Composite electrode material for electrolysis of water to produce hydrogen and preparation method thereof
By loading ruthenium nanoclusters on a molybdenum carbide-nitrogen-doped carbon skeleton, a composite electrode material with a three-dimensional ordered macroporous structure is formed, which solves the scarcity and catalytic instability problems of platinum-based electrocatalysts and achieves rapid hydrogen production. The improvement of precipitation and catalyst performance provides an efficient and stable electrochemical hydrogen production method.
Patent Information
- Application Number
- CN202111554822.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-17
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-12-17
AI Technical Summary
The scarcity, high cost and catalytic instability of existing platinum-based electrocatalysts limit the wide application of electrochemical hydrogen production, and the inconvenient release of hydrogen under alkaline conditions leads to a decrease in catalyst performance.
Molybdenum carbide-nitrogen-doped carbon skeleton is used to support ruthenium nanoclusters to form a composite electrode material with a three-dimensional ordered macroporous structure. It is prepared by suction filtration and high-temperature annealing, which provides a continuous precipitation path for hydrogen and promotes the synergistic effect of the catalyst.
It achieves rapid hydrogen evolution and improved catalyst performance. It has abundant active sites and good stability. The process is simple and its performance is better than that of commercial catalysts. It provides the possibility for large-scale production of new electrode materials for hydrogen production by electrolysis of water.
Smart Images

Figure CN114086208B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inorganic nanocomposite materials, and in particular to a composite electrode material for producing hydrogen by electrolyzing water and a preparation method thereof. Background Art
[0002] Hydrogen has a high combustion enthalpy and emits no carbon during combustion, making it a very promising sustainable clean energy source. Electrocatalytic water splitting technology is an important method for producing hydrogen. At present, the commercial electrode materials used for hydrogen production by this technology are platinum-based electrocatalysts. However, the scarcity, high cost and catalytic instability of platinum limit its widespread application. The development of alternatives with high economic benefits and high performance is considered to be an important way to solve the large-scale application of electrochemical hydrogen production catalysts. The price of ruthenium is about 5% of platinum, and it has a similar metal-hydrogen bond and obvious hydrogen production activity as platinum. Therefore, it is of great significance to optimize ruthenium-based catalysts to achieve or even exceed the performance of platinum-based catalysts, but there are great challenges.
[0003] Under alkaline conditions, the electrocatalytic hydrogen production process includes the dissociation of water molecules to form hydrogen adsorbed on the catalyst surface and the desorption of adsorbed hydrogen from the catalyst surface to release hydrogen molecules. Therefore, the development of multiphase catalysts to exert the synergistic effect between catalysts can promote the entire catalytic process. At the same time, if there is no convenient gas channel for hydrogen molecules to overflow from the catalyst surface in time after release, hydrogen will cover some active sites, thereby affecting the performance of the catalyst. Therefore, constructing gas escape channels through morphology engineering is crucial to improving the performance of catalysts.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The purpose of the present invention is to provide a composite electrode material for producing hydrogen by electrolysis of water and a preparation method thereof. The composite electrode material provided in the embodiment of the present invention can provide a continuous path for the precipitation of hydrogen in the process of electrocatalytic hydrogen production, which is conducive to the rapid precipitation of hydrogen.
[0006] The present invention is achieved in that:
[0007] In a first aspect, the present invention provides a composite electrode material for electrolyzing water to produce hydrogen, wherein the composite electrode material comprises a molybdenum carbide-nitrogen doped carbon skeleton and transition metal nanoclusters supported on the molybdenum carbide-nitrogen doped carbon skeleton.
[0008] In an optional embodiment, the transition metal nanoclusters are ruthenium nanoclusters;
[0009] Preferably, the composite electrode material has a three-dimensional ordered macroporous structure;
[0010] Preferably, the pore size of the three-dimensional ordered macroporous structure is 180-450 nm.
[0011] In a second aspect, the present invention provides a method for preparing a composite electrode material for electrolyzing water to produce hydrogen as described in the aforementioned embodiment, comprising: loading transition metal nanoclusters on a molybdenum carbide-nitrogen doped carbon skeleton.
