second particles (of a second type), wherein the average diameter of the second particles is smaller than the average diameter of the first particles.
[0011] For example, the first particles may include micron-sized particles, and the second particles may include nano-sized particles, as described above. The method may then include forming a necking bridge between the first particles while applying a magnetic field so as to bridge the first particles due to the second particles and along the first direction. The formation of the necking bridge may also rely on a sintering process to sinter the first particles and the second particles.
[0012] Finally, if desired, the chains are fixed in the formed composite material, for example by crosslinking a matrix material, which may be, for example, a photopolymer or a heat-cured epoxy resin. Note that the composite material may be formed by successively forming layers of the composite material, which may be achieved by repeating the above-described method steps.
[0013] In a preferred embodiment, the matrix material is provided in a structured template to constrain the shape of the final formed composite material.
[0014] For the sake of completeness, the magnetic core obtained can finally be integrated in a device in order to obtain, for example, an inductor, an amplifier or a transformer, a power supply device, etc.
[0015] Apparatus and methods embodying the invention will now be described by way of non-limiting examples and with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The accompanying drawings, in which like reference numerals refer to the same or functionally similar elements in the individual views, and together with the following detailed description, are incorporated into and form a part of this specification and are used to further illustrate various embodiments and to explain various principles and advantages according to the present disclosure, wherein:
[0017] Figure 1 is a top view showing a particle chain formed in a magnetic core according to an embodiment;
[0018] Figure 2A and 2B The embodiment involved in the example Figure 1 Neck bridges formed between particles of the chain shown;
[0019] Figure 3 is a microscope photograph of an actual core according to an embodiment, including Figure 1 The linear chain in ;
[0020] Figure 4 yes Figure 1 Top view of a variant of a linear configuration of the device. Figure 4 A magnetic core showing concentric chains according to an embodiment is shown.
[0021] Figure 5 is a 3-dimensional (3D) view of another variation of a magnetic core according to an embodiment, wherein the chain involves a percolation path between two perpendicular but not parallel chain rows;
[0022] Figure 6 is a 3D view of a toroidal inductor including a magnetic core according to an embodiment;
[0023] Figure 7 is a graph showing a possible multimodal distribution of ferromagnetic grain size in a magnetic core according to an embodiment; and
[0024] Figure 8 is a flow chart showing high-level steps of a method for manufacturing a magnetic core according to an embodiment.
[0025] Figure 1 , 2A , 2B and 4-6 show simplified representations of devices or parts thereof as involved in the embodiments. In particular, Figure 1 , 2A, 2B, 4 and 5 are intended to be schematic representations. The technical features depicted in the drawings are not necessarily drawn to scale. Unless otherwise specified, similar or functionally similar elements in the drawings have been assigned the same reference numerals. DETAILED DESCRIPTION
[0026] refer to Figure 1-5 First, an aspect of the present invention is described, which relates to magnetic cores 10, 10a, 10b. Note that reference numerals 10a, 10b refer to variations of core 10. Although the features of the present magnetic core are mainly referred to Figure 1 2A-2B, it will be apparent to one skilled in the art that the cores 10a, 10b may include similar features.
[0027] Basically, the core 10 comprises an anisotropic composite material comprising a matrix material 30 and magnetically aligned ferromagnetic particles 11 , 12 .
[0028] like Figure 1-3 As can be seen in FIG. 1 , such particles 11, 12 form particle chains 20 in the matrix material 30. Such chains 20 form permeable paths for magnetic conduction. The conduction paths are along a first direction (parallel to Figure 1-2A That is, each chain 20 forms a conductive path and thus extends along the first direction. In contrast, the conductive paths extend in a second direction perpendicular to the first direction (parallel to the x-axis in FIG. 2B). Figure 1-2A , z-axis in 2B), the chains are different and therefore far away from each other.
[0029] In other words, the magnetically aligned particles 11, 12 form distinct chains 20 ensuring a percolation path extending along a first direction. Such chains extend along the direction of the magnetic field applied during manufacture, as discussed later with reference to another aspect of the invention. As a result, the chains are substantially parallel to this first direction, while being distinct from each other and therefore away from each other in a perpendicular direction.
