Composition, positive electrode layer, all-solid-state secondary battery and method for preparing the same

By using a combination of low-reactivity dispersion medium and sulfide solid electrolyte, the problem of high reactivity between sulfide solid electrolyte and solvent in all-solid-state secondary batteries is solved, achieving high-performance formation of the positive electrode layer and improving battery performance, enhancing improve battery safety.

CN114122328BActive Publication Date: 2024-10-18SAMSUNG SDI CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202111002069.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-30
Publication Date
2024-10-18
Estimated Expiration
2041-08-30

AI Technical Summary

Technical Problem

During the preparation process of existing all-solid-state secondary batteries, there is high reactivity between the sulfide solid electrolyte and the solvent, which causes the binder to be insoluble and affects the formation of the positive electrode layer and battery performance.

Method used

Using a dispersion medium with low reactivity and excellent solubility characteristics for the binder, such as a mixture of octyl acetate and octanol, as a component of the positive active material layer, combined with a sulfide solid electrolyte and a conductive agent, through a wet method The positive electrode layer is prepared by a coating process, and drying conditions are controlled to reduce dispersion medium residue.

Benefits of technology

The high-performance formation of the positive electrode layer is achieved, the capacity characteristics and life of the all-solid-state secondary battery are improved, the internal resistance is reduced, and the safety of the battery is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114122328B_ABST
    Figure CN114122328B_ABST
Patent Text Reader

Abstract

A composition, a positive electrode layer, an all-solid-state secondary battery and a method for preparing the same are provided. The positive electrode layer includes a positive electrode current collector and a positive electrode active material layer on the positive electrode current collector, wherein the positive electrode active material layer includes a positive electrode active material, a binder, a conductive agent, a sulfide solid electrolyte and a dispersion medium, and the dispersion medium includes a compound represented by Formula 1 and a compound represented by Formula 2, wherein Formula 1R 1 ‑C(=O)O‑R 2 In formula 1, R 1 is C1-C2 alkyl and R 2 is a C7-C9 alkyl group, formula 2R 2’ ‑OH In formula 2, R 2’ It is a C7-C9 alkyl group.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application is based upon and claims the benefit of priority from Korean Patent Application No. 10-2020-0110587 filed on August 31, 2020, in the Korean Intellectual Property Office, the disclosure of which is incorporated herein in its entirety by reference. Technical Field

[0003] Embodiments relate to a positive electrode layer for an all-solid-state secondary battery, an all-solid-state secondary battery including the same, and a method of preparing the positive electrode layer. Background Art

[0004] In recent years, there has been a strong push to develop batteries with improved energy density and high safety. For example, lithium-ion batteries have been put into practical use in the automotive industry, as well as in information-related and communication equipment. Safety is paramount in the automotive industry. Summary of the Invention

[0005] An embodiment may be implemented by providing a positive electrode layer for an all-solid-state secondary battery, the positive electrode layer including a positive electrode current collector and a positive electrode active material layer on the positive electrode current collector, wherein the positive electrode active material layer includes a positive electrode active material, a binder, a conductive agent, a sulfide solid electrolyte, and a dispersion medium, the dispersion medium including a compound represented by Formula 1 and a compound represented by Formula 2,

[0006] Formula 1

[0007] R 1 -C(=O)OR 2

[0008] In formula 1, R 1 is a C1-C2 alkyl group and R 2 is a C7-C9 alkyl group,

[0009] Formula 2

[0010] R 2’ -OH

[0011] In formula 2, R 2’ It is a C7-C9 alkyl group.

[0012] The dispersion medium may include a mixture of octyl acetate as the compound represented by Formula 1 and octanol as the compound represented by Formula 2, nonyl acetate as the compound represented by Formula 1 and nonanol as the compound represented by Formula 2, or heptyl acetate as the compound represented by Formula 1 and heptanol as the compound represented by Formula 2.

[0013] The amount of the compound represented by Formula 1 in the positive electrode layer may be about 500 ppm or less.

[0014] The amount of the compound represented by Formula 2 in the positive electrode layer may be about 500 ppm or less.

[0015] The amount of the compound represented by Formula 2 in the positive electrode layer may be in the range of about 5 ppm to about 500 ppm relative to 100 ppm of the compound represented by Formula 1 in the positive electrode layer.

[0016] The binder may include polyvinylidene fluoride, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, a vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, or a combination thereof.

[0017] The conductive agent may include graphite, carbon black, acetylene black, carbon nanofibers, carbon nanotubes, or a combination thereof.

[0018] Sulfide solid electrolytes may include Li2S-P2S5; Li2S-P2S5-LiX (wherein X is a halogen element); Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S-P2S5-Z m S n , wherein m and n are each positive numbers, and Z is Ge, Zn or Ga; Li2S-GeS2; Li2S-SiS2-Li3PO4; Li2S-SiS2-Li p MO q , wherein p and q are each positive numbers, and M is P, Si, Ge, B, Al, Ga, or In; Li 7-x PS 6-x Cl x , where 0≤x≤2; Li 7-x PS 6-x Br x , where 0≤x≤2, or Li 7-x PS 6-x I x , where 0≤x≤2.

[0019] The sulfide solid electrolyte may be an argyrodite-type solid electrolyte including Li6PS5Cl, Li6PS5Br, or Li6PS5I.

[0020] The embodiment may be implemented by providing an all-solid-state secondary battery including the positive electrode layer according to the embodiment; a negative electrode layer; and a solid electrolyte between the positive electrode layer and the negative electrode layer, the solid electrolyte including a sulfide solid electrolyte.

[0021] The negative electrode layer may include a negative electrode collector and a first negative electrode active material layer, the second negative electrode active material layer may be on the first negative electrode active material layer, between the negative electrode collector and the first negative electrode active material layer, or on the first negative electrode active material layer and between the negative electrode collector and the first negative electrode active material layer, and the second negative electrode active material layer may include lithium or a lithium alloy.

[0022] The negative electrode layer may include a negative electrode current collector and a first negative active material layer, and the all-solid-state secondary battery may further include a carbon layer between the first negative active material layer and the solid electrolyte.

[0023] An embodiment may be implemented by providing a method for preparing an all-solid-state secondary battery, the method comprising mixing a positive electrode active material, a binder, a sulfide solid electrolyte, and a compound represented by Formula 1 to prepare a composition for forming a positive electrode active material layer; forming a positive electrode active material layer by coating and drying the composition for forming a positive electrode active material layer on a positive electrode current collector to form a positive electrode layer on the positive electrode current collector; providing a negative electrode layer including a negative electrode current collector and a first negative electrode active material layer; preparing a laminate by providing a solid electrolyte between the negative electrode layer and the positive electrode layer, the solid electrolyte including a sulfide solid electrolyte; and pressing the laminate,

[0024] Formula 1

[0025] R 1 -C(=O)OR 2

[0026] In Formula 1, R 1 is a C1-C2 alkyl group, and R 2 It is a C7-C9 alkyl group.

[0027] Drying the composition may include performing a first heat treatment at a temperature in a range of about 25° C. to about 100° C.; and performing a second heat treatment in a vacuum at a temperature in a range of about 40° C. to about 100° C.

[0028] After drying the composition, the positive electrode layer may include a dispersion medium including the compound represented by Formula 1 and the compound represented by Formula 2, an amount of the compound represented by Formula 1 in the positive electrode layer may be about 500 ppm or less, and an amount of the compound represented by Formula 2 in the positive electrode layer may be about 500 ppm or less.

[0029] Formula 2

[0030] R 2’ -OH

[0031] In formula 2, R 2’ It is a C7-C9 alkyl group.

[0032] The dispersion medium may include a mixture of octyl acetate as the compound represented by Formula 1 and octanol as the compound represented by Formula 2, nonyl acetate as the compound represented by Formula 1 and nonanol as the compound represented by Formula 2, or heptyl acetate as the compound represented by Formula 1 and heptanol as the compound represented by Formula 2.

[0033] The embodiment can be achieved by providing a composition for forming a positive electrode active material layer for an all-solid-state secondary battery, the composition including a positive electrode active material; a binder; a conductive agent; a sulfide solid electrolyte; and a compound represented by Formula 1,

[0034] Formula 1

[0035] R 1 -C(=O)OR 2

[0036] In Formula 1, R 1 is a C1-C2 alkyl group, and R 2 It is a C7-C9 alkyl group.

[0037] The compound represented by Formula 1 may be included in the composition in an amount of about 25 parts by weight to about 65 parts by weight, based on 100 parts by weight of solids in the composition.

[0038] The compound represented by Formula 1 may include octyl acetate, nonyl acetate, heptyl acetate, or a combination thereof.

[0039] The composition may further include a solvent including heptane, xylene, toluene, diethylbenzene, diethyl carbonate, or dimethyl carbonate. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Features will become apparent to those skilled in the art by describing exemplary embodiments in detail with reference to the accompanying drawings, in which:

[0041] Figure 1 Graph showing voltage and specific capacity in the all-solid-state secondary batteries of Example 1 and Comparative Example 4.

[0042] Figure 2A and Figure 2B Results of head space sampler (HSS) gas chromatography / mass spectrometry (HSS-GC / MS) analysis for analyzing components of the residual dispersion medium in the positive electrode layer prepared in Example 1 are shown.

[0043] Figures 3 to 5 is a cross-sectional view of an all-solid-state secondary battery according to example embodiments.

[0044] Figure 6A Images showing the results of evaluating the reactivity of octyl acetate as a dispersion medium with the sulfide solid electrolyte Li6PS5Cl, in part (a), the initial state after mixing; and in part (b), the state of solid electrolyte dispersion after 3 days.

[0045] Figure 6B Images showing the results of evaluating the reactivity of butyl acetate as a dispersion medium with the sulfide solid electrolyte Li6PS5Cl, in part (a), the initial state after mixing; and in part (b), the state of solid electrolyte dispersion after 3 days. DETAILED DESCRIPTION

[0046] Example embodiments will now be described more fully hereinafter with reference to the accompanying drawings; however, they may be embodied in different forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey exemplary implementations to those skilled in the art.