[0012] In an optional embodiment, the preparation step of the molybdenum carbide-nitrogen doped carbon skeleton comprises: impregnating a molybdenum salt into a polystyrene template by a suction filtration method, and then performing high temperature annealing to form a molybdenum carbide-nitrogen doped carbon skeleton;
[0013] Preferably, the preparation steps of the molybdenum carbide-nitrogen doped carbon skeleton include: immersing the molybdenum salt into the polystyrene template by suction filtration, and then drying it, and then annealing it at high temperature in a mixed gas atmosphere of reducing gas-inert gas to form the molybdenum carbide-nitrogen doped carbon skeleton.
[0014] In an optional embodiment, the molybdenum carbide-nitrogen doped carbon skeleton has a three-dimensional ordered macroporous structure;
[0015] Preferably, the molybdenum salt is ammonium molybdate solution;
[0016] Preferably, the concentration of the ammonium molybdate solution is 2-5 mmol / ml;
[0017] Preferably, the thickness of the polystyrene template is 1-10 mm;
[0018] Preferably, the reducing gas in the mixed gas is hydrogen, and the inert gas in the mixed gas is argon;
[0019] Preferably, the volume of the reducing gas in the mixed gas is 5-20%; the flow rate of the mixed gas is 50-200 ml / min;
[0020] Preferably, the high temperature annealing is performed at a temperature of 650-850° C., for a time of 2-5 hours, and at a heating rate of 2-10° C. / min.
[0021] In an optional embodiment, the step of preparing the polystyrene template comprises: mixing treated styrene, a surfactant, an initiator and a solvent to form a monodisperse polystyrene microsphere emulsion, and then filtering;
[0022] Preferably, the preparation step of the polystyrene template comprises: mixing the treated styrene with water, adding a surfactant, and then heating under an inert gas atmosphere, then adding a solution containing an initiator, reacting at a constant temperature to form a monodisperse polystyrene microsphere emulsion, and then filtering.
[0023] In an optional embodiment, the surfactant is selected from N-vinylamide polymers, preferably polyvinyl pyrrolidone;
[0024] Preferably, the inert gas is selected from nitrogen;
[0025] Preferably, the initiator is an oxidizing agent, preferably potassium persulfate;
[0026] Preferably, the temperature of the mixed reaction is 60-95°C, and the stirring speed is 300-600 rpm / min;
[0027] Preferably, the concentration of the solution containing the initiator is 2-20 mg / ml;
[0028] Preferably, the volume ratio of the styrene, water and the solution containing the initiator is: 1:(5-15):1;
[0029] Preferably, the amount of the surfactant used is 0.1-3 times the amount of the initiator used.
[0030] In an optional embodiment, the styrene treatment process includes: removing a stabilizer from the styrene feedstock;
[0031] Preferably, the treatment process of styrene comprises: mixing the styrene raw material with a strong alkaline solution to remove the stabilizer in the styrene raw material, and then washing with water to remove the strong alkaline;
[0032] Preferably, the ethylene treatment process comprises: mixing the styrene raw material with a sodium hydroxide solution to remove the stabilizer in the styrene raw material, and then washing with water to remove the sodium hydroxide.
[0033] In an optional embodiment, the loading process includes: loading the transition metal nanoclusters on the molybdenum carbide-nitrogen doped carbon skeleton by a reduction method;
[0034] Preferably, the loading process comprises: mixing a ruthenium salt, a molybdenum carbide-nitrogen doped carbon framework and a reducing agent, followed by separation and calcination;
[0035] Preferably, the loading process includes: mixing and dispersing the ruthenium salt and the molybdenum carbide-nitrogen doped carbon skeleton to form a suspension, placing the suspension at 0-4°C, then adding a reducing agent and stirring and mixing, and then centrifuging to form an intermediate, and then calcining the intermediate in an inert gas atmosphere.
