A production process and cold drawing die for a ribbed thin-walled cladding tube
Through multiple drawing processes and machining of thick-walled tubes, combined with twisting to form spiral ribs, the problem of difficulty in matching the thickness of thin-walled ribs and tube wall in the existing technology has been solved, and the high efficiency of ribbed thin-walled cladding tubes has been achieved. production and stable performance.
Patent Information
- Application Number
- CN202111389087.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-22
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-11-22
AI Technical Summary
The existing production process of ribbed thin-walled cladding tubes makes it difficult to process thin-walled ribs and tube walls that meet the requirements. Especially when the rib height is thicker than the tube wall, the plastically deformed metal is difficult to fill, and the solder joints are not resistant to high temperatures and pressures. Easy to fall off.
Thick-walled tubes are drawn through a perforated outer drawing die and a prismatic cylindrical core die. A blank tube with straight ribs on the outer wall and grooves on the inner wall is first formed, and then the cross-section and rib cross-section are reduced through multiple drawings. The thickness of the pipe wall, combined with machine processing to remove the grooves on the inner wall, gradually reaches the finished size, and is twisted to form a spiral rib.
It achieves efficient production of ribbed thin-walled cladding tubes, ensures dimensional accuracy and stable performance, avoids high-temperature and high-pressure problems in solder joints, and improves overall strength.
Smart Images

Figure CN114082803B_ABST
Abstract
Description
Technical field:
[0001] The invention relates to the field of ribbed thin-wall cladding tubes, in particular to a production process and a cold drawing die for ribbed thin-wall cladding tubes. Background technology:
[0002] The fuel assembly of a sodium-cooled fast reactor is mainly composed of a stainless steel cladding tube and a hexagonal outer sleeve. The stainless steel fuel cladding tubes in the hexagonal outer sleeve are isolated from each other by spirally winding stainless steel wires on spot welding. The disadvantage of this isolation method is that the stainless steel welding points are not resistant to high temperature and high pressure, and the welding points are easy to fall off under the erosion of high temperature and high pressure coolant. In addition, the welding points destroy the overall strength of the cladding tube.
[0003] The Chinese patent with authorization announcement number CN203055470U discloses a radially positioned ribbed cladding tube for a fuel rod. The cladding tube is cylindrical in shape as a whole, and its interior is a cavity structure. One or more ribs are distributed on the outer wall of the tube. The ribs are spirally distributed along the axis. The ribs and the tube are an integrated structure, and the cladding tube is isolated and distributed by the spiral ribs.
[0004] The Chinese patent application with publication number CN105723465A discloses a fuel element cladding, which is characterized by an integral tubular element with spirally wound fins (ribs) on the outer wall. The fin height is not less than 0.75 mm, and the wall thickness does not exceed 0.60 mm. The fin height is preferably 0.75 mm, and the tube wall thickness is preferably 0.40 mm.
[0005] The above patent designs a ribbed (finned) cladding tube, but does not mention what process is used to manufacture this cladding tube. Considering the neutron economy and heat transfer effect of nuclear fuel reaction, the wall thickness of this cladding tube is designed to be small, generally less than 0.50mm. However, due to the isolation requirements between fuel cladding tubes, the rib height requirement is relatively high, generally reaching 0.75mm. The cladding tube length is more than 2 meters. This ribbed thin-walled cladding tube with a rib height greater than the wall thickness is difficult to process. Summary of the invention:
[0006] The object of the present invention is to provide a production process and a cold drawing die for a ribbed thin-walled cladding tube, which can efficiently produce the ribbed thin-walled cladding tube, the cladding tube has overall plastic deformation, accurate size and stable performance.
