A negative electrode sheet, solid-state battery and preparation method thereof

By adopting the structural design of the silicon alloy negative electrode active layer and pre-lithium layer in the sulfide all-solid-state battery, the problem of crushing and cracking caused by the volume expansion of the silicon-based negative electrode sheet during the charge and discharge process is solved, and the cycle performance and first life of the battery are improved. Effectively, it promotes the industrial application of sulfide all-solid-state batteries.

CN113991058BActive Publication Date: 2024-10-22SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111247875.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-26
Publication Date
2024-10-22
Estimated Expiration
2041-10-26

AI Technical Summary

Technical Problem

The volume expansion of existing silicon-based sulfide negative electrode sheets during charging and discharging causes crushing and cracking, resulting in poor battery cycle life and reduced energy density. The first efficiency is low, making it difficult to promote the industrial application of sulfide all-solid-state batteries.

Method used

The structural design of the silicon alloy negative active layer and the pre-lithium layer is adopted. Through the stacking arrangement of the first silicon alloy negative active layer and the second silicon alloy negative active layer, the surface capacity is controlled to avoid powdering and cracking, and the pre-lithium layer is reasonably replenished. Lithium source improves the charge and discharge efficiency and cycle performance of the battery.

Benefits of technology

It effectively improves the cycle capacity retention rate and first charge and discharge efficiency of all-solid-state batteries, reduces battery costs and pollution risks, and enhances battery safety and energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113991058B_ABST
    Figure CN113991058B_ABST
Patent Text Reader

Abstract

The present invention provides a negative electrode plate, a solid-state battery and a preparation method thereof, wherein the negative electrode plate comprises a negative electrode current collector, and a first silicon alloy negative electrode active layer, a pre-lithium layer and a second silicon alloy negative electrode active layer are sequentially stacked on the surface of the current collector. The present invention effectively increases the cycle capacity retention rate of a silicon negative electrode all-solid-state battery through the silicon alloy negative electrode metal active layer and the pre-lithium layer, which is conducive to promoting the commercial application of all-solid-state batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of batteries and relates to a negative electrode plate, a solid-state battery and a preparation method thereof. Background Art

[0002] Solid-state batteries use non-flammable solid electrolytes to replace flammable organic liquid electrolytes, which greatly improves the safety of the battery system and achieves a simultaneous increase in energy density. Among various new battery systems, solid-state batteries are the next generation technology closest to industrialization, which has become a consensus in the industry and scientific community. Among them, sulfide electrolytes have relatively high lithium ion conductivity, and the room temperature ion conductivity can reach 10 -3 ~10 -2 S / cm, which is close to or even exceeds that of organic electrolytes. It also has the characteristics of high thermal stability, good safety performance, and a wide electrochemical stability window (above 5V). It has outstanding advantages in high-power and high- and low-temperature solid-state batteries, and has broad prospects in the research and development of high-safety, high-energy density batteries.

[0003] When using sulfide solid electrolytes to prepare all-solid-state battery cell systems, in order to ensure the energy density advantage, the all-solid-state battery negative electrode usually uses a silicon-containing negative electrode or a lithium metal negative electrode. Currently, the application cost and technical difficulty of lithium metal negative electrodes are still very high.

[0004] CN105489931A discloses the application of sulfide electrolyte in the preparation of all-solid-state batteries. The application is specifically as follows: mixing raw materials containing sulfide electrolyte and binder to obtain mixed dry powder; fully grinding the mixed dry powder into a viscous powder, and pressing it into shape. The invention further protects the positive electrode layer, electrolyte layer, negative electrode layer or / and the battery cell composed of the positive electrode layer, electrolyte layer and negative electrode layer of the all-solid-state battery prepared using sulfide electrolyte. The application method provided by the invention and the all-solid-state battery based on sulfide electrolyte do not use any solvent, thereby avoiding the reaction between the solvent and the sulfide electrolyte and destroying the performance of the solid electrolyte; at the same time, it eliminates the toxic effects of organic solvents and the cumbersome removal and recovery processes, and the operation method is simple and easy.

[0005] CN112467085A discloses a method for preparing a silicon alloy negative electrode for an all-solid-state battery. The method utilizes the high cycle durability of high-performance silicon alloy active materials. Through a mechanical alloying preparation method, silicon and other element alloy active material particles can be "amorphized" and "multi-element alloyed". Other additions have good mechanical and conductive properties, improve the conductivity of the composite material, and at the same time limit the volume expansion of silicon during lithiation / delithiation.

[0006] Therefore, how to provide a negative electrode sheet that can effectively improve the battery's initial efficiency and cycle performance and promote the industrial application of sulfide all-solid-state batteries has become an urgent problem that needs to be solved. Summary of the Invention

[0007] In response to the shortcomings of the existing technology, the purpose of the present invention is to provide a negative electrode plate, a solid-state battery and a preparation method thereof. Through the silicon alloy negative electrode metal active layer and the pre-lithium layer, the cycle capacity retention rate of the silicon negative electrode all-solid-state battery is effectively increased, which is conducive to promoting the commercial application of all-solid-state batteries.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a negative electrode plate, comprising a negative electrode current collector, the surface of which is sequentially stacked with a first silicon alloy negative electrode active layer, a pre-lithium layer, and a second silicon alloy negative electrode active layer.

[0010] The present invention provides a silicon alloy negative electrode active layer and a pre-lithium layer. The silicon alloy negative electrode active layer contains an alloy formed with silicon, which prevents the problem of pulverization and cracking of the negative electrode plate, further avoids short-circuit failure of the battery after lithium supplementation, and effectively improves the charge and discharge initial efficiency and cycle performance of the high-silicon content negative electrode all-solid-state battery. It has the advantages of high mass specific capacity and high volume specific capacity, low cost, non-toxicity and pollution-free, and low lithium insertion platform.

[0011] In existing technology, silicon-based sulfide negative electrode sheets are generally composed of a sulfide electrolyte (ionic conductor), silicon material, conductive agent, and graphite material. Silicon material itself has low electrical conductivity. As an active material, silicon undergoes a volume change of up to 270% when it inserts and removes lithium during the charge / discharge cycle, resulting in poor cycle life. This volume expansion can lead to the pulverization of silicon particles, repeated cracking of the electrode sheet during charge and discharge, and separation of the electrode sheet coating from the copper current collector, resulting in pulverization and degradation, ultimately leading to lithium-ion battery failure. Furthermore, silicon negative electrode sheets have low initial efficiency without lithium supplementation, reducing the battery's capacity.

