Use of nanoparticle compositions as heat transfer fluids in battery or other electrical device systems
By using heat transfer fluids between nanoparticles and polymer compositions in hydrophobic media, the stability and heat transfer performance of nanoparticles at high temperatures and long-term times are solved, and efficient cooling and energy efficiency improvement of electrical equipment are achieved.
Patent Information
- Application Number
- CN202080051229.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-07-17
- Filing Date
- 2020-07-13
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-07-13
AI Technical Summary
The prior art is difficult to maintain the stability and heat transfer properties of nanoparticles in hydrophobic media, especially at high temperatures and long-term times, and the increase in the viscosity of the heat transfer fluid leads to an increase in pressure loss, affecting the efficiency and life of electrical equipment.
The composition of nanoparticles and polymer composition is used as heat transfer fluid, and the mixture contains metal or metalloid nitrides, carbon nanotubes, carbon black and other nanoparticles and functional monomer polymers to form a stable hydrophobic medium. Enhance heat transfer and thermal conductivity, and improve the dispersion of nanoparticles through ultrasound or ball milling.
Long-term stable dispersion of nanoparticles in hydrophobic media is achieved, heat transfer and thermal conductivity are improved, friction performance is reduced, the service life of electrical equipment is extended, and energy efficiency is improved.
Smart Images

Figure FDA0005076680420000041 
Figure FDA0005076680420000042 
Figure FDA0005076680420000043
Abstract
Description
Technical Field
[0001] The present invention relates to the use of nanoparticle compositions as heat transfer fluids in battery systems or other electrical devices, particularly batteries, electric motors, electric vehicle transmissions, power transformers, capacitors, fluid-filled transmission lines, fluid-filled power cables, computers and power electronic components, such as power converters. Background Art
[0002] In recent years, energy shortages and environmental issues have had a huge impact on technological progress. The increase in environmental awareness has led to a growing interest in so-called green technologies, especially in the automotive industry. The demand for emission-free vehicles fueled by renewable energy, such as pure electric vehicles (EVs), hybrid electric vehicles (HEVs), and fuel cell electric vehicles, has gradually become more and more significant and is expected to increase dramatically in the next 20 years. The energy for such vehicles is provided and stored in batteries with high specific energy density. EVs and HEVs can use a variety of batteries, such as lead-acid, zinc / halogen, metal / air, sodium-β, nickel metal hydride (Ni-MH), and lithium ion (Li-ion).
[0003] To improve the performance of electric vehicles, large batteries with high current discharge are required. Due to their size and power output, these large batteries generate a lot of heat during rapid charge and discharge cycles at high current levels. Therefore, the battery must be thermally managed by cooling or heat dissipation to avoid battery failure and extend the life of the battery.
[0004] Furthermore, the performance of batteries is temperature-dependent. Depending on the type of battery, they can only reach their optimum performance within a certain temperature range. Therefore, proper thermal management enables optimization of battery performance.
[0005] In addition, there is increasing interest in using nanoparticles in lubricant formulations. Lubricants typically contain a base fluid and a variable amount of additives. Some additives in lubricant formulations are used to reduce friction and wear between contacts, which is important for the energy efficiency and durability of the device being lubricated. The nanoparticles are particularly useful for achieving boundary lubrication and keeping surfaces apart. Studies have shown that adding nanoparticles can greatly improve wear and friction properties (Zhou et al., Tribology Letters 8, 213-218 (2000); Qiu et al., J. Tribol. 123 (3), 441-443 (2001)).
[0006] However, constructing stable dispersions of nanoparticles is problematic. Most untreated nanoparticles, such as hBN and metal disulfides, are hydrophilic in nature and therefore form poor dispersions in oil or non-polar environments. In addition, the poor dispersibility of the particles and weak forces draw the particles together, resulting in agglomerations. These agglomerates will result in sedimentation, which is undesirable and ineffective for the formulation.
