Composite materials and copper-clad laminates made therefrom

By using smooth copper foil and an adhesive layer with a specific composition, the problem of difficult reduction of conductor loss and dielectric loss in the prior art is solved, achieving high peel strength and low loss in high-frequency signal transmission, making it a copper-clad laminate suitable for high-speed and high-frequency signal transmission.

CN113942277BActive Publication Date: 2026-11-10DUPONT ELECTRONICS INC
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202110789487.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-07-15
Filing Date
2021-07-13
Publication Date
2026-11-10
Estimated Expiration
2041-07-13

AI Technical Summary

Technical Problem

Existing technologies struggle to reduce conductor and dielectric losses in copper-clad laminates while maintaining high peel strength, especially in high-speed and high-frequency applications, leading to decreased signal transmission reliability and performance.

Method used

It uses a smooth copper foil and an adhesive layer with a specific composition. The copper foil has a surface roughness of less than 2.0 μm, a nodule density of less than 1 piece/μm2, and a non-copper metal element content of less than 350 μg/dm2. The adhesive layer is composed of reactive resin, styrene-based rubber, and additives. After curing, the Dk value is less than 3.0 and the Df value is less than 0.006, avoiding the need for adhesion promoter pretreatment.

Benefits of technology

It achieves a combination of low conductor loss, low dielectric loss and high peel strength under high frequency conditions, ensuring the reliability of signal transmission and the heat resistance of copper-clad laminates, and is suitable for high-speed and high-frequency signal transmission.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113942277B_ABST
    Figure CN113942277B_ABST
Patent Text Reader

Abstract

A composite material and a copper-clad laminate made therefrom are disclosed. The composite material for manufacturing the copper-clad laminate comprises a copper foil and an adhesive layer, wherein the copper foil has a Ω / m² content of 0.170 gΩ / m². 2 or lower resistance, at least one smooth surface with a surface roughness (Rz) of 2.0 μm or less, less than 1 piece / μm 2 The density of nodule-like growths, and having a density of 350 μg / dm³ on the smooth surface. 2 The total content of non-copper metal elements is less than or equal to that of copper; the adhesive layer is derived from a mixture comprising: a resin matrix containing about 5-25 parts by weight of a reactive resin, about 0.1-3 parts by weight of a curing agent and about 72-94.9 parts by weight of a styrene-based rubber; and about 0-100 parts by weight of additives based on 100 parts by weight of the resin matrix; the adhesive layer is in contact with the smooth surface of the copper foil; the cured adhesive layer has a Dk of 3.0 or less and a Df of 0.006 or less at 10 GHz according to the method described in the test method; and provided that the smooth surface of the copper foil has not been pretreated with an adhesion promoter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to composite materials for manufacturing copper clad laminates that exhibit reduced conductor loss, dielectric loss, and high peel strength. Background Technology

[0002] Currently, to improve the information processing speed of electronic devices and handle high-frequency wireless communications, electronic components require high-speed transmission of electrical signals. The application of high-frequency matching boards is also advancing. Therefore, low insertion loss has become one of the key characteristics of copper-clad laminates (CCLs) used in the fabrication of printed circuit boards for high-speed and / or high-frequency applications.

[0003] Reducing total insertion loss (which is the sum of conductor loss and dielectric loss) can be achieved by reducing conductor loss and / or dielectric loss. Reducing dielectric loss can be achieved by carefully selecting dielectric materials with low Dk (dielectric constant, also known as relative permittivity) and Df (dissipation factor, also known as loss tangent, tanδ), which comprise a substrate, prepreg, and binder (if present at the interface between the copper foil and the substrate). Under high-speed / high-frequency conditions, the current for signal transmission is primarily conducted through the surface of the copper foil, a phenomenon known as the skin effect. The skin effect is the phenomenon where a relatively large amount of current is concentrated at a higher frequency on the surface portion of the conductor. The current density decreases at a greater depth from this surface portion. The depth at which the current density value is provided on the surface by 1 / e (e is the natural logarithm) is called the skin depth and serves as an indicator of the depth of current flow. The skin depth depends on the frequency and decreases as the frequency increases.

[0004] Typically, in copper foil used for copper-clad laminates, the surface of the side to be laminated to the substrate is processed to form a roughened surface with protrusions (or nodules). This roughened surface exhibits an anchoring effect on the substrate. The adhesion strength between the substrate and the copper foil can then be improved to ensure the reliability of the printed circuit board made from it. While reducing surface roughness is one of the most effective ways to reduce conductor losses, this compromise weakens adhesion strength, as measured by peel strength between the copper foil and the substrate. Therefore, the final product (printed circuit board) may exhibit degraded reliability and performance in the high-frequency range (i.e., >1 GHz). One method to maintain peel strength with lower surface roughness is to modify the morphology of the nodules during the Cu surface roughening process, such as shape, density, and size. For example, this is disclosed by S.-Q. Lin et al. in TW M543248 and TW M543249.

[0005] Another approach is to pretreat the unroughened surface of the copper foil with an adhesion promoter or coupling agent. For example, T. Sato et al. disclosed in U.S. Patent No. 8,815,387 a method of forming a silane coupling agent layer on the unroughened surface of the copper foil, and then forming a primer resin layer thereon. A significant drawback is that the additional adhesion promoter applied to the primer resin typically increases dielectric loss due to its high Dk / Df characteristics, and results in higher overall insertion loss for the copper clads or PCB devices, regardless of the reduced conductor loss of the copper foil.

[0006] T. Matsunaga et al. also disclosed in TW I339222 the use of large amounts of non-copper elements such as nickel or silane to increase the peel strength, rust resistance, heat resistance, or chemical resistance of copper foil. However, these non-copper elements have higher permeability or higher resistivity, which significantly increases the insertion loss of the copper clad layer or PCB.

