Photovoltaic conversion layer, solar cell, multi-junction solar cell, solar cell module and photovoltaic power generation system
By using elements such as Ge, Ta, and In as p-type dopants in the cuprous oxide-based photoelectric conversion layer and controlling the doping concentration within a specific range, the problems of difficult bandgap improvement and carrier recombination in multi-junction solar cells were solved, achieving high-efficiency photoelectric conversion and power generation.
Patent Information
- Application Number
- CN202080037618.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-07-26
- Filing Date
- 2020-03-10
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-03-10
AI Technical Summary
In existing multijunction solar cells, it is difficult to improve efficiency without reducing the band gap of the cuprous oxide-based photoelectric conversion layer, and the use of dopants can easily lead to band gap changes and carrier recombination problems.
Using elements such as Ge, Ta, and In as p-type dopants, the doping concentration of the photoelectric conversion layer is controlled within the range of 1×10¹⁵ atoms/cm³ to 1×10²⁰ atoms/cm³, ensuring that the band gap is between 2.10 eV and 2.30 eV, and a transparent Cu₂O thin film is formed by sputtering.
It improves the hole concentration and transparency of the photoelectric conversion layer, reduces carrier recombination, and achieves a high-efficiency photoelectric conversion effect, making it suitable for multi-junction solar cells and photovoltaic power generation systems.
Smart Images

Figure CN114041209B_ABST
Abstract
Description
Technical Field
[0001] The embodiments described herein generally relate to a photoelectric conversion layer, a solar cell, a multi-junction solar cell, a solar cell module, and a photovoltaic power generation system. Background Art
[0002] As a high-efficiency solar cell, a multi-junction (tandem) solar cell is known. Since a tandem solar cell can use a cell with high spectral sensitivity in each wavelength range, its efficiency is higher than that of a single-junction solar cell. As the top cell of a tandem solar cell, it is expected to use a cuprous oxide compound or the like, which has a low material cost but a wide band gap.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: JP2018-46196A Summary of the invention
[0006] Problems to be solved by the invention
[0007] Embodiments provide a solar cell, a multi-junction solar cell, a solar cell module, and a photovoltaic power generation system having improved characteristics.
[0008] Means for solving problems
[0009] The photoelectric conversion layer of the embodiment is based on Cu 2 O and contains at least one p-type dopant selected from Ge, Ta and In, and has a band gap of 2.10 eV to 2.30 eV. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 This is a conceptual cross-sectional view of a photoelectric conversion layer in an embodiment.
[0011] Figure 2 This is a conceptual perspective view of a photoelectric conversion layer in an embodiment.
[0012] Figure 3 This is a conceptual diagram of a solar cell in an embodiment.
[0013] Figure 4 is a conceptual cross-sectional view of a multi-junction solar cell in an embodiment.
[0014] Figure 5 This is a conceptual diagram of a solar cell module in an embodiment.
[0015] Figure 6 This is a conceptual cross-sectional view of a solar cell module in an embodiment.
[0016] Figure 7is a conceptual diagram of a photovoltaic power generation system in an embodiment.
[0017] Figure 8 This is a conceptual diagram of a vehicle in the embodiment. DETAILED DESCRIPTION
[0018] (First Embodiment)
[0019] The first embodiment relates to a photoelectric conversion layer 10 . Figure 1 1 is a conceptual diagram of the photoelectric conversion layer 10 in the first embodiment. The photoelectric conversion layer 10 is, for example, a semiconductor layer provided on a substrate, on which a transparent electrode is formed. The photoelectric conversion layer 10 is a p-type semiconductor layer and is mainly composed of cuprous oxide (Cu2O) (more than 90 wt% of the photoelectric conversion layer 10 is composed of Cu2O).
[0020] The photoelectric conversion layer 10 contains a p-type dopant. Previously, Si and N were considered to be p-type dopants in the Cu2O layer, and the inventors have newly discovered an element that can serve as a p-type dopant in the Cu2O layer through research. As the p-type dopant of the photoelectric conversion layer 10 in the embodiment, it is preferably at least one element selected from Ge, Ta and In. The p-type dopant increases the hole concentration of the photoelectric conversion layer 10, and by adding a small amount of p-type dopant, the characteristics of the photoelectric conversion layer as a solar cell are further improved. As the p-type dopant contained in the photoelectric conversion layer 10 described in the embodiment, Ge and / or Ta are preferred, and Ge is more preferred.
[0021] The band gap of the undoped Cu2O layer is above 2.10eV and below 2.30eV, which depends on the quality of the crystal. Since the band gap of Cu2O is much higher than that of Si, Cu2O can transmit almost all wavelengths of the Si absorption band. Therefore, even if a solar cell using a Cu2O layer (photoelectric conversion layer based on a Cu2O layer) and a solar cell using Si are stacked, the performance required by the solar cell using Si can be fully utilized. Therefore, we hope to improve the Cu2O-based photoelectric conversion layer 10 to achieve more efficient power generation without reducing the Cu2O band gap.
[0022] The photoelectric conversion layer 10 of the embodiment contains a very small amount of p-type dopant. Although a very small amount of dopant increases the hole concentration to make the Cu2O layer more p-type, specifically, from p-type to p-type, the band gap of the Cu2O layer does not change substantially because the doping amount is small. When the amount of p-type dopant added reaches the extent that causes the band gap to change, the photoelectric conversion layer 10 is in a state of excessive holes, and the carrier electrons generated by the photoelectric conversion are easily recombined with the holes. Therefore, from the perspective of obtaining an efficient solar cell, the doping amount of the p-type dopant in the Cu2O layer cannot reach the extent that causes the band gap to change. In addition, due to the narrowing of the band gap, from the perspective of combining with a solar cell using Si, it is not preferred to add a dopant including a p-type dopant to the extent that the band gap can be less than 2.10 eV. In the technology that cannot prepare a transparent Cu2O layer, when there is no viewpoint of preparing a multi-junction type (due to the non-transmissive type, the multi-junction type cannot be prepared), a large amount of dopants other than p-type dopants are sometimes doped in Cu2O to change the band gap, which is done for purposes unrelated to the present invention. However, in a multi-junction solar cell in which a solar cell using the transparent photoelectric conversion layer 10 is combined with a solar cell having a narrow band gap, doping to narrow the band gap of the Cu2O layer has no advantage.