[0007] WO 2018 / 019783 A1 discloses stabilizing oxide and oxidized metal nanoparticles by covalently bonding the nanoparticles to a polymer having (meth) alkyl acrylate monomer units. The document does not mention thermal management applications.
[0008] Naser Ali et al., Review article (2018): “A review on nanofluids: fabrication, stability and thermophysical properties” deals with the development of nanofluids and states that the stability of nanofluids is a very important factor in commercial nanofluids because it prolongs the shelf life of the product while retaining its thermophysical properties. It also states that a major disadvantage of using this type of fluid is the increase in pressure loss in the piping system caused by the increased viscosity of the nanofluid. In this document, mainly hydrophilic heat transfer fluids are described as the prior art.
[0009] WO 2013 / 115925 A1 discloses a nanocomposite fluid comprising a fluid medium and a nanoparticle composition comprising the following nanoparticles, which are electrically insulating and thermally conductive. The document does not give any specific examples for preparing the nanocomposite fluid. No details are given about the stability of the nanocomposite fluid, nor is any comparison of viscosity and thermal conductivity with a corresponding reference base fluid described.
[0010] US2004 / 069454 A1 discloses a composition for use in a heat transfer system, wherein the composition comprises a metal nanoparticle powder dispersed in a heat transfer medium, wherein the nanoparticles are coated with a coating for imparting corrosion resistance and acting as a dispersant.
[0011] US2015 / 048272 A1 also discloses a method for preparing a nanofluid having heat transfer capability, wherein the heat transfer fluid may contain water, ethylene glycol or a mixture thereof and a metal oxide, such as aluminum oxide (see Table 1 of US2015 / 048272 A1).
[0012] WO2017 / 132122A1 relates to a heat transfer fluid for a battery, comprising functionalized carbon nanoparticles and particles of one or more semi-crystalline polymers dispersed in a polar liquid. It is described that the disclosed composition has the ability to absorb thermal energy by melting the semi-crystalline polymer particles, while the addition of the carbon nanoparticles provides thermal conductivity to the disclosed composition. There is no disclosure about stabilizing the particles in a non-polar medium. Summary of the invention
[0013] The object of the present invention is to provide a kind of in the electrical equipment with moving parts such as motor and electric vehicle transmission, or in the electrical equipment without any moving parts such as battery, power transformer, capacitor, fluid-filled transmission line, fluid-filled power cable, computer or power electronic component (for example power converter) The novel method of heat transfer.Usually, if it is possible to directly contact with metal parts, the hydrophobic dielectric fluid producing electrical insulation is preferred because of safety reasons, because they prevent electrical contact.Therefore, the object of the present invention is to provide improved heat transfer nanofluid, it has the stability that nanoparticles increase in hydrophobic medium.When using in electrical device, described heat transfer nanofluid should keep stable and meet the standard of application over time, for example in the improved heat transfer performance for a long time and at different temperatures.If described electrical equipment has moving parts, described heat transfer nanofluid should also have good tribological properties and stability (so-called cooling lubricant) under adverse conditions. SUMMARY OF THE INVENTION
[0015] In the present invention, it has been surprisingly found that the nanoparticle composition comprising nanoparticles and polymers according to the present invention can be used as a heat transfer fluid for batteries and other electrical devices. The challenge is to combine good heat transfer properties while keeping the nanoparticles contained in the heat transfer fluid in a good dispersed state for a long time at high temperature. This target use is achieved using the composition according to the present invention.
[0016] Another advantage of using the nanoparticle composition according to the invention as a heat transfer fluid in electrical equipment with mechanical moving parts is that the moving parts also acquire anti-friction properties due to the nanoparticles being very well dispersed in the lubricating oil.