[0007] There remains a continued need for composite materials with low conductor loss, low dielectric loss, and sufficiently high peel strength to fabricate copper-clad laminates and printed circuit boards suitable for high-speed and / or high-frequency applications. Summary of the Invention

[0008] This invention provides a composite material for manufacturing copper-clad laminates, the composite material comprising a copper foil and an adhesive layer, wherein...

[0009] The copper foil has a strength of 0.170 gΩ / m 2 Or even lower resistance and at least one smooth surface, said smooth surface having a surface roughness (Rz) of 2.0 μm or less, less than 1 μm / μm. 2 The density of the nodule on the smooth surface is 350 μg / dm³. 2 Or even lower total content of non-copper metal elements;

[0010] The adhesive layer is derived from a mixture comprising: a resin matrix containing about 5-25 parts by weight of a reactive resin, about 0.1-3 parts by weight of a curing agent and about 72-94.9 parts by weight of a styrene-based rubber; and about 0-100 parts by weight of additives based on 100 parts by weight of the resin matrix.

[0011] The adhesive layer is in contact with the smooth surface of the copper foil;

[0012] The cured adhesive layer has a Dk value of 3.0 or less and a Df value of 0.006 or less at 10 GHz; and

[0013] The premise is that the smooth surface of the copper foil has not been pretreated with an adhesion promoter.

[0014] The present invention also provides copper-clad laminates, copper-clad circuits, and devices incorporating the composite material of the present invention. Attached Figure Description

[0015] Figure 1 An enlarged side view of an embodiment of the composite laminate material 100 of the present invention is shown, which has the following layer structure: a copper foil 1 having a first surface 11 and a second surface 12, and an adhesive layer 2, wherein the second surface 12 is a smooth surface and is in contact with the adhesive layer 2.

[0016] Figure 2 An enlarged side view of an embodiment of the copper-clad laminate 200 of the present invention is shown, which is a single-sided CCL having a layer structure in the following order: a composite material 100 of the present invention, which is composed of a copper foil 1 and an adhesive layer 2; and a substrate 3, wherein the substrate 3 is in contact with the adhesive layer 2.

[0017] Figure 3 An enlarged side view of an embodiment of the copper-clad laminate 300 of the present invention is shown, which is a double-sided CCL having a layer structure in the following order: composite material 100 of the present invention, which is composed of copper foil 1 and adhesive layer 2; substrate 3; optional adhesive layer 4 and second copper foil 5; wherein the second copper foil 5 and copper foil 1 may be the same or different; when adhesive layer 4 is present, adhesive layer 4 and second copper foil 5 may also be embodiments of composite material 110 of the present invention (which may be the same or different from composite material 100).

[0018] Figure 4 The smooth surface of copper foil 4A (with a surface roughness (Rz) of 0.62 μm) is shown compared to that of copper foil 4B (purchased from Fukuda Corporation), which has a surface roughness of 3.57 μm and a surface roughness of 1.5 μm / μm. 2 Visual comparison of micrographs of roughened surfaces (density of nodules). Detailed Implementation

[0019] Unless otherwise stated, all publications, patent applications, patents and other references mentioned herein are expressly incorporated herein by reference in their entirety for all purposes, as if fully expounded.

[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. In case of conflict, this specification, including its definitions, shall prevail.

[0021] Unless otherwise stated, all percentages, parts, ratios, etc. are by weight.

[0022] As used herein, the term “made from” is synonymous with “comprising”. As used herein, the terms “comprises,” “comprising,” “includes,” “including,” “has,” “having,” “contains,” or “containing,” or any other variation thereof, are intended to cover non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that includes a list of elements is not necessarily limited to those elements, but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0023] The connecting phrase "composed of..." excludes any unspecified element, step, or ingredient. If in a claim, such a phrase makes the claim closed, excluding materials other than those described, except typically associated with impurities. When the phrase "composed of..." appears in a clause of the body of a claim, rather than immediately following the preamble, it only limits the elements described in that clause; other elements are not excluded from the claim as a whole.

[0024] The connecting phrase "substantially composed of" is used to define a composition, method, or apparatus that includes, in addition to those literally discussed, materials, steps, features, components, or elements, provided that such additional materials, steps, features, components, or elements do not materially affect one or more essential and novel features of the claimed invention. The term "substantially composed of" falls between "comprising" and "composed of".

[0025] The term "comprising" is intended to include embodiments covered by the terms "substantially consisting of" and "consisting of". Similarly, the term "substantially consisting of" is intended to include embodiments covered by the term "consisting of".

[0026] When a quantity, concentration, or other value or parameter is given as a range, preferred range, or a series of upper and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any upper or preferred value with any lower or preferred value, regardless of whether the range is disclosed individually. For example, when a range of “1 to 5” is listed, the listed range should be interpreted as including ranges such as “1 to 4”, “1 to 3”, “1-2”, “1-2 and 4-5”, “1-3 and 5”, etc. When describing numerical ranges herein, unless otherwise stated, the range is intended to include its endpoints, as well as all integers and fractions within that range.

[0027] When the term “about” is used in the description of a value or endpoint, this disclosure should be understood to include the specific value or endpoint mentioned.

[0028] Furthermore, unless explicitly stated otherwise, "or" refers to an inclusive "or," not an exclusive "or." For example, any of the following satisfy condition A "or" B: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); and both A and B are true (or exist).

[0029] "Mol%" or "mole%" refers to the percentage of moles.

[0030] The embodiments of the invention described in the summary of the invention include any other embodiments described herein, which may be combined in any way, and the description of variables in the embodiments relates not only to the composite laminates of the invention, but also to articles made therefrom.

[0031] The present invention will be described in detail below.