[0030] The magnetic alignment of particles 11, 12 is converted into a recognizable pattern of aligned particles. That is, although not completely aligned, a clear alignment direction as well as distinct chains can still be observed, see Figure 2A , 2B . And as in Figure 2A , 2B As can be seen further in FIG. 1 , each chain 20 may actually involve a link consisting of small 3D clusters of particles 11, 12, which is consistent with Figure 1 , 2B, 4 and 5, the latter showing a chain formed by a single particle 11. Therefore, a particle "chain" as used herein should be interpreted in a broad sense, such as a filament or a line of particles 11, 12, i.e. as a longitudinal composite structure (e.g., a cylindrical shell with local distortion) formed by ferromagnetic particles 11, 12. A particle chain may, for example, include a plurality of particles in a direction perpendicular to the percolation path, such as Figure 3 as shown, while keeping away from each other.
[0031] The first direction may be a straight line parallel to a given axis (e.g., the x-axis), resulting in a configuration of parallel lines, such as Figure 1-2A , as assumed in 2B. In other cases, the first direction can also be curvilinear (due to the magnetic field applied during the manufacturing process), resulting in the chains still remaining parallel, such as Figure 4 Note that in the radial portion P of the core 10a (eg Figure 4 ), the chains can be considered to extend parallel to the same, approximately straight direction. In general, the applied magnetic field can be designed to cause the chains 20 to be arranged substantially according to a desired pattern, such as a configuration of concentric rings (such as Figure 4 ), runway configuration or parallel line configuration (as shown in Figure 1 or 5).
[0032] The present solution relies on the magnetic assembly of the particles 11, 12 in the matrix material 30. Permeation of the particles is applied in the direction of the applied magnetic field during manufacturing, while it is suppressed (or at least substantially mitigated) in the perpendicular direction. As one may appreciate, this increases the effective magnetic permeability in the direction of the applied magnetic field while suppressing (or at least mitigating) eddy currents in the perpendicular direction. That is, the magnetic flux is enhanced along the direction of the chain, while the eddy currents are reduced in the perpendicular direction, hence the importance of anisotropic permeability. Note that the percolation path means that there is sufficient mechanical contact between the ferromagnetic portions of the particles 11, 12 to allow magnetic conduction (i.e., the magnetic resistance at the contact point is low).
[0033] Interestingly, the percolation path of magnetoconduction may extend along two perpendicular directions, e.g. Figure 5 As shown in the core 10b, that is, along the first direction x and the third direction (parallel to Figure 5 The axis y in the direction of the particle is perpendicular to the first direction and the second direction. Therefore, the particle chains form parallel chain rows. According to tests conducted by the inventors, it was found that this configuration provides the best results in terms of effective permeability. Figure 5 The core 10b shown can be manufactured layer by layer (in the y direction), as discussed later. Again, it should be remembered that Figure 5 The description is schematic; in practice, a real chain looks more like Figure 3 The chain in.
[0034] In all cases, the present method allows for a rapid and low-cost manufacturing process, especially when compared to thin film microfabrication processes. The resulting magnetic cores 10, 10a, 10b can be used in a variety of applications such as electromagnets, transformers, amplifiers, power supplies, motors, generators, inductors, tape heads, and other magnetic components.
[0035] All of this will now be described in detail with reference to specific embodiments of the present invention. First, the ferromagnetic particles 11, 12 preferably comprise micron-sized particles. Micro (e.g., spherical and / or rod-shaped) particles can be used at various loading concentrations. As observed by the inventors, the composite material obtained based on such microparticles provides stable permeability over a wide frequency range.
[0036] Micron-sized particles are particles whose characteristic dimension (e.g. their average diameter for spherical particles or average cross-sectional diameter for rod-shaped particles) is in the micrometer length range, i.e. between 1 μm and 100 μm. In a variant of or in addition to micron-sized particles, particles in the submicrometer range, e.g. particles in the nanometer range (having a characteristic dimension between 1 nanometer and 100 nanometers) can be used. However, preference is given to relying primarily on microparticles. However, for the reasons explained below, it is preferred to use additional, for example nanometer-sized particles 12 in addition to micron-sized particles 11.