[0047] In the drawings, the dimensions of layers and regions may be exaggerated for clarity of illustration. It will also be understood that when a layer or element is referred to as being "on" another layer or element, it can be directly on the other layer or element, or intervening layers may also be present. Additionally, it will be understood that when a layer is referred to as being "between" two layers, it can be the only layer between the two layers, or one or more intervening layers may also be present. Like reference numerals refer to like elements throughout.

[0048] As used herein, the terms "or" and "and / or" include any and all combinations of one or more of the associated listed items, for example, "A or B" will include A, B, or A and B. Expressions such as "at least one of," when preceding a list of elements, modify the entire list of elements and do not modify the individual elements of the list.

[0049] Hereinafter, according to one or more embodiments, a positive electrode layer for an all-solid-state secondary battery, an all-solid-state secondary battery including the same, and a method of preparing the positive electrode layer will be described in detail.

[0050] According to an embodiment, a positive electrode layer for an all-solid-state secondary battery including a sulfide solid electrolyte may be provided. In an embodiment, the positive electrode layer may include a positive electrode current collector and a positive electrode active material layer on the positive electrode current collector. In an embodiment, the positive electrode layer may include, for example, a positive electrode active material, a binder, a conductive agent, a sulfide solid electrolyte, and a dispersion medium. In an embodiment, the dispersion medium may include, for example, a compound represented by Formula 1 and a compound represented by Formula 2.

[0051] Formula 1

[0052] R 1 -C(=O)OR 2

[0053] In formula 1, R 1 may be or include, for example, a C1-C2 alkyl group, and R 2 It may be or include, for example, a C7-C9 alkyl group.

[0054] Formula 2

[0055] R 2’ -OH

[0056] In formula 2, R 2’ It may be or include, for example, a C7-C9 alkyl group.

[0057] Sulfide solid electrolytes can be used as solid electrolytes for all-solid-state secondary batteries, and the positive electrode layer can include the sulfide solid electrolyte. For commercialization of all-solid-state secondary batteries, the positive electrode layer can be prepared using a wet coating process.

[0058] In the preparation of the positive electrode layer using a wet coating process, due to the high reactivity of the solvent used for the wet coating process with the sulfide solid electrolyte, a non-polar solvent (e.g., heptane) can be used. However, the non-polar solvent may not dissolve the binder, and therefore it is expected that there will be improvement in this regard. When using a polar solvent with excellent solubility characteristics for the binder, the polar solvent can dissolve the sulfide solid electrolyte, and a positive electrode layer and an all-solid-state secondary battery may not be prepared.

[0059] One or more embodiments may provide a positive electrode layer for an all-solid-state secondary battery including a sulfide solid electrolyte with improved performance using a composition for forming a positive active material layer through a wet coating process, the composition including a dispersion medium having excellent solubility characteristics for a binder and low reactivity with the sulfide solid electrolyte.

[0060] In implementations, the composition for forming a positive active material layer for an all-solid-state secondary battery may include, for example, a positive active material, a binder, a conductive agent, a sulfide solid electrolyte, and a compound represented by Formula 1 as a dispersion medium.

[0061] Formula 1

[0062] R 1 -C(=O)OR 2

[0063] In formula 1, R 1 may be or include, for example, a C1-C2 alkyl group, and R2 It may be or include, for example, a C7-C9 alkyl group.

[0064] The compound represented by Formula 1 may have a bulky C7-C9 alkyl group as R 2 , and due to steric hindrance, it has low reactivity with sulfide solid electrolytes, so that it can be used as a dispersion medium in a positive electrode layer including a sulfide solid electrolyte and in an all-solid-state secondary battery. In practice, the compound represented by Formula 1 may have a C1-C2 alkyl group as R 1 , and can exhibit excellent solubility characteristics for binders.

[0065] When the compound of Formula 1 is used as a dispersion medium, the cell resistance may not be high, and a small amount of the dispersion medium may remain in the positive electrode layer after the drying process during the preparation of the positive electrode layer. The amount (e.g., residual amount, weight, or concentration) of the compound of Formula 1 in the positive electrode layer may be negligible, for example, as low as about 500 ppm (by weight) or less.

[0066] In an embodiment, the boiling point of the compound of Formula 1 may be in the range of about 190° C. to about 230° C., for example, about 193° C. to about 228° C. When the boiling point of the compound of Formula 1 is within these ranges, the amount of the dispersion medium in the positive electrode layer finally obtained after the vacuum drying process may be reduced, and thus an all-solid-state secondary battery having excellent capacity and average voltage characteristics and improved lifespan may be prepared.

[0067] When a positive electrode layer is prepared using the composition for forming a positive active material layer by a wet coating process using the compound of Formula 1 as a dispersion medium, a positive electrode layer having the same properties as those prepared by a dry process can be prepared.

[0068] Only the compound of Formula 1 can be used in the composition, and the compound of Formula 2 (in addition to the compound of Formula 1) may remain or exist in the final positive electrode layer prepared using the composition. After the drying process in the preparation of the positive active material layer, the compound of Formula 1 may remain in the positive electrode layer, and the compound of Formula 2 may be derived from the compound of Formula 1.

[0069] In an embodiment, the amount of the dispersion medium in the composition may be, for example, about 25 parts by weight to about 65 parts by weight based on 100 parts by weight of the solid in the composition for the positive active material layer. The amount of the dispersion medium represents the amount of the compound of Formula 1, and the total weight of the solid in the composition for the positive active material layer may be the total weight of the positive active material, the binder, the conductive agent, and the sulfide solid electrolyte.

[0070] The dispersion medium in the positive electrode layer according to the embodiment may include, for example, a mixture of octyl acetate and octanol, a mixture of nonyl acetate and nonanol, or a mixture of heptyl acetate and heptanol.

[0071] The composition may further include a non-polar solvent, for example, heptane, xylene, toluene, or diethylbenzene. The amount of the non-polar solvent based on 100 parts by weight of the dispersion medium and the non-polar solvent may be, for example, about 0.1 parts by weight or greater, about 5 parts by weight or greater, or about 10 parts by weight or greater. In implementation, the amount of the non-polar solvent based on 100 parts by weight of the dispersion medium and the non-polar solvent may be in the range of about 0.1 parts by weight to about 10 parts by weight.

[0072] The composition may further include an organic solvent, for example, diethyl carbonate, dimethyl carbonate or ethylene carbonate (for example, as a part of a dispersion medium). Based on 100 parts by weight of a dispersion medium, the amount of the organic solvent may be about 65 parts by weight or less, for example, in the range of about 0.5 parts by weight to about 65 parts by weight, about 1 part by weight to about 50 parts by weight, about 3 parts by weight to about 40 parts by weight or about 5 parts by weight to about 25 parts by weight. In an implementation, based on 100 parts by weight of the solid in the composition for the positive active material layer, the amount of the organic solvent may be, for example, in the range of about 5 parts by weight to about 40 parts by weight or about 5 parts by weight to about 15 parts by weight.

[0073] In the composition for forming a positive electrode active material layer, the amount of the sulfide solid electrolyte may be, for example, in the range of about 5 parts by weight to about 30 parts by weight or about 8 parts by weight to about 15 parts by weight, based on 100 parts by weight of the solid in the composition for forming a positive electrode active material layer.

[0074] The positive electrode layer prepared using the above composition may include a positive electrode current collector and a positive electrode active material layer on the positive electrode current collector. The positive electrode active material layer may include, for example, a positive electrode active material, a binder, a conductive agent, a sulfide solid electrolyte, a compound represented by Formula 1, and a compound represented by Formula 2.

[0075] Formula 1

[0076] R 1 -C(=O)OR 2

[0077] In formula 1, R 1 may be or include, for example, a C1-C2 alkyl group, and R 2 It may be or include, for example, a C7-C9 alkyl group.

[0078] Formula 2

[0079] R 2’ -OH

[0080] In formula 2, R 2’ It may be or include, for example, a C7-C9 alkyl group.

[0081] According to another embodiment, an all-solid-state secondary battery may include, for example, a positive electrode layer; a negative electrode layer; and a solid electrolyte layer between the positive electrode layer and the negative electrode layer. The solid electrolyte layer may include, for example, a sulfide solid electrolyte. In implementations, the positive electrode layer may be the same as the positive electrode layer according to aspects of the embodiment.

[0082] An all-solid-state secondary battery according to an embodiment may include a positive electrode layer; a negative electrode layer; and a solid electrolyte layer between the positive electrode layer and the negative electrode layer. In an embodiment, the positive electrode layer may include a positive electrode current collector and a positive electrode active material layer on the positive electrode current collector, and the negative electrode layer may include a metal-carbon composite material.

[0083] [All-solid-state secondary battery]

[0084] refer to Figure 3 The all-solid-state secondary battery 1 may include a positive electrode layer 10 , a negative electrode layer 20 , and a solid electrolyte layer 30 between the positive electrode layer 10 and the negative electrode layer 20 , the solid electrolyte layer 30 including a sulfide solid electrolyte.

[0085] The positive electrode layer 10 may include a positive electrode collector 11 and a positive active material layer 12 on the positive electrode collector 11. The positive active material layer 12 may include a positive active material, a binder, a sulfide solid electrolyte, a compound represented by Formula 1, and a compound represented by Formula 2.

[0086] Formula 1

[0087] R 1 -C(=O)OR 2

[0088] In formula 1, R 1 may be or include, for example, a C1-C2 alkyl group, and R 2 It may be or include, for example, a C7-C9 alkyl group.

[0089] Formula 2

[0090] R 2’ -OH

[0091] In formula 2, R 2’ It may be or include, for example, a C7-C9 alkyl group.

[0092] R in Formula 1 2 Can be compared with R in formula 2 2’ The same.