[0007] The technical solution of the present invention is:
[0008] A production process for a ribbed thin-walled clad tube, firstly using a hole-type drawing outer die and a prism-shaped cylindrical core die for forming straight ribs on the outer wall, processing a blank tube with straight ribs on the outer wall and grooves on the inner wall through a first drawing process of a thick-walled tube, and removing the grooves on the inner wall by machining to form a blank tube with straight ribs on the outer wall and a cylindrical shape on the inner wall; then using a hole-type drawing outer die and a cylindrical core die to draw the blank tube, reducing the outer diameter, wall thickness and rib cross section of the blank tube, and processing a thin-walled clad tube with straight ribs that meets the size requirements through one or more drawing processes.
[0009] The production process of the thin-wall cladding tube with ribs further obtains the thin-wall cladding tube with spiral ribs by twisting the thin-wall cladding tube with straight ribs.
[0010] In the production process of the ribbed thin-walled cladding tube, the outer diameter of the thick-walled tube is greater than 3 mm of the outer diameter of the finished ribbed thin-walled cladding tube, and the wall thickness is greater than 1.5 mm of the sum of the outer wall rib height and the wall thickness of the finished ribbed thin-walled cladding tube.
[0011] The production process of the ribbed thin-walled cladding tube, the cold drawing die includes a hole-type drawing outer die and a prismatic cylindrical core die for forming the outer wall straight ribs, the surface of the center hole of the hole-type drawing outer die is divided into a sizing section and an extrusion deformation section, the inner wall of the hole-type drawing outer die is provided with grooves corresponding to the shape of the outer wall straight ribs of the ribbed thin-walled cladding tube, and the rib distribution on the prismatic cylindrical core die is consistent with the groove distribution on the hole-type drawing outer die.
[0012] The production process of the ribbed thin-walled cladding tube is to draw out a blank tube with straight ribs on the outer wall and grooves on the inner wall, wherein the outer straight ribs of the blank tube with straight ribs on the outer wall and grooves on the inner wall correspond to the inner grooves; the hole-type drawing outer die and the ribbed cylindrical core die are adjusted so that the rib grooves of the hole-type drawing outer die are aligned with the straight edges on the ribbed cylindrical core die, the ribbed cylindrical core die is fixed with a connecting rod, and the tube is drawn at a uniform speed by a hydraulic drawing machine or a chain drawing machine, and the drawing speed ranges from 0.5m / min to 3m / min.
[0013] In the production process of the ribbed thin-walled cladding tube, in order to ensure that the metal is fully filled and the ribs are completely formed, the deformation of the blank tube is designed to have an outer diameter reduction greater than or equal to 10% and a wall thickness reduction rate greater than or equal to 10%.
[0014] The production process of the ribbed thin-walled clad tube adopts a machining method to remove the inner wall grooves to form a blank tube with straight ribs on the outer wall, and the straight ribs are retained on the outer side of the blank tube with straight ribs on the outer wall. The blank tube is machined by a reamer or a honing method. When machining the inner wall of the blank tube, the reamer or the honing head is designed to be floating and adapt to the change of the straightness of the blank tube. After machining, the thickness of the blank tube is greater than the wall thickness of the finished ribbed thin-walled clad tube by more than 0.20 mm.
[0015] The production process of the ribbed thin-walled cladding tube adopts a hole-type drawing outer die and a cylindrical core die for drawing. The hole-type drawing outer die has the same structure as the hole-type drawing outer die used in the first pass. The rib groove shape of the hole-type drawing outer die is the same as the straight rib shape. The cross-sectional size of the rib groove of the hole-type drawing outer die is smaller than the cross-sectional size of the rib groove of the hole-type drawing outer die in the first pass. The deformation elongation of the ribs on the blank tube is consistent with the elongation of the blank tube to ensure the overall plastic deformation of the ribs and the blank tube.