[0012] As a preferred technical solution of the present invention, the areal capacity of the first silicon alloy negative electrode active layer is greater than the areal capacity of the pre-lithium layer, and is less than the areal capacity of the second silicon alloy negative electrode active layer.

[0013] The present invention ensures that the surface capacity of the first silicon alloy negative electrode active layer is greater than the surface capacity of the pre-lithiation layer and less than the surface capacity of the second silicon alloy negative electrode active layer, thereby ensuring that the first silicon alloy layer will not be completely pre-lithiated (embrittled) and fall off from the current collector after pre-lithiation. The second silicon alloy layer serves as the main active layer, which not only undertakes the main task of lithium insertion and removal during the battery charging and discharging process, but also serves as a protective layer for the pre-lithiation layer. This ensures the capacity of the negative electrode and avoids the reduction of the battery energy density. If the above-mentioned surface capacity requirements are not met, there is a problem that short circuit and reduced energy density may occur during the battery charging and discharging process.

[0014] Preferably, the surface capacity of the first silicon alloy negative electrode active layer is 0.6 to 4.1 mAh / cm 2 , for example 0.6 mAh / cm 2 、1.0mAh / cm 2 、1.4mAh / cm 2 、1.8mAh / cm 2 , 2.2mAh / cm 2 , 2.6mAh / cm 2 、3.0mAh / cm 2 、3.4mAh / cm 2 、3.8mAh / cm 2 or 4.1mAh / cm 2 .

[0015] Preferably, the surface capacity of the pre-lithium layer is 0.5 to 4 mAh / cm 2 , for example 0.5 mAh / cm 2 , 0.8mAh / cm 2 、1.1mAh / cm 2 、1.4mAh / cm 2 , 1.7mAh / cm 2 , 2.0mAh / cm 2 , 2.3mAh / cm 2 , 2.6mAh / cm 2 , 2.9mAh / cm 2 、3.2mAh / cm 2 、3.5mAh / cm 2 、3.8mAh / cm 2 or 4.0mAh / cm 2 .

[0016] The present invention controls the surface capacity of the pre-lithium layer to 0.5-4 mAh / cm 2 , can reasonably supplement the lithium source, improve the battery charge and discharge efficiency and cycle performance, if the surface capacity is lower than 0.5mAh / cm 2, the pre-lithium amount is not enough, resulting in no obvious improvement in the first efficiency and cycle performance. If the pre-lithium surface capacity is higher than 4mAh / cm 2 , resulting in an increase in the corresponding negative electrode thickness, which in turn increases the length of the lithium ion channel, thereby increasing the polarization of the battery charge and discharge process, and an excessively high pre-lithium amount will increase the risk of battery short circuit.

[0017] Preferably, the surface capacity of the second silicon alloy negative electrode active layer is 4.2 to 10 mAh / cm 2 , for example, 4.2 mAh / cm 2 , 4.5mAh / cm 2 、5.0mAh / cm 2 、5.5mAh / cm 2 、6.0mAh / cm 2 、6.5mAh / cm 2 、7.0mAh / cm 2 , 7.5mAh / cm 2 、8.0mAh / cm 2 、8.5mAh / cm 2 、9.0mAh / cm 2 、9.5mAh / cm 2 or 10.0mAh / cm 2 .

[0018] Preferably, the pre-lithium layer comprises a metallic lithium strip.

[0019] Preferably, the negative electrode current collector comprises carbon-coated copper foil.

[0020] Preferably, the first silicon alloy negative electrode active layer comprises a negative electrode active material, a negative electrode electrolyte, metal powder, a conductive agent and a negative electrode binder.

[0021] Preferably, the first silicon alloy negative electrode active layer and the second silicon alloy negative electrode active layer have the same composition.

[0022] Preferably, the mass ratio of the negative electrode active material, negative electrode electrolyte, metal powder, conductive agent and negative electrode binder is (69.4~90):(0~10):(3~30):(0.1~5):(0.5~5), for example, 69.4:0:30:0.1:0.5, 70:7:18:2.5:2.5, 75:8:16:0.5:0.5, 80:5:10:3:2, 85:10:3:1:1 or 90:4:3:1.5:1.5.

[0023] The present invention controls the mass ratio of the negative electrode active material, the negative electrode electrolyte, the metal powder, the conductive agent and the negative electrode binder to be (69.4-90):(0-10):(3-30):(0.5-5):(0.5-5), and generates a silicon alloy by reacting the metal powder and the silicon-based active material. The silicon alloy has the advantages of little effect on the first efficiency and stable cycle performance. If the amount of metal powder added is too low, there is a problem of lack of alloy network structure, which easily leads to battery short circuit. If the amount of metal powder added is too high, there is a problem of reduced first efficiency.

[0024] As a preferred technical solution of the present invention, the negative electrode active material includes one or a combination of at least two of silicon, silicon oxide, silicon carbide or silicon nitride.

[0025] Preferably, the negative electrode electrolyte comprises a sulfide electrolyte.

[0026] Preferably, the sulfide electrolyte includes thio-LISICON, Li 10 GeP2S 12 、Li6PS5Cl、Li 10 SnP2S 12 , Li2S-P2S5, Li2S-SiS2, Li2S-B2S3 or a combination of at least two of them.

[0027] Preferably, the metal powder includes one or a combination of at least two of Fe, Co, Sb, Bi, Pb, Ni, Cu, Zn, Ge, In, Sn or Ti.

[0028] Preferably, the conductive agent includes one or a combination of at least two of a zero-dimensional conductive agent, a one-dimensional conductive agent or a two-dimensional conductive agent.

[0029] In one embodiment, the zero-dimensional conductive agent includes conductive carbon black and / or acetylene black; the one-dimensional conductive agent includes carbon nanotubes and / or carbon fibers; and the two-dimensional conductive agent includes graphene.

[0030] Preferably, the negative electrode binder includes one or a combination of at least two of PAA, Li-PAA, SBR, NBR, HNBR, SBR, SBS, SEBS or PEO.