[0036] In an optional embodiment, the ruthenium salt is RuCl3;
[0037] Preferably, the reducing agent comprises: sodium borohydride;
[0038] Preferably, the mass ratio of the ruthenium salt to the molybdenum carbide-nitrogen doped carbon skeleton is 5-30:100, and the mass ratio of the ruthenium salt to the reducing agent is 0.1-0.6:1;
[0039] Preferably, the centrifugal speed is 8000-15000 rpm / min;
[0040] Preferably, the inert gas includes nitrogen or argon, and the flow rate of the inert gas is 50 to 200 ml / min;
[0041] Preferably, the calcination conditions include: temperature of 250-450°C, time of 0.5-2 hours, and heating rate of 2-10°C.
[0042] The present invention has the following beneficial effects: the composite electrode material provided by the embodiment of the present invention can provide a continuous path for the precipitation of hydrogen in the process of electrocatalytic hydrogen production, which is conducive to the rapid precipitation of hydrogen. At the same time, the composite electrode material has abundant active sites, and ruthenium and molybdenum carbide can form a synergistic effect to jointly promote the kinetics of electrocatalytic hydrogen production. The preparation method provided by the embodiment of the present invention has a simple process and is easy to operate. The performance of the obtained material is better than that of commercial catalysts, which provides the possibility for large-scale production of new water electrolysis hydrogen production electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0044] Figure 1 This is a SEM image of the polystyrene template prepared in Example 1 of the present invention;
[0045] Figure 2 This is a SEM image of the Ru / Mo2C@NC composite electrode material prepared in Example 1 of the present invention;
[0046] Figure 3 This is the XRD pattern of the Ru / Mo2C@NC composite electrode material prepared in Example 1 of the present invention;
[0047] Figure 4 This is a comparison diagram of polarization curves of Ru / Mo2C@NC prepared in Example 1 of the present invention and commercial Pt / C catalyst in 1M KOH electrolyte;
[0048] Figure 5 This is a diagram showing the electrocatalytic hydrogen production stability of Ru / Mo2C@NC prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0049] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0050] The embodiment of the present invention provides a method for preparing a composite electrode material for electrolyzing water to produce hydrogen, comprising:
[0051] S1, preparing a polystyrene template;
[0052] First, the stabilizer in the styrene raw material is removed; specifically, the styrene raw material is mixed with a strong alkali solution to remove the stabilizer in the styrene raw material, and then water is used to wash to remove the strong alkali; wherein the strong alkali is sodium hydroxide.
[0053] The treated styrene, surfactant, initiator and solvent are mixed to react to form a monodisperse polystyrene microsphere emulsion, which is then filtered; specifically, the treated styrene is mixed with water, a surfactant is added, and then heated under an inert gas atmosphere, and then a solution containing an initiator is added, and the monodisperse polystyrene microsphere emulsion is reacted at a constant temperature to form a monodisperse polystyrene microsphere emulsion, and then the monodisperse polystyrene microsphere emulsion is filtered using a vacuum filtration device and a filter membrane for 1-2 hours to form a polystyrene template.
[0054] Wherein, the surfactant is selected from N-vinylamide polymers, preferably polyvinyl pyrrolidone; the inert gas is selected from nitrogen; the initiator is an oxidant, preferably potassium persulfate; the concentration of the solution containing the initiator is 2-20 mg / ml; the temperature of the mixed reaction is 60-95°C, and the stirring speed is 300-600 rpm / min; the volume ratio of styrene, water and the solution containing the initiator is: 1: (5-15): 1; the amount of the surfactant is 0.1-3 times the amount of the initiator. The selection of the above substances and the selection of the above conditions is conducive to the formation of the polystyrene template, and then to the subsequent formation of the skeleton.
[0055] S2, preparing a molybdenum carbide-nitrogen doped carbon skeleton;
[0056] The nitrogen-containing molybdenum salt is impregnated into a polystyrene template by a suction filtration method, and then a high-temperature annealing is performed to form a molybdenum carbide-nitrogen doped carbon skeleton; specifically, a nitrogen-containing molybdenum salt solution is prepared, and then poured into a suction filtration device for filtration, the molybdenum salt is impregnated into the polystyrene template, and then dried, and then a high-temperature annealing is performed in a mixed gas atmosphere of reducing gas-inert gas to form a molybdenum carbide-nitrogen doped carbon skeleton (denoted as Mo2C@NC).