[0037] For example, refer to Figure 2A , 2B , the particles 11, 12 may include first particles 11 (i.e., first type of particles) and second particles 12 (of the second type), wherein the average diameter of the second particles 12 is smaller than that of the first particles 11. Figure 2A As can be seen in FIG. 1 , the second particles 12 can form neck bridges 15 between the larger particles 11, thereby bridging the particles 11 in the first direction (see also FIG. 1 ). Figure 2B As previously described, the neck bridges 15 between the first particles (e.g., microparticles) are preferably achieved by introducing nano-sized ferromagnetic particles into the composite material 30. The sizes of the first particles 11 and the second particles 12 are typically distributed according to a bimodal or multimodal distribution, such as Figure 7 As shown, where D(ρ) represents the distribution of the average diameter ρ of the particles. Of course, different distributions can be considered, for example extended to larger particle sizes.
[0038] Accordingly, the second particles 12 can form a neck 15 around the contact area of the first particles 11, which gives additional mechanical stability to the entire permeation path. Figure 2A As shown, the second particles 12 can form additional magnetic permeability paths. This enhances the magnetic permeability by providing a magnetic field path of lower magnetic resistance at the contact points of the particles. Due to the edge and contraction fields caused by the particle assembly when the magnetic field is applied, necking can be automatically achieved when the magnetic field is applied.
[0039] Note that the necking bridges 15 are also anisotropic - they are applied in the magnetic field direction (along the path) and suppressed in the perpendicular direction (no necks are formed between particles of different chains). The distance between chains will usually be larger (or of the same order of magnitude) than the diameter of the largest particles (e.g., micron-sized particles). This distance depends on the volume fraction of the particles.
[0040] Although the necking bridge can already be obtained due to the appropriately applied magnetic field, a sintering process can be considered in addition to improve the mechanical stability and the magnetic conductivity. To this end, the particles 11, 12 will preferably have an average sintering temperature that is significantly lower than the melting temperature of the host material 30. For example, permalloy (nickel iron) particles can be used, which have a melting temperature of about 1450 degrees Celsius, but in the case of nanoparticles can be sintered at 200 degrees Celsius. However, this sintering process is optional, because the particles can be fixed in the matrix material and thus remain in contact, for example by solidifying the matrix material.
[0041] In this regard, the main (matrix) material 30 is preferably a dielectric, a non-magnetic material or a paramagnetic material. Diamagnetic materials should preferably be avoided, and ferromagnetic materials are excluded in principle. For example, the matrix material 30 can be composed of or include an epoxy resin material. It can be particularly based on an epoxy-based negative photoresist, such as SU-8 polymer or a heat-cured epoxy resin. Silicone resin and other adhesive materials can also be used. More generally, other materials can be considered, such as photoresist materials and photosensitive adhesive photopolymers.
[0042] Various types of ferroelectric materials can be considered for producing particles 11, 12, starting from materials containing transition metal elements (Fe, Co, Ni), such as transition metal-metalloid alloys, and rare earth magnets. Suitable particles 11, 12 are commercially available as micro- or nanoparticles. Microparticles are preferably produced by a thermal spraying process, and nanoparticles are preferably produced by a plasma spraying or liquid precipitation process.
[0043] In practice, the magnetic core 10 may include, for example, between 10 and 50 volume percent (vol%) of ferromagnetic particles 11, 12. This percentage reflects the composition of the core 10, including the matrix material 30 and the first type of ferromagnetic particles 11, and, if desired, the second type of particles 12. It corresponds to the volume fraction of all ferromagnetic particles multiplied by 100. That is, a fraction of 50 volume percent refers to a mixture of 50 volume units of either or both types of ferromagnetic particles 11, 12 with enough matrix material 30 (and additional materials, if desired) to make a final volume of 100 units. Although slightly larger volume fractions may be considered, the volume fraction of ferromagnetic particles 11, 12 generally needs to be limited to prevent penetration in undesired directions. Preferably, the volume fraction of ferromagnetic particles 11, 12 is between 30 and 45 volume percent. For example, in Figure 2A-2B The volume fraction is assumed to be 38 volume percent.