[0031] In a second aspect, the present invention provides a solid-state battery, comprising a positive electrode, an electrolyte layer and a negative electrode, wherein the negative electrode adopts the negative electrode sheet described in the first aspect.

[0032] As a preferred technical solution of the present invention, the NP ratio of the negative electrode to the positive electrode is 1.08 to 1.8, for example, 1.08, 1.10, 1.20, 1.30, 1.40, 1.50, 1.60, 1.70 or 1.80.

[0033] It should be noted that the NP ratio is the capacity margin of the negative electrode over the positive electrode at the same stage and under the same conditions. The calculation formula is: gram capacity of negative electrode active material * negative electrode surface density * negative electrode active material content ratio / (gram capacity of positive electrode active material * positive electrode surface density * positive electrode active material content ratio).

[0034] Preferably, the positive electrode of the solid-state battery includes a positive electrode current collector and a positive electrode active layer provided on at least one side surface of the positive electrode current collector.

[0035] The positive electrode active layer includes a positive electrode active material, a positive electrode electrolyte, a conductive agent and a positive electrode binder.

[0036] Preferably, the mass ratio of the positive electrode active material, positive electrode electrolyte, conductive agent and positive electrode binder is (40-91.4): (8-50): (0.5-8): (0.1-8), for example, 40:50:5:5, 50:34:8:8, 60:32:3:5, 70:20:4:6, 80:15:2:3 or 91.4:8:0.5:0.1.

[0037] Preferably, the positive electrode current collector comprises carbon-coated aluminum foil.

[0038] Preferably, the positive electrode active material comprises LiNi having an ion conductor coating layer. x Co y M z O2, x≥0, y≥0, z≥0, x+y+z=1, M includes one or a combination of at least two of Mn, Al, Zr, Ti, V, Mg, Fe or Mo.

[0039] Preferably, the cathode electrolyte comprises a sulfide electrolyte.

[0040] Preferably, the material of the ion conductor coating layer includes one or a combination of at least two of Li2TiO3, LiNbO3, Li3BO3, Li2ZrO3, LiCoO3, LiPO3, Li2MnO4, Al(PO3)3, La(PO3)3 or NaPO3.

[0041] Preferably, the thickness of the ion conductor coating layer is 1 to 10 nm, for example, 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm or 10 nm.

[0042] As a preferred technical solution of the present invention, the thickness of the electrolyte layer is 15 to 50 μm, for example, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm or 50 μm.

[0043] Preferably, the electrolyte layer comprises a sulfide electrolyte and an electrolyte binder.

[0044] Preferably, in the electrolyte layer, the mass ratio of the sulfide electrolyte to the electrolyte binder is (90-99.5):(0.5-10), for example, 90:10, 91:9, 92:8, 93:7, 94:6, 95:5, 96:4, 97:3, 98:2, 99:1 or 99.5:0.5.

[0045] Preferably, the electrolyte binder includes one or a combination of at least two of PVDF5130, PVDF75130, PVDF21216, PVD, F6020, PVDF-HVS900, PVDF-HFP, PVDF-LBG, NBR, HNBR, SBR, SBS or SEBS.

[0046] In one embodiment, the preparation method of the electrolyte layer includes: weighing a sulfide electrolyte and an electrolyte binder, mixing a solvent and the electrolyte binder to form a slurry, then adding the sulfide electrolyte and ball milling to mix the slurry, wherein the solid content of the slurry is 70%, coating the obtained slurry on PET, and drying at 100°C to obtain an electrolyte layer disposed on the PET.

[0047] In a third aspect, the present invention provides a method for preparing the solid-state battery described in the second aspect, the method for preparing the solid-state battery comprising: setting a first silicon alloy negative electrode active layer on one side surface of the negative electrode current collector, and performing pre-lithiation on the surface of the first silicon alloy negative electrode active layer to obtain a pre-lithiation layer, and then setting a second silicon alloy negative electrode active layer on the other side surface of the negative electrode current collector to prepare the negative electrode plate, and after encapsulating and pressing the negative electrode plate, positive electrode and electrolyte layer, the solid-state battery is prepared.

[0048] As a preferred technical solution of the present invention, the first silicon alloy negative electrode active layer is obtained by coating a negative electrode active slurry.

[0049] Preferably, the step of providing the first silicon alloy negative electrode active layer comprises: coating the negative electrode active slurry on the negative electrode current collector, drying it, and then rolling it to obtain the first silicon alloy negative electrode active layer.

[0050] In one embodiment, the rolling temperature of the first silicon alloy negative electrode active layer is 50-70°C and the pressure is 8-12 MPa / cm 2 .

[0051] Preferably, the solvent in the negative electrode active slurry includes one or a combination of at least two of water, dichloromethane, tetrahydrofuran, n-hexane, n-heptane, toluene, 2,4-dimethyl-3-pentanone, monochlorobenzene, xylene, anisole, cyclohexanone, 1,3,5-trimethylbenzene, n-decane and methylformamide, and more preferably water.

[0052] As a preferred technical solution of the present invention, the pre-lithiation method includes pressing lithium strips.

[0053] Preferably, the step of pressing the lithium ribbon comprises: performing at least one warm isostatic pressing to press the lithium ribbon having a PET substrate onto the surface of the first silicon alloy negative electrode active layer, and removing the PET to obtain a pre-lithium layer.

[0054] Preferably, the second silicon alloy negative electrode active layer is obtained by pressing.

[0055] Preferably, the pressing step of the second silicon alloy negative electrode active layer includes: coating the negative electrode slurry on aluminum foil, drying it, and performing at least one warm isostatic pressing with the pre-lithium negative electrode sheet, and removing the aluminum foil to obtain the second silicon alloy negative electrode active layer.

[0056] Preferably, the preparation step of the positive electrode comprises: mixing a positive electrode active material, a positive electrode electrolyte, a conductive agent and a positive electrode binder, dry rolling them, and then compounding them on the surface of a positive electrode current collector to prepare the positive electrode.

[0057] Preferably, the packaging and pressing method includes: laminating the negative electrode sheet and the electrolyte layer, performing at least one warm isostatic pressing to obtain the negative electrode sheet of the composite electrolyte layer, laminating the positive electrode and welding the tabs, and then packaging, performing at least one warm isostatic pressing to prepare the battery.