[0017] Thus, according to a first aspect, the present invention relates to the use of a nanoparticle composition according to the invention as a heat transfer fluid. The nanoparticle composition according to the invention is advantageously used as a heat transfer fluid for electrical devices such as batteries, electric motors, electric vehicle transmissions, power transformers, capacitors, fluid-filled transmission lines, fluid-filled power cables, computers or power electronic components, such as power converters. DETAILED DESCRIPTION OF THE INVENTION
[0019] Thus, the present invention relates to the use of a nanoparticle composition as a heat transfer fluid in a battery or other electrical device system, wherein the nanoparticle composition is obtainable by grinding a mixture comprising one or more nanoparticle compounds (A) and one or more polymer compounds (B),
[0020] (A) wherein the one or more nanoparticle compounds are selected from:
[0021] - Metal or metalloid nitride nanoparticles;
[0022] -Multi-walled or single-walled carbon nanotubes;
[0023] - carbon black;
[0024] - has the molecular formula MX 2 A metal chalcogenide of wherein M is a metal element selected from titanium (Ti), vanadium (V), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), zirconium (Zr), niobium (Nb), molybdenum (Mo), tantalum (Ta), tungsten (W), osmium (Os), and combinations thereof, and X is a chalcogen element selected from sulfur (S), oxygen (O), and combinations thereof;
[0025] - or a mixture thereof,
[0026] and
[0027] (B) wherein the one or more polymer compounds are obtainable by polymerizing the following monomer composition, the monomer composition comprising:
[0028] a) 1 to 30 wt % of one or more functional monomers, based on the total weight of the monomer composition, selected from:
[0029] a1) Aminoalkyl (meth)acrylates and aminoalkyl (meth)acrylamides, such as N-(3-dimethylaminopropyl)methacrylamide, 3-diethylaminopentyl (meth)acrylate, 3-dibutylaminohexadecyl (meth)acrylate;
[0030] a2) alkyl(meth)acrylic acid nitriles and other nitrogen-containing (meth)acrylic acid esters, such as N-(methacryloyloxyethyl)diisobutylketimine, N-(methacryloyloxyethyl)di(hexadecyl)ketimine, (meth)acrylamidoacetonitrile, 2-methacryloyloxyethylmethylcyanamide, cyanomethyl(meth)acrylate;
[0031] a3) (Meth)acrylic esters of ether alcohols, such as tetrahydrofurfuryl (meth)acrylate, methoxyethoxyethyl (meth)acrylate, 1-butoxypropyl (meth)acrylate, cyclohexyloxyethyl (meth)acrylate, propoxyethoxyethyl (meth)acrylate, benzyloxyethyl (meth)acrylate, furfuryl (meth)acrylate, 2-butoxyethyl (meth)acrylate, 2-ethoxy-2-ethoxyethyl (meth)acrylate, 2-methoxy-2-ethoxypropyl (meth)acrylate, ethoxylated (meth)acrylates, 1-ethoxybutyl (meth)acrylate, methoxyethyl (meth)acrylate, 2-ethoxy-2-ethoxy-2-ethoxyethyl (meth)acrylate, esters of (meth)acrylic acid and methoxypolyethylene glycol;
[0032] a4) epoxyalkyl (meth)acrylates, such as 2,3-epoxybutyl (meth)acrylate, 3,4-epoxybutyl (meth)acrylate, 10,11-epoxyundecyl (meth)acrylate, 2,3-epoxycyclohexyl (meth)acrylate, epoxyalkyl (meth)acrylates, such as 10,11-epoxyhexadecyl (meth)acrylate, glycidyl (meth)acrylate;
[0033] a5) phosphorus-, boron- and / or silicon-containing alkyl (meth)acrylates, such as 2-(dimethylphosphato)propyl (meth)acrylate, 2-(ethylphosphite)propyl (meth)acrylate, 2-dimethylphosphinomethyl (meth)acrylate, dimethylphosphonoethyl (meth)acrylate, diethyl methacryloylphosphonate, dipropyl methacryloylphosphate, 2-(dibutylphosphono)ethyl (meth)acrylate, 2,3-butylene methacryloylethylborate, methyldiethoxymethacryloylethoxysilane, diethylphosphatoethyl (meth)acrylate;