[0044] If desired, for example when molded in a structured template, the thickness of the core 10 may be less than one (or a few) millimeters, and may be as small as 100 microns. The sample may also be mechanically and / or chemically thinned if necessary. Depending on the application sought, the transverse dimensions (length and width) of the sample 10 will typically be larger, for example in the millimeter to centimeter range.
[0045] More specifically refer to Figure 6 , another aspect of the invention is now described, relating to a magnetic device 1 or apparatus comprising a magnetic core 10, 10a, 10b as described above. That is, the core comprises an anisotropic composite material comprising a matrix material 30 and magnetically aligned ferromagnetic particles 11, 12 assembled into chains 20, the chains 20 forming a percolation path for magnetic conduction, as described above. In an embodiment, such a device may in particular be realized as an inductor, a transformer, an amplifier or a power supply device, i.e. various applications may be envisaged, including servers, microservers, power supplies in data centers, e.g. for cloud computing, and integrated regulators, e.g. for IoT applications. Such a magnetic device may also be realized as a miniaturized transformer for isolation in various information technology, automotive and aerospace applications, or as a miniaturized inductor for resonant circuits, for various applications, such as transceivers.
[0046] Figure 6 An example of a realization of such a device 1 as a toroidal inductor based on printed circuit board (PCB) technology is shown, for example for use in an integrated voltage regulator. The inductor utilizes the free space inside the PCB to carry the magnetic core 10a, such as Figure 4As shown. The winding typically involves PCB metal traces and vias. The magnetic core 10a is embedded in a cavity formed inside the PCB. Manufacturing constraints typically impose an upper limit on the core thickness, such as a few millimeters. It is well known that both sides of the PCB can be used to mount electronic components, or one side can be used for cooling purposes.
[0047] Reference now Figure 8 , describes a final aspect of the invention, relating to a method of manufacturing a magnetic core 10, 10a, 10b, as previously described with reference to Figure 1-5 Aspects of the method have already been described implicitly; they are only briefly described below.
[0048] In one embodiment, the method relies on Figure 8 The matrix material 30 is provided in step S10 of the flowchart of FIG. The material 30 may already include ferromagnetic particles 11, 12. In a variant, the ferromagnetic particles 11, 12 may be introduced into the matrix material 30, for example, after the matrix material is filled into the cavity, such as Figure 8 As assumed in step S20 of the flowchart of . A magnetic field S30 is then applied to magnetically align the ferromagnetic particles 11, 12 in the matrix material 30. As previously described, this is done to obtain an anisotropic composite material for the magnetic core 10, wherein chains 20 of ferromagnetic particles 11, 12 are formed within the matrix material 30. The chains 20 form magnetically conductive percolation paths extending in a first direction, whereby the chains 20 each extend in the first direction while being different and distant from each other in a second direction perpendicular to the first direction.
[0049] Permanent magnets and / or one or more electromagnets are usually used to apply the magnetic field S32. For example, before or after the introduction of the particles, permanent (dipole) magnets can be arranged on each side of the sample holder, and the matrix material is placed on each side of the sample holder. For example, the magnetic field of a cylindrical dipole magnet can be used, with a gap of a nearly constant field at its center to align the particles 11, 12. In a variant, a similar field configuration can be obtained from a stacked current loop. Other variants rely on electromagnets (e.g., horseshoe magnets), which can actually be used as a supplement or variant of permanent magnets. In all cases, the magnetic field lines should preferably be aligned with the direction of the gravitational field to avoid magnetic field interference from deforming the chain 20. Another less preferred possibility is to rotate the system consisting of the sample, sample holder and magnet in the gravitational field during chain formation and fixation. Therefore, the gravitational field can be processed during manufacturing to minimize or conversely utilize its influence on the chain 20 to obtain the desired chain design. However, in principle, the effect of gravity on the chain geometry is very small.
