Tin-antimony electroplating solution and preparation method thereof
High specific capacity tin-antimony alloys and tin-antimony-nickel-phosphorus alloys are prepared through a simple mixing and stirring method of tin-antimony electroplating liquid, which solves the problems of long preparation cycle and high cost in the existing technology, and achieves uniform and efficient electroplating effects.
Patent Information
- Application Number
- CN202111561469.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-20
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-12-20
AI Technical Summary
The existing tin-antimony alloy preparation method has a long cycle, high cost, is not easy to be produced on a large scale, and is difficult to meet the demand for high specific capacity.
A tin-antimony plating solution is used, which contains boric acid, complexing agent, antimony salt and tin salt. It is prepared through a simple mixing and stirring method. An appropriate amount of saccharin and 2-aminopyridine are added to improve stability and uniformity, and a high specific capacity is prepared. Tin antimony alloy and tin antimony nickel phosphorus alloy.
It achieves uniform tin-antimony alloy coating, high specific capacity, good electroplating solution stability, simple preparation process, safety and environmental protection, shortened preparation cycle, and good performance repeatability.
Smart Images

Figure SMS_1 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electroplating, and in particular to a tin-antimony electroplating solution and a preparation method thereof. Background Art
[0002] Electroplating is the process of plating a thin layer of other metals or alloys on certain metal surfaces using the principle of electrolysis. Electroplating has the advantages of low cost, simple operation and easy scalability, and is widely used. Electroplating of single metals is far from meeting the modern demand for functional materials. Therefore, electroplating of multi-element alloys has developed rapidly in recent years, with a wide variety of types and excellent material properties. It has been widely used in the magnetic industry, energy field, etc.
[0003] At present, the lithium / sodium storage capacity of tin is as high as 990 mAh / g, and the lithium / sodium storage capacity of antimony is as high as 660 mAh / g, which is much higher than the current commercial carbon materials. Tin and its alloys are a class of energy storage materials with very good prospects. At present, the methods for preparing tin-antimony alloys mainly include high-energy ball milling, hydrothermal, etc., but these preparation methods have the disadvantages of long cycle, high cost, and difficulty in large-scale production and application. Therefore, it is of great significance to seek low-cost electrodeposition technology to prepare tin-antimony alloys and tin-antimony-nickel-phosphorus alloys with high specific capacity. Summary of the invention
[0004] The purpose of the present invention is to provide a tin-antimony electroplating solution and a preparation method thereof in view of the above problems existing in the prior art.
[0005] In order to achieve the first object of the above invention, the present invention adopts the following technical scheme: the tin-antimony electroplating solution comprises boric acid, a complexing agent and an appropriate amount of water, the electroplating solution further comprises an antimony salt and a tin salt, and the components and contents of the electroplating solution are 10-60 g / L of boric acid, 5-80 g / L of complexing agent, 0.5-10 g / L of antimony salt and 0.5-40 g / L of tin salt;
[0006] Among them, the antimony salt is potassium antimony tartrate, antimony acetate or sodium pyroantimonate; the tin salt is stannous sulfate or stannous chloride; the complexing agent is disodium ethylenediaminetetraacetate, ammonium acetate, citric acid or glycine.
[0007] Working principle and beneficial effects: 1. Compared with the prior art, the tin-antimony electroplating solution of the present application can be used to obtain a uniform tin-antimony alloy by electroplating method, with a uniform coating, beautiful color, high specific capacity, and good stability of the electroplating solution. The electroplating solution of this ratio has a stable polarization curve, and can be used with a relatively simple operation to obtain a product with good performance repeatability and uniformity.
[0008] Furthermore, the components and contents of the electroplating solution are 30 g / L of boric acid, 50 g / L of complexing agent, 5 g / L of antimony salt and 20 g / L of tin salt.
[0009] Furthermore, the pH value of the electroplating solution is 0.5-3.0.
[0010] Furthermore, the working temperature of the electroplating solution is 10-80°C.
[0011] Furthermore, the electroplating solution also includes additives, and the components and contents of the additives are 0.5-2 g / L of saccharin and 2-5 g / L of 2-aminopyridine. Since the electroplating solution is an alloy electroplating solution of tin salt and antimony salt, the above two substances are added to improve the stability during storage and to improve the uniformity and stability of the deposited coating of the electroplating solution during the electroplating process.