[0032] copper foil

[0033] Copper foil includes rolled annealed (RA) copper foil and electrodeposited (ED) copper foil. Typically, ED copper foil has a rough surface (deposited surface) and a glossy, shiny surface (drum surface), while RA copper foil has smooth surfaces on both sides. Since the composite material of this invention is intended to be incorporated into CCLs and PCBs for high-frequency and / or high-speed applications, suitable copper foils possess high purity and a purity of 0.170 gΩ / m 2 Or even lower resistance. The copper foil has at least one smooth surface, characterized by a surface roughness (Rz) of 2.0 μm or less, as measured by the method described in the Examples section below. Furthermore, the smooth surface has a surface roughness of less than 1 μm / μm. 2 or 0.5 pieces / μm 2 or 0.3 blocks / μm 2 or 0.1 blocks / μm 2 The density of nodules, or no roughening at all. For roughened copper foil surfaces, a density greater than 3 nodules / μm is generally expected. 2 The density of the nodule-like growth.

[0034] As used herein, the smooth surface of the copper foil is also referred to as the "laminated side" because it is the substrate-facing side when the composite material of the present invention is used to manufacture the CCL. The opposite side of the copper foil is referred to as the "resist side" (or wiring side).

[0035] In some cases, one or more passivation layers can be applied to one or both surfaces of copper foil to provide additional desired properties such as rust prevention, heat resistance, and chemical resistance. Suitable materials for forming the passivation layer include non-copper metal elements such as zinc, nickel, chromium, cobalt, molybdenum, tungsten, and combinations thereof. The total content of non-copper metal elements on the smooth surface of the copper foil should be maintained at 350 μg / dm³. 2 Or smaller allows the desired characteristics to be maintained without compromising the low conductor loss characteristics.

[0036] It should be noted that the surface properties of the resist surface undergo many subsequent printed circuit manufacturing processes, such as micro-etching, pickling, brown oxide coating, black oxide coating, and pre-soldering treatment. Understandably, there are no requirements regarding the surface roughness and total content of the deposited non-copper metal elements.

[0037] Regardless of the presence of any passivation layer, the smooth surface of the copper foil is not treated with any adhesion promoters to improve the adhesion between the copper foil and the substrate. Known adhesion promoters (also known as coupling agents) for treating copper surfaces include silanes and silylamines disclosed in U.S. Patent No. 5,861,076 to Adlam et al. and U.S. Patent No. 8,8815,387 to Sato et al.; allyl phosphites and allyl phosphates disclosed in U.S. Patent No. 4,521,558 to Mowdood; azole silanes disclosed in U.S. Patent No. 9,688,704 to Miura et al.; unsaturated amide-substituted heterocyclic compounds disclosed in EP-A-0251490; aminotriazine-based compounds in U.S. Patent No. 10,385,076 to Mori et al.; and some of the references cited therein.

[0038] The copper foil of the composite material of the present invention has a thickness of about 6 μm to about 400 μm, or about 12 μm to about 70 μm, or about 18 μm to about 35 μm.

[0039] The copper foil suitable for the composite material of the present invention can be purchased from, for example, Changchun Petrochemical Co.; Nan Ya Plastics Co.; Mitsui Mining & Smelting Co.; Furukawa Electric Co.; or Fukuda Metal Foil & Powder Co.

[0040] Adhesive layer

[0041] The adhesive layer of the composite material of the present invention contacts the smooth surface of the copper foil and is intended to provide good adhesion to the substrate for producing copper-clad laminates with dielectric loss not exceeding that of the substrate itself.

[0042] The adhesive layer is derived from a mixture comprising: a resin matrix containing about 5-25 parts by weight of a reactive resin, about 0.1-3 parts by weight of a curing agent and about 72-94.9 parts by weight of a styrene-based rubber; and about 0-100 parts by weight of additives based on 100 parts by weight of the resin matrix.

[0043] Examples of reactive resins include epoxy resins, acrylic resins, phenolic resins, imide resins, or combinations thereof; preferably, epoxy resins.

[0044] Various epoxy resins can be used, including bisphenol A type epoxy resin, bisphenol F type epoxy resin, phenol-phenolic varnish type epoxy resin, cresol-phenolic varnish type epoxy resin, glycidyl ether type epoxy resin, naphthalene type epoxy resin, etc. However, for proper control of the reaction, it is preferable to use epoxy resins containing at least two epoxy groups per molecule. The epoxy resins mentioned above can be used alone or in combination of two or more.

[0045] Depending on the type of epoxy resin used, those skilled in the art can readily select a suitable curing agent and then determine the appropriate amount based on the molar equivalent of the reactive resin. For example, curing agents may include amines such as dicyandiamide, imidazole, and aromatic amines; phenols such as bisphenol A and brominated bisphenol A; phenolic varnishes such as phenolic varnish resins and cresol varnish resins; and acid anhydrides such as phthalic anhydride, etc.

[0046] Examples of styrene-based rubbers include polystyrene and block copolymers such as styrene-isoprene-styrene (SIS), styrene-butadiene-styrene (SBS), styrene-ethylene-butadiene-styrene (SEBS), styrene-ethylene-propylene-styrene (SEPS), or mixtures thereof.

[0047] Styrene-based rubbers can be grafted or copolymerized with unsaturated carboxylic acids and / or their anhydrides to obtain acid-modified rubbers. Examples of suitable unsaturated carboxylic acids or their anhydrides for acid modification include maleic acid, acrylic acid, itaconic acid, crotonic acid, maleic anhydride, and itaconic anhydride. Maleic anhydride is particularly useful. By using acid-modified rubbers, adhesive reliability can be further enhanced without increasing the Dk and / or Df values.

[0048] The grafting rate for acid modification is, for example, based on the styrene-based rubber to be grafted, about 0.05% to 10.0% by weight, preferably about 0.1% to 5.0% by weight. When the grafting rate is less than the above range, the adhesive strength may be insufficient. On the other hand, when the grafting rate is greater than the above range, the styrene-based rubber may aggregate and its compatibility and dispersibility may decrease, resulting in a tendency for reduced production efficiency.

