Wafer pad structure and forming method thereof
By adopting the design of high-hardness protective layer and buffer layer in the wafer bonding pad structure, the problem of insufficient performance of the bonding pad structure in the existing technology is solved, the impact resistance and waterproof performance are improved, and the overall performance of the semiconductor structure is improved.
Patent Information
- Application Number
- CN202010814822.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-08-13
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-08-13
AI Technical Summary
The wafer bonding pad structure formed during the packaging process of the existing technology has insufficient structural performance and is susceptible to migration deformation and water vapor entry caused by impact force, affecting the performance of the semiconductor structure.
The pad design adopts a multi-layer structure, including the first and second protective layers, whose hardness is higher than the passivation layer, and a buffer layer is formed on the pad structure to absorb impact force, reduce expansion force and water vapor ingress.
Improves the performance of the semiconductor structure and extends its service life by enhancing the impact resistance and waterproof performance of the pad structure.
Smart Images

Figure CN114078795B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of semiconductor manufacturing, and in particular to a wafer pad structure and a forming method thereof. Background Art
[0002] Wafer Lever BGA (WLBGA) packaging is based on BGA (Ball Grid Array) technology and is an improved and enhanced CSP packaging technology. Wafer-level BGA technology uses wafers as processing objects, packages, ages and tests multiple chips on the wafer at the same time, and then cuts the wafer into a single device, which can be directly mounted on a substrate or printed circuit board.
[0003] Wafer-level BGA technology has the advantages of small package size and supports a wide range of bonding requirements, making the application of wafer-level BGA technology more and more extensive, and the demand for products packaged with wafer-level BGA technology is also increasing.
[0004] However, the performance of the wafer pad structure formed in the packaging process of the prior art still needs to be improved. Summary of the invention
[0005] The technical problem solved by the present invention is to provide a wafer pad structure and a method for forming the same, which can effectively improve the performance of the finally formed semiconductor structure.
[0006] To solve the above problems, the present invention provides a wafer pad structure, comprising: a first substrate, the first substrate comprising a device structure and an electrical interconnection structure; a first passivation layer located on the electrical interconnection structure; a first protective layer located on the first passivation layer, the first passivation layer and the first protective layer having a first opening therein, the first opening exposing the top surface of the electrical interconnection structure; a connecting layer located in the first opening; a pad structure located on the first protective layer and the connecting layer, the connecting layer connecting the pad structure and the electrical interconnection structure; a second protective layer located on the side and top surface of the pad structure; a second passivation layer located on the second protective layer, the second passivation layer and the second protective layer having a second opening therein, the second opening exposing the top surface of the pad structure.
[0007] Optionally, the hardness of the first protection layer and the second protection layer is greater than the hardness of the first passivation layer and the second passivation layer.
[0008] Optionally, the material of the first protective layer includes one or more combinations of silicon nitride, silicon oxynitride, aluminum oxide, strontium oxide, titanium oxide, oxygen-doped silicon nitride, nitrogen-doped silicon carbide and silicon oxide under a low-temperature process; the material of the second protective layer includes one or more combinations of silicon nitride, silicon oxynitride, aluminum oxide, strontium oxide, titanium oxide, oxygen-doped silicon nitride, nitrogen-doped silicon carbide and silicon oxide under a low-temperature process.
[0009] Optionally, the thickness of the first protective layer is 50 angstroms to 1000 angstroms; the thickness of the second protective layer is 50 angstroms to 1000 angstroms.
[0010] Optionally, the pad structure has a thickness of 2500 angstroms to 3500 angstroms.
[0011] Optionally, materials of the first passivation layer and the second passivation layer include silicon oxide and silicon nitride.
[0012] Optionally, the second passivation layer has a thickness of 600 angstroms to 1500 angstroms.
[0013] Optionally, the method further includes: a buffer layer located on the second passivation layer and the pad structure.
[0014] Optionally, the material of the buffer layer includes: a polyimide composite material.
[0015] Optionally, it also includes: a conductive structure, wherein the conductive structure is in contact with the pad structure.
[0016] Optionally, the conductive structure includes: a conductive column or a solder ball.
[0017] Optionally, the conductive pillar includes: a seed layer and a conductive layer located on the seed layer.
[0018] Optionally, the material of the conductive layer includes: copper.
[0019] Optionally, the material of the pad structure includes: aluminum.