[0034] a6) Heterocyclic alkyl (meth)acrylates, such as 2-(1-imidazolyl)ethyl (meth)acrylate, 2-(4-morpholinyl)ethyl (meth)acrylate, oxazolidinyl ethyl ester and N-methacryloyl morpholine;
[0035] a7) Vinyl halides, such as vinyl chloride, vinyl fluoride, vinylidene chloride and vinylidene fluoride;
[0036] a8) Vinyl esters, such as vinyl acetate;
[0037] a9) vinyl monomers containing aromatic groups, such as styrene, substituted styrenes having alkyl substituents in the side chains, for example α-methylstyrene and α-ethylstyrene, substituted styrenes having alkyl substituents on the ring, for example vinyltoluene and p-methylstyrene, halogenated styrenes, for example monochlorostyrene, dichlorostyrene, tribromostyrene and tetrabromostyrene;
[0038] a10) Heterocyclic vinyl compounds, such as 2-vinylpyridine, 3-vinylpyridine, 2-methyl-5-vinylpyridine, 3-ethyl-4-vinylpyridine, 2,3-dimethyl-5-vinylpyridine, vinylpyrimidine, vinylpiperidine, 9-vinylcarbazole, 3-vinylcarbazole, 4-vinylcarbazole, 1-vinylimidazole, 2-methyl-1-vinylimidazole, N-vinylpyrrolidone, 2-vinylpyrrolidone, N-vinylpyrrolidine, 3-vinylpyrrolidine, N-vinylcaprolactam, N-vinylbutyrolactam, vinyloxolane, vinylfuran, vinylthiophene, vinylthiolane, vinylthiazole and hydrogenated vinylthiazole, vinyl Azoles and Hydrogenated Vinyl Azoles;
[0039] a11) vinyl and prenyl ethers;
[0040] a12) methacrylic acid and acrylic acid,
[0041] b) 30 to 80 weight percent, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylate monomers, wherein each of the alkyl groups of the one or more alkyl (meth)acrylate monomers is independently linear, cyclic or branched and contains 1 to 40 carbon atoms, and
[0042] c) 20 to 60 wt % of one or more (meth)acrylic acid esters and one or more monomers having a number average molecular weight (M) of 500 to 10,000 g / mol, based on the total weight of the monomer composition. n ) is a hydroxylated hydrogenated polybutadiene formed by a reaction product,
[0043] and wherein the weight ratio of the one or more nanoparticle compounds (A) to the one or more polymer compounds (B) is 9:1 to 1:5.
[0044] According to a preferred embodiment, the weight ratio of the one or more nanoparticle compounds (A) to the one or more polymer compounds (B) is preferably 9:1 to 1:2, more preferably 5:1 to 1:2, most preferably 3:1 to 1:2.
[0045] According to another preferred embodiment, the amount of monomers a), b) and c) totals 100% by weight, based on the total weight of the monomer composition.
[0046] As used herein, "one or more" means that at least one or more than one of the described components or elements can be used as disclosed.
[0047] As used herein, "other electrical equipment systems" means electrical equipment such as batteries, electric motors, electric vehicle transmissions, power transformers, capacitors, fluid-filled transmission lines, fluid-filled power cables, computers, or power electronics components such as power converters.
[0048] The use defined above also means a method for enhancing heat transfer and thermal conductivity in a heat transfer fluid used in a battery or other electrical device system, wherein the nanoparticle composition is obtainable by grinding a mixture comprising one or more nanoparticle compounds (A) and one or more polymer compounds (B), as mentioned herein.
[0049] As demonstrated in the experimental part herein, the heat transfer nanofluids according to the invention show an increased stability of the nanoparticles in hydrophobic media.
[0050] According to the present invention, preferably the heat transfer fluid further comprises a base fluid (C) having a kinematic viscosity at 40°C of 3 to 30 cSt according to ASTM D-445 and a flash point above 110°C according to ASTM D-93.