[0093] The compound represented by Formula 1 may include, for example, heptyl acetate, octyl acetate, nonyl acetate, or a combination thereof. The compound represented by Formula 2 may include, for example, heptanol, octanol, nonyl alcohol, or a combination thereof (for example, and depending on the structure of Formula 1).

[0094] For example, in the positive electrode active material layer 12, the amount or concentration of the compound represented by Formula 1 and the compound represented by Formula 2 may each be, for example, about 500 ppm (by weight) or less, about 400 ppm or less, about 200 ppm or less, about 100 ppm or less, about 50 ppm or less, or about 10 ppm or less.

[0095] In implementations, the amount of the compound represented by Formula 1 and the compound represented by Formula 2 may each be in the range of, for example, about 50 ppm to about 500 ppm, about 100 ppm to about 500 ppm, about 200 ppm to about 500 ppm, about 300 ppm to about 500 ppm, or about 400 ppm to about 500 ppm.

[0096] In implementations, the amount of the compound represented by Formula 1 and the compound represented by Formula 2 may each be in a range of about 1 ppm to about 50 ppm, about 5 ppm to about 30 ppm, or about 5 ppm to about 10 ppm.

[0097] The amount of the compound represented by Formula 2 may be, for example, in the range of about 5 ppm to about 500 ppm, about 5 ppm to about 300 ppm, about 5 ppm to about 200 ppm, about 5 ppm to about 150 ppm, or about 5 ppm to about 100 ppm, based on or relative to 100 ppm of the compound represented by Formula 1 in the positive electrode layer 10. When the mixing ratio of the compound represented by Formula 1 and the compound represented by Formula 2 is within these ranges, an all-solid-state secondary battery having excellent ion conductivity and life characteristics can be prepared.

[0098] The compound represented by Formula 1 and the compound represented by Formula 2 may include, for example, octyl acetate and octanol. In an implementation, the amount of octanol may be, for example, in the range of about 5 ppm to about 100 ppm based on 100 ppm of octyl acetate.

[0099] The compound represented by Formula 1 and the compound represented by Formula 2 may be able to dissolve a binder used in the preparation of the positive electrode layer and may be chemically unreactive or almost completely chemically unreactive to the sulfide solid electrolyte.

[0100] [Positive electrode layer: positive electrode current collector]

[0101] The positive electrode current collector 11 may be, for example, a plate or foil formed of indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or alloys thereof. In embodiments, the positive electrode current collector 11 may be omitted. In embodiments, a carbon layer having a thickness ranging from about 0.1 μm to about 4 μm may be provided on the positive electrode current collector 11 to help increase the bonding strength between the positive electrode current collector 11 and the positive electrode layer 10.

[0102] [Positive electrode layer: positive electrode active material]

[0103] The positive active material layer 12 may include, for example, a positive active material, a sulfide solid electrolyte, a binder, a compound of Formula 1, and a compound of Formula 2.

[0104] The positive active material layer 12 may include a conductive agent. The conductive agent may include, for example, graphite, carbon black, acetylene black, carbon nanofiber, or carbon nanotube.

[0105] The sulfide solid electrolyte included in the positive electrode layer 10 may be the same as or different from the sulfide solid electrolyte included in the solid electrolyte layer 30 .

[0106] The positive electrode active material may be a positive electrode active material that can reversibly absorb and desorb lithium ions. Examples of the positive electrode active material may include lithium transition metal oxides such as lithium cobalt oxide (LCO), lithium nickel oxide, lithium nickel cobalt oxide, lithium nickel cobalt aluminum oxide (NCA), lithium nickel cobalt manganese oxide (NCM); lithium manganese oxide; lithium iron phosphate; nickel sulfide; copper sulfide; lithium sulfide; iron oxide; or vanadium oxide. The positive electrode active material may be formed from a single one of these examples or a mixture of at least two selected from these examples.

[0107] The positive electrode active material may include, for example, a compound represented by one of the following formulas: Li a A 1-b B' b D2 (where 0.90≤a≤1 and 0≤b≤0.5); Li a E 1-b B' b O 2-c D c (where 0.90≤a≤1, 0≤b≤0.5 and 0≤c≤0.05); LiE 2-b B' b O 4-c D c (where 0≤b≤0.5 and 0≤c≤0.05); Li a Ni 1-b-c Co b B'c D α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05 and 0<α≤2); Li a Ni 1-b-c Co b B' c O 2-α F' α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Li a Ni 1-b-c Co b B' c O 2-α F'2 (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Li a Ni 1-b-c Mn b B' c D α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05 and 0<α≤2); Li a Ni 1-b-c Mn b B' c O 2-α F' α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Li a Ni 1-b- c Mn b B' c O 2-α F'2 (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Li a Ni b E c G d O2 (where 0.90≤a≤1, 0≤b≤0.9, 0≤c≤0.5 and 0.001≤d≤0.1); Li a Ni b Co c Mn d G e O2 (where 0.90≤a≤1, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5 and 0.001≤e≤0.1); Li a NiG b O2 (where 0.90≤a≤1 and 0.001≤b≤0.1); Li a CoG bO2 (where 0.90≤a≤1 and 0.001≤b≤0.1); Li a MnG b O2 (where 0.90≤a≤1 and 0.001≤b≤0.1); Li a Mn2G b O4 (where 0.90≤a≤1 and 0.001≤b≤0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiI'O2; LiNiVO4; Li (3-f) J2(PO4)3(where 0≤f≤2);Li (3-f) Fe2(PO4)3 (where 0≤f≤2); or LiFePO4. In the compound, A can be nickel (Ni), cobalt (Co), manganese (Mn), or a combination thereof; B' can be aluminum (Al), nickel (Ni), cobalt (Co), manganese (Mn), chromium (Cr), iron (Fe), magnesium (Mg), strontium (Sr), vanadium (V), a rare earth element, or a combination thereof; D can be oxygen (O), fluorine (F), sulfur (S), phosphorus (P), or a combination thereof; E can be cobalt (Co), manganese (Mn), or a combination thereof; F' can be fluorine (F), sulfur (S), phosphorus (P), or a combination thereof. ; G may be Al, chromium (Cr), manganese (Mn), iron (Fe), magnesium (Mg), lanthanum (La), cerium (Ce), strontium (Sr), vanadium (V), or a combination thereof; Q may be titanium (Ti), molybdenum (Mo), manganese (Mn), or a combination thereof; I' may be chromium (Cr), vanadium (V), iron (Fe), scandium (Sc), yttrium (Y), or a combination thereof; and J may be vanadium (V), chromium (Cr), manganese (Mn), cobalt (Co), nickel (Ni), copper (Cu), or a combination thereof. The compound may have a surface coating (hereinafter, also referred to as a "coating"). In practice, a mixture of a compound without a coating and a compound with a coating may be used, the compound being selected from the compounds listed above. In practice, the coating may include a compound of a coating element, for example, an oxide, hydroxide, oxyhydroxide, oxycarbonate, or hydroxycarbonate of the coating element. In practice, the compound used for the coating may be amorphous or crystalline. In an embodiment, the coating element for the coating layer may include, for example, magnesium (Mg), aluminum (Al), cobalt (Co), potassium (K), sodium (Na), calcium (Ca), silicon (Si), titanium (Ti), vanadium (V), tin (Sn), germanium (Ge), gallium (Ga), boron (B), arsenic (As), zirconium (Zr) or a mixture thereof. In an embodiment, an appropriate method that does not adversely affect the physical properties of the positive active material when a compound of the coating element is used can be used to form the coating layer. In an embodiment, a spraying method or an immersion method can be used to form the coating layer.

[0108] The positive electrode active material may include, for example, a lithium salt of a transition metal oxide having a layered rock salt-type structure among examples of lithium transition metal oxides. In an implementation, the "layered rock salt-type structure" refers to a structure in which oxygen atom layers and metal atom layers are alternately and regularly arranged in the <111> direction in a cubic rock salt-type structure, where each atom layer forms a two-dimensional flat plane. The "cubic rock salt-type structure" refers to a sodium chloride (NaCl)-type structure, which is one of the crystal structures. For example, it refers to a structure in which face-centered cubic (fcc) lattices formed by anions and cations, respectively, are offset by only half of the ridge of each unit lattice. Examples of lithium transition metal oxides having a layered rock salt-type structure may include those represented as LiNi x Co y Al z O2 (NCA) or LiNi x Co y Mn z O2 (NCM) (where 0 < x < 1, 0 < y < 1, 0 < z < 1 and x + y + z = 1) of ternary lithium transition metal oxides. When the positive electrode active material includes a ternary transition metal oxide having a layered rock salt-type structure, the energy density and thermal stability of the all-solid-state secondary battery 1 can be improved.

[0109] The positive electrode active material may be covered with the above-described coating. The coating may include a suitable material that can be used as a coating for the positive electrode active material of the all-solid-state secondary battery. The coating may include, for example, Li2O-ZrO2 (LZO).

[0110] When the positive electrode active material includes a ternary lithium transition metal oxide containing nickel (Ni), such as NCA or NCM, the capacity density of the all-solid-state secondary battery 1 is increased, and thus the metal dissolution from the positive electrode active material in the charged state can be reduced. As a result, the all-solid-state secondary battery 1 according to the implementation may have improved cycle characteristics in the charged state.

[0111] The shape of the positive electrode active material may be, for example, a particulate shape, such as a true spherical shape, an oval shape, or a spherical shape. The particle size of the positive electrode active material may be within a suitable range for the positive electrode active material of the all-solid-state secondary battery. The amount of the positive electrode active material in the positive electrode layer 10 may be within a suitable range for the positive electrode layer of the all-solid-state secondary battery.

[0112] [Positive electrode layer: Solid electrolyte]

[0113] The positive electrode active material layer 12 may, for example, include a solid electrolyte. The solid electrolyte in the positive electrode layer 10 may be the same as or different from the solid electrolyte in the solid electrolyte layer 30. Details of the solid electrolyte may be the same as those defined with reference to the solid electrolyte layer 30.