[0016] A cold drawing die for a ribbed thin-walled cladding tube, comprising a hole-type drawing outer die and a prism-shaped cylindrical core die for forming straight ribs on the outer wall, the surface of the center hole of the hole-type drawing outer die comprises an extrusion deformation section and a sizing section arranged in sequence, the extrusion deformation section is truncated cone-shaped, the sizing section is cylindrical, the extrusion deformation section and the sizing section are an integrally connected structure, the cross-sections of the extrusion deformation section and the sizing section at the connection are the same, the diameter of the end face of the extrusion deformation section located on the outside is larger than the diameter of the end face of the extrusion deformation section located on the inside; grooves are arranged in the axial direction of the extrusion deformation section and the sizing section, each group of grooves is an integrally connected structure of a rib groove with a uniform cross-section and a transition groove with a variable cross-section, the rib groove runs through the sizing section in the axial direction, the transition groove runs through the extrusion deformation section in the axial direction, the cross-sections of the rib groove and the transition groove at the connection are the same, the diameter of the end face of the transition groove located on the outside is larger than the diameter of the end face of the transition groove located on the inside;
[0017] The ribbed cylindrical core mold is a cylinder of equal diameter. The side of the ribbed cylindrical core mold has straight edges distributed along the circumference. The distribution of the straight edges is consistent with the distribution of the rib grooves and transition grooves of the hole-type drawing outer mold. The shape of the straight edges is consistent with the shape of the straight ribs or is semi-cylindrical; the height of the straight edges is consistent with the depth of the rib grooves of the corresponding hole-type drawing outer mold.
[0018] The cold drawing die of the ribbed thin-walled cladding tube has the same shape of the rib grooves on the sizing section as the straight ribs, and the side taper α of the transition grooves on the extrusion deformation section is 6 to 16 degrees; the number and distribution of the rib grooves and transition grooves are consistent with the number and distribution of the ribs on the outer wall of the ribbed thin-walled cladding tube.
[0019] The advantages and beneficial effects of the present invention are:
[0020] like Figure 1 As shown, the ribbed thin-walled cladding tube 1 can be used for the fuel cladding of a nuclear reactor with a liquid metal coolant, and can also be used in other heat transfer and heat exchange equipment. The ribbed thin-walled cladding tube 1 is an integral tubular element, and the outer wall is spirally surrounded by ribs 11. It is characterized by a thin tube wall, a large ratio of outer diameter to wall thickness, and a large rib height, which is greater than the wall thickness of the ribbed thin-walled cladding tube 1.
[0021] With respect to this type of thin-walled high-rib cladding tube, the problems existing in the existing production technology are analyzed. The height of the ribs is greater than the wall thickness of the cladding tube. Whether it is extrusion, drawing or rolling, it is difficult for the plastically deformed metal to fill the mold, and it is difficult to process the ribs (fins) and tube walls that meet the required size at one time. The present invention proposes to use a thick-walled tube, and use a hole-type drawing outer die and a prism-shaped cylindrical core die to first draw out a blank tube with straight ribs on the outer wall and grooves on the inner wall. The height and width of the ribs are greater than the height and width of the ribs of the finished ribbed thin-walled cladding tube, and the thickness of the thick-walled tube is also greater than the thickness of the finished ribbed thin-walled cladding tube. Use a reamer or a grinding head machine to grind the inner wall of the tube and remove the grooves to obtain a blank tube with a smooth inner wall. Then use a hole-type drawing outer die and a cylindrical core die to draw, which can be done once or multiple times, gradually reducing the cross-section of the ribs, reducing the outer diameter and wall thickness of the blank tube, and finally reaching the size of the finished ribbed thin-walled cladding tube, obtaining a thin-walled cladding tube with straight ribs, and twisting the thin-walled cladding tube with straight ribs to form a cladding tube with spiral ribs. Description of the drawings:
[0022] Figure 1 The cross-sectional structure diagram of the ribbed thin-walled cladding tube is shown in FIG. 1 , ribbed thin-walled cladding tube, and 11 ribs.
[0023] Figure 2 The cross-sectional structure diagram of the drawn blank tube with straight ribs on the outer wall and grooves on the inner wall is shown in FIG. 2 , the blank tube with straight ribs on the outer wall and grooves on the inner wall, 21 is the straight rib, and 22 is the groove.