[0049] In this invention, various additives can be added to the mixture forming the adhesive layer to provide beneficial functions. Suitable additives include, but are not limited to, adhesion promoters, antioxidants, antistatic agents, colorants, fillers, flame retardants, impact modifiers, lubricants, processing aids, heat stabilizers, UV absorbers, etc. These additives can be added to the resin mixture as long as they do not impair the effects of this invention.

[0050] Examples of fillers and flame retardants useful for the mixtures of the present invention include, but are not limited to, alumina, organophosphates, silica, calcium carbonate, magnesium carbonate, calcium magnesium carbonate, calcium oxide, magnesium oxide, talc, magnesium silicate, aluminum silicate, aluminum magnesium silicate, calcium silicate, clay, mica, barium sulfate, boron nitride, aluminum nitride, barium titanate, strontium titanate, alumina trihydrate, and calcium sulfate.

[0051] The mixture forming the adhesive layer is preferably mixed with a solvent capable of dissolving or dispersing the reactive resin, a styrene-based rubber, optional additives, and a curing agent.

[0052] Suitable solvents include, for example, methyl ethyl ketone (MEK), toluene, methylcyclohexane, tetrahydrofuran, chlorobenzene, trichloroethylene, or dichloromethane, provided that the solvent does not adversely affect the adhesive properties of the resin mixture. These solvents may be optionally mixed according to the composition of the resin mixture. For example, a mixture of MEK and toluene in a 1:1-100 ratio may be used.

[0053] The solids content of the mixture forming the adhesive layer is based on the total weight of the mixture, from about 10% by weight to about 60% by weight, or from about 15% by weight to about 45% by weight.

[0054] In addition to good adhesive strength, a suitable resin mixture preferably has low Df and Dk values ​​after curing. Evaluation can be performed by applying the resin mixture to a releasable substrate to form an adhesive layer with a thickness of 25 μm. After stacking, drying, and complete curing, Df and Dk are measured according to the methods described in the Examples section below.

[0055] The inventors have discovered that the cured adhesive layer preferably has a Dk of 3.0 or less, or 2.5 or less at 10 GHz, and a Df of 0.0060 or less, or 0.0040 or less, or 0.0020 or less at 10 GHz.

[0056] Suitable resin mixtures can be prepared according to the adhesive compositions disclosed in U.S. Patent Application No. 2016 / 0137889A1, or can be purchased from commercial sources (such as those from DuPont). GPL or GFL).

[0057] The composite material of the present invention

[0058] The composite material 100 of the present invention comprises a copper foil 1 and an adhesive layer 2, wherein the copper foil has a first surface 11 and a second surface 12 (i.e., a smooth surface). A mixture forming the adhesive layer is applied to the smooth surface 12 of the copper foil, such as... Figure 1 As shown.

[0059] The mixture forming the adhesive layer 2 can be applied by various coating methods well known in the art, including spraying, curtain coating, roller coating, air knife coating, slot die coating, casting, direct gravure printing, reverse gravure printing, offset gravure printing, roll coating, dip coating, or immersion coating. Note that when using dip coating or immersion coating, the resist side of the copper foil can be covered with a releasable protective layer. In some embodiments, slot die coating can be used.

[0060] The resin mixture can be applied using any suitable application method readily determined by those skilled in the art. As used herein, the term "coating" is not intended to limit the method of applying it to a smooth surface of copper foil.

[0061] After coating, the solvent or mixed solvent can be removed by heating in an oven at a temperature of 60°C–160°C to ensure that the mixture is partially cured in stage B. The temperature and duration in the oven will depend on the solvent used and the thickness of the coating. Alternatively, the composite material of the present invention can be manufactured by first coating a layer of the mixture onto a release liner or carrier film, and then transferring the coating layer to the smooth surface of the copper foil by lamination.

[0062] The thickness of the adhesive layer in the composite material of the present invention varies depending on the end use of the composite material. Before lamination with the substrate, the adhesive layer of the composite material of the present invention has a thickness of about 0.1 μm to about 200 μm, or about 0.5 μm to about 100 μm, or about 1 μm to about 50 μm, or about 3 μm to about 20 μm. While such thicknesses are preferred, it should be understood that other thicknesses can be produced to meet specific needs and still fall within the scope of the present invention.

[0063] The composite material of the present invention typically has a total thickness of about 6.1 to about 600 μm, or about 10 μm to about 150 μm, or about 15 μm to about 100 μm. The total thickness of the composite material of the present invention can be adjusted according to the substrate type by changing the thickness of the adhesive layer, the thickness of the copper foil, or both.

[0064] copper-clad laminate

[0065] The composite material of the present invention can be incorporated into a copper-clad laminate (CCL) by laminating it onto a substrate. Suitable substrates for forming the CCL of the present invention can be rigid or flexible.

[0066] Flexible substrates include, but are not limited to, polyimide (PI) films, polyamide-imide (PAI) films, liquid crystal polymer films, or fluorine-based polymer films. Commercially available polyimide films include those from DuPont. APICAL from Kaneka Chemical Co., Ltd. TM From Ube Corporation Polyamide-imide films, such as those from Solvay.

[0067] Rigid substrates are typically derived from prepregs, which are formed by impregnating polymeric materials into fiber-reinforced members. Examples of fiber-reinforced members include woven glass fabrics such as E-glass (aluminosilicate glass) cloth, nonwoven glass fabrics, and nonwoven aramid fabrics.

[0068] Suitable polymeric materials for impregnation include, but are not limited to, epoxy resins, polyphenylene ether (PPE), polyphenylene oxide (PPO), liquid crystal polymers (LCP), polyimide (PI), polyamide-imide (PAI), polyether-imide (PEI), polyesters, polyolefins, poly(meth)acrylates, polyphenylene sulfide (PPS), polyoxymethylene (POM), polyaryletherketone (PAEK), polyetheretherketone (PEEK), polysulfone (PSU), polyethersulfone (PES), cyanate esters, polyethers, or fluorine-based polymers.