[0023] The concentration of the p-type dopant in the photoelectric conversion layer 10 is preferably 1×10 15 atoms / cm 3 Above and 1×10 20 atoms / cm 3 That is, the lowest value of the concentration of the p-type dopant in the photoelectric conversion layer 10 is preferably equal to or greater than 1×10 15 atoms / cm 3 , whose maximum value is equal to or less than 1×10 20 atoms / cm 3 The photoelectric conversion layer 10 having the p-type dopant concentration may contain about 1×10 14 atoms / cm 3 or less of n-type dopant. When the photoelectric conversion layer 10 contains an n-type dopant, the concentration of the p-type dopant is treated as a value obtained by subtracting the concentration of the n-type dopant from the actual concentration of the p-type dopant. Since it will cause the characteristics of the photoelectric conversion layer 10 to be different, it is not preferred that the p-type dopant is present only in a part of the photoelectric conversion layer 10, or that the photoelectric conversion layer contains a part that does not satisfy the above range. It is not preferred that the p-type dopant concentration is too low because the p-type dopant does not substantially provide an effect. Therefore, it is preferred that the p-type dopant is prevalent in the entire photoelectric conversion layer 10, and the p-type dopant concentration in the photoelectric conversion layer 10 as a whole is 1×10 15 atoms / cm3 Above and 1×10 20 atoms / cm 3 the following.
[0024] Moreover, if the concentration of the p-type dopant is too high, the photoelectric conversion layer 10 becomes p+ type and the band gap tends to be narrowed, so the concentration of the p-type dopant is preferably within the above preferred range. The more preferred range of the concentration of the p-type dopant in the photoelectric conversion layer 10 is 1×10 15 atoms / cm 3 Above and 1×10 18 atoms / cm 3 the following.
[0025] Preferably, a low concentration of p-type dopant is included in the entire photoelectric conversion layer 10 so as to make it more transparent than an undoped Cu 2 O layer.
[0026] High concentration doping is not preferred because it is not advisable to add a metal other than Cu containing a p-type dopant at a high concentration (e.g., equal to or greater than 1×10 22 atoms / cm 3 ) doped into the Cu2O layer will cause the Cu2O layer to no longer be the Cu2O layer.
[0027] The concentration of the p-type dopant in the photoelectric conversion layer 10 is 1×10 15 atoms / cm 3 Above and 1×10 20 atoms / cm 3 This fact is determined by the following method. Figure 2 As shown in the three-dimensional conceptual diagram of the photoelectric conversion layer 10 in FIG. 1 , for nine analysis points A1 to A9, it is necessary to determine the composition of the photoelectric conversion layer 10 to measure the concentration of the p-type dopant. The following nine analysis points were analyzed at three depths: a depth of 100 nm from the front side of the photoelectric conversion layer 10; a depth of half (D / 2) of the thickness (D) of the photoelectric conversion layer 10; and a depth of 100 nm from the back side of the photoelectric conversion layer 10. Each analysis point is about 5 mm in size. 2 square or circle, and the center of each analysis step is analyzed. When the concentration of p-type dopant obtained in the points is 1×10 15 atoms / cm 3 Above and 1×10 20 atoms / cm 3 When the concentration of the p-type dopant in the photoelectric conversion layer 10 is 1×10 15 atoms / cm 3 Above and 1×10 20 atoms / cm 3Below (the minimum value of the concentration of the p-type dopant in the photoelectric conversion layer 10 is equal to or greater than 1×10 15 atoms / cm 3 , and the maximum value of the concentration of the p-type dopant in the photoelectric conversion layer 10 is equal to or less than 1×10 20 atoms / cm 3 ). As the analysis method, secondary ion mass spectrometry (SIMS) and the like can be cited.
[0028] The nine analysis points are defined as follows. Assume that the width and length of the plane (main surface) seen from the front or back of the photoelectric conversion layer 10 are W1 and W2 (W1≤W2), respectively. Draw a virtual line at a distance of W3 (=W1 / 10) inward on both sides of the width direction facing the photoelectric conversion layer 10, draw a virtual line at a distance of W4 (=D2 / 10) inward on both sides of the length direction facing the solar cell 100, and draw a virtual line parallel to the width direction through the center of the solar cell 100 (a virtual line at a distance of W5 (=W1 / 2) inward from the side in the width direction facing the photoelectric conversion layer 10), draw a virtual line parallel to the length direction through the center of the photoelectric conversion layer 10 (a virtual line at a distance of W6 (=W2 / 2) inward from the side in the length direction facing the photoelectric conversion layer 10), and the area centered on the nine intersections of the virtual lines is defined as analysis points A1-A9. When the photoelectric conversion layer 10 is not rectangular, as in Figure 2 As shown, the analysis position is defined based on a rectangle inscribed in the photoelectric conversion layer 10 .
[0029] Preferably, the average value of the concentration of the p-type dopant at three depths of the nine analysis points (the average value of the concentration of all p-type dopants) is 1×10 15 atoms / cm 3 Above and 1×10 19 atoms / cm 3 In the following, the three depths are: a depth of 100 nm from the front side of the photoelectric conversion layer 10, a depth of half (D / 2) of the thickness (D) of the photoelectric conversion layer 10, and a depth of 100 nm from the back side of the photoelectric conversion layer 10. When the average value is less than 1×10 15 atoms / cm 3 When the average value is greater than 1×10 19 atoms / cm 3 Therefore, it is more preferred that the average value of the entire p-type dopant concentration is 1×10 15 atoms / cm 3 Above and 1×10 19atoms / cm 3 the following.
[0030] The maximum value of the concentration of the p-type dopant in the photoelectric conversion layer 10 (the maximum value of the p-type dopant concentration obtained by analyzing the analysis point) is preferably more than 1 times and less than 10,000 times the minimum value of the concentration of the p-type dopant in the photoelectric conversion layer 10 (the minimum value of the p-type dopant concentration obtained by analyzing the analysis point), and more preferably more than 1 times and less than 100 times. Therefore, a slight deviation in the p-type dopant concentration reduces the unevenness of the energy potential, which is caused by the concentration deviation of the dopant concentration in the conduction band and valence band of the photoelectric conversion layer 10 in the film thickness direction, thereby the electrons of the photocarrier diffuse to the n-type layer 2 without staying in the unevenness of the energy potential, and the holes between the photocarriers diffuse to the first electrode 1 without staying in the unevenness of the energy potential. Therefore, the advantage of a small amount of carrier recombination is revealed.