[0024] Figure 3 The cross-sectional structure diagram of the outer wall straight rib blank tube after the inner wall groove is removed by machining. In the figure, 3 is the outer wall straight rib blank tube, 31 is the straight rib.
[0025] Fig. 4 is a schematic diagram of the drawing outer die structure with two grooves, wherein Fig. 4(a) is a front view, and Fig. 4(b) is a side cross-sectional view. In the figure, 4 is a hole-type drawing outer die, 41 is an extrusion deformation section, 42 is a sizing section, 43 is a rib groove, and 44 is a transition groove.
[0026] Fig. 5 is a schematic diagram of the structure of a cylindrical core mold with edges, wherein Fig. 5(a) is a front view and Fig. 5(b) is a top view. In the figure, 5 is a cylindrical core mold with edges, and 51 is a straight edge.
[0027] Figure 6 This is a physical picture of a thin-walled cladding tube with two ribs (before twisting). Specific implementation method:
[0028] In the specific implementation process, the cold drawing die of the present invention includes a hole-type drawing outer die and a prism-shaped cylindrical core die for forming the outer wall straight ribs. The surface of the center hole of the hole-type drawing outer die is divided into a sizing section and an extrusion deformation section. The inner wall of the hole-type drawing outer die is provided with grooves corresponding to the shape of the outer wall straight ribs of the ribbed thin-walled cladding tube. The distribution of the edges on the prism-shaped cylindrical core die is consistent with the distribution of the grooves on the hole-type drawing outer die. First, a blank tube with straight ribs on the outer wall and grooves on the inner wall is processed by drawing a thick-walled tube. The inner wall grooves are removed by a reamer or a grinding head to form a blank tube with straight ribs on the outer wall and a cylindrical inner wall. Then, the hole-type drawing outer die and the cylindrical core die are used to draw the blank tube to reduce the outer diameter, wall thickness and cross-section of the ribs of the blank tube. Through one or more drawing, a thin-walled cladding tube with straight ribs that meets the requirements is processed. Furthermore, a thin-walled cladding tube with spiral ribs can be obtained by twisting a thin-walled cladding tube with straight ribs.
[0029] like Figure 1-Figure 6 As shown, the production process of the ribbed thin-walled cladding tube of the present invention is as follows:
[0030] 1. Thick-walled tube, the outer diameter is more than 3mm larger than the outer diameter of the finished ribbed thin-walled cladding tube, and the wall thickness is more than 1.5mm larger than the sum of the outer wall rib height and wall thickness of the finished ribbed thin-walled cladding tube. Because it is necessary to extrude and deform the rib height on the thick-walled tube billet, and remove the inner wall groove, and then use the hole-type drawing outer die and cylindrical core die to draw the billet tube to reduce the outer diameter and wall thickness of the billet tube, so the thick-walled tube is designed to have sufficient outer diameter and wall thickness.
[0031] 2. If Figure 2 As shown in Fig. 4-Fig. 5, a cold drawing die for processing a ribbed thin-walled cladding tube comprises a hole-type drawing outer die 4 and a prism-shaped cylindrical core die 5 for forming the outer wall straight ribs 21. The center hole surface of the hole-type drawing outer die 4 comprises an extrusion deformation section 41 and a sizing section 42 arranged in sequence, the extrusion deformation section 41 is truncated cone-shaped, the sizing section 42 is cylindrical, the extrusion deformation section 41 and the sizing section 42 are an integral connection structure, the cross-section of the connection between the extrusion deformation section 41 and the sizing section 42 is the same, and the diameter of the end face of the extrusion deformation section 41 located on the outside is larger than the diameter of the end face of the extrusion deformation section 41 located on the inside. Grooves are axially arranged on the extrusion deformation section 41 and the sizing section 42. Each group of grooves is an integrally connected structure of a rib groove 43 with a uniform cross-section and a transition groove 44 with a variable cross-section. The rib groove 43 axially penetrates the sizing section 42, and the transition groove 44 axially penetrates the extrusion deformation section 41. The cross-sections of the rib groove 43 and the transition groove 44 at the connection are the same, and the end face diameter of the transition groove 44 on the outside is larger than the end face diameter of the transition groove 44 on the inside.