[0050] As mentioned above, the particles 11, 12 introduced in step S20 preferably include microparticles 11, possibly supplemented with nanoparticles 12. The ferromagnetic particles 11, 12 introduced into the matrix material 30 will preferably account for 10 to 50 volume percent of the composite material finally obtained. Generally, the applied magnetic field needs to have a strength of at least 20 mT to obtain the desired chains 20.
[0051] Assuming that the particles 11, 12 include ferromagnetic particles 12 having an average diameter smaller than that of the first particles 11, the method may further include forming S34 a necking bridge 15 between the first particles 11. The bridge is formed while applying S32 a magnetic field so as to bridge the first particles along the first direction due to the second particles 12. As previously described, the chains 20 remain unconnected (or not connected) along the vertical direction.
[0052] Due to the only magnetic field S32 applied during manufacturing, necking can be achieved, which results in an edge and / or a shrinkage field horizontal to the contact area. The necking is anisotropic because it is applied in the direction of the applied magnetic field and is suppressed (or at least mitigated) in the perpendicular direction. As previously mentioned, a sintering process S34 is preferably included to strengthen the conduction path. That is, the necking bridge 15 can be perfected by sintering S34 the first and second particles 11, 12, by applying heat, thereby compacting the particles and forming a chain 20 that penetrates as much as possible in the first direction. The sintering is carried out while the magnetic field is still present. The particles 11, 12 are typically sintered S34 at a temperature substantially below the melting temperature of the matrix material 30.
[0053] Finally, the chain 20 may need to be fixed S36 in the obtained anisotropic composite material. This is usually achieved by curing the matrix material (for example, by cross-linking a photopolymer or heat-curing an epoxy resin) while the magnetic field is still present. More generally, fixation can be achieved by heating the matrix material while maintaining the magnetic field.
[0054] In an embodiment, the matrix material is provided in a structured template (e.g., formed on a surface of the device 1) to constrain the shape of the final composite material. For example, one or more micro-machined grooves, cavities, etc. can be used to constrain the final shape of the composite material 11, 12, 30 as a whole in a particular direction. As described above, thicknesses as low as 100 microns can be achieved, while lateral dimensions can be much larger (indeed up to millimeters to centimeters).
[0055] If desired, the anisotropic composite material is formed as a layer-by-layer process, i.e. by successively forming layers of the composite material, which can be easily achieved, for example, by repeating steps S10-S36 as described above at S50. Figure 5The core 10b shown can be produced, for example, using such a layer-by-layer process. That is, particle chains 20 can be obtained, extending along a first direction x but away from each other in a second perpendicular direction z, and forming magnetically conductive percolation paths extending along the first direction x and a third direction y, wherein the latter is perpendicular to the first direction x and the second direction z, to improve performance.
[0056] Finally, the core material obtained S36 may be packaged for transport or integrated S60 in a device 1 for a specific purpose such as described above, for example using common manufacturing techniques for such devices.
[0057] Although the present invention has been described with reference to a limited number of embodiments, variants and drawings, it will be understood by those skilled in the art that various changes may be made and equivalents may be substituted without departing from the scope of the present invention. In particular, the features (similar devices or methods) shown in a given embodiment, variant or figure may be combined with or replace another feature in another embodiment, variant or figure without departing from the scope of the present invention. Various combinations of features described with respect to any of the above embodiments or variants may be envisaged accordingly, and these combinations are still within the scope of the appended claims. In addition, many small modifications may be made to adapt specific situations or materials to the teachings of the present invention without departing from the scope of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed, but the present invention will include all embodiments falling within the scope of the appended claims. In addition, many other variations other than those explicitly mentioned above may be envisaged. For example, other materials other than those explicitly mentioned may be envisaged, as long as they exhibit the desired magnetic properties. If desired, additional materials may be used to adjust the chemical (e.g., cross-linking properties of polymer chains) or mechanical (e.g., rheology, viscosity, etc.) properties of the composite material.