[0114] The average particle size D50 of the solid electrolyte in the positive electrode active material layer 12 may be smaller than the average particle size D50 of the solid electrolyte in the solid electrolyte layer 30. In an implementation, the average particle size D50 of the solid electrolyte in the positive electrode active material layer 12 may be, for example, about 90% or less, about 80% or less, about 70% or less, about 60% or less, about 50% or less, about 40% or less, about 30% or less, or about 20% or less of the average particle size D50 of the solid electrolyte in the solid electrolyte layer 30.

[0115] [Positive electrode layer: binder]

[0116] The positive active material layer 12 may include a binder. Examples of the binder may include polyvinylidene fluoride, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, a vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, and polymethyl methacrylate.

[0117] [Positive electrode layer: conductive agent]

[0118] The positive electrode active material layer 12 may include a conductive agent. The conductive agent may include, for example, graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or metal powder.

[0119] [Positive electrode layer: additives]

[0120] The positive electrode layer 10 may further include, for example, additives such as a filler, a coating agent, a dispersant, and an ion conductive agent in addition to the positive active material, the solid electrolyte, the binder, and the conductive agent.

[0121] The filler, coating agent, dispersant, and ion conductive agent that may be included in the positive electrode layer 10 may be appropriate materials for an electrode of an all-solid-state secondary battery.

[0122] [Solid electrolyte layer]

[0123] The solid electrolyte in the solid electrolyte layer 30 may be a sulfide solid electrolyte having excellent lithium ion conductivity characteristics.

[0124] [Solid electrolyte layer: sulfide solid electrolyte]

[0125] refer to Figures 3 to 5 , the solid electrolyte layer 30 may include a sulfide solid electrolyte between the positive electrode layer 10 and the negative electrode layer 20 .

[0126] The sulfide solid electrolyte may include, for example, Li2S-P2S5, Li2S-P2S5-LiX (wherein X is a halogen), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (wherein m and n are each positive numbers, and Z is one of Ge, Zn and Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q (wherein p and q are each positive numbers, and M is one of P, Si, Ge, B, Al, Ga, and In), Li 7-x PS 6-x Cl x (where 0≤x≤2), Li 7-x PS 6-x Br x (where 0≤x≤2), or Li 7-x PS 6-x I x (where 0≤x≤2). The sulfide solid electrolyte can be prepared by, for example, melting and quenching or mechanically grinding a starting material (e.g., Li2S or P2S5). Subsequently, the resultant can be heat-treated. The sulfide solid electrolyte can be amorphous or crystalline and can be in a mixed form. In an embodiment, the sulfide solid electrolyte can be a material comprising sulfur (S), phosphorus (P) and / or lithium (Li) as component elements. In an embodiment, the sulfide solid electrolyte can be a material comprising Li2S-P2S5. In an embodiment, when a material comprising Li2S-P2S5 is used as a sulfide solid electrolyte material, the mixing molar ratio of Li2S and P2S5 (Li2S:P2S5) can be, for example, in the range of about 50:50 to about 90:10.

[0127] In practice, the sulfide solid electrolyte may include, for example, Li 7-x PS 6-x Cl x (where 0≤x≤2), Li 7- x PS 6-x Br x (where 0≤x≤2) or Li 7-x PS 6-x I x(wherein 0≤x≤2) an argyrodite-type compound. In an implementation, the sulfide solid electrolyte may be an argyrodite-type solid electrolyte including, for example, Li6PS5Cl, Li6PS5Br, or Li6PS5I.

[0128] The density of the argyrodite-type solid electrolyte may be, for example, in the range of about 1.5 g / cc to about 2.0 g / cc. When the density of the argyrodite-type solid electrolyte is about 1.5 g / cc or higher, the internal resistance of the all-solid-state secondary battery may be reduced, and the penetration of the solid electrolyte layer by Li migration may be effectively suppressed.

[0129] The elastic modulus of the sulfide solid electrolyte may be, for example, in the range of about 15 GPa to about 35 GPa.

[0130] [Solid electrolyte layer: binder]

[0131] The solid electrolyte layer 30 may include, for example, a binder. In an embodiment, the binder in the solid electrolyte layer 30 may include, for example, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, or another suitable material. The binder in the solid electrolyte layer 30 may be the same as or different from the binder in the positive electrode active material layer 12 and the binder in the negative electrode active material layer 22. The negative electrode active material layer 22 may be, for example, a first negative electrode active material layer 22.

[0132] [Negative electrode layer]

[0133] [Negative electrode layer: negative electrode active material]

[0134] The negative electrode layer 20 may include a negative electrode current collector 21 and a first negative active material layer 22 on the negative electrode current collector 21. The first negative active material layer 22 may include, for example, a negative active material and a binder.

[0135] The negative electrode active material in the first negative electrode active material layer 22 may be, for example, in the form of particles. The average particle size of the negative electrode active material in the form of particles may be, for example, about 4 μm or less, about 2 μm or less, about 1 μm or less, or about 900 nm or less. The average particle size of the negative electrode active material in the form of particles may be, for example, in the range of about 10 nm to about 4 μm, about 10 nm to about 2 μm, or about 10 nm to about 900 nm. When the average particle size of the negative electrode active material is within these ranges, it may further facilitate the reversible absorption and / or desorption of lithium during the charge / discharge process. The average particle size of the negative electrode active material may be a median particle size (D50) as measured by, for example, a laser diffraction particle size distribution analyzer.

[0136] In an implementation, the negative electrode active material may include, for example, a carbonaceous negative electrode active material or a metal or metalloid negative electrode active material.

[0137] The carbonaceous negative electrode active material may include, for example, amorphous carbon. Examples of amorphous carbon may include carbon black (CB), acetylene black (AB), furnace black (FB), Ketjen black (KB), graphene, or other suitable materials. Amorphous carbon refers to carbon with no or very low crystallinity and is distinguished from crystalline carbon or graphite carbon.

[0138] The metal or metalloid negative electrode active material may include, for example, gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), zinc (Zn), or other suitable metal negative electrode active materials or metalloid negative electrode active materials that can form alloys or compounds with lithium. In practice, nickel (Ni) does not form an alloy with lithium and therefore may not be used as the metal negative electrode active material.

[0139] In an embodiment, the first negative electrode active material layer 22 may include one of the negative electrode active materials listed above or a mixture of the above-mentioned multiple negative electrode active materials. In an embodiment, the first negative electrode active material layer 22 may include only amorphous carbon, or may include gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), or zinc (Zn). In an embodiment, the first negative electrode active material layer 22 may include a mixture of amorphous carbon and gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), or zinc (Zn). In a mixture of amorphous carbon and, for example, gold (Au), the mixing ratio of amorphous carbon to gold (Au) may be, for example, about 10:1 to about 1:2, about 5:1 to about 1:1, or about 4:1 to about 2:1, or the mixing ratio may be appropriately selected according to the desired characteristics of the all-solid-state secondary battery 1. When the negative electrode active material of the first negative electrode active material layer 22 has the composition described above, the all-solid-state secondary battery 1 can have further improved cycle characteristics.

[0140] The negative electrode active material of the first negative electrode active material layer 22 may include, for example, a mixture of first particles composed of amorphous carbon and second particles composed of metal or metalloid. Examples of metals or metalloids may include gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn) and zinc (Zn). In an embodiment, the metalloid may be a semiconductor. Based on the total weight of the mixture, the amount of the second particles may be, for example, in the range of about 8 weight % (wt%) to about 60 wt%, about 10 wt% to about 50 wt%, about 15 wt% to about 40 wt%, or about 20 wt% to about 30 wt%. When the amount of the second particles is within these ranges, the all-solid-state secondary battery 1 may have further improved cycle characteristics.

[0141] [Negative electrode layer: binder]

[0142] Examples of the binder in the first negative electrode active material layer 22 may include styrene-butadiene rubber (SBR), polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, or other suitable materials. The binder may be formed of a single one of these examples of the binder or a plurality of different binders.

[0143] When the first negative electrode active material layer 22 includes a binder, it can be stably attached to the negative electrode current collector 21. In practice, cracking of the first negative electrode active material layer 22 can be suppressed despite changes in volume and / or relative position of the first negative electrode active material layer 22 during the charge / discharge process. In practice, when the first negative electrode active material layer 22 does not include a binder, the first negative electrode active material layer 22 can be easily separated from the negative electrode current collector 21. When a portion of the separated negative electrode current collector 21 is exposed, the exposed portion may contact the solid electrolyte layer 30, increasing the likelihood of a short circuit. The first negative electrode active material layer 22 can be prepared, for example, by coating the negative electrode current collector 21 with a slurry in which the materials constituting the first negative electrode active material layer 22 are dispersed, and then drying the slurry and the negative electrode current collector 21. When a binder is included in the first negative electrode active material layer 22, the negative electrode active material can be stably dispersed in the slurry. In implementation, when the negative electrode current collector 21 is coated with the slurry using the screen printing method, clogging of the screen (eg, clogging by aggregates of the negative active material) may be suppressed.

[0144] [Negative electrode layer: additives]

[0145] The first negative active material layer 22 may further include additives for all-solid-state secondary batteries, such as a filler, a coating agent, a dispersant, and an ion conductive agent.

[0146] [Structure of negative electrode layer]

[0147] The thickness of the first negative electrode active material layer 22 may be, for example, about 50% or less, about 40% or less, about 30% or less, about 20% or less, about 10% or less, or about 5% or less of the thickness of the positive electrode active material layer 12. The thickness of the first negative electrode active material layer 22 may be, for example, in the range of about 1 μm to about 20 μm, about 2 μm to about 10 μm, or about 3 μm to about 7 μm. If the first negative electrode active material layer 22 is too thin, the first negative electrode active material layer 22 may collapse due to lithium dendrites that may form between the first negative electrode active material layer 22 and the negative electrode current collector 21, which may degrade the cycle characteristics of the all-solid-state secondary battery 1. If the first negative electrode active material layer 22 is too thick, the all-solid-state secondary battery 1 may have a reduced energy density and increased internal resistance, and thus the all-solid-state secondary battery 1 may have poor cycle characteristics.