[0020] Optionally, it also includes: a second substrate located on the conductive structure.
[0021] Optionally, the device structure includes a transistor, a resistor, an inductor or a capacitor, and the electrical interconnection structure is electrically connected to the device structure.
[0022] Correspondingly, the present invention also provides a method for forming a wafer pad structure, comprising: providing a first substrate, the first substrate comprising a device structure and an electrical interconnection structure; forming an initial first passivation layer on the electrical interconnection structure; forming an initial first protective layer on the initial first passivation layer; performing a first patterning process on the initial first passivation layer and the initial first protective layer to form a first passivation layer and a first protective layer, wherein the first passivation layer and the first protective layer have a first opening, and the first opening exposes the top surface of the electrical interconnection structure; forming a metal layer on the first opening and the first protective layer; performing a second patterning process on the metal layer and the first protective layer to form a pad structure and a connection layer, wherein the connection layer is located in the first opening and the connection layer connects the pad structure and the electrical interconnection structure; forming an initial second protective layer on the side and top surface of the pad structure; forming an initial second passivation layer on the initial second protective layer; performing a third patterning process on the initial second protective layer and the initial second passivation layer to form a second protective layer and a second passivation layer, wherein the second protective layer and the second passivation layer have a second opening, and the second opening exposes the top surface of the pad structure.
[0023] Optionally, the hardness of the first protection layer and the second protection layer is greater than the hardness of the first passivation layer and the second passivation layer.
[0024] Optionally, the material of the first protective layer includes one or more combinations of silicon nitride, silicon oxynitride, aluminum oxide, strontium oxide, titanium oxide, oxygen-doped silicon nitride, nitrogen-doped silicon carbide and silicon oxide under a low-temperature process; the material of the second protective layer includes one or more combinations of silicon nitride, silicon oxynitride, aluminum oxide, strontium oxide, titanium oxide, oxygen-doped silicon nitride, nitrogen-doped silicon carbide and silicon oxide under a low-temperature process.
[0025] Optionally, the thickness of the first protective layer is 50 angstroms to 1000 angstroms; the thickness of the second protective layer is 50 angstroms to 1000 angstroms.
[0026] Optionally, the device structure includes: a transistor, a resistor, an inductor or a capacitor, and the electrical interconnection structure is electrically connected to the device structure.
[0027] Optionally, the pad structure has a thickness of 2500 angstroms to 3500 angstroms.
[0028] Optionally, materials of the first passivation layer and the second passivation layer include silicon oxide and silicon nitride.
[0029] Optionally, the second passivation layer has a thickness of 600 angstroms to 1500 angstroms.
[0030] Optionally, after forming the second passivation layer, the method further includes: forming a buffer layer on a surface of the second passivation layer and a portion of the pad structure.
[0031] Optionally, the material of the buffer layer includes: a polyimide composite material.
[0032] Optionally, after forming the buffer layer, the method further includes: forming a conductive structure on the pad structure, wherein the conductive structure contacts the pad structure.
[0033] Optionally, the conductive structure includes: a conductive column or a solder ball.
[0034] Optionally, the conductive pillar includes: a seed layer and a conductive layer located on the seed layer.
[0035] Optionally, the material of the conductive layer includes: copper.
[0036] Optionally, the material of the pad structure includes: aluminum.
[0037] Optionally, after forming the conductive structure, the method further includes: providing a second substrate; and bonding the first substrate and the second substrate.
[0038] Optionally, the method of bonding the first substrate and the second substrate includes: connecting the second substrate to the conductive structure.
[0039] Compared with the prior art, the technical solution of the present invention has the following advantages:
[0040] In the structure of the technical solution of the present invention, the first protective layer and the second protective layer are located on the surface of the pad structure, and the hardness of the first protective layer and the second protective layer is greater than the hardness of the first passivation layer and the second passivation layer. When the pad structure is subjected to a greater impact force causing migration deformation, the first protective layer and the second protective layer are not easily subjected to a greater expansion force and cracks, thereby reducing the entry of external water vapor, thereby improving the final semiconductor structure.
[0041] Furthermore, it also includes: a buffer layer located on the second passivation layer and the pad structure. Since the buffer layer has good elastic deformation ability, when subjected to a greater impact force, the buffer layer can also absorb part of the impact force, effectively reducing the impact force borne by the pad structure, thereby reducing the expansion force of the pad structure caused by migration deformation, thereby protecting the first protective layer and the second protective layer.