[0057] Among them, the nitrogen-containing molybdenum salt is ammonium molybdate solution; the concentration of the ammonium molybdate solution is 2-5mmol / ml; the thickness of the polystyrene template is 1-10mm; the reducing gas in the mixed gas is hydrogen, and the inert gas in the mixed gas is argon; the volume of the reducing gas in the mixed gas is 5-20%; the flow rate of the mixed gas is 50-200ml / min; the temperature of high-temperature annealing is 650-850℃, the time is 2-5 hours, and the heating rate is 2-10℃ / min. The use of the above substances and conditions is conducive to the formation of molybdenum carbide-nitrogen doped carbon skeleton, and is also conducive to the formation of a three-dimensional ordered macroporous structure.
[0058] Furthermore, the polystyrene template prepared in the above steps is a regularly arranged polystyrene sphere as a template for macropores. During the high temperature annealing process, the polystyrene decomposes into small molecular gases and evaporates, thereby forming regularly ordered macropores. At the same time, the size of the polystyrene spheres can be adjusted by adjusting the preparation conditions of the polystyrene template. Using polystyrene spheres of different sizes can obtain molybdenum carbide-nitrogen-doped carbon skeletons with different pore sizes, that is, the pore size of the macropores can be adjusted.
[0059] S3, preparing composite electrode materials;
[0060] Transition metal nanoclusters are loaded on a molybdenum carbide-nitrogen doped carbon skeleton by a reduction method; specifically, a transition metal salt, such as a ruthenium salt, is dissolved in water, added to the above-mentioned Mo2C@NC and ultrasonically dispersed to form a suspension, the above-mentioned suspension is placed at 0-4°C (generally an ice water bath), and then a reducing agent is added and stirred and mixed, and then centrifuged to form an intermediate, and then the intermediate is calcined in an inert gas atmosphere.
[0061] Wherein, the ruthenium salt is RuCl3, the reducing agent includes sodium borohydride; the mass ratio of the ruthenium salt and the molybdenum carbide-nitrogen doped carbon skeleton is 5-30:100; the mass ratio of the ruthenium salt and the reducing agent is 0.1-0.6:1; the centrifugal speed is 8000-15000rpm / min; the inert gas includes nitrogen or argon, and the flow rate of the inert gas is 50-200ml / min; the calcination conditions include: temperature of 250-450℃, time of 0.5-2 hours, and heating rate of 2-10℃.
[0062] The use of the above substances and conditions is beneficial to the formation of composite electrode materials and is also beneficial to improving their performance.
[0063] In the second aspect, an embodiment of the present invention provides a composite electrode material for electrolyzing water to produce hydrogen, which is prepared by the above-mentioned preparation method, and the composite electrode material includes a molybdenum carbide-nitrogen-doped carbon skeleton and a transition metal nanocluster supported on the molybdenum carbide-nitrogen-doped carbon skeleton. Among them, the transition metal nanocluster is a ruthenium nanocluster; it can also be a precious metal nanocluster such as palladium, platinum, iridium, rhodium, etc., but it cannot be a metal such as nickel, cobalt, iron, etc., because the use of the above metals will generate metal borides.
[0064] This composite electrode material can provide a continuous path for the evolution of hydrogen during electrocatalytic hydrogen production, which is beneficial to the rapid evolution of hydrogen; it has abundant active sites, and ruthenium and molybdenum carbide can form a synergistic effect to jointly promote the kinetics of electrocatalytic hydrogen production.
[0065] The composite electrode material has a three-dimensional ordered macroporous structure; the three-dimensional ordered macroporous structure is arranged in a matrix; the pore size of the three-dimensional ordered macroporous structure is adjustable; and the pore size of the three-dimensional ordered macroporous structure is 180-450nm.