[0012] A method for preparing a tin-antimony electroplating solution, for preparing the above-mentioned tin-antimony electroplating solution, comprises the following steps:
[0013] S00, add 10-60g of boric acid and 5-80g of complexing agent into deionized water, stir and dissolve to form a mixed solution;
[0014] S10, adjusting the pH of the mixed solution to 1.0-3.0 with hydrochloric acid or sulfuric acid;
[0015] S20, adding 0.5-10 g of antimony salt and 0.5-40 g of tin salt to the mixed solution, stirring to dissolve, then adding the remaining amount of deionized water to make the volume to 1 L, adjusting the pH of the mixed solution to 0.5-3.0, to obtain a tin-antimony electroplating solution.
[0016] In this way, during the preparation process of the electroplating solution of the present application, there is no need to perform operations such as high-energy ball milling, but only simple mixing and stirring, which greatly shortens the preparation cycle, is safe and environmentally friendly, has high chemical stability, a simple and controllable preparation process, and good stability.
[0017] In order to achieve the second object of the above invention, the present invention adopts the following technical scheme: tin-antimony-nickel-phosphorus electroplating solution, based on the above tin-antimony electroplating solution, the electroplating solution also includes nickel salt and phosphate, and the components and contents of the electroplating solution are boric acid 10-80 g / L, complexing agent 10-80 g / L, antimony salt 1-20 g / L, tin salt 1-20 g / L, nickel salt 1-20 g / L and phosphate 5-60 g / L;
[0018] Among them, the nickel salt is sulfate or chloride; the phosphate is sodium dihydrogen hypophosphite or sodium phosphate; the antimony salt is potassium antimony tartrate or antimony chloride; the tin salt is sulfate or chloride; and the complexing agent is sodium acetate, sodium alginate, glycine or tartaric acid.
[0019] Working principle and beneficial effects: 1. Compared with the prior art, the tin-antimony-nickel-phosphorus electroplating solution of the present application adds nickel salt and phosphate on the basis of the above-mentioned tin-antimony electroplating solution, and adjusts the content of each component. Therefore, the tin-antimony-nickel-phosphorus electroplating solution of the present application can also be used to obtain a uniform tin-antimony-nickel-phosphorus alloy by electroplating method, with uniform coating, beautiful color, high specific capacity, and good stability of the electroplating solution. The electroplating solution of this ratio has a stable polarization curve, and can be used with a relatively simple operation to obtain a product with good performance repeatability and uniformity.
[0020] Furthermore, the components and contents of the electroplating solution are 40 g / L boric acid, 60 g / L complexing agent, 4 g / L antimony salt, 5 g / L tin salt, 10 g / L nickel salt, and 40 g / L phosphate.
[0021] Furthermore, the pH value of the electroplating solution is 0.5-4.0.
[0022] Furthermore, the working temperature of the electroplating solution is 10-60°C.
[0023] Furthermore, the electroplating solution also includes additives, which are 0.5-3 g / L polyethylene glycol and 0.5-2 g / L 2-amino-4-methylpyridine.
[0024] A method for preparing a tin-antimony-nickel-phosphorus electroplating solution, used for the above-mentioned tin-antimony electroplating solution, comprises the following steps:
[0025] S00, add 10-80 g of boric acid and 10-80 g of complexing agent into deionized water, stir and dissolve to form a mixed solution;
[0026] S10, adjusting the pH of the mixed solution to 1.0-4.0 with hydrochloric acid or sulfuric acid;
[0027] S20, add 1-10 g of antimony salt, 1-20 g of tin salt, 1-20 g of nickel salt and 5-60 g of phosphate to the above mixed solution, stir to dissolve, then add the remaining amount of deionized water to make the volume 1L, adjust the pH of the mixed solution to 0.5-4.0, and obtain a tin-antimony-nickel-phosphorus electroplating solution.
[0028] In this way, during the preparation process of the electroplating solution of the present application, there is no need to perform operations such as high-energy ball milling, and only simple mixing and stirring is required, which greatly shortens the preparation cycle, is safe and environmentally friendly, has high chemical stability, a simple and controllable preparation process, and good stability. DETAILED DESCRIPTION
[0029] Below in conjunction with the accompanying drawings in the embodiments of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described. Obviously, the described embodiments are only a part of embodiments of the present invention, rather than all embodiments. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art belong to the scope of protection of the present invention. If there are no special instructions, the raw materials used in the embodiments of the present invention are the raw materials commonly used in this area, and the methods used in the embodiments are the conventional methods in this area.