[0042] Furthermore, the thickness of the first protective layer and the second protective layer are both 50 angstroms to 1000 angstroms. When the thickness of the first protective layer and the second protective layer is less than 50 angstroms, the first protective layer and the second protective layer are easily affected by the expansion force and cracks are generated; when the thickness of the first protective layer and the second protective layer is greater than 1000 angstroms, residues are easily formed when etching the initial second protective layer, and the subsequently formed buffer layer cannot completely cover the side wall of the second protective layer, and the buffer layer cannot provide good buffer protection for the second protective layer.
[0043] In the formation method of the technical solution of the present invention, by forming a first protective layer and a second protective layer, the first protective layer and the second protective layer surround the pad structure, and the hardness of the first protective layer and the second protective layer is greater than the hardness of the first passivation layer and the second passivation layer. When the pad structure is subjected to a greater impact force causing migration deformation, the first protective layer and the second protective layer are not easily subjected to a large expansion force and cracks, thereby reducing the entry of external water vapor, thereby improving the final semiconductor structure.
[0044] Furthermore, after forming the second passivation layer, the method further includes: forming a buffer layer on the second passivation layer and the pad structure. Since the buffer layer has good elastic deformation capability, when subjected to a greater impact force, the buffer layer can also absorb a portion of the impact force, effectively reducing the impact force borne by the pad structure, thereby reducing the expansion force of the pad structure caused by migration deformation, thereby protecting the first protective layer and the second protective layer.
[0045] Furthermore, the thickness of the first protective layer and the second protective layer are both 50 angstroms to 1000 angstroms. When the thickness of the first protective layer and the second protective layer is less than 50 angstroms, the first protective layer and the second protective layer are easily affected by the expansion force and cracks are generated; when the thickness of the first protective layer and the second protective layer is greater than 1000 angstroms, residues are easily formed when etching the initial second protective layer, and the subsequently formed buffer layer cannot completely cover the side wall of the second protective layer, and the buffer layer cannot provide good buffer protection for the second protective layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 It is a schematic diagram of the structure of a semiconductor structure;
[0047] Figures 2 to 10 It is a schematic diagram of the structures of the steps of an embodiment of a method for forming a semiconductor structure of the present invention. DETAILED DESCRIPTION
[0048] As described in the background art, the performance of the wafer pad structure formed in the packaging process of the prior art still needs to be improved.
[0049] Please refer to Figure 1 , including: providing a first substrate 100, wherein the first substrate 100 has a device structure 101 and an electrical interconnection structure 102; forming a first passivation layer 103 on the electrical interconnection structure 102; forming a pad structure 104 on the first passivation layer 103, wherein the pad structure 104 is electrically connected to the electrical interconnection structure 102; and forming a second passivation layer 105 on the sidewall and top surface of the pad structure 104.
[0050] In this embodiment, the pad structure 104 is surrounded by the first passivation layer 103 and the second passivation layer 105, and the first passivation layer 103 and the second passivation layer 105 are used to protect the pad structure 104. However, the first passivation layer 103 and the second passivation layer 105 are structurally brittle. As the characteristic size of the semiconductor structure becomes smaller and smaller, when the pad structure 104 is subjected to a larger impact force, the stress generated in the pad structure 104 is also greater, which easily causes the material of the pad structure 104 to migrate and deform, so that the first passivation layer 103 and the second passivation layer 105 surrounding the pad structure 104 are subjected to a larger expansion force and generate microcracks. Due to the existence of the microcracks, external water vapor is easy to contact the pad structure 104 through the microcracks, thereby affecting the performance of the formed semiconductor structure.
[0051] On this basis, the present invention provides a wafer pad structure and a method for forming the same, wherein a first protective layer and a second protective layer are formed, wherein the first protective layer and the second protective layer surround the pad structure, and the hardness of the first protective layer and the second protective layer is greater than the hardness of the first passivation layer and the second passivation layer. Since the hardness of the first protective layer and the second protective layer is greater than the hardness of the first passivation layer and the second passivation layer, when the pad structure undergoes migration deformation due to a greater impact force, the first protective layer and the second protective layer are not easily subject to a greater expansion force and cracks are generated, thereby reducing the entry of external water vapor, thereby improving the semiconductor structure finally formed.
[0052] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0053] Figures 2 to 10 , is a structural schematic diagram of a formation process of a semiconductor structure according to an embodiment of the present invention.