[0031] At the same time, the average value of the p-type dopant concentration at a depth of 100 nm from the front side of the photoelectric conversion layer 10 (the average value of the front side p-type dopant concentration: α (alfa)) is preferably 1 or more and 100 or less (β≤α≤1000β) of the average value of the p-type dopant concentration at a depth of half the thickness of the photoelectric conversion layer 10 (the average value of the central p-type dopant concentration: β (beta)), and the average value of the p-type dopant concentration at a depth of 100 nm from the back side of the photoelectric conversion layer 10 (the average value of the back side p-type dopant concentration: γ (gamma)) is preferably 10 or more and 1000 or less (10β≤γ≤1000β) of the average value of the p-type dopant concentration at a depth of half the thickness of the photoelectric conversion layer 10 (the average value of the central p-type dopant concentration: β (beta)). The average value of the back side p-type dopant concentration is preferably 10 or more and 1000 or less than the average value of the front side p-type dopant concentration. The slight deviation of the p-type dopant concentration in the thickness direction of the photoelectric conversion layer 10 reduces the unevenness of the energy potential caused by the concentration deviation of the dopant concentration in the conduction band and the valence band of the photoelectric conversion layer 10, whereby the electrons of the photocarriers diffuse to the n-type layer 2 without staying in the unevenness of the energy potential, and the holes between the photocarriers diffuse to the first electrode 1 without staying in the unevenness of the energy potential. Therefore, the advantage of a small amount of carrier recombination is revealed.
[0032] Therefore, the average value (α) of the p-type dopant concentration at a depth of 100 nm from the front side of the photoelectric conversion layer 10 is preferably 1 or more and 50 or less (β≤α≤50β) of the average value (β) of the p-type dopant concentration at a depth of half the thickness of the photoelectric conversion layer 10, and more preferably, the average value (γ) of the p-type dopant concentration at a depth of 100 nm from the back side of the photoelectric conversion layer 10 is 10 or more and 500 or less (10β≤γ≤500β) of the average value (β) of the p-type dopant concentration at a depth of half the thickness of the photoelectric conversion layer 10. Specifically, the average value (β) of the p-type dopant concentration at a depth of half the thickness of the photoelectric conversion layer 10 is preferably 1×10 15 atoms / cm 3 Above and 1×10 16 atoms / cm 3 the following.
[0033] The photoelectric conversion layer 10 has light-transmitting properties and has a transmittance of 90% or more for light having a wavelength of 700 nm to 1000 nm, which is the wavelength of the main absorption band of Si.
[0034] The thickness of the photoelectric conversion layer 10 is preferably 500 nm or more and 10 μm or less. The photoelectric conversion layer 10 may contain additives as long as the requirements of the band gap and the p-type doping concentration are satisfied.
[0035] More than 95% of the photoelectric conversion layer 10 is preferably composed of cuprous oxide. That is, the photoelectric conversion layer 10 contains almost (substantially) no heterogeneous phase such as CuO or Cu. The photoelectric conversion layer 10 preferably contains no heterogeneous phase such as CuO or Cu, and is substantially a thin film of a Cu2O single phase for achieving high light transmittance. The fact that the photoelectric conversion layer 10 is substantially a Cu2O single phase can be confirmed by measurement using a photoluminescence method (PL method).
[0036] The photoelectric conversion layer 10 is preferably prepared by sputtering. The atmosphere during the sputtering process is preferably a mixed gas atmosphere of an inert gas such as Ar and oxygen. Although it depends on the type of substrate supporting the solar cell 10 ( Figure 6 The substrate 20 is heated by using a target material containing Cu and a p-type dopant to achieve sputtering, so that the substrate temperature is above 100° C. and below 600° C. For example, by adjusting the temperature and oxygen partial pressure during sputtering, a transparent cuprous oxide film with a large particle size can be formed.
[0037] (Second Embodiment)
[0038] The second embodiment relates to a solar cell using the photoelectric conversion layer 10 of the first embodiment. Figure 32 is a conceptual diagram of a solar cell in the second embodiment. Figure 3 As shown, in this embodiment, the solar cell 100 includes a first electrode 1, a photoelectric conversion layer 10 on the first electrode 1, an n-type layer 2 on the photoelectric conversion layer 10, and a second electrode 3 on the n-type layer 2. An interlayer (not shown) may be included between the first electrode 1 and the photoelectric conversion layer 10, or between the n-type layer 2 and the second electrode 3. The light may enter from the first electrode 1 side or from the second electrode 3 side. The light enters the solar cell 100, thereby generating electricity.
[0039] (First Electrode)
[0040] In the embodiment, the first electrode 1 is a transparent conductive layer disposed on the photoelectric conversion layer 10 side. Figure 3 In the embodiment, the first electrode 1 is in direct contact with the photoelectric conversion layer 10. The first electrode 1 is preferably a transparent conductive film, and a stacked structure consisting of a transparent conductive film and a metal film. Examples of transparent conductive films include, but are not limited to, indium tin oxide (ITO), aluminum-doped zinc oxide (AZO), boron-doped zinc oxide (BZO), gallium-doped zinc oxide (GZO), fluorine-doped tin oxide (FTO), antimony-doped tin oxide (ATO), titanium-doped indium oxide (ITiO), indium zinc oxide (IZO), indium gallium zinc oxide (IGZO), tantalum-doped tin oxide (SnO2:Ta), niobium-doped tin oxide (SnO2:Nb), tungsten-doped tin oxide (SnO2:W), molybdenum-doped tin oxide (SnO2:Mo), fluorine-doped tin oxide (SnO2:F) and indium hydroxide-doped (IOH). The transparent conductive film may be a stacked film having a plurality of films, and the stacked film may also include a tin oxide film or the like in addition to the above-mentioned oxides. Examples of dopants in tin oxide films and the like include, but are not limited to, In, Si, Ge, Ti, Cu, Sb, Nb, F, Ta, W, Mo, Br, I and Cl. Examples of the metal film include, but are not limited to, films of Mo, Au, Cu, Ag, Al, Ta or W. The first electrode 1 may be an electrode having a dot-shaped, linear or mesh-shaped metal under a transparent conductive film. At this time, the dot-shaped, linear or mesh-shaped metal is arranged on the opposite side of the photoelectric conversion layer 10 of the transparent conductive layer. The dot-shaped, linear or mesh-shaped metal preferably has a porosity of 50% or more relative to the transparent conductive film. Examples of dot-shaped, linear or mesh-shaped metal include, but are not limited to, Mo, Au, Cu, Ag, Al, Ta and W. When a metal thin film is used as the first electrode 1, the film thickness is preferably approximately equal to or less than 5 nm from the perspective of transmittance.