[0030] Embodiment 1:
[0031] A method for preparing a tin-antimony electroplating solution is as follows:
[0032] Add 10 g of boric acid and 5 g of disodium ethylenediaminetetraacetate to deionized water, stir and dissolve to prepare a mixed solution, adjust the pH to 1.0 with aqueous hydrogen chloride solution, add 0.5 g of potassium antimony tartrate and 0.5 g of stannous chloride to the mixed solution, stir and dissolve, add the remaining amount of deionized water to a total volume of 1 L, adjust the pH to 0.5, and obtain a tin-antimony electroplating solution.
[0033] Embodiment 2:
[0034] A method for preparing a tin-antimony electroplating solution is as follows:
[0035] Add 60 g of boric acid and 80 g of ammonium acetate to deionized water, stir and dissolve to prepare a mixed solution, adjust the pH to 3.0 with aqueous hydrogen chloride solution, add 10 g of potassium antimony tartrate and 40 g of stannous chloride to the mixed solution, stir and dissolve, add the remaining amount of deionized water to a total volume of 1 L, adjust the pH to 3.0, and obtain a tin-antimony electroplating solution.
[0036] Embodiment 3:
[0037] A method for preparing a tin-antimony electroplating solution is as follows:
[0038] Add 40 g of boric acid and 60 g of citric acid to deionized water, stir and dissolve to prepare a mixed solution, adjust the pH to 2.0 with aqueous hydrogen chloride solution, add 5 g of potassium antimony tartrate and 20 g of stannous chloride to the mixed solution, stir and dissolve, add the remaining amount of deionized water to a total volume of 1 L, adjust the pH to 1.5, and obtain a tin-antimony electroplating solution.
[0039] Embodiment 4:
[0040] A method for preparing a tin-antimony electroplating solution is as follows:
[0041] Add 60 g of boric acid and 50 g of glycine to deionized water, stir and dissolve to prepare a mixed solution, adjust the pH to 1.0 with aqueous hydrogen chloride solution, add 4 g of antimony acetate and 5 g of stannous sulfate to the mixed solution, stir and dissolve, add the remaining amount of deionized water to a total volume of 1 L, adjust the pH to 1.0, and obtain a tin-antimony electroplating solution.
[0042] Embodiment 5:
[0043] A method for preparing a tin-antimony electroplating solution is as follows:
[0044] Add 40 g of boric acid and 40 g of sodium ethylenediaminetetraacetate to deionized water, stir and dissolve to prepare a mixed solution, adjust the pH to 3.0 with aqueous hydrogen chloride solution, add 6 g of sodium pyroantimonate and 5 g of stannous chloride to the mixed solution, stir and dissolve, add the remaining amount of deionized water to a total volume of 1 L, adjust the pH to 1.5, and obtain a tin-antimony electroplating solution.
[0045] Embodiment 6:
[0046] A method for preparing a tin-antimony electroplating solution is as follows:
[0047] Add 30 g of boric acid and 50 g of glycine to deionized water, stir and dissolve to prepare a mixed solution, adjust the pH to 2.0 with an aqueous hydrogen chloride solution, add 4 g of potassium antimony tartrate and 20 g of stannous sulfate to the mixed solution, stir and dissolve, add the remaining amount of deionized water to a total volume of 1 L, adjust the pH to 1.5, and obtain a tin-antimony electroplating solution.
[0048] Embodiment 7:
[0049] On the basis of Example 5, 0.5 g / L saccharin and 2 g / L 2-aminopyridine were added, and the timing of addition was the same as that of boric acid.
[0050] Embodiment 8:
[0051] On the basis of Example 6, 2 g / L saccharin and 5 g / L 2-aminopyridine were added, and the timing of addition was the same as that of boric acid.