[0054] Please refer to Figure 2, providing a first substrate 200 , wherein the first substrate 200 includes a device structure 202 and an electrical interconnection structure 201 .
[0055] In this embodiment, the material of the first substrate 200 is silicon; in other embodiments, the material of the first substrate may also be germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium.
[0056] In this embodiment, the device structure 202 includes a transistor, a resistor, an inductor or a capacitor, and the electrical interconnection structure 201 is electrically connected to the device structure 202 .
[0057] The material of the electrical interconnection structure 201 includes metal, and the metal includes: tungsten, aluminum, copper, titanium, silver, gold, lead or nickel. In this embodiment, the material of the electrical interconnection structure 201 is copper.
[0058] Please refer to Figure 3 , forming an initial first passivation layer 208 on the electrical interconnect structure.
[0059] In this embodiment, the initial first passivation layer 208 is used to cover the electrical interconnection structure 201 and also to surround the subsequently formed pad structure.
[0060] Please refer to Figure 4 After forming the initial first passivation layer 208, an initial first protective layer (not shown) is formed on the initial first passivation layer 208; the initial first passivation layer 208 and the initial first protective layer are subjected to a first patterning process to form a first passivation layer 203 and a first protective layer 204, wherein the first passivation layer 203 and the first protective layer 204 have a first opening 205, and the first opening 205 exposes the top surface of the electrical interconnect structure 201.
[0061] In this embodiment, the method for the first patterning treatment includes: forming a first patterning layer (not shown) on the initial first protective layer, the first patterning layer exposing a portion of the top surface of the initial first protective layer; etching the initial first protective layer and the initial first passivation layer using the first patterning layer as a mask until the top surface of the electrical interconnection structure 201 is exposed, thereby forming the first passivation layer 203 and the first protective layer 204, the first passivation layer 203 and the first protective layer 204 having a first opening 205 therein, and the first opening 205 exposing the top surface of the electrical interconnection structure 201.
[0062] In this embodiment, the first opening 205 is used to define the position and size of a subsequent connection layer, and the electrical connection between the pad structure and the electrical interconnection structure 201 is achieved through the connection layer.
[0063] Please refer to Figure 5 , forming a metal layer (not shown) on the first opening 205 and the first protective layer 204; performing a second graphic processing on the metal layer and the first protective layer 204 to form a pad structure 209 and a connecting layer 207, wherein the connecting layer 207 is located in the first opening 205, and the connecting layer 207 connects the pad structure 209 and the electrical interconnection structure 201.
[0064] In this embodiment, the second patterning method includes: forming a second patterning layer (not shown) on the metal layer, the second patterning layer exposing a portion of the top surface of the metal layer; etching the metal layer and the first protective layer 204 using the second patterning layer as a mask until the top surface of the first passivation layer 203 is exposed, thereby forming the connecting layer 207 and the pad structure 209.
[0065] In this embodiment, after the connection layer 207 and the pad structure 209 are formed, the second patterned layer is removed.
[0066] In this embodiment, the connection layer 207 and the pad structure 209 are formed simultaneously after the metal layer undergoes a patterning process, which effectively reduces the number of process steps and improves production efficiency.
[0067] In this embodiment, the material of the pad structure 209 is aluminum; the thickness of the pad structure 209 is 2500 angstroms to 3500 angstroms, and the thickness direction is a direction perpendicular to the top surface of the first substrate 200 .
[0068] The material of the first protective layer 204 includes one or more combinations of silicon nitride, silicon oxynitride, aluminum oxide, strontium oxide, titanium oxide, oxygen-doped silicon nitride, nitrogen-doped silicon carbide and silicon oxide in a low temperature process. In this embodiment, the material of the first protective layer 204 is titanium oxide.
[0069] In this embodiment, the hardness of the first protection layer 204 is greater than the hardness of the first passivation layer formed subsequently.
[0070] In this embodiment, the thickness of the first protection layer 204 is 50 angstroms to 1000 angstroms, and the thickness direction is a direction perpendicular to the top surface of the first substrate 200 .
[0071] After forming the first protective layer 204 and the pad structure 209, the method further includes: forming an initial second protective layer on the side and top surface of the pad structure 209; forming an initial second passivation layer on the initial second protective layer; performing a third patterning process on the initial second protective layer and the initial second passivation layer to form a second protective layer and a second passivation layer, wherein the second protective layer and the second passivation layer have a second opening, and the second opening exposes the top surface of the pad structure. For the specific formation process, please refer to Figure 6 to Figure 7 .