[0032] The rib groove 43 on the sizing section 42 is consistent with the shape of the straight rib 21, and the side taper α of the transition groove 44 on the extrusion deformation section 41 is 6 degrees to 16 degrees. The number and distribution of the rib grooves 43 and the transition grooves 44 are consistent with the number and distribution of the ribs on the outer wall of the ribbed thin-walled cladding tube 1. In this embodiment, the cross section of the rib groove 43 on the sizing section 42 can be semi-cylindrical, and the cross section of the transition groove 44 on the extrusion deformation section 41 can be semi-conical.
[0033] The ribbed cylindrical core mold 5 is a cylinder of equal diameter, and the side of the ribbed cylindrical core mold 5 is distributed with straight edges 51 along the circumference, and the distribution of the straight edges 51 is consistent with the distribution of the rib grooves 43 and the transition grooves 44 of the hole-type drawing outer mold 4. The shape of the straight edges 51 can be consistent with the shape of the straight ribs 21, or it can be semi-cylindrical. The height of the straight edges 51 is consistent with the depth of the rib grooves 43 of the corresponding hole-type drawing outer mold 4. The function of the straight edges 51 is to squeeze the metal inside the thick-walled tube so that it enters the rib grooves 43 of the hole-type drawing outer mold 4 to form straight ribs 21, and at the same time form grooves 22 in the thick-walled tube.
[0034] 3. If Figure 2 As shown, a blank tube 2 with straight ribs on the outer wall and grooves on the inner wall is drawn out, and the outer straight ribs 21 of the blank tube 2 with straight ribs on the outer wall and grooves on the inner wall correspond to the inner grooves 22. The thick-walled tube blank is lubricated, and the hydraulic press head is used to reduce the end diameter. The reduction amount is greater than 3mm, and the length of the diameter reduction section is 150mm. Adjust the hole-type drawing outer die 4 and the ribbed cylindrical core die 5 so that the rib groove 43 of the hole-type drawing outer die 4 is aligned with the straight edge 51 on the ribbed cylindrical core die 5, and the ribbed cylindrical core die 5 is fixed with a connecting rod. Use a hydraulic drawing machine or a chain drawing machine to draw at a uniform speed, and the appropriate speed range is 0.5m / min to 3m / min. In order to ensure that the metal is fully filled and the ribs are completely formed, the deformation of the blank tube is designed to have an outer diameter reduction greater than or equal to 10%, and a wall thickness reduction rate greater than or equal to 10%.
[0035] 4. If Figure 3 As shown, the inner wall groove is removed by machining to form a blank tube 3 with straight ribs on the outer wall. The outer side of the blank tube 3 with straight ribs on the outer wall retains straight ribs 31. The blank tube 3 can be machined by reaming or honing. When machining the inner wall of the blank tube, the reamer or honing head is designed to be floating, which can adapt to the change of the straightness of the blank tube. The thickness of the blank tube after machining is greater than the wall thickness of the finished ribbed thin-walled cladding tube by more than 0.20 mm. A certain amount of wall thickness is left to prepare for the subsequent cylindrical core die drawing.
[0036] 5. Use a hole-type drawing outer die and a cylindrical core die for drawing. The core die of this drawing pass has no edges and is a cylindrical smooth die. The purpose of drawing is to reduce the outer diameter and wall thickness of the blank tube and reduce the cross section of the ribs. The hole-type drawing outer die has the same structure as the first pass. The hole-type drawing outer die has rib grooves and transition grooves. The shape of the rib grooves is the same as the shape of the ribs. The cross-sectional size of the rib grooves of this pass is slightly smaller than the cross-sectional size of the rib grooves of the first pass hole-type drawing outer die. The specific design principle is: the deformation elongation of the ribs on the blank tube is consistent with the elongation of the blank tube to ensure the overall plastic deformation of the ribs and the blank tube. During the drawing process, the ribs on the blank tube move forward with the tube in the rib grooves, and the ribs will only deform after the inner wall of the blank tube contacts the core die. After drawing, the outer diameter and wall thickness of the blank tube are reduced respectively, and the tube wall becomes uniform under the extrusion deformation of the outer die and the core die. The shape of the ribs remains unchanged, and the cross-sectional size becomes smaller.