Claims
1. A magnetic core, comprising: Anisotropic composite material, comprising at least: Base material; and magnetically aligned ferromagnetic particles form chains of said particles within said matrix material, said chains forming magnetically conductive percolation paths extending along a first direction, whereby said chains each extend along the first direction while being distinct and remote from one another along a second direction perpendicular to the first direction, wherein said chains of magnetically aligned ferromagnetic particles are arranged in concentric rings or a racetrack configuration, in: The particles include first particles of a first type and second particles of a second type, the second particles having an average diameter smaller than the first particles; and The second particles form neck bridges between the first particles along the first direction.
2. The magnetic core according to claim 1, wherein: The particles include micron-sized particles.
3. The magnetic core according to claim 1, wherein: The first particles include micron-sized particles, and the second particles include nano-sized particles.
4. The magnetic core according to claim 1, wherein: The first particles and the second particles have an average sintering temperature that is significantly lower than the melting temperature of the matrix material.
5. The magnetic core according to claim 1, wherein: The matrix material is a dielectric, non-magnetic material.
6. The magnetic core according to claim 5, wherein: The matrix material is a paramagnetic material.
7. The magnetic core according to claim 1, wherein: The composite material contains 10 to 50 volume percent of ferromagnetic particles.
8. The magnetic core according to claim 1, wherein: The particle chains form magnetically conductive permeable paths extending along a first direction and a third direction, the third direction being perpendicular to the first direction and the second direction.
9. A magnetic device comprising a magnetic core, the magnetic core comprising: Anisotropic composite material, comprising at least: Base material; and magnetically aligned ferromagnetic particles form chains of said particles within said matrix material, said chains forming magnetically conductive percolation paths extending along a first direction, whereby said chains each extend along the first direction while being distinct and remote from one another along a second direction perpendicular to the first direction, wherein said chains of magnetically aligned ferromagnetic particles are arranged in concentric rings or a racetrack configuration, in: The particles include first particles of a first type and second particles of a second type, the second particles having an average diameter smaller than the first particles; and The second particles form neck bridges between the first particles along the first direction.
10. The magnetic device according to claim 9, wherein: The device is one of the following: inductor, transformer, amplifier, and power supply.
11. A method for manufacturing a magnetic core, the method comprising: providing a matrix material comprising ferromagnetic particles; and applying a magnetic field to magnetically align ferromagnetic particles in a matrix material to form an anisotropic composite material for a magnetic core, wherein chains of said particles are formed within said matrix material, said chains forming magnetically conductive percolation paths extending along a first direction, whereby said chains each extend along the first direction while being distinct and remote from one another along a second direction perpendicular to the first direction, wherein said chains of magnetically aligned ferromagnetic particles are arranged in concentric rings or a racetrack configuration, in: The ferromagnetic particles include first particles of a first type and second particles of a second type, the second particles having an average diameter smaller than the first particles, and The method further comprises forming a necking bridge between the first particles while applying the magnetic field so as to bridge the latter along the first direction due to the second particle.
12. The method according to claim 11, wherein: The ferromagnetic particles include micron-sized particles.
13. The method according to claim 12, wherein: The strength of the applied magnetic field is at least 20 mT.
14. The method according to claim 11, wherein: The ferromagnetic particles in the matrix material account for 10 to 50 volume percent of the formed composite material.
15. The method of claim 11, wherein: Forming the neck bridge includes sintering the first particles and the second particles.
16. The method of claim 11, wherein: The method also includes fixing the chains in the formed anisotropic composite material.
17. The method of claim 11, wherein: The first particles include micron-sized particles, and the second particles include nano-sized particles.
18. The method of claim 11, wherein: The magnetic field is applied using one or each of a permanent magnet and an electromagnet.
19. The method of claim 11, wherein: The anisotropic composite material is formed by repeating the steps of claim 13 to successively form layers of the composite material.
20. The method of claim 11, wherein: The matrix material is disposed in a structured template to constrain the shape of the final composite material.
21. The method of claim 11, wherein: The method further comprises integrating the obtained magnetic core in a device.