[0052] In summary, the tin-antimony coatings obtained through Examples 1-6 are uniform, beautiful in color, and have a relatively high sodium storage capacity. Table 1 below shows the test results of the electrochemical performance test of the coatings of Examples 1-6:
[0053]
[0054] Table 1
[0055] Examples 7-8 are further improvements. Since the electroplating solution is based on tin salt and antimony salt, the existing complexing agent cannot improve the storage stability of the electroplating solution. Therefore, it is necessary to modify its storage stability in order to reduce the impact of storage time on the performance of the coating. The following Table 2 shows the test results of the coating obtained in Examples 7-8 using electrochemical performance tests:
[0056]
[0057] Table 2
[0058] It can be seen from the above table that the tin-antimony coating obtained by using the electroplating solution of the present invention has a high specific capacity and exhibits good electrochemical performance. Examples 7-8 ensure the stability of its storage performance. After long-term storage, the process operation difficulty of Examples 1-6 increases, and the stability of the plating solution decreases. After long-term storage, the plating solution becomes turbid and the coating performance decreases by 3%-10%. After the improvement of Examples 7-8, the plating solution remains clear and transparent within two months, and has little effect on the coating performance.
[0059] Based on Examples 1-8, further steps were performed to add nickel salt and phosphate to obtain a tin-antimony-nickel-phosphorus electroplating solution. The preparation method of the tin-antimony-nickel-phosphorus electroplating solution is as shown in the following example:
[0060] Embodiment 9:
[0061] A method for preparing a tin-antimony-nickel-phosphorus electroplating solution is as follows:
[0062] Add 10 g of boric acid and 10 g of sodium acetate to deionized water, stir and dissolve to prepare a mixed solution, adjust the pH to 1.0 with an aqueous hydrogen chloride solution, add 1 g of potassium antimony tartrate, 1 g of stannous chloride, 1 g of nickel chloride and 5 g of sodium hypophosphite to the mixed solution, stir and dissolve, add the remaining amount of deionized water to a total volume of 1 L, adjust the pH to 0.5, and obtain a tin-antimony-nickel-phosphorus electroplating solution.
[0063] Embodiment 10:
[0064] A method for preparing a tin-antimony-nickel-phosphorus electroplating solution is as follows:
[0065] Add 80 g of boric acid and 80 g of sodium alginate to deionized water, stir and dissolve to prepare a mixed solution, adjust the pH to 4.0 with an aqueous hydrogen chloride solution, add 10 g of antimony chloride, 2 g of stannous chloride, 20 g of nickel chloride and 60 g of sodium phosphate to the mixed solution, stir and dissolve, add the remaining amount of deionized water to a total volume of 1 L, adjust the pH to 4.0, and obtain a tin-antimony-nickel-phosphorus electroplating solution.
[0066] Embodiment 11:
[0067] A method for preparing a tin-antimony-nickel-phosphorus electroplating solution is as follows:
[0068] Add 40 g of boric acid and 60 g of glycine to deionized water, stir and dissolve to prepare a mixed solution, adjust the pH to 2.5 with an aqueous hydrogen chloride solution, add 4 g of potassium antimony tartrate, 20 g of stannous chloride, 10 g of nickel sulfate and 40 g of sodium hypophosphite to the mixed solution, stir and dissolve, add the remaining amount of deionized water to a total volume of 1 L, adjust the pH to 2.0, and obtain a tin-antimony-nickel-phosphorus electroplating solution.
[0069] Embodiment 12:
[0070] A method for preparing a tin-antimony-nickel-phosphorus electroplating solution is as follows:
[0071] Add 60 g of boric acid and 40 g of tartaric acid to deionized water, stir and dissolve to prepare a mixed solution, adjust the pH to 1.5 with an aqueous hydrogen chloride solution, add 2 g of potassium antimony tartrate, 15 g of stannous sulfate, 5 g of nickel sulfate and 20 g of phosphate to the mixed solution, stir and dissolve, add the remaining amount of deionized water to a total volume of 1 L, adjust the pH to 3.5, and obtain a tin-antimony-nickel-phosphorus electroplating solution.
[0072] Embodiment 13:
[0073] A method for preparing a tin-antimony-nickel-phosphorus electroplating solution is as follows:
[0074] Add 40 g of boric acid and 40 g of tartaric acid to deionized water, stir and dissolve to prepare a mixed solution, adjust the pH to 3.0 with an aqueous hydrogen chloride solution, add 6 g of antimony chloride, 5 g of stannous chloride, 10 g of nickel chloride and 10 g of hypophosphite to the mixed solution, stir and dissolve, add the remaining amount of deionized water to a total volume of 1 L, adjust the pH to 2.0, and obtain a tin-antimony-nickel-phosphorus electroplating solution.