[0037] 6. If Figure 6 As shown, the actual thin-wall cladding tube with straight ribs is formed by twisting the thin-wall cladding tube with straight ribs to form a thin-wall cladding tube with spiral ribs.
[0038] Below, the present invention is further described in detail by examples.
[0039] Example
[0040] In this embodiment, the production process of the ribbed thin-walled cladding tube is as follows:
[0041] 1. Thick-walled tube, material: 1Cr18Ni9Ti stainless steel, size (outer diameter * wall thickness): 27.3*2.5mm. Lubricate, press head, prepare for drawing.
[0042] 2. The inner wall of the 25mm diameter hole-type drawing die is provided with two rib grooves, which are 180 degrees apart and 1mm deep. The outer wall of the 21mm diameter cylindrical core die is provided with two straight edges, which are 180 degrees apart and are in the shape of a semi-cylinder with a radius of 1mm.
[0043] 3. Pull out a blank tube with straight ribs on the outer wall and grooves on the inner wall. The outer diameter of the blank tube is 25mm, the inner diameter is 21mm, the wall thickness of the blank tube is 2.0mm, there are 2 straight ribs, and the rib height is 1mm. There are 2 straight grooves on the inner wall of the blank tube, with a depth of 1mm.
[0044] 4. Use a floating reamer to add inner wall. First straighten the blank tube, then use a floating reamer to add chip remover, divided into 4 processing, each processing amount is 0.25mm. After processing, the blank tube has an outer diameter of 25mm, an inner diameter of 23mm, a wall thickness of 1mm, a smooth inner wall, and a rib height of 1mm.
[0045] 5. The first drawing with hole-type drawing outer die and cylindrical core die. The diameter of the hole-type drawing outer die is 22mm, with 2 rib grooves and a groove depth of 0.92mm. The core die is cylindrical, without edges, and has a diameter of 20.4mm. After drawing, the outer diameter of the blank tube is 22mm, the inner diameter is 20.40mm, the wall thickness is 0.80mm, there are 2 straight ribs, and the rib height is 0.92mm.
[0046] 6. The second drawing with hole-type drawing outer die and cylindrical core die. The diameter of the hole-type drawing outer die is 19mm, with 2 rib grooves and a groove depth of 0.88mm. The cylindrical core die has no edges and a diameter of 17.50mm. After drawing, the billet tube has an outer diameter of 19mm, an inner diameter of 17.50mm, a wall thickness of 0.75mm, 2 straight ribs, and a rib height of 0.88mm.
[0047] 7. The third drawing with hole-type drawing outer die and cylindrical core die. The diameter of the hole-type drawing outer die is 17mm, with 2 rib grooves and a groove depth of 0.82mm. The cylindrical core die has no edges and a diameter of 15.70mm. After drawing, the billet tube has an outer diameter of 17mm, an inner diameter of 15.70mm, a wall thickness of 0.65mm, 2 straight ribs, and a rib height of 0.82mm.
[0048] 8. The fourth drawing with hole-type drawing outer die and cylindrical core die. The diameter of the hole-type drawing outer die is 15mm, with 2 rib grooves and a groove depth of 0.79mm. The cylindrical core die has no edges and a diameter of 13.80mm. After drawing, the blank tube has an outer diameter of 15mm, an inner diameter of 13.80mm, a wall thickness of 0.60mm, 2 straight ribs, and a rib height of 0.79mm.