[0051] Advantageously, it has been observed that nanoparticle compositions used as heat transfer fluids in batteries or other electrical equipment systems with metal moving parts not only enhance heat transfer and thermal conductivity, but also provide good tribological properties. Table 11 in the experimental section illustrates this additional beneficial friction reduction performance, which can be directly converted into energy efficiency in automotive and industrial applications.
[0052] Nanoparticles (A)
[0053] According to the present invention, the nanoparticle compound (also referred to as "particle" or "nanoparticle" in this article) is a microscopic particle having at least one dimension between 1 and 500 nm, preferably between 10 and 300 nm, and more preferably between 30 and 200 nm (measured using a transmission electron microscope, TEM). Such particles can either be independently characterized or exist in a structure of aggregation and / or agglomeration. In the latter case, at least one dimension of the size of the primary particle is between the above-mentioned sizes. The size of the structure of the aggregation / agglomeration can be between 50 and 150,000 nm, preferably between 100 and 100,000 nm, and more preferably between 400 and 70,000 nm (measured using a static light scattering technique, d50 SLS).
[0054] In the present invention, the SLS (static light scattering) measurement is carried out using a Beckmann Coulter LS 13 320 device. 0.1 to 2 wt % of the corresponding powder is added to a 0.05 wt % sodium pyrophosphate aqueous solution and homogenized for one minute using ultrasound. 0.2 to 2 g of this solution is added to a measuring device containing about 200 mL of water. The mathematical calculation of d50 is based on volume and is carried out using the Fraunhofer optical model.
[0055] All above-noted dimensions are provided for illustrative purposes only and are not intended to limit the present disclosure.
[0056] According to a preferred aspect of the present invention, the nanoparticles are selected from nitrides of the following elements: boron or aluminum or a mixture thereof, more preferably hBN.
[0057] According to another preferred aspect of the present invention, the nanoparticles are carbon black.
[0058] According to another preferred aspect of the present invention, the nanoparticle (A) has a molecular formula of MX 2 wherein M is a metal element selected from titanium (Ti), vanadium (V), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), zirconium (Zr), niobium (Nb), molybdenum (Mo), tantalum (Ta), tungsten (W), osmium (Os) and combinations thereof, and X is a chalcogen element selected from sulfur (S) and / or oxygen (O) and combinations thereof. Preferably, the metal chalcogenide has a molecular formula MX 2 , wherein the metal element M is tungsten (W) or molybdenum (Mo), and the chalcogen element X is sulfur (S).
[0059] According to the present invention, "MX 2The "compound" may be an intercalation compound, meaning a compound that can be inserted between elements or layers. The intercalation compound generally has a fullerene-like geometry. The core of the fullerene-like geometry may be hollow, solid, amorphous, or a combination thereof. Fullerene-like geometry may also be referred to as having a cage-like geometry. More specifically, in some embodiments, the intercalation compound having an inorganic fullerene-like geometry may be a cage-like geometry that is hollow or solid at its core and layered at its periphery. For example, the intercalation compound having an inorganic fullerene-like geometry may be a single-layer or double-layer structure. The intercalation compound is not limited to a single-layer or double-layer structure, as the intercalation compound may have any number of layers. These structures are also referred to in the art as nested layer structures. Preferably, the intercalation compound is selected from WS 2 or MoS 2 or a mixture thereof, more preferably WS 2 .
[0060] In a preferred embodiment, the inorganic fullerene-like geometry of the intercalation compound may be spherical, nearly spherical, polyhedral, elongated, rod-like, cubic, plate-like or tubular, or mixtures thereof, with or without a hollow core.
[0061] According to a preferred aspect of the present invention, the nanoparticles are selected from a mixture of the above structures, more preferably selected from hexagonal boron nitride (hBN) nanoparticles; carbon black; nanoparticles having a molecular formula of MX 2 A metal chalcogenide, wherein the metal element M is tungsten (W) or molybdenum (Mo), and the chalcogen element X is sulfur (S); or a mixture thereof.