[0058] Preferably, the temperature of the warm isostatic pressing is 50-120°C, for example, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C or 120°C.

[0059] Preferably, the warm isostatic pressing pressure is 5 to 650 MPa, for example, 5 MPa, 10 MPa, 50 MPa, 100 MPa, 150 MPa, 200 MPa, 250 MPa, 300 MPa, 350 MPa, 400 MPa, 450 MPa, 500 MPa, 550 MPa, 600 MPa or 650 MPa.

[0060] Preferably, the holding time of the warm isostatic pressing is 1 to 720 min, for example, 1 min, 30 min, 60 min, 120 min, 180 min, 240 min, 300 min, 360 min, 420 min, 480 min, 540 min, 600 min, 660 min or 720 min.

[0061] Preferably, the warm isostatic pressing is performed 1 to 5 times, for example, 1 time, 2 times, 3 times, 4 times or 5 times.

[0062] As a preferred technical solution of the present invention, the preparation method specifically comprises the following steps:

[0063] The negative electrode active slurry is coated on the negative electrode current collector, and after drying, the negative electrode active slurry is rolled to obtain the first silicon alloy negative electrode active layer;

[0064] Placing a lithium strip with a PET substrate on the surface of the first silicon alloy negative electrode active layer, performing at least one warm isostatic pressing at 50-120° C. and 5-650 MPa for a holding time of 1-720 minutes, and removing the PET to prepare a pre-lithium layer;

[0065] The negative electrode slurry is coated on aluminum foil, dried, and laminated with a negative electrode sheet provided with a pre-lithium layer. Warm isostatic pressing is performed at least once at 50-120° C. and 5-650 MPa for a holding time of 1-720 min. After removing the aluminum foil, a second silicon alloy negative electrode active layer is obtained to prepare the negative electrode sheet.

[0066] The positive electrode active material, positive electrode electrolyte, conductive agent and positive electrode binder are mixed, dry-rolled and then composited onto the surface of the positive electrode current collector to prepare the positive electrode;

[0067] The negative electrode sheet is laminated to the electrolyte layer, and warm isostatic pressing is performed at least once at 50-120° C. and 5-650 MPa for a holding time of 1-720 min to obtain a negative electrode sheet with a composite electrolyte layer. The positive electrodes are laminated, the tabs are welded, and then packaged. Warm isostatic pressing is performed at least once at 50-120° C. and 5-650 MPa for a holding time of 1-720 min to prepare the battery.

[0068] The process of laminating the negative electrode sheet and the electrolyte layer specifically includes: laminating and encapsulating the negative electrode sheet and the electrolyte layer provided on the PET, performing warm isostatic pressing at least once, and after removing the PET, completing the composite of the electrolyte layer and the negative electrode sheet; the encapsulation and pressing process specifically includes: punching the sheet through a die (for example, with a size of 4.2*6.2cm), then punching the positive electrode sheet (for example, with a size of 4*6cm), welding the tabs after lamination and encapsulating, and performing warm isostatic pressing at least once to prepare the solid-state battery. For example, the temperature of warm isostatic pressing is 50-120°C, the pressure is 5-650MPa, and the holding time is 1-720min.

[0069] The numerical range described in the present invention includes not only the point values ​​listed above, but also any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0070] Compared with the prior art, the present invention has the following beneficial effects:

[0071] The present invention provides a silicon alloy negative electrode active layer and a pre-lithium layer. The silicon alloy negative electrode active layer contains an alloy formed with silicon, which prevents the problem of pulverization and cracking of the negative electrode plate, further avoids short-circuit failure of the battery after lithium supplementation, and effectively improves the charge and discharge initial efficiency and cycle performance of the high-silicon content negative electrode all-solid-state battery. It has the advantages of high mass specific capacity and high volume specific capacity, low cost, non-toxicity and pollution-free, and low lithium insertion platform. BRIEF DESCRIPTION OF THE DRAWINGS

[0072] Figure 1 This is a schematic structural diagram of the negative electrode sheet provided in Example 1 of the present invention;

[0073] Figure 2 This is a flow chart of the process for preparing the negative electrode sheet provided in Example 1 of the present invention;

[0074] Figure 3 2 is a comparison chart of the cycle performance of Example 1 of the present invention and Comparative Example 1.

[0075] Among them, 1 is the negative electrode current collector; 2 is the first silicon alloy negative electrode active layer; 3 is the pre-lithium layer; 4 is the second silicon alloy negative electrode active layer. DETAILED DESCRIPTION

[0076] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, the present invention is further described in detail below. However, the following embodiments are merely simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0077] Example 1

[0078] This embodiment provides a negative electrode plate, such as Figure 1 As shown, the negative electrode current collector 1 of the negative electrode sheet is a carbon-coated copper foil, and a first silicon alloy negative electrode active layer 2, a pre-lithium layer 3, and a second silicon alloy negative electrode active layer 4 are sequentially stacked on one side of the carbon-coated copper foil. The pre-lithium layer 3 is a lithium strip, and the surface capacity of the first silicon alloy negative electrode active layer 2 is 1.1 mAh / cm 2 , the surface capacity of lithium strip is 0.5mAh / cm 2 The second silicon alloy negative electrode active layer 4 has a surface capacity of 5.5 mAh / cm 2 The first silicon alloy negative electrode active layer 2 and the second silicon alloy negative electrode active layer 4 have the same composition.

[0079] This embodiment further provides a solid-state battery using the above-mentioned negative electrode sheet, and a method for preparing the solid-state battery specifically includes:

[0080] like Figure 2 As shown, nano-silicon, Li6PS5Cl, Zn powder, CNT and SBR with a mass ratio of 70:10:16:1:3 were weighed, SBR was dissolved in trimethylbenzene, mixed with other components, and then coated on carbon-coated copper foil, dried at 100°C for 12h, and rolled on a roller press at 60°C and 10MPa / cm 2 The electrode surface is compacted under a force of , to obtain the first silicon alloy negative electrode active layer 2;

[0081] A lithium tape with a PET substrate is attached to the surface of the first silicon alloy negative electrode active layer 2, and is subjected to a warm isostatic pressing at 50°C and 300 MPa for 30 minutes. After removing the PET, a pre-lithium layer 3 is prepared;

[0082] The negative electrode slurry is coated on aluminum foil, dried at 100°C for 12 hours, and then laminated with the negative electrode sheet provided with the pre-lithium layer 3. Warm isostatic pressing is performed twice at 90°C and 400 MPa for 10 minutes. After removing the aluminum foil, a second silicon alloy negative electrode active layer 4 is obtained, thereby preparing the negative electrode sheet.