[0072] Please refer to Figure 6 , forming an initial second protection layer 210 on the sidewall and top surface of the pad structure 209 ; and forming an initial second passivation layer 211 on the initial second protection layer 210 .
[0073] In this embodiment, the initial second protection layer 210 and the initial second passivation layer 211 are formed by an atomic layer deposition process. The initial second protection layer 210 and the initial second passivation layer 211 formed by the atomic layer deposition process have better uniformity and step coverage.
[0074] Please refer to Figure 7 The initial second protective layer 210 and the initial second passivation layer 211 are subjected to a third graphical processing to form a second protective layer 212 and a second passivation layer 213 , wherein the second protective layer 212 and the second passivation layer 213 have a second opening 214 , and the second opening 214 exposes the top surface of the pad structure 209 .
[0075] In this embodiment, the method of the third graphic processing includes: forming a third graphic layer (not shown) on the initial second passivation layer 211, and the third graphic layer exposes a portion of the top surface of the initial second passivation layer 211; etching the initial second passivation layer 211 and the initial second protective layer 210 using the third graphic layer as a mask until the top surface of the pad structure 209 is exposed, thereby forming the second protective layer 212 and the second passivation layer 213, and the second protective layer 212 and the second passivation layer 213 have a second opening 214 exposing a portion of the top surface of the pad structure 209.
[0076] In this embodiment, after the second protection layer 212 and the second passivation layer 213 are formed, the third patterned layer is removed.
[0077] In this embodiment, the second opening 214 is used to define the position of the subsequent conductive structure, while ensuring that the conductive structure can be electrically connected to the pad structure 209 .
[0078] The material of the second protective layer 212 includes one or more combinations of silicon nitride, silicon oxynitride, aluminum oxide, strontium oxide, titanium oxide, oxygen-doped silicon nitride, nitrogen-doped silicon carbide and silicon oxide in a low temperature process. In this embodiment, the material of the second protective layer 212 is titanium oxide.
[0079] In this embodiment, the hardness of the second protection layer 212 is greater than the hardness of the second passivation layer 213 .
[0080] By forming the first protective layer 204 and the second protective layer 212, the first protective layer 204 and the second protective layer 212 surround the pad structure 209, and the hardness of the first protective layer 204 and the second protective layer 212 is greater than the hardness of the first passivation layer 203 and the second passivation layer 213. Since the hardness of the first protective layer 204 and the second protective layer 212 is greater than the hardness of the first passivation layer 203 and the second passivation layer 213, when the pad structure 209 undergoes migration deformation due to a greater impact force, the first protective layer 204 and the second protective layer 212 are not easily subjected to a greater expansion force and cracks are generated, thereby reducing the entry of external water vapor, thereby improving the final semiconductor structure.
[0081] In this embodiment, the thickness of the second protective layer 212 is 50 angstroms to 1000 angstroms. The thickness direction of the second protective layer 212 located on the side wall of the pad structure 209 is perpendicular to the side wall of the pad structure 209, and the thickness direction of the second protective layer 212 located on the top surface of the pad structure 209 is perpendicular to the top surface of the first substrate 200.
[0082] In this embodiment, the thickness of the first protective layer 204 and the second protective layer 212 are both 50 angstroms to 1000 angstroms. When the thickness of the first protective layer 204 and the second protective layer 212 is less than 50 angstroms, the first protective layer 204 and the second protective layer 212 are easily affected by the expansion force and cracks are generated; when the thickness of the first protective layer 204 and the second protective layer 212 is greater than 1000 angstroms, residues are easily formed when etching the initial second protective layer 210, and the subsequently formed buffer layer cannot completely cover the side walls of the second protective layer 212, and the buffer layer cannot provide good buffer protection for the second protective layer 212.
[0083] In this embodiment, the material of the second passivation layer 213 includes silicon oxide and silicon nitride. The thickness of the second passivation layer 213 is 600 angstroms to 1500 angstroms, and the thickness direction is perpendicular to the side wall of the pad structure 209 .
[0084] Please refer to Figure 8 After forming the second protection layer 212 and the second passivation layer 213, a buffer layer 215 is formed on the second passivation layer 213 and the pad structure 209.