[0148] When the thickness of the first negative active material layer 22 decreases, for example, the first negative active material layer 22 may have a reduced charge capacity. In embodiments, the charge capacity of the first negative active material layer 22 may be about 50% or less, about 40% or less, about 30% or less, about 20% or less, about 10% or less, about 5% or less, or about 2% or less of the charge capacity of the positive active material layer 12. The charge capacity of the first negative active material layer 22 may be, for example, about 0.1% to about 50%, about 0.1% to about 40%, about 0.1% to about 30%, about 0.1% to about 20%, about 0.1% to about 10%, about 0.1% to about 5%, or about 0.1% to about 2% of the charge capacity of the positive active material layer 12. If the charge capacity of the first negative electrode active material layer 22 is too small, the thickness of the first negative electrode active material layer 22 may become so thin that the first negative electrode active material layer 22 may be broken due to lithium dendrites formed between the first negative electrode active material layer 22 and the negative electrode current collector 21 during repeated charge / discharge processes, and thus the all-solid-state secondary battery 1 may have poor cycle characteristics. If the charge capacity of the first negative electrode active material layer 22 is excessively increased, the all-solid-state secondary battery 1 may have reduced energy density and increased internal resistance, and thus the all-solid-state secondary battery 1 may have poor cycle characteristics.

[0149] The charge capacity of the positive active material layer 12 can be obtained by multiplying the charge capacity density (mAh / g) of the positive active material in the positive active material layer 12 by the weight of the positive active material. When different positive active materials are used, the charge capacity density of each positive active material layer can be multiplied by the weight of each positive active material layer, and the sum of the products can be calculated as the charge capacity of the positive active material layer 12. The charge capacity of the first negative active material layer 22 can be calculated in the same manner. That is, the charge capacity of the first negative active material layer 22 can be obtained by multiplying the charge capacity density (mAh / g) of the negative active material in the first negative active material layer 22 by the weight of the negative active material. When different negative active materials are used, the charge capacity density of each negative active material layer can be multiplied by the weight of each negative active material layer, and the sum of the products can be calculated as the charge capacity of the first negative active material layer 22. Here, the charge capacity densities of the positive and negative active materials are estimated capacity densities obtained using an all-solid-state half-cell including lithium metal as a counter electrode. The charge capacity of the positive electrode active material layer 12 and the first negative electrode active material layer 22 can be directly calculated by measuring the charge capacity of an all-solid-state half-cell. The measured charge capacity of each of the positive electrode active material and the negative electrode active material can be divided by the weight of the corresponding active material to obtain the charge capacity density. In practice, the charge capacity of the positive electrode active material layer 12 and the first negative electrode active material layer 22 can be the initial charge capacity measured after the first charge cycle.

[0150] In an implementation, the all-solid-state secondary battery 1 may further include a carbon layer between the first negative electrode active material layer 22 and the solid electrolyte layer 30 .

[0151] [Negative electrode layer: negative electrode current collector]

[0152] In an embodiment, the negative electrode current collector 21 may be formed of a material that does not react with lithium to form an alloy or compound. Examples of the material of the negative electrode current collector 21 may include copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or other suitable materials. The thickness of the negative electrode current collector 21 may be, for example, in the range of about 1 μm to about 20 μm, about 5 μm to about 15 μm, or about 7 μm to about 10 μm.

[0153] The negative electrode current collector 21 may be formed of one of the metal examples or an alloy or coating material of at least two metals selected from the examples. The negative electrode current collector 21 may be in the form of, for example, a plate or foil.

[0154] In implementation, reference Figure 4, the all-solid-state secondary battery 1 may further include a thin film 24 on the negative electrode current collector 21, the thin film 24 including an element that can form an alloy with lithium. The thin film 24 may be between the negative electrode current collector 21 and the first negative electrode active material layer 22. The thin film 24 may include, for example, an element that can form an alloy with lithium. Examples of elements that can form an alloy with lithium may include gold, silver, zinc, tin, indium, silicon, aluminum, bismuth or other suitable elements. The thin film 24 may be formed of one of these metals or of an alloy of various metals. When the thin film 24 is provided on the negative electrode current collector 21, for example, the precipitation form of the second negative electrode active material layer precipitated between the thin film 24 and the first negative electrode active material layer 22 can be further flattened, and thus the cycle characteristics of the all-solid-state secondary battery 1 can be further improved.

[0155] The thickness of the film 24 may be, for example, in the range of about 1 nm to about 800 nm, about 10 nm to about 700 nm, about 50 nm to about 600 nm, or about 100 nm to about 500 nm. If the thickness of the film 24 is less than about 1 nm, the function of the film 24 may not be exhibited. If the film 24 is too thick, the film 24 itself may absorb lithium, so that the precipitation of lithium on the negative electrode layer 20 may be reduced, which may lead to degradation of the energy density of the all-solid-state secondary battery 1, and therefore the cycle characteristics of the all-solid-state secondary battery 1 may be degraded. The film 24 may, for example, be provided on the negative electrode current collector 21 by vacuum vapor deposition, sputtering, electroplating or other appropriate methods.

[0156] [Negative electrode layer: precipitation layer]

[0157] In implementation, reference Figure 5 , the all-solid-state secondary battery 1 may further include a second negative electrode active material layer 23 between the negative electrode current collector 21 and the first negative electrode active material layer 22 by charging. In an embodiment, the all-solid-state secondary battery 1 may further include a second negative electrode active material layer (not shown) between the solid electrolyte layer 30 and the first negative electrode active material layer 22 by charging, or may include only a single second negative electrode active material layer 23. The second negative electrode active material layer 23 may be a metal layer including lithium or a lithium alloy. The metal layer may include lithium or a lithium alloy. The second negative electrode active material layer 23 may be a metal layer including lithium, and the second negative electrode active material layer 23 may be used as, for example, a lithium storage. The lithium alloy may include, for example, a Li-Al alloy, a Li-Sn alloy, a Li-In alloy, a Li-Ag alloy, a Li-Au alloy, a Li-Zn alloy, a Li-Ge alloy, a Li-Si alloy, or other suitable lithium alloys. The second negative electrode active material layer 23 may be formed of one of these alloys or lithium or may be formed of various alloys.

[0158] In implementations, the thickness of the second negative electrode active material layer 23 may be, for example, in the range of about 1 μm to about 1,000 μm, about 1 μm to about 500 μm, about 1 μm to about 200 μm, about 1 μm to about 150 μm, about 1 μm to about 100 μm, or about 1 μm to about 50 μm. If the second negative electrode active material layer 23 is too thin, the second negative electrode active material layer 23 may not function as a lithium storage. If the second negative electrode active material layer 23 is too thick, the weight and volume of the all-solid-state secondary battery 1 may increase, and the cycle characteristics of the all-solid-state secondary battery 1 may deteriorate. The second negative electrode active material layer 23 may be, for example, a metal foil having a thickness within these ranges.

[0159] In the all-solid-state secondary battery 1, the second negative electrode active material layer 23 may be provided between the negative electrode collector 21 and the first negative electrode active material layer 22, for example, before assembly of the all-solid-state secondary battery 1, or may be precipitated between the negative electrode collector 21 and the first negative electrode active material layer 22, for example, by charging after assembly of the all-solid-state secondary battery 1.

[0160] When the second negative electrode active material layer 23 is provided between the negative electrode current collector 21 and the first negative electrode active material layer 22 before assembling the all-solid-state secondary battery 1, the second negative electrode active material layer 23, as a metal layer including lithium, can function as a lithium reservoir. In this regard, the cycle characteristics of the all-solid-state secondary battery 1 including the second negative electrode active material layer 23 can be further improved. In practice, lithium foil can be provided between the negative electrode current collector 21 and the first negative electrode active material layer 22 before assembling the all-solid-state secondary battery 1.

[0161] When the second negative electrode active material layer 23 is provided by charging after assembly of the all-solid-state secondary battery 1, the second negative electrode active material layer 23 may not be present during assembly of the all-solid-state secondary battery 1, and thus the all-solid-state secondary battery 1 may have an increased energy density. In practice, the all-solid-state secondary battery 1 may be charged beyond the charge capacity of the first negative electrode active material layer 22. In practice, the first negative electrode active material layer 22 may be overcharged. During the initial charging phase, lithium may be absorbed into the first negative electrode active material layer 22. In practice, the negative electrode active material in the first negative electrode active material layer 22 may form an alloy or compound with lithium ions that have migrated from the positive electrode layer 10. When the first negative electrode active material layer 22 is charged beyond its capacity, lithium may precipitate on the rear surface of the first negative electrode active material layer 22, for example, between the negative electrode current collector 21 and the first negative electrode active material layer 22, thereby forming a metal layer corresponding to the second negative electrode active material layer 23 from the precipitated lithium. The second negative electrode active material layer 23 may be a metal layer including lithium (e.g., metallic lithium or non-composite lithium) as a main component. This may be attributed to, for example, the negative electrode active material in the first negative electrode active material layer 22 including a material capable of forming an alloy or compound with lithium. During discharge, the lithium in the first negative electrode active material layer 22 and the second negative electrode active material layer 23, e.g., a lithium metal layer, may be ionized and then move toward the positive electrode layer 10. Accordingly, lithium may be used as the negative electrode active material in the all-solid-state secondary battery 1. Furthermore, the first negative electrode active material layer 22 may coat the second negative electrode active material layer 23, and the first negative electrode active material layer 22 may serve as a protective layer for the second negative electrode active material layer 23 and may simultaneously help suppress the precipitation and growth of lithium dendrites. Therefore, short circuiting and capacity reduction of the all-solid-state secondary battery 1 may be suppressed, and as a result, the cycle characteristics of the all-solid-state secondary battery 1 may be improved. Furthermore, when the second negative electrode active material layer 23 is provided by charging after assembly of the all-solid-state secondary battery 1, the negative electrode collector 21, the first negative electrode active material layer 22, and the area between the negative electrode collector 21 and the first negative electrode active material layer 22 may be, for example, a lithium-free area that does not contain lithium (Li) in the initial state or the discharged state of the all-solid-state secondary battery 1.