[0083] NCM811 coated with LiNbO3 (coating thickness of 5 nm), Li6PS5Cl, SP and PTFE were weighed in a mass ratio of 85:13:1.5:0.5, mixed and ground, dry-rolled at 180°C, and then composited onto the surface of carbon-coated aluminum foil to prepare the positive electrode. The NP ratio of the positive electrode to the negative electrode was 1.15.

[0084] The negative electrode sheet and the electrolyte layer were laminated and subjected to warm isostatic pressing three times at 85°C and 500 MPa with a holding time of 20 min to obtain a negative electrode sheet of the composite electrolyte layer (die punched sheet 4.2*6.2 cm), the positive electrode was laminated (die punched sheet 4*6 cm) and the tabs were welded and packaged, and warm isostatic pressing was performed once at 90°C and 400 MPa with a holding time of 15 min to prepare the battery.

[0085] The electrolyte layer was prepared by weighing NBR and Li6PS5Cl in a 95:5 mass ratio, mixing trimethylbenzene and NBR to form a paste, then ball-milling the mixture with Li6PS5Cl to obtain a slurry with a solid content of 70%, coating it on PET, and drying it at 100°C to obtain an electrolyte layer with a thickness of 25 μm.

[0086] Example 2

[0087] This embodiment provides a negative electrode plate, which includes a carbon-coated copper foil. A first silicon alloy negative electrode active layer 2, a lithium strip, and a second silicon alloy negative electrode active layer 4 are sequentially stacked on one side of the carbon-coated copper foil. The surface capacity of the first silicon alloy negative electrode active layer 2 is 2.1 mAh / cm 2 , the surface capacity of lithium strip is 2mAh / cm 2 The second silicon alloy negative electrode active layer 4 has a surface capacity of 5.5 mAh / cm 2 The first silicon alloy negative electrode active layer 2 and the second silicon alloy negative electrode active layer 4 have the same composition.

[0088] This embodiment further provides a solid-state battery using the above-mentioned negative electrode sheet, and a method for preparing the solid-state battery specifically includes:

[0089] Silica powder, thio-LISICON, nano Cu powder, SP and HNBR were weighed in a mass ratio of 69.4:0:30:0.1:0.5. HNBR was dissolved in xylene, mixed with other components, and then coated on carbon-coated copper foil. The mixture was dried at 100°C for 12 h and rolled on a roller press at 60°C and 10 MPa / cm 2 The electrode surface is compacted under a force of , to obtain the first silicon alloy negative electrode active layer 2;

[0090] A lithium tape with a PET substrate is attached to the surface of the first silicon alloy negative electrode active layer 2, and is subjected to a warm isostatic pressing at 80°C and 650 MPa for 200 minutes. After removing the PET, a pre-lithium layer 3 is prepared;

[0091] The negative electrode slurry is coated on aluminum foil, dried at 100°C for 12 hours, and then laminated with the negative electrode sheet provided with the pre-lithium layer 3. Warm isostatic pressing is performed twice at 70°C and 300 MPa for 80 minutes. After removing the aluminum foil, a second silicon alloy negative electrode active layer 4 is obtained, thereby preparing the negative electrode sheet.

[0092] NCM811 coated with Li2TiO3 (coating thickness of 1 nm), thio-LISICON, SP, and PTFE were weighed in a mass ratio of 40:50:5:5, mixed and ground, dry-rolled at 180°C, and then composited onto the surface of a carbon-coated aluminum foil to prepare the positive electrode. The NP ratio of the positive electrode to the negative electrode was 1.08.

[0093] The negative electrode sheet and the electrolyte layer were laminated and subjected to warm isostatic pressing three times at 75°C and 400 MPa with a holding time of 40 min to obtain a negative electrode sheet of the composite electrolyte layer (die punched sheet 4.2*6.2 cm), the positive electrode was laminated (die punched sheet 4*6 cm) and the tabs were welded and packaged, and warm isostatic pressing was performed twice at 80°C and 500 MPa with a holding time of 20 min to prepare the battery.

[0094] The preparation process of the electrolyte layer is as follows: SEBS and thio-LISICON are weighed in a mass ratio of 99.5:0.5, trimethylbenzene and SEBS are mixed to make a glue, and then ball-milled with thio-LISICON to obtain a slurry with a solid content of 70%, which is coated on PET and dried at 100°C to obtain an electrolyte layer with a thickness of 15 μm.

[0095] Example 3

[0096] This embodiment provides a negative electrode plate, which includes a carbon-coated copper foil. A first silicon alloy negative electrode active layer 2, a lithium strip, and a second silicon alloy negative electrode active layer 4 are sequentially stacked on one side of the carbon-coated copper foil. The surface capacity of the first silicon alloy negative electrode active layer 2 is 4.1 mAh / cm 2 , the surface capacity of lithium strip is 4mAh / cm 2 The second silicon alloy negative electrode active layer 4 has a surface capacity of 5.5 mAh / cm 2 The first silicon alloy negative electrode active layer 2 and the second silicon alloy negative electrode active layer 4 have the same composition.

[0097] This embodiment further provides a solid-state battery using the above-mentioned negative electrode sheet, and a method for preparing the solid-state battery specifically includes:

[0098] Silicon carbide, Li2S-P2S5, nano-Ni powder, graphene and SBS were weighed in a mass ratio of 90:4:3:1.5:1.5. SBS was dissolved in n-decane, mixed with other components, and then coated on a carbon-coated copper foil. The mixture was dried at 100°C for 12 h and rolled on a roller press at 60°C and 10 MPa / cm 2 The electrode surface is compacted under a force of , to obtain the first silicon alloy negative electrode active layer 2;

[0099] A lithium tape with a PET substrate is attached to the surface of the first silicon alloy negative electrode active layer 2, and is subjected to a warm isostatic pressing at 120°C and 50 MPa for 600 minutes. After removing the PET, a pre-lithium layer 3 is prepared;

[0100] The negative electrode slurry is coated on aluminum foil, dried at 100°C for 12 hours, and then laminated with the negative electrode sheet provided with the pre-lithium layer 3. Warm isostatic pressing is performed three times at 100°C and 200 MPa, with a holding time of 60 minutes. After removing the aluminum foil, a second silicon alloy negative electrode active layer 4 is obtained, thereby preparing the negative electrode sheet.