[0085] In this embodiment, the material of the buffer layer 215 is a polyimide composite material.
[0086] Since the buffer layer 215 has good elastic deformation ability, when subjected to a greater impact force, the buffer layer 215 can also absorb part of the impact force, effectively reducing the impact force borne by the pad structure 209, and further reducing the expansion force generated by the migration deformation of the pad structure 209, thereby protecting the first protective layer 204 and the second protective layer 212.
[0087] Please refer to Fig. 9 After the buffer layer 215 is formed, a conductive structure is formed on the pad structure 209 , and the conductive structure is in contact with the pad structure 209 .
[0088] In this embodiment, the conductive structure adopts a conductive column, and the conductive column includes: a seed layer 216 and a conductive layer 206 located on the seed layer 216; in other embodiments, the conductive structure may also adopt a solder ball.
[0089] In this embodiment, the method for forming the seed layer 216 and the conductive layer 206 includes: forming the seed layer 216 in the second opening 214 and on a portion of the top surface of the buffer layer 215 ; and forming the conductive layer 206 on the seed layer 216 using a metal growth process.
[0090] In this embodiment, the seed layer 216 is formed by an atomic layer deposition process.
[0091] In this embodiment, the conductive layer 206 is made of copper.
[0092] Please refer to Fig.10 After forming the conductive structure, providing a second substrate 300; bonding the first substrate 200 and the second substrate 300.
[0093] In this embodiment, the second substrate 300 includes a second device structure and a second electrical interconnection structure (not shown).
[0094] In this embodiment, the material of the second substrate 300 is silicon; in other embodiments, the material of the second substrate may also be germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium.
[0095] In this embodiment, the second device structure includes a transistor, a resistor, an inductor or a capacitor, and the second electrical interconnection structure is electrically connected to the second device structure.
[0096] In this embodiment, the method of bonding the first substrate 200 and the second substrate 300 includes: connecting the second substrate 300 to the conductive structure.
[0097] Correspondingly, an embodiment of the present invention further provides a wafer pad structure, please continue to refer to Fig.10 , comprising: a first substrate 200, the first substrate 200 comprising a device structure 202 and an electrical interconnection structure 201; a first passivation layer 203 located on the electrical interconnection structure 201; a first protective layer 204 located on the first passivation layer 203, the first passivation layer 203 and the first protective layer 204 having a first opening (not marked), the first opening exposing the top surface of the electrical interconnection structure 201; a connection layer 207 located in the first opening; a pad structure 209 located on the first protective layer 204 and the connection layer 207, the connection layer 207 connecting the pad structure 209 and the electrical interconnection structure 201; a second protective layer 212 located on the side and top surface of the pad structure 209; a second passivation layer 213 located on the second protective layer 212, the second passivation layer 213 and the second protective layer 212 having a second opening (not marked), the second opening exposing the top surface of the pad structure 209.
[0098] In this embodiment, the hardness of the first protection layer 204 and the second protection layer 212 is greater than the hardness of the first passivation layer 203 and the second passivation layer 213 .
[0099] The first protective layer 204 and the second protective layer 212 are located on the surface of the pad structure 209, and the hardness of the first protective layer 204 and the second protective layer 212 is greater than the hardness of the first passivation layer 203 and the second passivation layer 213. When the pad structure 209 is subjected to a greater impact force and causes migration deformation, the first protective layer 204 and the second protective layer 212 are not easily subjected to a greater expansion force and cracks, thereby reducing the entry of external water vapor, thereby improving the final semiconductor structure.
[0100] The material of the first protective layer 204 includes: one or more combinations of silicon nitride, silicon oxynitride, aluminum oxide, strontium oxide, titanium oxide, oxygen-doped silicon nitride, nitrogen-doped silicon carbide and silicon oxide under a low-temperature process; in this embodiment, the material of the first protective layer 204 is titanium oxide.
[0101] The material of the second protective layer 212 includes one or more combinations of silicon nitride, silicon oxynitride, aluminum oxide, strontium oxide, titanium oxide, oxygen-doped silicon nitride, nitrogen-doped silicon carbide and silicon oxide in a low temperature process. In this embodiment, the material of the second protective layer 212 is titanium oxide.
[0102] In this embodiment, the thickness of the first protection layer 204 is 50 angstroms to 1000 angstroms; the thickness of the second protection layer 212 is 50 angstroms to 1000 angstroms.