[0162] According to another embodiment, a method of preparing an all-solid-state secondary battery will be described.

[0163] First, a positive active material, a binder, a sulfide solid electrolyte, a conductive agent, and a compound represented by Formula 1 as a dispersion medium may be mixed to prepare a composition for forming a positive active material layer.

[0164] Formula 1

[0165] R 1 -C(=O)OR 2

[0166] In formula 1, R 1 may be or include, for example, a C1-C2 alkyl group, and R 2 It may be or include, for example, a C7-C9 alkyl group.

[0167] In the composition, the amount of the dispersion medium may be, for example, in the range of about 25 parts by weight to about 65 parts by weight or about 35 parts by weight to about 45 parts by weight based on 100 parts by weight of the solids in the composition for forming the positive electrode active material layer. The amount of the sulfide solid electrolyte may be, for example, in the range of about 5 parts by weight to about 40 parts by weight or about 8 parts by weight to about 30 parts by weight based on 100 parts by weight of the solids in the composition for forming the positive electrode active material layer.

[0168] As used herein, the solid in the composition for forming the positive electrode active material layer refers to a mixture of the positive electrode active material, the binder, the sulfide solid electrolyte, and the conductive agent.

[0169] The composition for forming the positive active material layer may include a non-polar solvent, such as xylene or diethylbenzene, and may further include an organic solvent, such as diethyl carbonate (DEC), dimethyl carbonate, or ethylene carbonate.

[0170] The composition for forming a positive active material layer may be coated on a positive electrode current collector and dried to prepare a positive active material layer, thereby providing a positive electrode layer.

[0171] The drying process may include a first heat treatment (e.g., thermal treatment) process. The first heat treatment process may be performed at a temperature in the range of, for example, about 25°C to about 100°C, about 30°C to about 95°C, about 35°C to about 85°C, about 40°C to about 70°C, or at a temperature of about 40°C. The first heat treatment process may be performed, for example, on a hot plate or in a convection oven.

[0172] The drying process may further include a second heat treatment process. The second heat treatment process may be performed, for example, after the first heat treatment process under vacuum conditions at a temperature in the range of about 40°C to about 100°C, about 50°C to about 95°C, about 55°C to about 90°C, or about 60°C to about 80°C. In implementations, the vacuum conditions may be, for example, at a pressure in the range of about 380 Torr to about 760 Torr.

[0173] In implementation, when the amount of the dispersion medium is controlled as desired through the first heat treatment process for drying, the second heat treatment process may be omitted.

[0174] The heat treatment time for the first heat treatment process may vary according to the temperature range of the first heat treatment process, and, for example, the first heat treatment process may be performed for about 1 hour or more, about 2 hours or more, or about 2 hours to about 4 hours. In an implementation, the heat treatment time for the second heat treatment process may vary according to the temperature range of the second heat treatment process, and, for example, the second heat treatment process may be performed for about 2 hours or more, about 4 hours or more, or about 4 hours to about 8 hours.

[0175] The dried positive electrode layer may include the compound of Formula 1 and the compound of Formula 2, the amount (eg, residual amount) of the compound of Formula 1 may be about 500 ppm or less, and the amount of the compound of Formula 2 may be about 500 ppm or less.

[0176] In addition to the preparation of the positive electrode layer, the method may include providing a negative electrode layer including a negative electrode current collector and a first negative active material layer; providing a solid electrolyte layer between the negative electrode layer and the positive electrode layer to prepare a laminate; and pressing the laminate.

[0177] The pressing of the laminate can be carried out at a temperature in the range of about 25°C to about 90°C and at a pressure in the range of, for example, about 500 MPa or less, or about 400 MPa to about 500 MPa, thereby completing the manufacture of the all-solid-state secondary battery. The pressing time for pressing the laminate may vary depending on the temperature and pressure, and may be, for example, less than 30 minutes. In implementation, the pressing of the laminate may be carried out by, for example, isostatic pressing, roller pressing, or plate pressing.

[0178] The all-solid-state secondary battery according to the embodiment may be applicable to a medium- or large-sized battery or an energy storage system (ESS).

[0179] The following examples and comparative examples are provided to emphasize the characteristics of one or more embodiments, but it will be understood that the examples and comparative examples are not to be construed as limiting the scope of the embodiments, nor are the comparative examples to be construed as being outside the scope of the embodiments. Further, it will be understood that the embodiments are not limited to the specific details described in the examples and comparative examples.

[0180] Preparation Example 1: Preparation of a composition for forming a positive electrode active material layer

[0181] LiNi 0.8 Co 0.15 Mn 0.05O2(NCM) was prepared as the positive electrode active material. A crystalline argyrodite-type solid electrolyte (Li6PS5Cl) was used as a solid electrolyte. In addition, polyvinylidene fluoride (PVDF) (available from Arekema) was used as a binder, and carbon nanofiber (CNF) was used as a conductive agent. The positive electrode active material, solid electrolyte, carbon nanofiber and binder were mixed in a weight ratio of 86.91:11.85:0.25:0.99 and then mixed with a dispersion medium including octyl acetate and diethyl carbonate (DEC, for example, as an organic solvent) in the content ratio shown in Table 1 to prepare a composition for forming a positive electrode active material layer.

[0182] In the composition for forming the positive electrode active material layer, the amounts of octyl acetate and diethyl carbonate are approximately 25 parts by weight and approximately 15 parts by weight, respectively, based on 100 parts by weight of the solids in the composition for forming the positive electrode active material layer. Here, the weight of the solids in the composition for forming the positive electrode active material layer represents the total weight of the positive electrode active material, the solid electrolyte, the carbon nanofibers, and the binder.

[0183] Preparation Examples 2 to 6

[0184] Each composition for forming a positive electrode active material layer was prepared in the same manner as in Preparation Example 1, except that the amounts of octyl acetate as a dispersion medium and DEC as an organic solvent were changed according to Table 1. The amounts of acetate and diethyl carbonate are based on 100 parts by weight of the solids in the composition for forming a positive electrode active material layer. The weight of the solids in the composition for forming a positive electrode active material layer represents the total weight of the positive electrode active material, conductive agent, binder, and sulfide solid electrolyte.

[0185] Preparation Examples 7 and 8

[0186] Compositions for forming a positive electrode active material layer were each prepared in the same manner as in Preparation Example 1, except that heptyl acetate or nonyl acetate was used as a dispersion medium, respectively.

[0187] Table 1

[0188]

[0189] Preparation Example 9

[0190] A positive active material layer forming composition was prepared in the same manner as in Preparation Example 2, except that the amount of octyl acetate was changed to 65 parts by weight based on 100 parts by weight of the solid in the positive active material layer forming composition.

[0191] Comparative Preparation Examples 1 to 7

[0192] Compositions for forming a positive electrode active material layer were each prepared in the same manner as in Preparation Example 1, except that the dispersion medium of Table 2 was used instead of the dispersion medium of Table 1.

[0193] Table 2

[0194] sample dispersion medium Amount of dispersion medium (parts by weight) Comparative Preparation Example 1 Butyl acetate 25 Comparative Preparation Example 2 Amyl acetate 25 Comparative Preparation Example 3 Hexyl acetate 25 Comparative Preparation Example 4 Decyl acetate 25 Comparative Preparation Example 5 Undecyl acetate 25 Comparative Preparation Example 6 Lauryl acetate 25 Comparative Preparation Example 7 Octanol 25

[0195] The amounts of the dispersion medium in Table 2 are based on 100 parts by weight of the solid in the positive electrode active material layer.

[0196] Example 1

[0197] (Preparation of Positive Electrode Layer)

[0198] The composition for forming the positive active material layer of Preparation Example 1 was dispersed 5 times at a rate of 2,000 rpm for 30 seconds each time to prepare a coating slurry. The slurry was applied to a positive electrode substrate coated with a carbon layer having a thickness of about 1 μm using a rod coater to prepare a positive electrode. The positive electrode plate was then dried by performing a first heat treatment process in a convection constant temperature oven at about 40°C for about 2 hours. Subsequently, the positive electrode plate was dried by performing a second heat treatment process in a vacuum oven at about 80°C for about 4 hours to prepare a positive electrode layer.

[0199] (Preparation of Negative Electrode Layer)

[0200] A Ni foil having a thickness of about 10 μm was prepared as a negative electrode current collector, and carbon black (CB) having a primary particle size of about 30 nm and silver (Ag) particles having an average particle size of about 60 nm were prepared as negative electrode active materials.

[0201] 0.25 g of a mixture powder prepared by mixing carbon black (CB) and silver (Ag) particles in a weight ratio of about 3: 1 was placed in a container, and 2 g of an N-methyl-2-pyrrolidone (NMP) solution including about 7 weight % (wt %) of a PVDF binder (#9300 available from Kureha Co.) was added to the container to prepare a mixture solution. Next, while gradually adding NMP to the mixture solution, the mixture solution was stirred to prepare a slurry. The prepared slurry was applied to a Ni foil using a rod coater and dried in a convection oven at about 80°C for about 10 minutes to obtain a laminate. The laminate was vacuum dried at a temperature of about 100°C for about 10 hours. Through these processes, a negative electrode layer including a first negative active material layer prepared on a negative electrode collector was prepared.

[0202] (Preparation of Solid Electrolyte Layer)

[0203] An acrylic binder (SX-A334, Zeon Co., Ltd.) was added to octyl acetate to prepare a 4 wt% acrylic binder solution. The acrylic binder solution was added to a Li6PS5Cl solid electrolyte (D50 = 3 μm, crystalline) as an argyrodite-type crystal and mixed using a Thinky mixer to prepare a slurry. The slurry included approximately 1.5 parts by weight of an acrylic binder and 98.5 parts by weight of a solid electrolyte. The slurry was applied to a non-woven fabric using a rod coater and dried in a convection oven at approximately 50°C for approximately 5 minutes to obtain a laminate. The laminate was dried in a vacuum oven at a temperature of approximately 40°C for approximately 10 hours. Through these processes, a solid electrolyte layer was prepared.