[0069] Examples of epoxy resins include, but are not limited to, bifunctional or polyfunctional bisphenol A or bisphenol F resins, epoxy-phenolic varnish resins, or brominated epoxy resins.

[0070] Examples of polyesters include, but are not limited to, polybutylene terephthalate (PBT), polyethylene terephthalate (PET), or polyethylene naphthalate (PEN).

[0071] Examples of polyolefins include, but are not limited to, polypropylene (PP) or polyethylene (PE).

[0072] Examples of fluorine-based polymers include, but are not limited to, tetrafluoroethylene polymer (PTFE), tetrafluoroethylene hexafluoropropylene copolymer, tetrafluoroethylene perfluoro(alkyl vinyl ether) copolymer (PFA), tetrafluoroethylene copolymer, polychlorotrifluoroethylene, ethylene-chlorotrifluoroethylene copolymer, polyvinylidene fluoride, polyvinylidene fluoride hexafluoropropylene copolymer, or polyvinylidene fluoride.

[0073] Examples of commercially available prepregs include 2929 bondply material (PTFE-based, Dk=2.9 and Df=0.3 at 10 GHz) and RO4450, both available from Rogers Corp. TM Prepreg (Dk is 3.30-3.54 at 10 GHz, depending on thickness); R-5670 prepreg material (PPE-based, Dk = 3.35, Df = 0.004 at 12 GHz) is available from Panasonic Corp.; MCL-HS100 prepreg material (epoxy-based, Dk = 3.4-4.1, Df = 0.0025-0.0055 at 10 GHz) is available from Hitachi Chemical Co., Ltd.

[0074] The composite material of the present invention can be bonded to one or both surfaces of a substrate, corresponding to the application to form such as Figure 2 The single-sided CCL shown or as Figure 3 The double-sided CCL shown in the figure.

[0075] like Figure 2 As shown, the composite material 100 of the present invention is placed on the substrate 3, so that the adhesive layer 2 is in contact with the substrate 3, and then laminated by a method (such as hot pressing, continuous rolling, continuous band pressing, etc.) to provide a single-sided CCL, which is an embodiment of the present invention.

[0076] Similarly, such as Figure 3 As shown, the double-sided CCL 300 of the present invention can be manufactured by sequentially assembling the composite material 100, substrate 3, optional adhesive layer 4, and second copper foil 5; then laminating them together using the method described above; wherein the substrate 3 is in contact with the adhesive layer 2. Note that the second copper foil 5 may be the same as or different from the copper foil 1.

[0077] In some embodiments, when the adhesive layer 4 is absent, the second copper foil 5 of the double-sided CCL 300 of the present invention preferably has its roughened surface (i.e., also referred to herein as the laminated surface) in contact with the substrate 3 to ensure sufficient adhesion, and the roughened surface may be pretreated with an adhesion promoter.

[0078] In some embodiments, regardless of whether the second copper foil 5 is the same as or different from the copper foil 1, an adhesive layer 4 is present to enhance the adhesion between the second copper foil 5 and the substrate 3.

[0079] In other embodiments, the adhesive layer 4 and the second copper foil 5 are derived from the composite material 110 of the present invention, wherein the composite material 110 and the composite material 100 may be the same or different.

[0080] The process parameters used to prepare the copper-clad laminates of this invention, such as temperature, pressure, and time, generally depend on the material properties of the substrate and the preparation method. Those skilled in the art can therefore determine suitable process parameters.

[0081] In some embodiments, the copper-clad laminate of the present invention is prepared by hot pressing.

[0082] In some embodiments, hot pressing is performed at a temperature ranging from about 80°C to about 250°C, or from about 135°C to about 225°C; at a pressure ranging from about 0.2 MPa to about 17.4 MPa, or from about 0.5 MPa to about 5 MPa; and for a duration of about 30 minutes to about 300 minutes, or from about 60 minutes to about 240 minutes.

[0083] The copper-clad laminates of the present invention typically have a total thickness of about 30 μm to about 2000 μm, or about 50 μm to about 1500 μm, or about 90 μm to about 1000 μm. The total thickness of the copper-clad laminates of the present invention can be easily adjusted by using composite materials and substrates of the present invention of various thicknesses.

[0084] This invention utilizes a composite material to produce copper-clad laminates with good to excellent peel strength. The composite material comprises a copper foil having at least one smooth surface (which is unroughened and without adhesive accelerator pretreatment) and an adhesive layer composed of a resin material with low Dk and Df values. The peel strength of the CCL of this invention can be, for example, 0.4 kN / m or greater, or 0.6 kN / m or greater, or 0.8 kN / m or greater. Note that peel strength data may vary when the substrate is changed. In this document, peel strength is measured according to the methods described in the Examples section below.

[0085] Furthermore, the copper-clad laminate of the present invention also exhibits excellent heat resistance and is expected to withstand soldering and reflow steps during PCB manufacturing processes. For example, the CCL of the present invention can withstand heat treatment at 260°C, 288°C, or even 320°C or higher for at least 30 seconds or longer without blistering or delamination. In this document, the heat resistance to soldering temperatures is measured using the methods described in the Examples section below.

[0086] Printed circuit board (PCB)

[0087] The copper-clad laminate of the present invention can be subjected to known patterning methods (such as subtractive (photolithography) or additive (electroplating)) to form a predetermined conductor pattern (i.e., circuit) on the resist surface of the copper foil to produce a printed circuit board (PCB, or printed wiring board). Since the manufacturing process of PCBs is well known to those skilled in the art, its disclosure is omitted herein for the sake of brevity.

[0088] The printed circuit boards produced from the composite materials and CCLs of the present invention can then be assembled with other components (such as leads and holes) to form various electrical products utilizing high-speed signals with data rates of at least 1 Gbps and / or high-frequency signals of at least 1 GHz.