[0066] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0067] Example 1
[0068] This embodiment provides a method for preparing a composite electrode material for electrolyzing water to produce hydrogen, comprising:
[0069] (1) Preparation of polystyrene template:
[0070] 30 ml of styrene was mixed with 10 ml of 100 mg / ml NaOH solution and stirred to remove the stabilizer in the styrene, and the residual NaOH was washed with deionized water; then the obtained styrene was mixed with 250 ml of deionized water, 0.3 g of polyvinyl pyrrolidone was added and stirred at a stirring rate of 400 rpm / min, nitrogen was introduced to maintain the inert gas state in the reactor, the oil bath was heated to 75°C, and then 25 ml of 4 mg / ml potassium persulfate solution was added, and stirred at a constant temperature for 24 hours to obtain a monodisperse polystyrene microsphere emulsion; 20 ml of the emulsion was taken and filtered using a vacuum filtration device and a filter membrane (pore size: 0.22 μm) for 1.5 hours to obtain a polystyrene template.
[0071] (2) Preparation of Mo2C@NC skeleton:
[0072] Prepare 5ml of 5mmol / ml ammonium molybdate solution, pour it into the filtration device, continue filtration for 0.5h, immerse the ammonium molybdate solution into the polystyrene template, and then transfer the template to a 60℃ oven for drying; then use a tubular furnace to increase the temperature to 750℃ at a heating rate of 5℃ / min in a 10% H2-Ar atmosphere, keep it warm for 3h, and calcine it after natural cooling to form a Mo2C@NC three-dimensional ordered macroporous skeleton.
[0073] (3) Preparation of Ru / Mo2C@NC composite electrode materials:
[0074] 20 mg RuCl3 was dissolved in 80 ml deionized water, and 100 mg Mo2C@NC powder was added and ultrasonically dispersed evenly; the suspension was placed in an ice-water bath (about 0-4°C) and stirred, and then 5 ml 10 mg / ml NaBH4 solution was added dropwise and the reaction was continued with stirring for 0.5 h; the reaction solution was placed in a centrifuge tube and centrifuged at 11000 rpm / min for 5 min. The product obtained by centrifugation was placed in a 60°C oven for drying, and then a tubular furnace was used to increase the temperature to 300°C at a heating rate of 5°C / min in a N2 atmosphere, and the temperature was kept for 1 h for calcination to finally obtain a Ru / Mo2C@NC composite material with a three-dimensional ordered macroporous structure.
[0075] The composite electrode material prepared by the above method is a three-dimensional ordered macroporous structure with adjustable pore size. The main body of the material is composed of ruthenium nanoclusters loaded on a molybdenum carbide@nitrogen-doped carbon skeleton.
[0076] Example 2-3
[0077] The oil bath temperature in step (1) of Example 1 was changed to 60° C. and 90° C. respectively, and the remaining steps were the same as in Example 1.
[0078] Embodiment 4-5
[0079] The amounts of polyvinyl pyrrolidone in step (1) of Example 1 were changed to 0 g and 1.2 g respectively, and the remaining steps were the same as those of Example 1.
[0080] Embodiment 6-7
[0081] The concentrations of potassium persulfate in step (1) of Example 1 were changed to 0.5 g and 1.0 g respectively, and the remaining steps were the same as in Example 1.
[0082] Embodiment 8-9
[0083] The insulation time in step (2) of Example 1 was changed to 2 h and 4 h respectively, and the remaining steps were the same as Example 1.
[0084] Examples 10-13
[0085] The amount of RuCl3 in step (3) of Example 1 was changed to 5 mg, 10 mg, 15 mg and 25 mg respectively, and the remaining steps were the same as Example 1.
[0086] Examples 14-16
[0087] The calcination temperatures in step (3) of Example 1 were changed to 250°C, 350°C, and 400°C, respectively, and the remaining steps were the same as in Example 1.