[0103] In this embodiment, the thickness of the pad structure 209 is 2500 angstroms to 3500 angstroms.
[0104] In this embodiment, the materials of the first passivation layer 203 and the second passivation layer 213 include silicon oxide and silicon nitride.
[0105] In this embodiment, the thickness of the second passivation layer 213 is 600 angstroms to 1500 angstroms.
[0106] In this embodiment, the present invention further includes: a buffer layer 215 located on the second passivation layer 213 and the pad structure 209 .
[0107] In this embodiment, the material of the buffer layer 215 is a polyimide composite material.
[0108] Since the buffer layer 215 has good elastic deformation ability, when subjected to a greater impact force, the buffer layer 215 can also absorb part of the impact force, effectively reducing the impact force borne by the pad structure 209, and further reducing the expansion force generated by the migration deformation of the pad structure 209, thereby protecting the first protective layer 204 and the second protective layer 212.
[0109] In this embodiment, it further includes: a conductive structure, wherein the conductive structure is in contact with the pad structure 209 .
[0110] In this embodiment, the conductive structure adopts a conductive column; in other embodiments, the conductive structure may also adopt a solder ball.
[0111] In this embodiment, the conductive pillar includes a seed layer 216 and a conductive layer 206 located on the seed layer 216 .
[0112] In this embodiment, the conductive layer 206 is made of copper.
[0113] In this embodiment, the material of the pad structure 209 is aluminum.
[0114] In this embodiment, it further includes: a second substrate 300 located on the conductive structure.
[0115] In this embodiment, the device structure 202 includes a transistor, a resistor, an inductor or a capacitor, and the electrical interconnection structure 201 is electrically connected to the device structure 202 .
[0116] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A wafer pad structure, characterized in that: include: a first substrate, the first substrate comprising a device structure and an electrical interconnection structure; a first passivation layer located on the electrical interconnect structure; a first protection layer located on the first passivation layer, wherein the first passivation layer and the first protection layer have a first opening therein, and the first opening exposes a top surface of the electrical interconnection structure; a connecting layer located in the first opening; a pad structure located on the first protection layer and the connection layer, wherein the connection layer connects the pad structure and the electrical interconnection structure; A second protective layer located on the side and top surfaces of the pad structure; a second passivation layer located on the second protective layer, wherein the second passivation layer and the second protective layer have a second opening therein, and the second opening exposes a top surface of the pad structure; The hardness of the first protection layer and the second protection layer is greater than the hardness of the first passivation layer and the second passivation layer.
2. The wafer pad structure according to claim 1, characterized in that: The material of the first protective layer includes: one or more combinations of silicon nitride, silicon oxynitride, aluminum oxide, strontium oxide, titanium oxide, oxygen-doped silicon nitride, nitrogen-doped silicon carbide and silicon oxide under low temperature process; the material of the second protective layer includes: one or more combinations of silicon nitride, silicon oxynitride, aluminum oxide, strontium oxide, titanium oxide, oxygen-doped silicon nitride, nitrogen-doped silicon carbide and silicon oxide under low temperature process.
3. The wafer pad structure according to claim 1, characterized in that: The thickness of the first protective layer is 50 angstroms to 1000 angstroms; the thickness of the second protective layer is 50 angstroms to 1000 angstroms.
4. The wafer pad structure according to claim 1, wherein: The thickness of the pad structure is 2500 angstroms to 3500 angstroms.
5. The wafer pad structure according to claim 1, wherein: The materials of the first passivation layer and the second passivation layer include silicon oxide and silicon nitride.
6. The wafer pad structure according to claim 1, wherein: The thickness of the second passivation layer is 600 angstroms to 1500 angstroms.
7. The wafer pad structure according to claim 1, characterized in that: Also includes: A buffer layer is located on the second passivation layer and the pad structure.
8. The wafer pad structure as claimed in claim 7, characterized in that: The material of the buffer layer includes: a polyimide composite material.
9. The wafer pad structure according to claim 1, wherein: Also includes: A conductive structure is in contact with the pad structure.
10. The wafer pad structure according to claim 9, characterized in that: The conductive structure includes: a conductive column or a solder ball.
11. The wafer pad structure according to claim 10, characterized in that: The conductive pillar includes a seed layer and a conductive layer located on the seed layer.
12. The wafer pad structure according to claim 11, characterized in that: The material of the conductive layer includes: copper.