[0062] Polymer (B)
[0063] The polymers of the present invention are not crystalline or semi-crystalline polymers, but are amorphous polymers.
[0064] In a preferred embodiment of the present invention, the one or more polymer compounds (B) have a weight average molecular weight (MW) of 10,000 to 1,000,000 g / mol, more preferably 50,000 to 800,000 g / mol, even more preferably 100,000 to 500,000 g / mol, most preferably 150,000 to 350,000 g / mol. w ).
[0065] In the present invention, the weight average molecular weight (M w) was determined by gel permeation chromatography (GPC) using polymethyl methacrylate (PMMA) calibration standards and tetrahydrofuran (THF) as eluent (flow rate: 1 mL / min; injection volume: 100 μL).
[0066] Preferably, the one or more polymer compounds (B) prepared with a monomer composition comprising monomer components a), b) and c) are obtainable by polymerizing a monomer composition comprising:
[0067] a) 5 to 30 wt%, more preferably 10 to 20 wt%, of the one or more functional monomers as component a), based on the total weight of the monomer composition; and
[0068] b) 35 to 70 wt%, more preferably 40 to 60 wt%, of the one or more alkyl (meth)acrylate monomers, based on the total weight of the monomer composition, wherein each of the alkyl groups of the one or more alkyl (meth)acrylate monomers is independently linear, cyclic or branched and contains 1 to 40 carbon atoms; and
[0069] c) 25 to 55 wt %, more preferably 30 to 50 wt %, based on the total weight of the monomer composition, of one or more (meth)acrylic acid and one or more having a number average molecular weight (M) of 500 to 10,000 g / mol. n ) is an ester formed by hydroxylated hydrogenated polybutadiene.
[0070] In a preferred embodiment, the weight contents of the monomers a), b) and c) of the monomer composition add up to 100% by weight, based on the total weight of the monomer composition.
[0071] Functional monomer a)
[0072] As already defined above, the one or more functional monomers a) according to the invention are chosen from:
[0073] a1) Aminoalkyl (meth)acrylates and aminoalkyl (meth)acrylamides;
[0074] a2) alkyl(meth)acrylic nitriles and other nitrogen-containing alkyl(meth)acrylates;
[0075] a3) (meth)acrylates of ether alcohols;
[0076] a4) epoxyalkyl alkyl (meth)acrylate;
[0077] a5) phosphorus-, boron- and / or silicon-containing alkyl (meth)acrylates;
[0078] a6) Heterocycloalkyl (meth)acrylate;
[0079] a7) vinyl halides;
[0080] a8) vinyl esters;
[0081] a9) vinyl monomers containing aromatic groups;
[0082] a10) heterocyclic vinyl compounds;
[0083] a11) vinyl and prenyl ethers;
[0084] a12) Methacrylic acid and acrylic acid.
[0085] Preferably, the functional monomer a) is selected from aminoalkyl (meth)acrylates a1) or aminoalkyl (meth)acrylamides a1) or heterocycloalkyl (meth)acrylates a6) or vinyl monomers containing aromatic groups a9). More preferably, it is selected from aminoalkyl (meth)acrylamides a1) or vinyl monomers containing aromatic groups a9) or mixtures thereof.
[0086] Even more preferably, the functional monomer a) is selected from aminoalkyl(meth)acrylamides, most preferably N-(3-dimethylaminopropyl)methacrylamide, as first component a), and vinyl monomers containing aromatic groups, most preferably styrene, as second component a).
[0087] (Meth) acrylate monomer b)
[0088] The term "(meth)acrylic acid" refers to acrylic acid, methacrylic acid and a mixture of acrylic acid and methacrylic acid; preferably methacrylic acid. The term "(meth)acrylate" refers to an ester of acrylic acid, an ester of methacrylic acid or a mixture of esters of acrylic acid and methacrylic acid; preferably an ester of methacrylic acid.