[0101] NCM811 coated with Li3BO3 (coating thickness of 10 nm), Li2S-P2S5, SP and PTFE were weighed in a mass ratio of 91.4:8:0.5:0.1, mixed and ground, dry-rolled at 180°C, and then composited onto the surface of carbon-coated aluminum foil to prepare the positive electrode. The NP ratio of the positive electrode to the negative electrode was 1.8.

[0102] The negative electrode sheet and the electrolyte layer were laminated and subjected to warm isostatic pressing four times at 90°C and 450 MPa with a holding time of 60 min to obtain a negative electrode sheet of the composite electrolyte layer (die punched sheet 4.2*6.2 cm), the positive electrode was laminated (die punched sheet 4*6 cm) and the tabs were welded and packaged, and warm isostatic pressing was performed twice at 120°C and 360 MPa with a holding time of 40 min to prepare the battery.

[0103] The preparation process of the electrolyte layer is as follows: PVDF-LBG and Li2S-P2S5 with a mass ratio of 90:10 are weighed, trimethylbenzene and PVDF-LBG are mixed to make a glue, and then ball-milled with Li2S-P2S5 to obtain a slurry with a solid content of 70%, which is coated on PET and dried at 100°C to obtain an electrolyte layer with a thickness of 50μm.

[0104] Example 4

[0105] This embodiment provides a negative electrode plate and a solid-state battery. Compared with Example 1, the difference is that in the negative electrode plate, the mass ratio of nano-silicon, Li6PS5Cl, Zn powder, CNT and SBR is 75:5:16:1:3, and the remaining steps and operations are exactly the same as in Example 1.

[0106] Example 5

[0107] This embodiment provides a negative electrode plate and a solid-state battery. Compared with Example 1, the difference is that in the negative electrode plate, the mass ratio of nano-silicon, Li6PS5Cl, Sn powder, CNT and SBR is 90:5:3:0.5:1.5, and the remaining steps and operations are exactly the same as in Example 1.

[0108] Example 6

[0109] This embodiment provides a negative electrode sheet and a solid-state battery. Compared with Example 1, the difference is that the surface capacity of the first silicon alloy negative electrode active layer 2, the surface capacity of the pre-lithium layer 3, and the surface capacity of the second silicon alloy negative electrode active layer 4 are all equal, which are 0.5 mAh / cm 2 The remaining steps and operations are exactly the same as those in Example 1.

[0110] Example 7

[0111] This embodiment provides a negative electrode plate and a solid-state battery. Compared with embodiment 1, the difference is that the surface capacity of the pre-lithium layer 3 is 4.5 mAh / cm 2 The remaining steps and operations are exactly the same as those in Example 1.

[0112] Example 8

[0113] This embodiment provides a negative electrode plate and a solid-state battery. Compared with embodiment 1, the difference is that the surface capacity of the pre-lithium layer 3 is 0.2 mAh / cm 2 The remaining steps and operations are exactly the same as those in Example 1.

[0114] Example 9

[0115] This embodiment provides a negative electrode plate and a solid-state battery. Compared with Example 1, the difference is that in the negative electrode plate, the ratio of other components remains unchanged, and only the amount of Zn powder added is increased, so that the mass ratio of nano-silicon, Li6PS5Cl, nano-Zn powder, CNT and SBR is 54.2:7.7:35:0.8:2.3. The remaining steps and operations are exactly the same as in Example 1.

[0116] Example 10

[0117] This embodiment provides a negative electrode plate and a solid-state battery. Compared with Example 1, the difference is that in the negative electrode plate, the ratio of other components remains unchanged, and only the amount of Zn powder added is reduced, so that the mass ratio of nano-silicon, Li6PS5Cl, nano-Zn powder, CNT and SBR is 82.5:11.8:1:1.2:3.5. The remaining steps and operations are exactly the same as in Example 1.

[0118] Comparative Example 1

[0119] This comparative example provides a negative electrode plate. Compared with Example 1, the difference is that the pre-lithium layer 3 is not provided, and the remaining steps and operations are exactly the same as those in Example 1.

[0120] This comparative example also provides a solid-state battery, which differs from Example 1 in that the negative electrode adopts the above-mentioned negative electrode plate.

[0121] The performance of the batteries prepared in the above examples and comparative examples was tested under the following conditions: 2 , at 25 ° C, 0.1C first efficiency test was carried out, and the capacity retention rate of 100 charge and discharge cycles was carried out at 0.33C. The test results are shown in Table 1. The cycle performance comparison diagram of Example 1 and Comparative Example 1 is shown in Figure 3 shown.

[0122] Table 1

[0123]

[0124]

[0125] As can be seen from the table above:

[0126] (1) Compared with Examples 6-8, it can be seen that in the present invention, the surface capacity of the first silicon alloy negative electrode active layer is greater than the surface capacity of the pre-lithiation layer, and less than the surface capacity of the second silicon alloy negative electrode active layer, thereby ensuring that the first silicon alloy layer will not be completely pre-lithiated (embrittled) and fall off from the current collector after pre-lithiation. The second silicon alloy layer serves as the main active layer. It not only undertakes the main task of lithium insertion and removal during the battery charging and discharging process, but also exists as a protective layer for the pre-lithiation layer. This ensures the capacity of the negative electrode and avoids the reduction of the battery energy density. If the above-mentioned surface capacity requirements are not met, there is a problem that the battery charging and discharging process may cause short circuit and reduced energy density. Furthermore, the present invention controls the surface capacity of the pre-lithiation layer to be 0.5-4mAh / cm 2 , can reasonably supplement the lithium source, improve the battery charge and discharge efficiency and cycle performance, if the surface capacity is lower than 0.5mAh / cm 2 , the pre-lithium amount is not enough, resulting in no obvious improvement in the first efficiency and cycle performance. If the pre-lithium surface capacity is higher than 4mAh / cm 2, resulting in an increase in the corresponding negative electrode thickness, which in turn increases the length of the lithium ion channel, thereby increasing the polarization of the battery charge and discharge process, and an excessively high pre-lithium amount will increase the risk of battery short circuit.