[0088] Comparative Example 1
[0089] This comparative example provides a method for preparing a composite electrode material for electrolyzing water to produce hydrogen, comprising:
[0090] (1) Preparation of monodispersed polystyrene microsphere powder:
[0091] 30 ml of styrene was mixed with 10 ml of 100 mg / ml NaOH solution and stirred to remove the stabilizer in the styrene, and the residual NaOH was washed with deionized water; then the obtained styrene was mixed with 250 ml of deionized water, 0.3 g of polyvinyl pyrrolidone was added and stirred at a stirring rate of 400 rpm / min, nitrogen was introduced to maintain the inert gas state in the reactor, the oil bath was heated to 75°C, and then 25 ml of 4 mg / ml potassium persulfate solution was added, and the mixture was stirred at a constant temperature for 24 hours to obtain a monodisperse polystyrene microsphere emulsion; the above emulsion was centrifuged and washed, dried in an oven and ground evenly to obtain a monodisperse polystyrene microsphere powder.
[0092] (2) Preparation of disordered Mo2C@NC carrier:
[0093] Prepare 5ml of 5mmol / ml ammonium molybdate solution, pour it into the filtration device, continue filtration for 0.5h, immerse the ammonium molybdate solution into the polystyrene template, and then transfer the template to a 60℃ oven for drying; then use a tubular furnace to increase the temperature to 750℃ at a heating rate of 5℃ / min in a 10% H2-Ar atmosphere, keep it warm for 3h, and calcine it after natural cooling to form a Mo2C@NC three-dimensional ordered macroporous skeleton.
[0094] 1.46 g PS powder and 0.45 g ammonium molybdate were ground and mixed evenly, and then the mixture was placed in a tube furnace and heated to 750 °C at a heating rate of 5 °C / min in a 10% H2-Ar atmosphere, and calcined for 3 h. After natural cooling, a structurally disordered Mo2C@NC carrier (denoted as Mo2C@NC-2) was obtained.
[0095] (3) Preparation of structurally disordered Ru / Mo2C@NC-2 composite electrode materials:
[0096] 20 mg RuCl3 was dissolved in 80 ml deionized water, and 100 mg Mo2C@NC-2 powder was added and ultrasonically dispersed evenly; the suspension was placed in an ice-water bath (about 0-4°C) and stirred, and then 5 ml 10 mg / ml NaBH4 solution was added dropwise and the reaction was continued with stirring for 0.5 h; the reaction solution was placed in a centrifuge tube and centrifuged at 11000 rpm / min for 5 min. The product obtained by centrifugation was placed in a 60°C oven for drying, and then a tubular furnace was used to increase the temperature to 300°C at a heating rate of 5°C / min in a N2 atmosphere, and the temperature was kept for 1 h to calcine to obtain a structurally disordered Ru / Mo2C@NC-2 composite material.
[0097] The polystyrene microsphere powder prepared by the above method has a disordered structure and can only be used as a carbon source, so the prepared composite electrode material has a disordered structure.
[0098] Comparative Example 2
[0099] This comparative example provides a method for preparing an electrode material for electrolyzing water to produce hydrogen, comprising:
[0100] Preparation of Ru nanoparticles: 20 mg of RuCl3 was dissolved in 80 ml of deionized water, and the solution was placed in an ice water bath (about 0-4°C) and stirred. Then, 5 ml of 10 mg / ml NaBH4 solution was added dropwise and the reaction was continued with stirring for 0.5 h. The reaction solution was placed in a centrifuge tube and centrifuged at 11000 rpm / min for 5 min. The product obtained by centrifugation was placed in an oven at 60°C and dried to obtain the electrode material, namely Ru nanoparticles (denoted as Ru NPs).
[0101] Characterization
[0102] The polystyrene template and the Ru / Mo2C@NC composite material prepared in Example 1 were respectively subjected to electron microscope scanning, and the Ru / Mo2C@NC composite material prepared in Example 1 was subjected to X-ray diffraction. The test results are shown in Figure 1-Figure 3 .
[0103] Figure 1 This is the SEM image of the polystyrene template. It can be seen that after filtration, the uniform polystyrene spheres form a three-dimensional orderly arrangement.
[0104] Figure 2 This is the SEM image of the Ru / Mo2C@NC composite electrode material. It can be seen that the three-dimensional ordered macroporous Mo2C@NC skeleton formed by high-temperature calcination still maintains a three-dimensional ordered macroporous structure after loading Ru nanoclusters.