[0089] The printed circuit board comprising the composite material and CCL of this invention exhibits an insertion loss of 2.5 dB / 10 cm or less, or 2.0 dB / 10 cm or less, or 1.5 dB / 10 cm or less at a frequency of 10 GHz; and an insertion loss of 8.0 dB / 10 cm or less, or 7.0 dB / 10 cm or less, or 6.0 dB / 10 cm or less at a frequency of 39 GHz. In this document, the insertion loss is a value measured by the method described in the Examples section below.

[0090] Products utilizing high-performance PCBs include servers, routers, storage area networks, power amplifiers, transceiver modules, and high-speed data channels.

[0091] In addition, consumer devices requiring higher data rates and computing performance include mobile electronic devices such as laptops, tablets, e-readers, portable gaming devices, portable media players, digital cameras, mobile phones, or wearable devices; smart home devices; manned and autonomous vehicles; aviation equipment such as drones, airplanes, and spacecraft; and so on.

[0092] Without further detailed explanation, it is believed that those skilled in the art can utilize the foregoing description to the fullest extent possible. Therefore, the following examples should be interpreted as merely illustrative and not as limiting the scope of this disclosure in any way.

[0093] Example

[0094] The abbreviation "E" stands for "Example," and "CE" stands for "Comparative Example," with the numbers following them indicating the example number in which the copper-clad laminate was prepared. Examples and comparative examples were prepared and tested in a similar manner.

[0095] Material

[0096] CF1: is a copper foil with a thickness of 12 μm; the smooth surface of the foil has a surface roughness (Rz) of 0.62 μm and is plated with less than 100 μg / dm². 2 Non-copper elements. Copper foil with the same grade as CF1 but a thickness of 35 μm was tested and found to have 0.170 gΩ / m. 2 Or even smaller resistance.

[0097] CF2: is an ED copper foil with a thickness of 35 μm; the smooth surface of the foil has a surface roughness (Rz) of 1.06 μm and is plated with less than 100 μg / dm². 2 The non-copper elements. A piece of CF2 copper foil was tested and found to have 0.170 gΩ / m 2 Or even smaller resistance.

[0098] CF3: This is an ED copper foil with a thickness of 12μm, product number HVLP2; the laminated surface of the foil has a surface roughness (Rz) of 3.21μm and is plated with 300-350μg / dm². 2 Non-copper elements. Copper foil with the same grade as CF3 but a thickness of 35 μm was tested and found to have 0.170 gΩ / m. 2 Or even smaller resistance.

[0099] CF4: This is an ED copper foil with a thickness of 12μm, product number HVLP1; the laminated surface of the foil has a surface roughness (Rz) of 4.22μm and is plated with 350-400μg / dm². 2 Non-copper elements. Copper foil with the same grade as CF4 but a thickness of 35 μm was tested and found to have 0.170 gΩ / m. 2 Or even smaller resistance.

[0100] Adh1: This is an adhesive sheet available from DuPont. Product name: GPL. The Dk and Df of the cured Adh1 sample were tested according to the following procedure, and it was found that it had a Dk of 2.8 and a Df of 0.0035.

[0101] Adh2: An adhesive sheet available from DuPont. Product name: GFL. The Dk and Df of the cured Adh2 sample were tested according to the following procedure, and it was found that it had a Dk of 2.4 and a Df of 0.0017.

[0102] S1 is an ultra-low loss planar prepreg with a thickness of approximately 130 μm, which is composed of woven glass fiber fabric and impregnated with modified epoxy resin, and has Dk = 3.62 and Df = 0.005 at 10 GHz (tested according to the conditions specified by IPC-TM-650 No. 2.5.5.13).

[0103] S2 is a low-loss planar prepreg with a thickness of approximately 130 μm, which is composed of woven glass fiber fabric and impregnated with epoxy resin, and has Dk = 3.9-4.0 and Df = 0.005-0.006 at 1 GHz (tested according to the conditions specified by IPC-TM-650 No. 2.5.5.9).

[0104] Preparation of composite materials A and B

[0105] Adh1 is transferred from a carrier film (132 μm release paper) to the smooth surface of a copper foil (CF1, 29 cm × 20 cm) by lamination using a roller laminator at a linear speed of approximately 0.3 MPa and 0.5 m / min at a roller temperature of 120 °C to provide a composite material A, which is one embodiment of the present invention. The resulting composite material A has a thickness of approximately 16.5 μm and an adhesive layer thickness of 4.5 μm.

[0106] Composite material B was obtained according to the above procedure, except that Adh2 was applied to a smooth surface of a copper foil (CF2) instead of Adh1. The resulting composite material B has a thickness of approximately 39 μm and an adhesive layer thickness of 4 μm.

[0107] Preparation of copper-clad laminates in Examples 1-3

[0108] The copper-clad laminates in the working examples (E1-E3) have the following characteristics: Figure 3 The double-sided copper-clad laminate 300 has a structure in which optional layer 4 is absent. The CCL is manufactured as follows using a hot press (manufactured by LCM):

[0109] The substrate sheet (S1 or S2) is cut into 30cm × 30cm square sheets. The composite material (composite material A or B) obtained through the above procedure is placed on the substrate, with the adhesive layer in contact with the substrate. A copper foil (CF3) is applied to the opposite side of the substrate, with its laminated surface in direct contact with the substrate.

[0110] The lamination parameters were adjusted according to the recommended lamination parameters for the substrate. Lamination was performed under a vacuum of 0.99 atm (751 Torr), and the temperature and pressure characteristic curves are shown below:

[0111] Temperature characteristic curves: (1) Start at 80℃ and heat to 120℃ within 5 min, (2) Hold at 120℃ for 3 min and heat to 180℃ within 5 min, (3) Hold at 180℃ for 32 min and heat to 210℃ within 5 min, (4) Hold at 210℃ for 143 min and cool to 160℃ within 12 min, (5) Cool to 50℃ within 1 min and hold at 50℃ for 30 min.