[0127] (2) Compared with Examples 9-10, it can be seen that the present invention controls the mass ratio of the negative electrode active material, the negative electrode electrolyte, the metal powder, the conductive agent and the negative electrode binder to be (69.4-90):(0-10):(3-30):(0.5-5):(0.5-5), and generates a silicon alloy by reacting the metal powder and the silicon-based active material. The silicon alloy has the advantages of little effect on the first effect and stable cycle performance. If the amount of metal powder added is too low, there is a problem of lack of alloy network structure, which easily leads to battery short circuit. If the amount of metal powder added is too high, there is a problem of reduced first effect.

[0128] (3) Compared with Comparative Example 1, it can be seen that the present invention provides a silicon alloy negative electrode active layer and a pre-lithium layer 3. The silicon alloy negative electrode active layer contains an alloy formed with silicon, which prevents the problem of pulverization and cracking of the negative electrode plate, further avoids battery short circuit failure after lithium supplementation, improves the battery charge and discharge initial efficiency and cycle stability, has high mass specific capacity and high volume specific capacity, low cost, non-toxic and pollution-free, and a low lithium insertion platform. The initial efficiency reaches more than 85%, and the capacity retention rate reaches more than 93.2%.

[0129] The applicant declares that the above is only a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention fall within the scope of protection and disclosure of the present invention.

Claims

1. A negative electrode plate, characterized in that: The negative electrode sheet comprises a negative electrode current collector, and a first silicon alloy negative electrode active layer, a pre-lithium layer, and a second silicon alloy negative electrode active layer are sequentially stacked on the surface of the current collector; The surface capacity of the first silicon alloy negative electrode active layer is greater than the surface capacity of the pre-lithium layer, and less than the surface capacity of the second silicon alloy negative electrode active layer; the first silicon alloy negative electrode active layer includes a negative electrode active material, a negative electrode electrolyte, a metal powder, a conductive agent and a negative electrode binder; the first silicon alloy negative electrode active layer and the second silicon alloy negative electrode active layer have the same composition; the mass ratio of the negative electrode active material, the negative electrode electrolyte, the metal powder, the conductive agent and the negative electrode binder is (69.4~90):(0~10):(3~30):(0.1~5):(0.5~5); the negative electrode active material includes one or a combination of at least two of silicon, silicon oxide, silicon carbide or silicon nitride.

2. The negative electrode sheet according to claim 1, characterized in that: The surface capacity of the first silicon alloy negative electrode active layer is 0.6 to 4.1 mAh / cm 2 .

3. The negative electrode sheet according to claim 1, characterized in that: The surface capacity of the pre-lithium layer is 0.5 to 4 mAh / cm 2 .

4. The negative electrode sheet according to claim 1, characterized in that: The surface capacity of the second silicon alloy negative electrode active layer is 4.2 to 10 mAh / cm 2 .

5. The negative electrode sheet according to claim 1, characterized in that: The pre-lithium layer includes a metal lithium strip.

6. The negative electrode sheet according to claim 1, characterized in that: The negative electrode current collector includes carbon-coated copper foil.

7. The negative electrode sheet according to claim 1, characterized in that: The negative electrode electrolyte includes a sulfide electrolyte.

8. The negative electrode sheet according to claim 7, characterized in that: The sulfide electrolyte includes thio-LISICON, Li 10 GeP2S 12 、Li6PS5Cl、Li 10 SnP2S 12 , Li2S-P2S5, Li2S-SiS2, Li2S-B2S3 or a combination of at least two of them.

9. The negative electrode sheet according to claim 1, characterized in that: The metal powder includes one or a combination of at least two of Fe, Co, Sb, Bi, Pb, Ni, Cu, Zn, Ge, In, Sn or Ti.

10. The negative electrode sheet according to claim 1, characterized in that: The conductive agent includes one of a zero-dimensional conductive agent, a one-dimensional conductive agent, or a two-dimensional conductive agent, or a combination of at least two of them.

11. The negative electrode sheet according to claim 1, characterized in that: The negative electrode binder includes one or a combination of at least two of PAA, Li-PAA, SBR, NBR, HNBR, SBR, SBS, SEBS or PEO.

12. A solid-state battery, characterized in that: The solid-state battery comprises a positive electrode, an electrolyte layer and a negative electrode, and the negative electrode adopts the negative electrode sheet described in any one of claims 1-11.

13. The solid-state battery according to claim 12, characterized in that: The NP ratio of the negative electrode to the positive electrode is 1.05 to 2; The NP ratio is the capacity surplus of the negative electrode superpositive electrode at the same stage and under the same conditions, and the calculation formula is: negative electrode active material gram capacity * negative electrode surface density * negative electrode active material content ratio / (positive electrode active material gram capacity * positive electrode surface density * positive electrode active material content ratio).

14. The solid-state battery according to claim 12, characterized in that: The positive electrode of the solid-state battery includes a positive electrode current collector and a positive electrode active layer arranged on at least one side surface of the positive electrode current collector.

15. The solid-state battery according to claim 14, characterized in that: The positive electrode active layer includes a positive electrode active material, a positive electrode electrolyte, a conductive agent and a positive electrode binder.

16. The solid-state battery according to claim 15, characterized in that: The mass ratio of the positive electrode active material, the positive electrode electrolyte, the conductive agent and the positive electrode binder is (40-91.4): (8-50): (0.5-8): (0.1-8).

17. The solid-state battery according to claim 14, characterized in that: The positive electrode current collector includes carbon-coated aluminum foil.

18. The solid-state battery according to claim 15, characterized in that: The positive electrode active material includes LiNi having an ion conductor coating layer x Co y M z O2, x≥0, y≥0, z≥0, x+y+z=1, and M includes one or a combination of at least two of Mn, Al, Zr, Ti, V, Mg, Fe or Mo.

19. The solid-state battery according to claim 15, characterized in that: The positive electrode electrolyte includes a sulfide electrolyte.