[0105] Figure 3This is the XRD diagram of the Ru / Mo2C@NC composite electrode material. It can be seen that the peak package near 26° is the peak of nitrogen-doped carbon, and the other peaks are the peaks of Mo2C. There is no obvious Ru diffraction peak, indicating that Ru has formed a smaller-sized nanocluster structure.
[0106] Experimental Example 1
[0107] Method: The electrode materials prepared in Example 1, Comparative Example 1 and Comparative Example 2 of the present invention and commercial Pt / C catalysts purchased on the market (purchased from Shanghai Hesen Electric Co., Ltd.) were polarized in 1M KOH electrolyte to obtain polarization curves. Specifically, 5 mg of the electrode materials of the embodiment and comparative example and the Pt / C catalyst were ultrasonically dispersed in a mixed solution of 450 μl of isopropanol and 50 μl of 5% Nafion, and then 20 μL of the ultrasonically uniform dispersion was applied to an area of 0.25 cm 2 On carbon fiber paper (catalyst loading: 0.8 mg cm -2 ) to obtain the working electrode. The electrochemical test was carried out in a standard three-electrode system, where the counter electrode was a platinum sheet, the reference electrode was a Hg / HgO electrode, and the electrolyte was a 1 M KOH solution. The scan rate of the polarization curve was 2 mV / s.
[0108] Results Figure 4 ,according to Figure 4 It can be seen that at the same current density, the three-dimensional ordered macroporous structure of Ru / Mo2C@NC composite material has the lowest overpotential, which is lower than the overpotential of Pt / C, indicating that its electrocatalytic hydrogen production activity is the highest.
[0109] Experimental Example 2
[0110] Method: The Ru / Mo2C@NC composite powder prepared in Example 1 was ultrasonically dispersed into a mixed solution of 450 μl isopropanol and 50 μl 5% Nafion. Then, 20 μL of the ultrasonically uniform dispersion was applied to an area of 0.25 cm 2 On carbon fiber paper (catalyst loading: 0.8 mg cm -2 ) to obtain the working electrode. The electrochemical test was carried out in a standard three-electrode system, in which the counter electrode was a platinum sheet, the reference electrode was a Hg / HgO electrode, and the electrolyte was a 1M KOH solution. The chronopotentiometry was used to test at different current densities to observe the change in potential.
[0111] Test results see Figure 5 ,according to Figure 5 It can be seen that after the Ru / Mo2C@NC composite material was tested at different current densities for 100 hours, the voltage curve had almost no change, indicating its excellent stability. Stability means that it has good catalytic performance even after long-term use.
[0112] In summary, since the two indicators for evaluating catalyst performance are catalytic rate and sustainability, the corresponding electrocatalytic hydrogen evolution reaction is the overpotential at the same current density (see the overpotential provided by the present invention). Figure 4 ) and long-term stability test (see the present invention provided Figure 5 ), that is, the present invention provides Figure 4 This indicates that the hydrogen evolution rate is faster. Figure 5 This indicates that the catalyst has good catalytic performance even after long-term use.
[0113] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A composite electrode material for producing hydrogen by electrolysis of water, characterized in that: The composite electrode material comprises a molybdenum carbide-nitrogen doped carbon skeleton and a transition metal nanocluster loaded on the molybdenum carbide-nitrogen doped carbon skeleton; wherein the transition metal nanocluster is a ruthenium nanocluster; and the molybdenum carbide-nitrogen doped carbon skeleton has a three-dimensional ordered macroporous skeleton; The method for preparing a composite electrode material for electrolyzing water to produce hydrogen comprises: loading transition metal nanoclusters on a molybdenum carbide-nitrogen-doped carbon skeleton by a reduction method; The steps of preparing the molybdenum carbide-nitrogen doped carbon skeleton include: immersing nitrogen-containing molybdenum salt into a polystyrene template by suction filtration, and then performing high temperature annealing to form a molybdenum carbide-nitrogen doped carbon skeleton; The preparation steps of the polystyrene template include: mixing the treated styrene with water, adding a surfactant, and then heating under an inert gas atmosphere, then adding a solution containing an initiator, reacting at a constant temperature to form a monodisperse polystyrene microsphere emulsion, and then filtering; The loading process includes: mixing and dispersing the ruthenium salt and the molybdenum carbide-nitrogen doped carbon skeleton to form a suspension, placing the suspension at 0-4°C, then adding a reducing agent and stirring and mixing, and then centrifuging to form an intermediate, and then calcining the intermediate in an inert gas atmosphere.