13. The wafer pad structure according to claim 1, wherein: The material of the pad structure includes: aluminum.
14. The wafer pad structure according to claim 9, wherein: Also includes: A second substrate is located on the conductive structure.
15. The wafer pad structure according to claim 1, wherein: The device structure includes a transistor, a resistor, an inductor or a capacitor, and the electrical interconnection structure is electrically connected to the device structure.
16. A method for forming a wafer pad structure, characterized in that: include: Providing a first substrate, the first substrate comprising a device structure and an electrical interconnection structure; forming an initial first passivation layer on the electrical interconnect structure; forming an initial first protective layer on the initial first passivation layer; Performing a first patterning process on the initial first passivation layer and the initial first protection layer to form a first passivation layer and a first protection layer, wherein the first passivation layer and the first protection layer have a first opening therein, and the first opening exposes a top surface of the electrical interconnection structure; forming a metal layer on the first opening and the first protective layer; Performing a second patterning process on the metal layer and the first protective layer to form a pad structure and a connection layer, wherein the connection layer is located in the first opening and connects the pad structure and the electrical interconnection structure; forming an initial second protective layer on the side and top surfaces of the pad structure; forming an initial second passivation layer on the initial second protective layer; Performing a third patterning process on the initial second protection layer and the initial second passivation layer to form a second protection layer and a second passivation layer, wherein the second protection layer and the second passivation layer have a second opening therein, and the second opening exposes the top surface of the pad structure; The hardness of the first protection layer and the second protection layer is greater than the hardness of the first passivation layer and the second passivation layer.
17. The method for forming a wafer pad structure according to claim 16, wherein: The material of the first protective layer includes: one or more combinations of silicon nitride, silicon oxynitride, aluminum oxide, strontium oxide, titanium oxide, oxygen-doped silicon nitride, nitrogen-doped silicon carbide and silicon oxide under low temperature process; the material of the second protective layer includes: one or more combinations of silicon nitride, silicon oxynitride, aluminum oxide, strontium oxide, titanium oxide, oxygen-doped silicon nitride, nitrogen-doped silicon carbide and silicon oxide under low temperature process.
18. The method for forming a wafer pad structure according to claim 16, wherein: The thickness of the first protective layer is 50 angstroms to 1000 angstroms; the thickness of the second protective layer is 50 angstroms to 1000 angstroms.
19. The method for forming a wafer pad structure according to claim 16, wherein: The device structure includes: a transistor, a resistor, an inductor or a capacitor, and the electrical interconnection structure is electrically connected to the device structure.
20. The method for forming a wafer pad structure according to claim 16, wherein: The thickness of the pad structure is 2500 angstroms to 3500 angstroms.
21. The method for forming a wafer pad structure as claimed in claim 16, characterized in that: The materials of the first passivation layer and the second passivation layer include silicon oxide and silicon nitride.
22. The method for forming a wafer pad structure according to claim 16, wherein: The thickness of the second passivation layer is 600 angstroms to 1500 angstroms.
23. The method for forming a wafer pad structure as claimed in claim 16, characterized in that: After forming the second passivation layer, the method further includes: forming a buffer layer on a surface of the second passivation layer and a portion of the pad structure.
24. The method for forming a wafer pad structure as claimed in claim 23, characterized in that: The material of the buffer layer includes: a polyimide composite material.
25. The method for forming a wafer pad structure as claimed in claim 23, characterized in that: After forming the buffer layer, the method further includes: forming a conductive structure on the pad structure, wherein the conductive structure contacts the pad structure.
26. The method for forming a wafer pad structure as claimed in claim 25, characterized in that: The conductive structure includes: a conductive column or a solder ball.
27. The method for forming a wafer pad structure as claimed in claim 26, characterized in that: The conductive pillar includes a seed layer and a conductive layer located on the seed layer.
28. The method for forming a wafer pad structure as claimed in claim 27, characterized in that: The material of the conductive layer includes: copper.
29. The method for forming a wafer pad structure as claimed in claim 16, wherein: The material of the pad structure includes: aluminum.
30. The method for forming a wafer pad structure as claimed in claim 25, characterized in that: After forming the conductive structure, the method further includes: providing a second substrate; and bonding the first substrate and the second substrate.
31. The method for forming a wafer pad structure as claimed in claim 30, characterized in that: The method of bonding the first substrate and the second substrate includes: connecting the second substrate to the conductive structure.