[0204] (Preparation of All-Solid-State Secondary Batteries)

[0205] The solid electrolyte layer is arranged between the positive electrode layer and the negative electrode layer to prepare a laminate. The laminate is hot-plate pressed at a temperature of about 80°C and a pressure of about 500 MPa for about 30 minutes to prepare an all-solid-state secondary battery. The solid electrolyte layer is sintered by the pressing process, and the battery characteristics of the all-solid-state secondary battery are improved. The thickness of the pressed positive electrode active material layer is about 100 μm, the thickness of the negative electrode active material layer is about 7 μm, and the thickness of the solid electrolyte layer is about 60 μm.

[0206] Examples 2 to 8

[0207] The positive electrode layer and the all-solid-state secondary battery were prepared in the same manner as in Example 1, except that drying was performed by a heat treatment process under the conditions shown in Table 3, instead of performing a first heat treatment process in a convection constant temperature oven at about 40°C for about 2 hours and a second heat treatment process in a vacuum oven at about 80°C for about 4 hours during the preparation of the positive electrode layer.

[0208] Example 9

[0209] A positive electrode layer and an all-solid-state secondary battery were prepared in the same manner as in Example 1, except that the composition for forming a positive electrode active material layer of Preparation Example 9 was used instead of the composition for forming a positive electrode active material layer of Preparation Example 1 during the preparation of the positive electrode layer.

[0210] Comparative Examples 1 to 5

[0211] The negative electrode layer and the all-solid-state secondary battery were prepared in the same manner as in Example 1, except that during the preparation of the positive electrode layer, the compositions for forming the positive electrode active material layer of Comparative Preparation Examples 1 to 5 were used instead of the composition for forming the positive electrode active material layer of Preparation Example 1.

[0212] Table 3

[0213]

[0214] In Comparative Examples 1 and 2, the solid electrolyte reacted with the solvent and thus lost the ion conductivity characteristic of the battery, and thus no battery was formed.

[0215] Comparative Example 6

[0216] The negative electrode layer and the all-solid-state secondary battery were prepared in the same manner as in Example 1, except that the composition for forming the positive electrode active material layer of Comparative Preparation Example 6 was used instead of the composition for forming the positive electrode active material layer of Preparation Example 1 during the preparation of the positive electrode layer under the following conditions.

[0217] (Preparation of Positive Electrode Layer)

[0218] The composition for forming a positive electrode active material layer of Comparative Preparation Example 6 was dispersed 5 times for 30 seconds each time at a rate of 2,000 rpm using a Thinky mixer to prepare a coating slurry. The slurry was applied to a positive electrode substrate coated with a carbon layer having a thickness of about 1 μm using a rod coater to prepare a positive electrode. The positive electrode plate was then dried in a convection oven at about 40°C for about 2 hours. Subsequently, the positive electrode plate was dried in a vacuum oven at about 80°C for about 8 hours to prepare a positive electrode sheet.

[0219] According to Comparative Example 6, lauryl acetate has low reactivity with the sulfide solid electrolyte but a high boiling point, and therefore, the temperature of the drying process in Comparative Example 6 needs to be increased to about 100° C. to remove the lauryl acetate in the positive electrode layer. However, when the temperature of the drying process is increased in this manner, the sulfide solid electrolyte deteriorates, and thus, the capacity characteristics of the battery also deteriorate as a result.

[0220] Comparative Example 7

[0221] The same process as in Example 1 was performed except that the composition for forming a positive electrode active material layer of Comparative Preparation Example 7 was used during the preparation of the positive electrode layer instead of the composition for forming a positive electrode active material layer of Preparation Example 1.

[0222] However, according to Comparative Example 7, octanol dissolved the sulfide solid electrolyte Li 6 PS 5 Cl, and thus a positive electrode layer and an all-solid-state secondary battery could not be prepared.

[0223] Evaluation Example 1: Reactivity with sulfide solid electrolyte

[0224] The reactivity of the dispersion media used in Preparation Examples 1 to 8 and Comparative Preparation Examples 1 to 6 with respect to the sulfide solid electrolyte Li6PS5Cl was evaluated according to the following method.

[0225] After 2 g of the dispersion medium and 0.2 g of the sulfide solid electrolyte were mixed and stirred, the resultant was observed for 3 days to check color change to evaluate the reactivity of the dispersion medium and the sulfide solid electrolyte.

[0226] ○: Color changes immediately after mixing (highly reactive to sulfide solid electrolyte)

[0227] △: Color change 1 to 3 days after mixing (reactive to sulfide solid electrolyte)

[0228] X: No color change after 3 days (no reactivity to sulfide solid electrolyte)

[0229] The results of the evaluation are shown in Table 4.

[0230] The results are an evaluation of the reactivity of the sulfide solid electrolyte Li6PS5Cl using octyl acetate or butyl acetate.

[0231] Figure 6A shows the case when octyl acetate is used as a dispersion medium, and Figure 6B The case where butyl acetate is used as the dispersion medium is shown. Figure 6A and Figure 6B , part (a) shows the initial state after mixing, and part (b) shows the state in which the solid electrolyte is dispersed after 3 days.

[0232] refer to Figure 6A , it can be seen that when octyl acetate is used as the dispersion medium, the reactivity of the dispersion medium with the sulfide solid electrolyte is low. Figure 6B , it can be seen that, when butyl acetate was used as the dispersion medium, butyl acetate reacted with the sulfide solid electrolyte, and thus a change in the color of the mixture was observed.

[0233] Evaluation Example 2: Charge / Discharge Test

[0234] The charge / discharge characteristics of the all-solid-state secondary batteries prepared in Examples 1 to 8 and Comparative Examples 1 to 6 were evaluated by the following charge / discharge test.

[0235] The battery was charged at a constant current of about 0.1 C for 10 hours until the battery voltage was about 4.25 V, and then discharged at a constant current of about 0.1 C for 10 hours until the battery voltage was about 2.5 V (1st cycle). Subsequently, the battery was charged at a constant current of about 0.1 C for 10 hours until the battery voltage was about 4.25 V, and then discharged at a constant current of about 0.33 C for 3 hours until the battery voltage was about 2.5 V (2nd cycle). Then, the battery was charged at a constant current of about 0.1 C for 10 hours until the battery voltage was about 4.25 V. Subsequently, the battery was discharged at a constant current of about 1 C for 1 hour until the battery voltage was about 2.5 V (3rd cycle)

[0236] Thereafter, the battery was charged at a constant current of about 0.33 C for 3 hours until the battery voltage reached about 4.25 V. Next, the battery was charged at a constant current of about 0.33 C for 3 hours until the battery voltage reached about 2.5 V (4th cycle).

[0237] The cycle was repeated a total of 100 times. The life characteristics of the battery are shown in Table 4. In Table 4, the average voltage indicates the average voltage after 100 cycles.

[0238] The lifespan characteristic indicates a cycle in which the battery capacity is 60% without a short circuit occurring.

[0239] Table 4

[0240]

[0241]

[0242] As shown in Table 4, the all-solid-state secondary batteries of Examples 1 to 8 have excellent capacity, average voltage, and lifespan characteristics compared to those of the all-solid-state secondary batteries of Comparative Examples 3 to 6.

[0243] In contrast, the all-solid-state secondary batteries of Comparative Examples 1 and 2, which used butyl acetate and amyl acetate, respectively, as dispersion media, were highly reactive to the sulfide solid electrolyte, and thus single-cell performance of the batteries could not be measured.

[0244] Like the all-solid-state secondary battery of Comparative Example 1, the all-solid-state secondary battery of Comparative Example 3 using hexyl acetate as a dispersion medium is highly reactive to the sulfide solid electrolyte, and thus as a result, the single cell performance of the battery of Comparative Example 3 appears to be poor.

[0245] The boiling point of the dispersion medium used in the preparation of the positive electrode layer of the all-solid-state secondary batteries of Comparative Examples 4 to 6 was high, and the amount of the dispersion medium remaining after the vacuum drying process was high, which led to deterioration in the performance of the single cells. In particular, when a dispersion medium with a high boiling point is used to prepare the positive electrode layer, the solid electrolyte may deteriorate when the battery is heat-treated at a temperature of about 100°C or higher to remove the high-boiling-point dispersion medium, and thus the capacity characteristics of the all-solid-state secondary battery may deteriorate.

[0246] And, the voltage change according to the specific capacity of the all-solid-state secondary batteries of Example 1 and Comparative Example 4 was evaluated, and the results showed that Figure 1 middle.

[0247] refer to Figure 1 , it can be seen that the all-solid-state secondary battery of Example 1 (which used octyl acetate as a dispersion medium during the preparation of the positive electrode layer) has excellent capacity characteristics compared to those of the all-solid-state secondary battery of Comparative Example 4 (which used decyl acetate as a dispersion medium). In this regard, it can be seen that when the number of carbon atoms bonded to the oxygen atom of the ester group in the compound of Formula 1 is 8, the capacity characteristics of the all-solid-state secondary battery can be improved compared to those with 10 carbon atoms.

[0248] Also, the charge / discharge characteristics of the all-solid-state secondary battery of Example 9 were evaluated in the same manner as in the test method of the charge / discharge characteristics of the all-solid-state secondary battery of Example 1 described above.

[0249] As a result of evaluation, the all-solid-state secondary battery of Example 9 exhibited the same charge / discharge characteristics as those of the all-solid-state secondary battery of Example 1.