[0112] Pressure characteristic curves: (1) Increase to 0.3 MPa in 1 min, (2) Maintain at 0.3 MPa for 3 min and increase to 1.0 MPa in 1 min, (3) Maintain at 1.0 MPa for 11 min and increase to 3.4 MPa in 1 min, (4) Maintain at 3.4 MPa for 176 min and decrease to 2.7 MPa in 1 min, (5) Maintain at 2.7 MPa for 11 min and decrease to 0.1 MPa in 1 min, (6) Maintain at 0.1 MPa for 30 min.

[0113] Preparation of copper-clad laminates in comparative examples 1-6

[0114] Each copper-clad laminate of comparative examples (CE1-CE6) was prepared by directly laminating a copper foil (CF1, CF3, or CF4) onto a substrate (S1 or S2) (where the smooth surface of the copper foil or the laminated surface is in contact with the substrate). On the opposite side of the substrate, a copper foil (CF3) was also laminated onto the substrate, where its laminated surface is in direct contact with the substrate. Lamination was performed according to the lamination conditions described above for Examples 1-3.

[0115] Preparation of test specimens in Examples 1 and 3 and Comparative Examples 1-6

[0116] Each copper-clad laminate in the examples and comparative examples was further processed to form a microstrip structure having a total thickness of approximately 162 μm, a conductor length of 100 mm, a conductor thickness of 12 μm, and, respectively, a conductor width of 300 μm for the CCL using S1 as the substrate and a conductor width of 275 μm for the CCL using S2 as the substrate.

[0117] The test results are listed in Tables 1 to 3.

[0118] Test methods

[0119] Surface roughness (Rz): Measured at five points using a laser scanning microscope (manufactured by Keyence, model: VK-9700), and the data were averaged.

[0120] Layer thickness: The thickness of the adhesive layer of composite material A or B is determined using a contact thickness gauge. Each sample is measured 6-10 times at different locations, and the results are averaged.

[0121] Resistance test: According to IPC-TM-650 2.5.14, a copper foil sample with a thickness of 35μm was used, and the sample was annealed in an N2 oven at 200°C for 2 hours.

[0122] Solder Floating Test: This test simulates the thermal shock encountered during the reflow component assembly process of printed circuit board solder. Three samples (size: 5cm × 5cm) of each CCL are floated on a bath of molten solder (99.3% tin, 0.7% copper) by placing the CF3 side down at 260°C or 288°C for 3 minutes. The samples are then removed, cooled to ambient temperature, and visually inspected. The top surface of the sample (i.e., opposite to the CF3 side) is visually inspected, and if no deterioration (such as blistering and delamination) is found, it is marked as "pass".

[0123] Chemical resistance and aging performance: Each CCL instance underwent different chemical treatments. For the HCl resistance test, the sample was immersed in a container with an 18% HCl solution for 60 min, then removed from the container, rinsed with DI water, air-dried at room temperature for 24 h, and the appearance of the sample was visually inspected. A similar procedure was repeated by subjecting each sample made from the corresponding CCL instance to other chemical treatments, including 8% NaOH for 30 min and 3% H2SO4 at 50°C for 60 min. Finally, the sample was placed in an oven at 180°C for 10 days. Afterward, the sample was sent for peel strength testing to determine whether the chemical treatment or aging test caused any degradation.

[0124] Peel strength test: CCL samples, either prepared undisturbed or obtained after chemical treatment / aging tests, were cut into rectangular samples of 75mm × 30mm. The samples were then patterned using photolithography with straight lines, where the line / spacing was 1mm / 1mm. The patterned laminate sample was fixed to an FR4 board (i.e., fiberglass board, purchased from HONTEC) measuring 98mm (L) × 31mm (W) with double-sided tape and then mounted on a sliding sample holder. The front portion of the patterned laminate sample was then manually peeled off and clamped to the upper fixture. The peel strength was tested using a testing machine (manufactured by SHIMADZU, model: AG-IS) at a traction speed of 50.8mm / min, and the peel strength was measured and recorded in kN / m. The peel strength data from the three test lines were averaged and listed in Table 1-2.

[0125] Dk / Df Measurement: Adhesive samples (adh1 or adh2) were coated onto a releasable PET film with a thickness of approximately 25 μm. Adhesive layers were then stacked to a thickness of approximately 85–125 μm and fully cured at 200 °C for 90 min to produce cured adhesive samples. The cured adhesive samples were tested using a split post-dielectric resonator (SPDR) cavity and vector network analyzer (manufacturer: Keysight, model E5063A) at 10 GHz. Each sample was tested twice, and the two data points were averaged to obtain the Dk / Df data.

[0126] Insertion loss: Measurements were performed on CCL samples with microstrip structures and no cover film using an Agilent PNA network analyzer, scanning from 10 MHz to 40 GHz, with a reference impedance of 50 Ω, 4001 scan points, calibration: Keysight AFR, and temperature: 23 °C. The transmission loss (dB / m) corresponding to the frequencies of 10 GHz and 39 GHz is reported in Table 3. The improvement in insertion loss was calculated by dividing the difference between the measured insertion loss data of the comparative example and the reference example by the data of the comparative example.

[0127] Table 1

[0128]

[0129]

[0130] a For laminated structures, " / " is used to separate each individual layer from one or more adjacent layers.

[0131] From the results in Table 1, the following is obvious.

[0132] Comparing the data of E1 and E2 with CE1, the CCL of E1 and E2 showed better heat resistance and maintained high peel strength through various acid / alkali treatments.

[0133] Comparing the data for E1 with those for CE2 and CE3, for the same substrate (i.e., S1) and copper foil thickness, the E1 laminate exhibits similar heat resistance, peel strength, and maintains peel strength through various acid / alkali treatments. These results demonstrate that the composite material and CCL of this invention are suitable for providing PCBs with excellent performance and reliability, even after various harsh conditions in the manufacturing process.

[0134] Table 2

[0135]

[0136] aFor laminated structures, " / " is used to separate each individual layer from one or more adjacent layers.