[0041] (Photoelectric conversion layer)
[0042] The photoelectric conversion layer 10 in this embodiment is the photoelectric conversion layer in the first embodiment.
[0043] A cuprous oxide film may be formed on the first electrode 1. Examples of the substrate (substrate carrying the first electrode 1) for preparing the solar cell 100 include organic substrates such as acrylic, polyimide, polycarbonate, polyethylene terephthalate (PET), polypropylene (PP), fluororesins (polytetrafluoroethylene (PTFE), perfluoropropylene copolymer (FEP), ethylene tetrafluoroethylene copolymer (ETFE), polychlorotrifluoroethylene (PCTFE), perfluoroalkane (PFA), etc.), polyarylate, polysulfone, polyethersulfone, polyetherimide, and inorganic substrates such as soda-lime glass, white plate glass, chemically strengthened glass, and quartz.
[0044] (n-type layer)
[0045] The n-type layer 2 is a semiconductor layer disposed between the photoelectric conversion layer 10 and the second electrode 3. Preferably, the plane of the n-type layer 2 facing the photoelectric conversion layer 10 is in direct contact with the plane of the photoelectric conversion layer 10 facing the n-type layer 2. The n-type layer 2 is also called an n-type layer or a buffer layer. The n-type layer 2 is preferably an n-type semiconductor layer of an oxide or a sulfide. Preferably, the n-type layer 2 is an amorphous thin film. The oxide used in the n-type layer 2 is preferably, but not limited to: Zn x A y X z Ow (A represents at least one element selected from the group consisting of Si, Ge and Sn, M represents at least one element selected from the group consisting of B, Al, Ga, In and Ge, 0.90≤x+y≤1.00, 0.00≤z≤0.30, and 0.09≤w≤1.10), Cu (2-x) M x O (M=Mn, Mg, Ca, Zn, Sr, Ba, Al, Ga, In, Nb, lanthanide elements), Cu2O:F, Cu2O:N, Cu2O:B, Cu2O:Cl, Cu2O:Br, Cu2O:I, Al (2-x) Ga x The sulfide used in the n-type layer 2 is preferably but not limited to: Zn x In (2-2x) S (3-2x) , ZnS and In x Ga (1-x) At least one sulfide selected from the group consisting of S. The range of x is 0≤x≤1, and the range of y is 0≤y≤2.
[0046] When Si or Ge is contained in the n-type layer 2 and Si or Ge diffuses from the n-type layer 2 to the photoelectric conversion layer 10, the region on the n-type layer 2 side of the photoelectric conversion layer 10 (the region on the n-type layer 2 side of the photoelectric conversion layer 10) may contain a high concentration of Si or Ge. In one case, the average concentration of Si and / or Ge in the region on the n-type layer 2 side of the photoelectric conversion layer 10 (the average value of the p-type dopant concentration in the n-type layer side region) is the average concentration (atoms / cm2) of the p-type dopant in the photoelectric conversion layer 10. 3 ) is more than 1 times and less than 100 times. In the photoelectric conversion layer 10, the region on the n-type layer 2 side is a region with a depth of 10 nm from the interface between the photoelectric conversion layer 10 and the n-type layer 2 to the first electrode 1 side. Based on the same reasons as above, considering factors such as the band gap and the hole concentration, the p-type dopant concentration in the region on the n-type layer 2 side of the photoelectric conversion layer 10 is preferably 1×10 15 atoms / cm 3 Above and 1×10 20 atoms / cm 3 The boundary (interface) between the n-type layer 2 and the photoelectric conversion layer 10 is, for example, a position where the concentration of the main elements other than Cu, O, and the p-type dopant contained in the n-type layer 2 exceeds the Cu concentration measured by SIMS from the side of the n-type layer 2. The boundary (interface) between the n-type layer 2 and the photoelectric conversion layer 10 can also be determined by the interface of the layers and the composition using scanning electron microscopy-energy dispersive x-ray spectroscopy (SEM-EDX).
[0047] The film thickness of the n-type layer 2 is typically greater than 3nm and less than 100nm. If the thickness of the n-type layer 2 is equal to or less than 5nm, leakage current will be generated when the coverage of the n-type layer 2 is poor, which deteriorates its characteristics. When the coverage is good, the film thickness is not limited to the above range. If the thickness of the n-type layer 2 exceeds 100nm, the characteristics will deteriorate due to the excessive resistance of the n-type layer 2, or the short-circuit current will decrease due to the reduction in transmittance. Therefore, the thickness of the n-type layer 2 is more preferably greater than 5nm and less than 50nm, and further preferably greater than 5nm and less than 10nm. In order to achieve a thin film with good coverage, the n-type layer 2 has a surface roughness equal to or less than 5nm. When the quality of the n-type layer 2 is high, a solar cell 100 that can operate even when the film thickness is about 200nm can be configured.
[0048] The n-type layer 2 may be formed by atomic layer deposition (ALD), sputtering, or the like.