2. The composite electrode material for producing hydrogen by electrolysis of water according to claim 1, characterized in that: The composite electrode material has a three-dimensional ordered macroporous structure.
3. The composite electrode material for producing hydrogen by electrolysis of water according to claim 2, characterized in that: The pore size of the three-dimensional ordered macroporous structure is 180-450nm.
4. The composite electrode material for producing hydrogen by electrolysis of water according to claim 1, characterized in that: The preparation steps of the molybdenum carbide-nitrogen doped carbon skeleton include: immersing nitrogen-containing molybdenum salt into a polystyrene template by suction filtration, then drying, and then high-temperature annealing in a mixed gas atmosphere of reducing gas-inert gas to form a molybdenum carbide-nitrogen doped carbon skeleton.
5. The composite electrode material for producing hydrogen by electrolysis of water according to claim 4, characterized in that: The nitrogen-containing molybdenum salt is an ammonium molybdate solution; the concentration of the ammonium molybdate solution is 2-5mmol / ml; the thickness of the polystyrene template is 1-10mm; the reducing gas in the mixed gas is hydrogen, and the inert gas in the mixed gas is argon; the high-temperature annealing temperature is 650-850°C, the time is 2-5 hours, and the heating rate is 2-10°C / min.
6. The composite electrode material for producing hydrogen by electrolysis of water according to claim 4, characterized in that: The volume of the reducing gas in the mixed gas is 5-20%; the flow rate of the mixed gas is 50-200 ml / min.
7. The composite electrode material for producing hydrogen by electrolysis of water according to claim 1, characterized in that: The surfactant is selected from N-vinylamide polymers, the initiator is an oxidant, and the inert gas is selected from nitrogen; The temperature of the mixed reaction is 60~95°C, and the stirring speed is 300~600 rpm / min; The concentration of the solution containing the initiator is 2-20 mg / ml; The volume ratio of the styrene, water and the solution containing the initiator is: 1:(5-15):1; The amount of the surfactant used is 0.1-3 times the amount of the initiator used.
8. The composite electrode material for producing hydrogen by electrolysis of water according to claim 7, characterized in that: The surfactant is polyvinyl pyrrolidone; the initiator is potassium persulfate.
9. The composite electrode material for producing hydrogen by electrolysis of water according to claim 1, characterized in that: The processing of styrene includes removing stabilizers from the styrene raw material.
10. The composite electrode material for producing hydrogen by electrolysis of water according to claim 9, characterized in that: The treatment process of styrene includes: mixing the styrene raw material with a strong alkaline solution, removing the stabilizer in the styrene raw material, and then washing with water to remove the strong alkali.
11. The composite electrode material for producing hydrogen by electrolysis of water according to claim 9, characterized in that: The treatment process of styrene includes: mixing the styrene raw material with a sodium hydroxide solution to remove the stabilizer in the styrene raw material, and then washing with water to remove the sodium hydroxide.
12. The composite electrode material for producing hydrogen by electrolysis of water according to claim 1, characterized in that: The ruthenium salt is RuCl3; the reducing agent includes sodium borohydride; the mass ratio of the ruthenium salt to the molybdenum carbide-nitrogen doped carbon skeleton is 5-30:100, and the mass ratio of the ruthenium salt to the reducing agent is 0.1-0.6:1; the centrifugal speed is 8000-15000 rpm / min; The inert gas includes nitrogen or argon, and the flow rate of the inert gas is 50~200ml / min; The calcination conditions include: temperature of 250-450°C, time of 0.5-2 hours, and heating rate of 2-10°C.