[0049] 9. The fifth drawing with hole-type drawing outer die and cylindrical core die. The diameter of the hole-type drawing outer die is 13mm, with 2 rib grooves and a groove depth of 0.76mm. The cylindrical core die has no edges and a diameter of 11.90mm. After drawing, the outer diameter of the billet tube is 13mm, the inner diameter is 11.90mm, the wall thickness is 0.55mm, there are 2 straight ribs, and the rib height is 0.76mm.
[0050] 10. The sixth drawing with hole-type drawing outer die and cylindrical core die. The diameter of the hole-type drawing outer die is 12mm, with 2 rib grooves and a groove depth of 0.72mm. The cylindrical core die has no edges and a diameter of 11.0mm. After drawing, the outer diameter of the blank tube is 12mm, the inner diameter is 11.0mm, the wall thickness is 0.50mm, there are 2 straight ribs, and the rib height is 0.72mm. The thin-walled cladding tube with straight ribs that meets the requirements is processed.
[0051] 11. Twisting spiral line. The diameter of the hole-type drawing outer die is 12mm, with 2 rib grooves and a groove depth of 0.72mm. The cylindrical core die has no edges and a diameter of 11.0mm. The linear drawing speed is 700mm / min, and the rotation speed of the thin-walled cladding tube with straight ribs is 360 degrees / min. The spiral line with a pitch of 700mm is twisted to obtain a thin-walled cladding tube with spiral ribs.
[0052] In the present invention, the cladding tube material can be stainless steel, zirconium and zirconium alloy, ferrite martensitic alloy steel, oxide dispersion enhanced iron-chromium-aluminum stainless steel, but is not limited to the above materials. The processing flow of the present invention is suitable for a cladding tube with a ribbed outer wall and a smooth inner wall, and the outer wall can have one rib or more than two ribs.
Claims
1. A production process for a ribbed thin-walled cladding tube, characterized in that: Firstly, a hole-type drawing outer die and a cylindrical core die with prisms for forming straight ribs on the outer wall are used to process a blank tube with straight ribs on the outer wall and grooves on the inner wall through the first drawing of a thick-walled tube, and the grooves on the inner wall are removed by machining to form a blank tube with straight ribs on the outer wall and a cylindrical inner wall; then, a hole-type drawing outer die and a cylindrical core die are used to draw the blank tube, and the outer diameter, wall thickness and cross section of the ribs of the blank tube are reduced, and a thin-walled cladding tube with straight ribs that meets the requirements is processed through one or more drawing passes; The outer diameter of the thick-walled tube is more than 3mm larger than the outer diameter of the finished ribbed thin-walled cladding tube, and the wall thickness is more than 1.5mm larger than the sum of the outer wall rib height and wall thickness of the finished ribbed thin-walled cladding tube; The cold drawing die used in the production process includes a hole-type drawing outer die and a prismatic cylindrical core die for forming the outer wall straight ribs. The surface of the center hole of the hole-type drawing outer die is divided into a sizing section and an extrusion deformation section. The inner wall of the hole-type drawing outer die is provided with grooves corresponding to the shape of the straight ribs of the outer wall of the ribbed thin-walled cladding tube. The distribution of the ribs on the prismatic cylindrical core die is consistent with the distribution of the grooves on the hole-type drawing outer die. Drawing out a blank tube with straight ribs on the outer wall and grooves on the inner wall, wherein the outer straight ribs of the blank tube with straight ribs on the outer wall and grooves on the inner wall correspond to the inner grooves; adjusting the hole-type drawing outer die and the ribbed cylindrical core die so that the rib grooves of the hole-type drawing outer die are aligned with the straight edges on the ribbed cylindrical core die, the ribbed cylindrical core die is fixed with a connecting rod, and the tube is drawn at a uniform speed by a hydraulic drawing machine or a chain drawing machine, and the drawing speed ranges from 0.5 m / min to 3 m / min; The surface of the center hole of the hole-type drawing outer die includes an extrusion deformation section and a sizing section arranged in sequence, the extrusion deformation section is a truncated cone, the sizing section is a cylindrical section, the extrusion deformation section and the sizing section are an integrally connected structure, the cross-section of the