[0049] The conduction band offset (ΔE=Ecp-Ecn) refers to the difference between the position (Ecp (eV)) of the conduction band minimum (CBM) of the photoelectric conversion layer 10 and the position (Ecn (eV)) of the conduction band minimum of the n-type layer 2, which is preferably greater than -0.6eV and less than 0.2eV (-0.6eV≤ΔE≤+0.2eV). If the conduction band offset is greater than 0, the conduction band at the pn junction interface is discontinuous, resulting in a spike. If the conduction band offset is less than 0, the conduction band at the pn junction interface is also discontinuous, resulting in a cliff. Since the spike is an energy barrier for obtaining photogenerated electrons from the second electrode, and the cliff reduces the voltage of the driven photogenerated electrons, the smaller the absolute values of the spike and the cliff, the better. Therefore, the conduction band offset is more preferably greater than -0.4eV and less than 0.0eV (-0.4eV≤ΔE≤0.0eV). However, this does not apply to the case where conduction is performed by utilizing the energy level within the gap. The position of the CBM can be estimated using the following technique. The valence band top (VBM) is measured using photoelectron spectroscopy, which evaluates the energy level of electron occupation, and the CBM is calculated by assuming the band gap of the material being measured. However, since the actual pn junction interface cannot maintain an ideal interface, such as the mutual diffusion of cations or the generation of holes, the possibility of band gap changes is very large. Therefore, it is preferred to directly evaluate the CBM using inverse photoelectron spectroscopy, which directly utilizes the photoemission reversal process. Specifically, the electronic state of the pn junction interface can be evaluated by repeatedly measuring the surface of the solar cell with low-energy ion etching, photoelectron spectroscopy, and inverse photoelectron spectroscopy.
[0050] (Second Electrode)
[0051] The second electrode 3 of the embodiment is a transparent conductive layer arranged on the n-type layer 2. As the second electrode 3, it is preferred to use the same transparent electrode as the electrode used as the first electrode 1. The second electrode 3 can be an electrode provided with a dot-shaped, linear or mesh-shaped metal on a transparent conductive film. Relative to the transparent conductive film, the dot-shaped, linear or mesh-shaped metal preferably has a porosity of 50% or more. Examples of dot-shaped, linear or mesh-shaped metals include, but are not limited to, Mo, Au, Cu, Ag, Al, Ta and W. When a metal film is used as the second electrode 3, from the perspective of transmittance, the film thickness is preferably approximately equal to or less than 5 nm. As the second electrode 3, it is preferred to use the same transparent electrode as the electrode used as the first electrode 1. As the second electrode 3, other transparent electrodes such as multilayer graphene having a lead-out electrode containing a metal wire can also be used.
[0052] (Anti-reflective film)
[0053] The anti-reflection film of this embodiment is a film that facilitates the introduction of light into the photoelectric conversion layer 10, and is preferably formed on the side of the first electrode 1 or the second electrode 3 opposite to the photoelectric conversion layer 10. For example, MgF2 or SiO2, etc. can be used as the desired anti-reflection film. In this embodiment, the anti-reflection film can be omitted. Although it is necessary to adjust the film thickness according to the refractive index of each layer, it is preferred that the vapor deposition thickness is about 70nm to 130nm (preferably 80nm to 120nm).
[0054] (Third Embodiment)
[0055] A third embodiment relates to a multi-junction solar cell. Figure 4 is a conceptual cross-sectional view of a multi-junction solar cell 200 according to a third embodiment. Figure 4 The multi-junction solar cell 200 in the embodiment includes the solar cell (first solar cell) 100 located on the light incident side of the second embodiment and the second solar cell 201. The band gap of the photoelectric conversion layer in the second solar cell 201 is smaller than the band gap of the photoelectric conversion layer 10 in the solar cell 100 of the second embodiment. The multi-junction solar cell in this embodiment includes a solar cell in which three or more solar cells are connected.
[0056] Since the band gap of the photoelectric conversion layer 10 in the solar cell 100 according to the second embodiment is equal to or greater than 2.10 eV, the band gap of the photoelectric conversion layer in the second solar cell 201 is preferably 1.0 eV or more and 1.4 eV or less. The photoelectric conversion layer of the second solar cell 201 is preferably a layer composed of at least one of a GIGS-based compound semiconductor, a CIT-based compound semiconductor, a CdTe-based compound semiconductor, a copper oxide-based compound semiconductor, or crystalline silicon with a high In content.
[0057] By using the solar cell 100 according to the second embodiment as the first solar cell, the first solar cell transmits most of the light of the wavelength of the absorption band of the photoelectric conversion layer of the bottom cell, thereby preventing the conversion efficiency of the bottom cell (second solar cell) from deteriorating, and it is possible to realize a multi-junction solar cell with good efficiency.
[0058] (Fourth Embodiment)
[0059] The fourth embodiment relates to a solar cell module. Figure 5 This is a conceptual perspective view of a solar cell module 300 according to the fourth embodiment. Figure 5The solar cell module 300 is a solar cell module prepared by laminating a first solar cell module 301 and a second solar cell module 302. The first solar cell module 301 is located on the light incident side and uses the solar cell 100 of the second embodiment. The second solar cell 201 is preferably used for the second solar cell module 302.
[0060] Figure 6 It is a conceptual cross-sectional view of the solar cell module 300 . Figure 6 The structural details of the first solar cell module 301 are shown, but the structure of the second solar cell module 302 is not shown. In the second solar cell module 302, the structure of the solar cell module is appropriately selected according to the photoelectric conversion layer of the solar cell to be used, etc. Figure 6 The solar cell assembly in the figure includes a plurality of subassemblies 303 surrounded by dotted lines. Each subassembly 303 includes a plurality of solar cells 100 (solar cell elements) arranged laterally and electrically connected in series. The subassemblies 303 are electrically connected in parallel or in series.
[0061] The solar cell 100 is scribed (P1 to P3), and the second electrode 3 located on the upper side and the first electrode 1 located on the lower side are connected to each other in adjacent solar cells 100. The solar cell 100 in the third embodiment also has the first electrode 1, the photoelectric conversion layer 10, the n-type layer 2 and the second electrode 3, and further includes a substrate 20, similarly to the solar cell 100 in the second embodiment.
[0062] Variations in output voltage between components can result in reduced component output due to current flowing backwards to the lower voltage portion or excess heat generation.
[0063] Furthermore, by using the solar cell disclosed in the present invention, a solar cell suitable for each band can be used, which can produce higher power generation efficiency than when the solar cell is used alone as a top cell or a bottom cell. This is desirable because the output of the entire assembly is increased.