[0075] Embodiment 14:
[0076] A method for preparing a tin-antimony-nickel-phosphorus electroplating solution is as follows:
[0077] Add 20 g of boric acid and 30 g of citric acid to deionized water, stir and dissolve to prepare a mixed solution, adjust the pH to 3.0 with aqueous hydrogen chloride solution, add 4 g of potassium antimony tartrate, 20 g of nickel chloride, 15 g of stannous chloride and 5 g of phosphate to the mixed solution, stir and dissolve, add the remaining amount of deionized water to a total volume of 1 L, adjust the pH to 1.0, and obtain a tin-antimony-nickel-phosphorus electroplating solution.
[0078] Embodiment 15:
[0079] On the basis of Example 13, 0.5 g / L polyethylene glycol and 0.5 g / L 2-amino-4-methylpyridine were added, and the timing of addition was the same as that of boric acid.
[0080] Embodiment 16:
[0081] On the basis of Example 14, 3 g / L of polyethylene glycol and 2 g / L of 2-amino-4-methylpyridine were added, and the timing of addition was the same as that of boric acid. Since the electroplating solution is a tin-antimony-nickel-phosphorus alloy electroplating solution, the above two substances are added for the purpose of improving the stability during storage and improving the uniformity of the deposited coating of the electroplating solution during the electroplating process.
[0082] In summary, the tin-antimony coatings obtained in Examples 9-14 are uniform, beautiful in color, and have a relatively high sodium storage capacity.
[0083] Table 3 below shows the test results of the electrochemical performance test on the coatings of Examples 9-14:
[0084]
[0085] Table 3
[0086] Table 4 below shows the test results of the coatings obtained in Examples 15-16 using electrochemical performance tests:
[0087]
[0088] Table 4
[0089] It can be seen from the above table that the tin-antimony coating obtained by using the electroplating solution of the present invention has a high specific capacity and exhibits good electrochemical properties. Examples 15-16 are further improvements. Since the electroplating solution is a tin-antimony multi-element alloy electroplating solution, the existing complexing agent cannot improve the storage stability of the electroplating solution. Therefore, it is necessary to modify its storage stability in order to reduce the influence of storage time on the coating performance.
[0090] Examples 15-16 ensure the stability of storage performance. After long-term storage, the process operation difficulty of Examples 9-14 increases, and the stability of the plating solution decreases. After long-term storage, the plating solution becomes turbid and the coating performance decreases by 5%-10%. After the improvement of Examples 15-16, the plating solution remains clear and transparent within two months, and has little effect on the coating performance.
[0091] In the above Tables 1 to 4, only the sodium storage capacity is measured, but in fact lithium, potassium, etc. can also be stored.
[0092] The parts not described in detail in the present invention are prior art, so the present invention does not describe them in detail.
[0093] It is to be understood that the term "one" should be understood as "at least one" or "one or more", that is, in one embodiment, the number of an element may be one, while in another embodiment, the number of the element may be multiple, and the term "one" should not be understood as a limitation on the quantity.
[0094] Although the term "such as" is used more frequently in this article, the possibility of using other terms is not excluded. These terms are used only to more conveniently describe and explain the essence of the present invention; interpreting them as any additional limitation is contrary to the spirit of the present invention.
[0095] The present invention is not limited to the above-mentioned optimal implementation mode. Anyone can derive other various forms of products under the inspiration of the present invention. However, no matter what changes are made in the shape or structure, all technical solutions that are the same or similar to those of the present application fall within the protection scope of the present invention.
Claims
1. A tin-antimony electroplating solution comprising boric acid, a complexing agent and an appropriate amount of water, characterized in that: The electroplating solution also contains antimony salt, tin salt and a first additive, wherein the first additive is saccharin and 2-aminopyridine; The components and contents of the electroplating solution are 10-60 g / L of boric acid, 5-80 g / L of complexing agent, 0.5-10 g / L of antimony salt, 0.5-40 g / L of tin salt, 0.5-2 g / L of saccharin and 2-5 g / L of 2-aminopyridine; The antimony salt is potassium antimony tartrate, antimony acetate or sodium pyroantimonate; the tin salt is stannous sulfate or stannous chloride; the complexing agent is disodium ethylenediaminetetraacetate, ammonium acetate, citric acid or glycine; the pH value of the electroplating solution is 0.5-3.0; and the working temperature of the electroplating solution is 10-80°C.