extrusion deformation section and the sizing section at the connection is the same, and the diameter of the end face of the extrusion deformation section located on the outside is larger than the diameter of the end face of the extrusion deformation section located on the inside; the extrusion deformation section and the sizing section are provided with grooves along the axial direction, and each group of grooves is an integrally connected structure of a rib groove with a uniform cross-section and a transition groove with a variable cross-section, the rib groove runs through the sizing section along the axial direction, and the transition groove runs through the extrusion deformation section along the axial direction, the cross-section of the rib groove and the transition groove at the connection is the same, and the diameter of the end face of the transition groove located on the outside is larger than the diameter of the end face of the transition groove located on the inside; The ribbed cylindrical core mold is a cylinder of equal diameter. The side of the ribbed cylindrical core mold has straight edges distributed along the circumference. The distribution of the straight edges is consistent with the distribution of the rib grooves and transition grooves of the hole-type drawing outer mold. The shape of the straight edges is consistent with the shape of the straight ribs or is semi-cylindrical; the height of the straight edges is consistent with the depth of the rib grooves of the corresponding hole-type drawing outer mold.
2. The production process of the ribbed thin-walled cladding tube according to claim 1, characterized in that: Furthermore, a thin-walled cladding tube with spiral ribs is obtained by twisting the thin-walled cladding tube with straight ribs.
3. The production process of the ribbed thin-walled cladding tube according to claim 1, characterized in that: In order to ensure that the metal is fully filled and the ribs are completely formed, the deformation of the billet tube is designed to have an outer diameter reduction greater than or equal to 10% and a wall thickness reduction rate greater than or equal to 10%.
4. The production process of the ribbed thin-walled cladding tube according to claim 1, characterized in that: The inner wall grooves are removed by machining to form a blank tube with straight ribs on the outer wall. The straight ribs are retained on the outer side of the blank tube with straight ribs on the outer wall. The blank tube is machined by reamer processing or honing. When machining the inner wall of the blank tube, the reamer or honing head is designed to be floating and adapt to the change of the straightness of the blank tube. After machining, the thickness of the blank tube is greater than the wall thickness of the finished ribbed thin-wall cladding tube by more than 0.20 mm.
5. The production process of the ribbed thin-walled cladding tube according to claim 1, characterized in that: Drawing is performed using a hole-type drawing outer die and a cylindrical core die, the hole-type drawing outer die has the same structure as the hole-type drawing outer die used in the first pass, the rib groove shape of the hole-type drawing outer die is the same as the straight rib shape, and the rib groove cross-sectional size of the hole-type drawing outer die is smaller than the rib groove cross-sectional size of the hole-type drawing outer die in the first pass; the deformation elongation of the ribs on the blank tube is consistent with the elongation of the blank tube to ensure the overall plastic deformation of the ribs and the blank tube.
6. The production process of the ribbed thin-walled cladding tube according to claim 1, characterized in that: The rib grooves on the sizing section are consistent with the shape of the straight ribs, and the side taper α of the transition grooves on the extrusion deformation section is 6 to 16 degrees; the number and distribution of the rib grooves and transition grooves are consistent with the number and distribution of the ribs on the outer wall of the ribbed thin-walled cladding tube.
Citation Information
Patent Citations
Fuel rod cladding, fuel rod and fuel assembly
CN105723465A
Ribbed cladding tube for radial location of fuel rod
CN203055470U
Combined cutter system for outer finned pipe processing
CN106734337A
Bidirectional intermittent differential upsetting composite extrusion forming method for outer longitudinal rib cylindrical piece
CN112517816A
Spiral rib cladding tube torsion forming device and method
CN113500112A
Cited By
Fuel cladding covered by a mesh
US12700515B2
Fuel cladding covered by a mesh
US20230368931A1