[0064] If the conversion efficiency of the entire assembly is high, it is possible to reduce the energy ratio of applied light energy that is converted into heat. Therefore, it is possible to suppress the decrease in efficiency due to the increase in the temperature of the entire assembly.
[0065] (Fifth Embodiment)
[0066] The fifth embodiment relates to a photovoltaic power generation system. The solar cell assembly 300 of the fourth embodiment can be used as a generator for generating electricity in the photovoltaic power generation system of the fifth embodiment. The photovoltaic power generation system of this embodiment uses a solar cell assembly to generate electricity, and specifically includes: a solar cell assembly for generating electricity, a device for converting the generated electricity into electric power, and a storage device for storing the generated electricity or a load for consuming the generated electricity. Figure 7 4 is a conceptual diagram of the configuration of the photovoltaic power generation system 400 in the embodiment. Figure 7 The photovoltaic power generation system in includes a solar cell assembly 401 (300), a power converter 402, a battery 403 and a load 404. Any one of the battery 403 and the load 404 can be omitted. The load 404 can be configured to be able to utilize the electric energy stored in the battery 403. The power converter 402 is a device including a circuit or an element, wherein the circuit or element can perform voltage conversion and power conversion, such as DC / AC conversion. The power converter 402 can be preferably configured according to the configuration of the power generation voltage, the battery 403 or the load 404.
[0067] The solar cell included in the subassembly 301 that receives light in the solar cell assembly 300 generates electricity, and the electric energy is converted by the converter 402 and stored in the storage battery 403 or consumed in the load 404. Preferably, the solar cell assembly 401 is provided with a sunlight tracking device that can continuously guide the solar cell assembly 401 to the sun, or is provided with a concentrator that collects sunlight, or a device for improving power generation efficiency is added to the solar cell assembly 401.
[0068] Photovoltaic power generation system 400 is preferably used in real estate such as residences, commercial facilities, and factories, or in movable property such as vehicles, aircraft, and electronic equipment. By using the solar cell having good conversion efficiency in this embodiment in solar cell module 401, it is expected that the amount of power generation will increase.
[0069] As an application example of the photovoltaic power generation system 400 , a vehicle is shown. Figure 8 This is a conceptual diagram of the structure of vehicle 500. Figure 8The vehicle 500 shown has a vehicle body 501, a solar cell module 502, a power converter 503, a battery 504, a motor 505, and tires (wheels) 506. The electric energy generated by the solar cell module 502 disposed on the top of the vehicle body 501 is converted in the power converter 503 to charge the battery 504 or to be consumed in a load such as the motor 505. The vehicle 500 can be moved by rotating the tires (wheels) 506 by the motor 505 using the electric energy provided by the solar cell module 502 or the battery 504. The solar cell module 502 can be configured as only the first solar cell module having the solar cell 100 in the second embodiment, rather than the multi-junction type. When a solar cell module 502 having light transmittance is used, in addition to the top of the vehicle body 501, the solar cell module 502 on the side of the vehicle body 501 is preferably used as a power generation window.
[0070] The present invention will be described in more detail below based on examples, but the present invention is not limited to the following examples.
[0071] (Example 1)
[0072] Example 1 uses a white glass substrate as a substrate, and a transparent conductive film containing SnO2 doped with Sb is used as the first electrode on the back side. On the first electrode, Ge and Cu are used as targets, sputtered in a mixed atmosphere of oxygen and argon, and the substrate is heated at 450°C to deposit a Ge-doped cuprous oxide compound as a photoelectric conversion layer. Then, Zn-Ge-O as an n-type layer is formed on the photoelectric conversion layer by atomic layer deposition. Subsequently, an AZO transparent conductive film is deposited as the second electrode on the front side. MgF2 is deposited on the second electrode as an anti-reflection film to obtain a solar cell.
[0073] A solar simulator was used to simulate the light source of AM1.5G, and the amount of light was adjusted so that 1 sun (1sun) could be obtained using a reference Si cell under the light source. The atmospheric temperature was 25°C. The voltage was scanned and the current density was measured (obtained by dividing the current by the cell area). When the voltage is on the horizontal axis and the current density is on the vertical axis, the intersection with the horizontal axis is the open circuit voltage Voc, and the intersection with the vertical axis is the short circuit current density Jsc. On the measurement curve, the points where the product of voltage and current density is the largest are set as Vmpp and Jmpp (maximum power point), respectively, FF = (Vmpp*Jmpp) / (Voc*Jsc), and the efficiency is determined by Eff = Voc*Jsc*FF. The transmittance of the solar cell was measured, and the band gap of the photoelectric conversion layer was determined by the photoluminescence method. In addition, SIMS was used to observe the cross section of the obtained solar cell and determine the concentration of each element.
[0074] (Example 2)
[0075] A photoelectric conversion layer was formed in the same manner as in Example 1 except that Ta was used instead of Ge in the formation of the photoelectric conversion layer, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0076] (Example 3)
[0077] A photoelectric conversion layer was formed in the same manner as in Example 1 except that In was used instead of Ge in the formation of the photoelectric conversion layer, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0078] (Implementation 4)
[0079] The photoelectric conversion layer was formed in the same manner as in Example 1 except that Ta and In were further used in addition to Ge in the formation of the photoelectric conversion layer, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0080] (Implementation 5)
[0081] A photoelectric conversion layer was formed in the same manner as in Example 1 except that Ta was further used in addition to Ge in the formation of the photoelectric conversion layer, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0082] (Example 6)
[0083] A photoelectric conversion layer was formed in the same manner as in Example 1 except that Ta and In were used instead of Ge in the formation of the photoelectric conversion layer, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0084] (Example 7)
[0085] A photoelectric conversion layer was formed in the same manner as in Example 1 except that the sputtering amount of Ge was increased during the formation of the photoelectric conversion layer, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0086] (Example 8)
[0087] The photoelectric conversion layer was formed in the same manner as in Example 1, except that the sputtering amount of Ge was greatly increased compared with Example 7. Then, various measurements were performed in the same manner as in Example 1.
[0088] (Example 9)
[0089] A photoelectric conversion layer was formed in the same manner as in Example 1 except that the sputtering amount of Ge was reduced during the formation of the photoelectric conversion layer, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0090] (Example 10)
[0091] The photoelectric conversion layer was formed in the same manner as in Example 1, except that the sputtering amount of Ge was significantly reduced compared with Example 9. Then, various measurements were performed in the same manner as in Example 1.