[0250] Evaluation Example 3: Headspace Sampler Gas Chromatography / Mass Spectrometry (HSS-GC / MS)

[0251] The residual dispersion medium in the positive electrode layers prepared in Examples 1 to 8 and Comparative Examples 1 to 6 was analyzed using HSS-GC / MS. A GC6890N available from Agilent was used for HSS-GC / MS analysis. Analysis was performed using an RTX-200 column at a flow rate of 3 mL / min, with an inlet temperature of approximately 210°C, and the furnace temperature was increased from approximately 50°C to approximately 260°C at a rate of 15°C / min. The HSS furnace temperature was set to approximately 180°C, and the measurement time was set to 5 minutes.

[0252] The results of analyzing the amount of residual dispersion medium are shown in Table 5 and Figure 2A and Figure 2B middle.

[0253] Table 5

[0254]

[0255] Figure 2A and Figure 2B Results of analyzing the components of the residual dispersion medium in the positive electrode layer prepared in Example 1 are shown.

[0256] refer to Figure 2A The positive electrode layer of Example 1 has a main peak related to octyl acetate and a secondary peak related to octanol. In addition, peaks related to sulfur dioxide and 1-octanethiol were observed. Figure 2B As a decomposition product of the first dispersion medium, a second dispersion medium is generated. It is believed that adhesion with various surrounding materials occurs during the decomposition.

[0257] According to an embodiment, a composition for forming a positive electrode active material layer containing a dispersion medium that helps reduce degradation of a sulfide solid electrolyte and helps improve solubility characteristics for a binder can be used to prepare a positive electrode layer for an all-solid-state secondary battery. The all-solid-state secondary battery including the positive electrode layer can have excellent capacity characteristics and an improved lifespan.

[0258] By summarizing and reviewing, currently commercialized lithium-ion batteries may use electrolyte solutions containing flammable organic dispersion media, and therefore there is a possibility of overheating and fire when a short circuit occurs. As a result, all-solid-state batteries that use solid electrolytes instead of electrolyte solutions have been considered.

[0259] All-solid-state batteries do not use flammable organic dispersion media and, even if a short circuit occurs, significantly reduce the possibility of overheating and fire. Therefore, compared to lithium-ion batteries that use electrolyte solutions, these all-solid-state batteries can significantly enhance safety.

[0260] In addition to the positive active material, the positive electrode layer of an all-solid-state battery may contain a sulfide solid electrolyte with excellent ionic conductivity. For commercialization of all-solid-state batteries including a positive electrode layer containing a sulfide solid electrolyte, the positive electrode layer may be formed by a wet coating process. Sulfide solid electrolytes can be easily degraded by air, moisture, and / or polar solvents, and when a sulfide solid electrolyte is used to prepare a positive electrode layer by a wet coating process, the performance of the all-solid-state battery may deteriorate.

[0261] One or more embodiments may provide an all-solid-state secondary battery with improved performance by including a positive electrode layer.

[0262] Example embodiments have been disclosed herein, and although specific terms are employed, they are used and interpreted in a general and descriptive sense only and not for purposes of limitation. In some cases, as will be apparent to one of ordinary skill in the art of filing this application, features, characteristics, and / or elements described in conjunction with a particular embodiment may be used alone or in combination with features, characteristics, and / or elements described in conjunction with other embodiments, unless specifically indicated otherwise. Accordingly, it will be understood by those skilled in the art that various changes in form and detail may be made without departing from the spirit and scope of the invention as set forth in the appended claims.

Claims

1. A positive electrode layer for an all-solid-state secondary battery, the positive electrode layer comprising a positive electrode current collector and a positive electrode active material layer on the positive electrode current collector, in: The positive electrode active material layer comprises: Positive electrode active material, Binder, Conductive agent, Sulfide solid electrolyte, and A dispersion medium comprising a compound represented by Formula 1 and a compound represented by Formula 2, wherein Formula 1 R 1 -C(=O)O-R 2 In formula 1, R 1 is a C1-C2 alkyl group and R 2 is a C7-C9 alkyl group, Formula 2 R 2’ -OH In formula 2, R 2’ It is a C7-C9 alkyl group.

2. The positive electrode layer according to claim 1, wherein the dispersion medium comprises a mixture of: Octyl acetate as the compound represented by Formula 1 and octanol as the compound represented by Formula 2, Nonyl acetate as the compound represented by Formula 1 and nonanol as the compound represented by Formula 2, or Heptyl acetate as the compound represented by Formula 1 and heptanol as the compound represented by Formula 2. 3 . The positive electrode layer according to claim 1 , wherein an amount of the compound represented by Formula 1 in the positive electrode layer is 500 ppm or less. 4 . The positive electrode layer according to claim 1 , wherein an amount of the compound represented by Formula 2 in the positive electrode layer is 500 ppm or less. 5 . The positive electrode layer according to claim 1 , wherein the amount of the compound represented by Formula 2 in the positive electrode layer is in the range of 5 ppm to 500 ppm relative to 100 ppm of the amount of the compound represented by Formula 1 in the positive electrode layer. 6 . The positive electrode layer according to claim 1 , wherein the binder comprises polyvinylidene fluoride, styrene butadiene rubber, polytetrafluoroethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, or a combination thereof. 7 . The positive electrode layer of claim 1 , wherein the conductive agent comprises graphite, carbon black, carbon nanofibers, carbon nanotubes, or a combination thereof.

8. The positive electrode layer according to claim 7, wherein the carbon black comprises acetylene black.

9. The positive electrode layer according to claim 1, wherein the sulfide solid electrolyte comprises Li2S-P2S5; Li2S-P2S5-LiX, wherein X is a halogen element; Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S-P2S5-Z m S n , wherein m and n are each positive numbers, and Z is Ge, Zn or Ga; Li2S-GeS2; Li2S-SiS2-Li3PO4; Li2S-SiS2-Li p MO q , wherein p and q are each positive numbers, and M is P, Si, Ge, B, Al, Ga or In; Li 7-x PS 6-x Cl x , where 0≤x≤2; Li 7-x PS 6-x Br x , where 0<x≤2; or Li 7-x PS 6-x I x , where 0<x≤2. 10 . The positive electrode layer according to claim 1 , wherein the sulfide solid electrolyte is an argyrodite-type solid electrolyte including Li 6 PS 5 Cl, Li 6 PS 5 Br or Li 6 PS 5 I.

11. An all-solid-state secondary battery, comprising: The positive electrode layer according to any one of claims 1 to 10; negative electrode layer; and A solid electrolyte is provided between the positive electrode layer and the negative electrode layer, wherein the solid electrolyte comprises a sulfide solid electrolyte.

12. The all-solid-state secondary battery according to claim 11, wherein: The negative electrode layer includes a negative electrode current collector and a first negative electrode active material layer; or the negative electrode layer includes a negative electrode current collector, a first negative electrode active material layer and a second negative electrode active material layer, The second negative electrode active material layer: On the first negative electrode active material layer, between the negative electrode current collector and the first negative electrode active material layer, or on the first negative active material layer and between the negative electrode current collector and the first negative active material layer, and The second negative electrode active material layer includes lithium or a lithium alloy.

13. The all-solid-state secondary battery according to claim 11, wherein: The negative electrode layer includes a negative electrode current collector and a first negative electrode active material layer, and The all-solid-state secondary battery further includes a carbon layer between the first negative electrode active material layer and the solid electrolyte.

14. A method for preparing an all-solid-state secondary battery, the method comprising: mixing a positive electrode active material, a binder, a sulfide solid electrolyte, a conductive agent, and a compound represented by Formula 1 to prepare a composition for forming a positive electrode active material layer; forming a positive electrode active material layer by coating and drying the composition for forming a positive electrode active material layer on a positive electrode current collector to form a positive electrode layer on the positive electrode current collector; providing a negative electrode layer, the negative electrode layer comprising a negative electrode current collector and a first negative electrode active material layer; preparing a laminate by providing a solid electrolyte between the negative electrode layer and the positive electrode layer, the solid electrolyte comprising a sulfide solid electrolyte; and pressing the laminate, Formula 1 R 1 -C(=O)O-R 2 Among them, in formula 1, R 1 is a C1-C2 alkyl group, and R 2 It is a C7-C9 alkyl group.

15. The method of claim 14, wherein drying the composition comprises: performing a first heat treatment at a temperature in a range of 25° C. to 100° C.; and The second heat treatment is performed in vacuum at a temperature ranging from 40°C to 100°C.

16. The method of claim 14, wherein: After drying the composition, the positive electrode layer includes a dispersion medium containing the compound represented by Formula 1 and the compound represented by Formula 2, The amount of the compound represented by Formula 1 in the positive electrode layer is 500 ppm or less, The amount of the compound represented by Formula 2 in the positive electrode layer is 500 ppm or less, Formula 2 R 2’ -OH In formula 2, R 2’ It is a C7-C9 alkyl group.

17. The method according to claim 16, wherein the dispersion medium comprises a mixture of: Octyl acetate as the compound represented by Formula 1 and octanol as the compound represented by Formula 2, Nonyl acetate as the compound represented by Formula 1 and nonanol as the compound represented by Formula 2, or Heptyl acetate as the compound represented by Formula 1 and heptanol as the compound represented by Formula 2.

18. A composition for forming a positive electrode active material layer for an all-solid-state secondary battery, the composition comprising: Positive electrode active material; Binder; Conductive agent; Sulfide solid electrolyte; and The compound represented by Formula 1, Formula 1 R 1 -C(=O)O-R 2 Among them, in formula 1, R 1 is a C1-C2 alkyl group, and R 2 It is a C7-C9 alkyl group. 19 . The composition according to claim 18 , wherein the compound represented by Formula 1 is included in the composition in an amount of 25 parts by weight to 65 parts by weight based on 100 parts by weight of a solid in the composition.

20. The composition of claim 18, wherein the compound represented by Formula 1 comprises octyl acetate, nonyl acetate, heptyl acetate, or a combination thereof.

21. The composition of claim 18, further comprising a solvent comprising heptane, xylene, toluene, diethylbenzene, diethyl carbonate, or dimethyl carbonate.

Citation Information

Patent Citations

  • Display device and driving method thereof

    KR1020200110587A

  • Sulfide solid electrolyte

    CN113557616A