2. The tin-antimony electroplating solution according to claim 1, characterized in that: The components and contents of the electroplating solution are 40 g / L boric acid, 40 g / L disodium ethylenediaminetetraacetate, 6 g / L sodium pyroantimonate, 5 g / L stannous chloride, 0.5 g / L saccharin and 2 g / L 2-aminopyridine.
3. A method for preparing a tin-antimony electroplating solution, characterized in that: The method for preparing the tin-antimony electroplating solution according to claim 1 comprises the following steps: S00, add 10-60 g of boric acid, 5-80 g of complexing agent, 0.5-2 g of saccharin and 2-5 g of 2-aminopyridine to deionized water, stir and dissolve to prepare a mixed solution; S10, adjusting the pH of the mixed solution to 1.0-3.0 with hydrochloric acid or sulfuric acid; S20, add 0.5-10 g of antimony salt and 0.5-40 g of tin salt to the above mixed solution, stir to dissolve, then add the remaining amount of deionized water to make the volume to 1 L, adjust the pH of the mixed solution to 0.5-3.0, and obtain a tin-antimony electroplating solution.
4. Tin-antimony-nickel-phosphorus electroplating solution, characterized in that: Based on the tin-antimony electroplating solution of claim 1, the electroplating solution further comprises a nickel salt and a phosphate and a second additive, the second additive is used to replace the first additive, and the second additive is polyethylene glycol and 2-amino-4-methylpyridine; the components of the electroplating solution and their contents are adjusted to 10-80 g / L of boric acid, 10-80 g / L of complexing agent, 1-20 g / L of antimony salt, 1-20 g / L of tin salt, 1-20 g / L of nickel salt, 5-60 g / L of phosphate, 0.5-3 g / L of polyethylene glycol and 0.5-2 g / L of 2-amino-4-methylpyridine; Wherein, the nickel salt is sulfate or chloride; the phosphate is sodium dihydrogen hypophosphite or sodium phosphate; the pH value of the electroplating solution is 0.5-4.0; and the working temperature of the electroplating solution is 10-60°C.
5. The tin-antimony-nickel-phosphorus electroplating solution according to claim 4, characterized in that: The components and contents of the electroplating solution are 20 g / L boric acid, 30 g / L citric acid, 4 g / L potassium antimony tartrate, 15 g / L stannous chloride, 20 g / L nickel chloride, 5 g / L phosphate, 3 g / L polyethylene glycol and 2 g / L 2-amino-4-methylpyridine.
6. A method for preparing a tin-antimony-nickel-phosphorus electroplating solution, characterized in that: The method for preparing the tin-antimony-nickel-phosphorus electroplating solution according to claim 4 comprises the following steps: S00, add 10-80 g of boric acid, 10-80 g of a complexing agent, 0.5-3 g / L of polyethylene glycol and 0.5-2 g / L of 2-amino-4-methylpyridine to deionized water, and stir to dissolve to prepare a mixed solution; S10, adjusting the pH of the mixed solution to 1.0-4.0 with hydrochloric acid or sulfuric acid; S20. Add 1-10 g of antimony salt, 1-20 g of tin salt, 1-20 g of nickel salt and 5-60 g of phosphate to the above mixed solution, stir to dissolve, add the remaining amount of deionized water to make the volume to 1 L, adjust the pH of the mixed solution to 0.5-4.0, and obtain a tin-antimony-nickel-phosphorus electroplating solution.
Citation Information
Patent Citations
Method for manufacturing tin-stibium-nickel alloy cathode material of lithium ion battery
CN102332570A
Stabilizer for electroplating brightening tin and tin alloy and preparation method thereof
CN106521570A
Nickel-antimony electroplating liquid and preparing method thereof
CN109680310A
Antimony electroplating solution and preparation method thereof
CN109778259A
Tin or tin-alloy plating liquid, bump forming method, and circuit board production method
CN111788337A