[0092] (Example 11)
[0093] The photoelectric conversion layer was formed in the same manner as in Example 1 except that the variation in the amount of Ge to be doped was reduced during the formation of the photoelectric conversion layer, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0094] (Example 12)
[0095] The photoelectric conversion layer was formed in the same manner as in Example 1, and a solar cell was obtained in the same manner as in Example 1, except that the change in the amount of Ge to be doped during the formation of the photoelectric conversion layer was significantly reduced compared to Example 11. Next, various measurements were performed in the same manner as in Example 1.
[0096] (Example 13)
[0097] The photoelectric conversion layer was formed in the same manner as in Example 1 except that the amount of Ge to be doped was changed during the formation of the photoelectric conversion layer, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0098] (Example 14)
[0099] The photoelectric conversion layer was formed in the same manner as in Example 1 except that the amount of Ge to be doped was changed during the formation of the photoelectric conversion layer, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0100] (Example 15)
[0101] The photoelectric conversion layer was formed in the same manner as in Example 1. Next, a solar cell was obtained in the same manner as in Example 1, except that Zn-Si-O was deposited as an n-type layer and Si was diffused in the photoelectric conversion layer. Then, various measurements were performed in the same manner as in Example 1, and the p-type dopant concentration was measured from the surface of the n-type layer side of the photoelectric conversion layer to a depth of 10 nm.
[0102] (Example 16)
[0103] The photoelectric conversion layer was formed in the same manner as in Example 1. Next, a solar cell was obtained in the same manner as in Example 1, except that an n-type layer was formed and Ge was diffused from the n-type layer into the photoelectric conversion layer. Then, various measurements were performed in the same manner as in Example 1, and the p-type dopant concentration was measured from the surface of the n-type layer side of the photoelectric conversion layer to a depth of 10 nm.
[0104] (Example 17)
[0105] The photoelectric conversion layer was formed in the same manner as in Example 1 except that the amount of Ge to be doped was reduced during the formation of the photoelectric conversion layer, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0106] (Example 18)
[0107] The photoelectric conversion layer was formed in the same manner as in Example 2 except that the amount of Ta to be doped was reduced during the formation of the photoelectric conversion layer, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0108] (Example 19)
[0109] A photoelectric conversion layer was formed in the same manner as in Example 3 except that the amount of In to be doped was reduced during the formation of the photoelectric conversion layer, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0110] (Example 20)
[0111] The photoelectric conversion layer was formed in the same manner as in Example 1, except that the amount of Ge to be doped in the central portion in the thickness direction of the photoelectric conversion layer was reduced during the formation of the photoelectric conversion layer, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0112] (Example 21)
[0113] The photoelectric conversion layer was formed in the same manner as in Example 1 except that the amount of Ge to be doped on the first electrode side was reduced during the formation of the photoelectric conversion layer, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0114] (Example 22)
[0115] A photoelectric conversion layer was formed in the same manner as in Example 1 except that the deposition rate was reduced during the formation of the photoelectric conversion layer, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0116] (Comparative Example 1)
[0117] A photoelectric conversion layer was formed in the same manner as in Example 1 except that Ge, Ta and In were not used in the formation of the photoelectric conversion layer, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0118] (Comparative Example 2)
[0119] The photoelectric conversion layer was formed in the same manner as in Example 1 except that the amount of Ge to be doped was greatly increased during the formation of the photoelectric conversion layer, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0120] (Comparative Example 3)
[0121] The photoelectric conversion layer was formed in the same manner as in Example 2 except that the amount of Ta to be doped was greatly increased, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0122] (Comparative Example 4)
[0123] A photoelectric conversion layer was formed in the same manner as in Example 3 except that the amount of In to be doped was reduced during the formation of the photoelectric conversion layer, and a solar cell was obtained in the same manner as in Example 1. Next, various measurements were performed in the same manner as in Example 1.
[0124] Table 1 shows the results of the embodiments and comparative examples. For FF, Jsc, conversion efficiency and transmittance, when the characteristics are improved compared with Comparative Example 1, it is evaluated as A (A- when the characteristics are slightly improved), and when FF, Jsc, conversion efficiency and transmittance are lower than the values in Comparative Example 1, it is evaluated as B. The overall average value in the table is the average value of the overall p-type dopant concentration. The n-type layer side average value in the table is the average value of the front side p-type dopant concentration. The central average value in the table is the average value of the central p-type dopant concentration. The first electrode side average value in the table is the average value of the back side p-type dopant concentration. The n-type layer side region average value in the table is the average value of the n-type layer side region p-type dopant concentration.
[0125] Table 1A
[0126]
[0127] Table 1B
[0128]
[0129] For the solar cell in the embodiment, only when an element as a p-type dopant is added to the photoelectric conversion layer 10, FF and Jsc can be completely improved, thereby improving the efficiency of the solar cell in the embodiment. It can be inferred that by reducing crystal defects by adding elements, the recombination of photogenerated carriers in the photoelectric conversion layer 10 can be improved, which is proved by the following: the hole concentration in the photoelectric conversion layer 10 is controlled by adding a p-type dopant, and the crystallinity of the photoelectric conversion layer 10 itself is improved by adding a p-type dopant. As shown in the above embodiment, by adding appropriate elements in the mixed region 2a or the mixed layer 2b, a high-efficiency solar cell using a photoelectric conversion layer based on cuprous oxide can be realized.
[0130] In the specification, some elements are represented by only element symbols.
[0131] Next, the technical scheme of the embodiment will be described separately.
[0132] Technical Case 1
[0133] A photoelectric conversion layer, which is based on Cu2O and contains at least one p-type dopant selected from Ge, Ta and In, and has a band gap of 2.10 eV or more and 2.30 eV or less.
[0134] Technical Case 2
[0135] According to the photoelectric conversion layer of technical solution 1, the minimum value of the p-type dopant concentration in the photoelectric conversion layer is equal to or greater than 1×10 15 atoms / cm 3, and the maximum value of the p-type dopant concentration in the photoelectric conversion layer is equal to or less than 1×10 20 atoms / cm 3 .