20. The solid-state battery according to claim 18, characterized in that The material of the ion conductor coating layer includes one or a combination of at least two of Li2TiO3, LiNbO3, Li3BO3, Li2ZrO3, LiCoO3, LiPO3, Li2MnO4, Al(PO3)3, La(PO3)3 or NaPO3.

21. The solid-state battery according to claim 18, characterized in that: The thickness of the ion conductor coating layer is 1 to 10 nm.

22. The solid-state battery according to claim 12, characterized in that: The thickness of the electrolyte layer is 15 to 50 μm.

23. The solid-state battery according to claim 12, characterized in that: The electrolyte layer includes a sulfide electrolyte and an electrolyte binder.

24. The solid-state battery according to claim 12, characterized in that: In the electrolyte layer, the mass ratio of the sulfide electrolyte to the electrolyte binder is (90-99.5):(0.5-10).

25. The solid-state battery according to claim 23, characterized in that: The electrolyte binder includes one or a combination of at least two of PVDF5130, PVDF75130, PVDF21216, PVD, F6020, PVDF-HVS900, PVDF-HFP, PVDF-LBG, NBR, HNBR, SBR, SBS or SEBS.

26. A method for preparing a solid-state battery according to any one of claims 12 to 25, characterized in that: The method for preparing the solid-state battery comprises: A first silicon alloy negative electrode active layer is arranged on one side surface of the negative electrode current collector, and pre-lithiation is carried out on the surface of the first silicon alloy negative electrode active layer to obtain a pre-lithiation layer, and then a second silicon alloy negative electrode active layer is arranged on the other side surface of the negative electrode current collector to prepare the negative electrode pole piece, and the negative electrode pole piece, the positive electrode and the electrolyte layer are packaged and pressed to prepare the solid-state battery.

27. The method for preparing a solid-state battery according to claim 26, characterized in that: The first silicon alloy negative electrode active layer is obtained by coating a negative electrode active slurry.

28. The method for preparing a solid-state battery according to claim 26, characterized in that: The step of setting the first silicon alloy negative electrode active layer includes: coating the negative electrode active slurry on the negative electrode current collector, drying it and then rolling it to obtain the first silicon alloy negative electrode active layer.

29. The method for preparing a solid-state battery according to claim 28, characterized in that: The solvent in the negative electrode active slurry includes one or a combination of at least two of water, dichloromethane, tetrahydrofuran, n-hexane, n-heptane, toluene, 2,4-dimethyl-3-pentanone, monochlorobenzene, xylene, anisole, cyclohexanone, 1,3,5-trimethylbenzene, n-decane and methylformamide.

30. The method for preparing a solid-state battery according to claim 29, characterized in that: The solvent in the negative electrode active slurry is water.

31. The method for preparing a solid-state battery according to claim 26, characterized in that: The pre-lithiation method includes pressing lithium strips.

32. The method for preparing a solid-state battery according to claim 31, characterized in that: The step of pressing the lithium strip includes: performing at least one warm isostatic pressing to press the lithium strip whose substrate is PET onto the surface of the first silicon alloy negative electrode active layer, and obtaining a pre-lithium layer after removing the PET.

33. The method for preparing a solid-state battery according to claim 26, characterized in that: The second silicon alloy negative electrode active layer is obtained by pressing.

34. The method for preparing a solid-state battery according to claim 33, characterized in that: The pressing step of the second silicon alloy negative electrode active layer includes: coating the negative electrode slurry on aluminum foil, drying it, performing at least one warm isostatic pressing with the pre-lithium negative electrode sheet, and removing the aluminum foil to obtain the second silicon alloy negative electrode active layer.

35. The method for preparing a solid-state battery according to claim 26, characterized in that: The preparation steps of the positive electrode include: mixing a positive electrode active material, a positive electrode electrolyte, a conductive agent and a positive electrode binder, dry rolling them, and then compounding them on the surface of a positive electrode current collector to prepare the positive electrode.

36. The method for preparing a solid-state battery according to claim 26, characterized in that: The packaging and pressing method comprises: laminating the negative electrode sheet with the electrolyte layer, performing warm isostatic pressing at least once to obtain the negative electrode sheet of the composite electrolyte layer, laminating the positive electrode, welding the tabs, and then packaging, performing warm isostatic pressing at least once to prepare the battery.

37. The method for preparing a solid-state battery according to claim 36, characterized in that: The temperature of the warm isostatic pressing is 50-120°C.

38. The method for preparing a solid-state battery according to claim 36, characterized in that: The pressure of the warm isostatic pressing is 5-650 MPa.

39. The method for preparing a solid-state battery according to claim 36, characterized in that: The holding time of the warm isostatic pressing is 1 to 720 minutes.

40. The method for preparing a solid-state battery according to claim 36, characterized in that: The warm isostatic pressing is performed 1 to 5 times.

41. The method for preparing a solid-state battery according to claim 26, characterized in that: The preparation method specifically comprises the following steps: The negative electrode active slurry is coated on the negative electrode current collector, and after drying, the slurry is rolled to obtain the first silicon alloy negative electrode active layer; Placing a lithium strip with a PET substrate on the surface of the first silicon alloy negative electrode active layer, performing at least one warm isostatic pressing at 50-120° C. and 5-650 MPa for a holding time of 1-720 min, and removing the PET to prepare a pre-lithium layer; The negative electrode slurry is coated on an aluminum foil, and after drying, it is laminated with a negative electrode sheet provided with a pre-lithium layer, and warm isostatic pressing is performed at least once at 50-120° C. and 5-650 MPa for a holding time of 1-720 min. After removing the aluminum foil, a second silicon alloy negative electrode active layer is obtained, thereby preparing the negative electrode sheet; The positive electrode active material, the positive electrode electrolyte, the conductive agent and the positive electrode binder are mixed, dry-rolled, and then compounded on the surface of the positive electrode current collector to prepare the positive electrode; The negative electrode plate is laminated with the electrolyte layer, and warm isostatic pressing is performed at least once at 50-120° C. and 5-650 MPa for a holding time of 1-720 min to obtain a negative electrode plate with a composite electrolyte layer. The positive electrode is laminated and packaged after welding the tabs, and warm isostatic pressing is performed at least once at 50-120° C. and 5-650 MPa for a holding time of 1-720 min to prepare the battery.