[0137] From the results in Table 2, the following is obvious.

[0138] Comparing solder float data between E3 and CE4, the E3 CCL also exhibited unexpectedly better performance in heat resistance and peel strength through various acid / alkali treatments and aging tests. These results demonstrate that the composite material of the present invention is compatible with a variety of substrates, and that the CCL of the present invention can provide PCBs with excellent performance and reliability even at high operating temperatures.

[0139] Table 3

[0140]

[0141] a For laminated structures, " / " is used to separate each individual layer from one or more adjacent layers.

[0142] b Use the data from the example as a reference to calculate the improvement relative to the comparison example.

[0143] From the results in Table 3, the following is obvious.

[0144] Comparing the insertion loss data of E1 with those of CE2 and CE3, since they have the same substrate, the CCL of E1 unexpectedly provides a lower insertion loss value than the CCLs of CE2 and CE3.

[0145] Comparing the insertion loss data of E3 with those of CE5 and CE6, since they share the same substrate, the CCL of E3 also shows a significantly lower insertion loss value than that of the CCLs of CE5 and CE6. The results indicate that the composite material and CCL of the present invention are suitable for producing printed circuit boards with low insertion loss for high-frequency or high-speed circuit applications.

[0146] While the invention has been illustrated and described in typical embodiments, it is not intended to limit the details shown, as various modifications and substitutions may be made without departing from the spirit of the invention. Similarly, modifications and equivalents of the invention disclosed herein can be derived by those skilled in the art using only conventional experimentation, and all such modifications and equivalents are considered to be within the spirit and scope of the invention as defined in the following claims.

Claims

1. A composite material for manufacturing copper-clad laminates, the composite material comprising copper foil and an adhesive layer, in The copper foil has a strength of 0.170 gΩ / m 2 Or even smaller resistance, at least one smooth surface with a surface roughness Rz of 0.62 µm to 1.06 µm, less than 1 piece / µm 2 The density of nodules, and having 350 µg / dm² on the smooth surface. 2 Or even lower total content of non-copper metal elements; The adhesive layer is derived from a mixture comprising: a resin matrix containing 5-25 parts by weight of a reactive resin, 0.1-3 parts by weight of a curing agent, and 72-94.9 parts by weight of a styrene-based rubber; and 0-100 parts by weight of an additive based on 100 parts by weight of the resin matrix, wherein the reactive resin is selected from the group consisting of: phenol-phenolic varnish type epoxy resin, cresol-phenolic varnish type epoxy resin, glycidyl ether type epoxy resin, and various combinations thereof; The adhesive layer is in contact with the smooth surface of the copper foil; The cured adhesive layer has a Dk of 3.0 or less and a Df of 0.006 or less at 10 GHz, wherein Dk and Df are tested according to the following method: an adhesive sample is coated onto a releasable PET film with a thickness of 25 µm, then the adhesive layer is stacked to a thickness of 85–125 µm and fully cured at 200°C for 90 min to produce a cured adhesive sample. The cured adhesive sample is tested using a split post-dielectric resonator cavity and vector network analyzer at 10 GHz, with each sample tested twice and the two data points averaged; and The premise is that the smooth surface of the copper foil has not been pretreated with an adhesion promoter.

2. The composite material as described in claim 1, wherein, The copper foil has a thickness of 6 µm to 400 µm.

3. The composite material as described in claim 1, wherein, The adhesive layer has a thickness of 0.1 µm to 200 µm.

4. The composite material as described in claim 1, wherein, The adhesion promoter is selected from the group consisting of: silanes, silylamines, allyl phosphites, allyl phosphates, azole silanes, unsaturated amide-substituted heterocyclic compounds, and aminotriazine-based compounds.

5. A copper-clad laminate with improved low transmission loss, comprising a substrate and a composite material as described in any one of claims 1-4. The substrate is a film composed of polyimide, polyamide-imide, liquid crystal polymer, or fluorine-based polymer.

6. A copper-clad laminate with improved low transmission loss, comprising a substrate and a composite material as described in any one of claims 1-4, The substrate is a prepreg made of fiber-reinforced members impregnated with polymer material; The fiber-reinforced component is a woven glass fabric, a nonwoven glass fabric, or a nonwoven aramid fabric; and The polymer material is epoxy resin, polyphenylene ether, liquid crystal polymer, polyimide, polyamide-imide, polyether-imide, polyester, polyolefin, poly(meth)acrylate, polyphenylene sulfide, polyoxymethylene, polyaryletherketone, polyetheretherketone, polysulfone, polyethersulfone, cyanate ester, polyether, or fluorine-based polymer.

7. The copper-clad laminate as described in claim 5 or 6, wherein, The copper-clad laminate has a peel strength of 0.4 kN / m or greater, heat resistance of no blistering or delamination for more than 30 seconds at 260°C, and an insertion loss of 2.5 dB / 10 cm or less at 10 GHz or 8.0 dB / 10 cm or less at 39 GHz.

8. A printed circuit board manufactured from the copper-clad laminate as described in claim 5 or 6.

9. The printed circuit board as claimed in claim 8, wherein it is a flexible printed circuit board or a rigid printed circuit board.

10. Use of the printed circuit board of claim 8 in high-speed applications, high-frequency applications, or both; wherein the high-speed application has a data rate higher than 1 Gbps, and the high-frequency application has a frequency higher than 1 GHz.

Citation Information

Patent Citations

  • Metal-polymer adhesion

    EP0251490A2

  • Surface-treated copper foil, a method for manufacturing the same, and surface-treated copper foil with an extremely thin primer resin layer

    TWI339222B

  • Electrolysis copper foil with surface layer containing rugby-shape structure and circuit board component

    TWM543248U

  • Electrolysis copper foil with surface layer containing fur-shape structure and circuit board component

    TWM543249U

  • Surface treatment agent and novel compound

    US10385076B2