[0136] Technical Case 3
[0137] The photoelectric conversion layer according to claim 1 or 2, wherein the average value of the p-type dopant concentration in the photoelectric conversion layer is 1×10 15 atoms / cm 3 Above and 1×10 19 atoms / cm 3 the following.
[0138] Technical Case 4
[0139] The photoelectric conversion layer according to any one of claims 1 to 3, wherein the maximum value of the p-type dopant concentration in the photoelectric conversion layer is 1 to 10,000 times the minimum value of the p-type dopant concentration in the photoelectric conversion layer.
[0140] Technical Case 5
[0141] A photoelectric conversion layer according to any one of Technical Cases 1 to 4, wherein, in the photoelectric conversion layer, an average value of the p-type dopant concentration at a depth of 100 nm from the front side of the photoelectric conversion layer is equal to or less than 100 times the average value of the p-type dopant concentration at a depth of half the thickness of the photoelectric conversion layer, and an average value of the p-type dopant concentration at a depth of 100 nm from the back side of the photoelectric conversion layer is equal to or less than 1000 times the average value of the p-type dopant concentration at a depth of half the thickness of the photoelectric conversion layer.
[0142] Technical Case 6
[0143] The photoelectric conversion layer according to any one of technical solutions 1 to 5, wherein the proportion of Cu2O is equal to or greater than 90wt%.
[0144] Technical Case 7
[0145] A solar cell comprising:
[0146] A transparent first electrode,
[0147] The photoelectric conversion layer described in any one of technical solutions 1 to 6 on the first electrode,
[0148] an n-type layer on the photoelectric conversion layer, and
[0149] A transparent second electrode is on the n-type layer.
[0150] Technical Case 8
[0151] According to the solar cell described in Technical Case 7, the average concentration of Si and / or Ge in a region up to a depth of 50 nm from the interface between the photoelectric conversion layer and the n-type layer to the first electrode side is more than 1 times and less than 100 times the average concentration of p-type dopants in the photoelectric conversion layer.
[0152] Technical Case 9
[0153] A multi-junction solar cell, comprising the solar cell described in technical case 7 or 8.
[0154] Technical Case 10
[0155] A solar cell assembly comprises the solar cell described in technical case 7 or 8.
[0156] Technical Case 11
[0157] A photovoltaic power generation system is configured to generate electricity using the solar cell assembly described in technical case 10.
[0158] Although certain embodiments have been described, these embodiments are presented by way of example only and are not intended to limit the scope of the invention. In fact, the novel embodiments described herein may be embodied in a variety of other forms; furthermore, various omissions, substitutions, and changes may be made in the form of the embodiments described herein without departing from the spirit of the invention. The accompanying claims and their equivalents are intended to cover forms or modifications that fall within the scope and spirit of the invention.
[0159] Explanation of symbols
[0160] 10 Photoelectric conversion layer
[0161] 100 Solar cells (first solar cell, top cell)
[0162] 1. First electrode
[0163] 2 n-type layer
[0164] 3 Second electrode
[0165] 200 multi-junction solar cells
[0166] 201 Second solar cell (bottom cell)
[0167] 300 Solar cell modules
[0168] 301 First Solar Cell Module
[0169] 302 Second solar cell module
[0170] 20 Base
[0171] 303 Subcomponents
[0172] 400 Photovoltaic power generation system
[0173] 401 Solar cell modules
[0174] 402 Power Converter
[0175] 403 Battery
[0176] 404 Payload
[0177] 500 vehicles
[0178] 501 Carbody
[0179] 502 Solar cell modules
[0180] 503 Power Converter
[0181] 504 Battery
[0182] 505 Motor
[0183] 506 Tire (Wheel)
Claims
1. A photoelectric conversion layer, which is based on Cu2O and contains at least one selected from Ge, Ta and In as a p-type dopant, wherein the band gap of the photoelectric conversion layer is greater than or equal to 2.10 eV and less than or equal to 2.30 eV, The average concentration of the p-type dopant in the photoelectric conversion layer is 1×10 15 atoms / cm 3 Above and 1×10 19 atoms / cm 3 the following, The p-type dopant increases the hole concentration of the photoelectric conversion layer.
2. The photoelectric conversion layer according to claim 1, wherein The minimum value of the p-type dopant concentration in the photoelectric conversion layer is equal to or greater than 1×10 15 atoms / cm 3 , and the maximum value of the p-type dopant concentration in the photoelectric conversion layer is equal to or less than 1×10 20 atoms / cm 3 .
3. The photoelectric conversion layer according to claim 1 or 2, wherein: The maximum value of the p-type dopant concentration in the photoelectric conversion layer is not less than 1 time and not more than 10000 times the minimum value of the p-type dopant concentration in the photoelectric conversion layer.
4. The photoelectric conversion layer according to any one of claims 1 to 3, wherein In the photoelectric conversion layer, the average value of the p-type dopant concentration at a depth of 100 nm from the front side of the photoelectric conversion layer is equal to or less than 100 times the average value of the p-type dopant concentration at a depth of half the thickness of the photoelectric conversion layer, and the average value of the p-type dopant concentration at a depth of 100 nm from the back side of the photoelectric conversion layer is equal to or less than 1000 times the average value of the p-type dopant concentration at a depth of half the thickness of the photoelectric conversion layer.
5. The photoelectric conversion layer according to any one of claims 1 to 4, wherein The proportion of Cu2O is equal to or greater than 90 wt%.
6. A solar cell comprising: A transparent first electrode, The photoelectric conversion layer according to any one of claims 1 to 5 on the first electrode, an n-type layer on the photoelectric conversion layer, and A transparent second electrode is disposed on the n-type layer.
7. The solar cell according to claim 6, wherein: An average concentration of Si and / or Ge in a region 50 nm deep from an interface between the photoelectric conversion layer and the n-type layer toward the first electrode is 1 to 100 times an average concentration of p-type dopants in the photoelectric conversion layer.
8. A multi-junction solar cell comprising the solar cell according to claim 6 or 7.
9. A solar cell module comprising the solar cell according to claim 6 or 7.
10. A photovoltaic power generation system, configured to generate electricity using the solar cell assembly according to claim 9.