[0089] The term "(meth)acrylic acid C 1-40 "Alkyl ester" refers to an ester formed from (meth)acrylic acid and a linear, cyclic or branched alcohol having 1 to 40 carbon atoms. The term includes a single (meth)acrylic acid ester formed with an alcohol of a specific length, and also includes a mixture of (meth)acrylic acid esters formed with alcohols of different lengths.
[0090] According to the present invention, it is preferred that, in optional component b) of the nanoparticle composition, each of the alkyl groups of the one or more alkyl (meth)acrylate monomers is independently linear, cyclic or branched and contains 1 to 40 carbon atoms.
[0091] As already indicated above, according to the present invention, the one or more alkyl (meth)acrylate monomers b) comprise
[0092] b1) one or more alkyl (meth)acrylates of formula (I):
[0093]
[0094] Where R is hydrogen or methyl, R 1 refers to a straight-chain, branched or cyclic alkyl group having 1 to 8 carbon atoms, preferably 1 to 5 carbon atoms, and more preferably 1 to 4 carbon atoms,
[0095] b2) one or more alkyl (meth)acrylates of formula (II):
[0096]
[0097] Where R is hydrogen or methyl, R 2 refers to a linear, branched or cyclic alkyl group having 9 to 15 carbon atoms, preferably 12 to 15 carbon atoms, and more preferably 12 to 14 carbon atoms,
[0098] b3) one or more alkyl (meth)acrylates of formula (III):
[0099]
[0100] Where R is hydrogen or methyl, R 3 It refers to a linear, branched or cyclic alkyl group having 16 to 40 carbon atoms, preferably 16 to 30 carbon atoms, and more preferably 16 to 22 carbon atoms.
[0101] The term "(meth)acrylic acid C 1-8 "Alkyl ester" refers to an ester formed from (meth)acrylic acid and a straight chain or branched alcohol having 1 to 8 carbon atoms. The term includes a single (meth)acrylic acid ester formed with an alcohol of a specific length, and also includes a mixture of (meth)acrylic acid esters formed with alcohols of different lengths.
[0102] According to the present invention, the one or more monomers according to formula (I) (ie (meth) acrylic acid C 1-8Each of the (meth)acrylates and alkyl esters) may be independently selected from (meth)acrylates derived from saturated alcohols, preferably methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cycloalkyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, heptyl (meth)acrylate, 2-tert-butylheptyl (meth)acrylate, n-octyl (meth)acrylate and 3-isopropylheptyl (meth)acrylate, the most preferred monomer according to formula (II) is methyl methacrylate.
[0103] Particularly preferred (meth)acrylic acid C 1-8 The alkyl esters are methyl (meth)acrylate and n-butyl (meth)acrylate; methyl methacrylate and n-butyl methacrylate are particularly preferred.
[0104] The term "(meth)acrylic acid C 9-15 "Alkyl ester" refers to an ester formed from (meth)acrylic acid and a straight chain or branched alcohol having 9 to 15 carbon atoms. The term includes a single (meth)acrylic acid ester formed with an alcohol of a specific length, and also includes a mixture of (meth)acrylic acid esters formed with alcohols of different lengths.
[0105] According to the present invention, the one or more monomers according to formula (II) (ie (meth) acrylic acid C 9-15 Each of the (meth)acrylates may also be independently selected from nonyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, 5-methylundecyl (meth)acrylate, n-dodecyl (meth)acrylate, 2-methyldodecyl (meth)acrylate, tridecyl (meth)acrylate, 5-methyltridecyl (meth)acrylate, n-tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, oleyl (meth)acrylate; cycloalkyl (meth)acrylate, cyclohexyl (meth)acrylate having a ring substituent, tert-butylcyclohexyl (meth)acrylate, trimethylcyclohexyl (meth)acrylate, bornyl (meth)acrylate, and isobornyl (meth)acrylate.
[0106] Particularly preferred (meth)acrylic acid C 9-15 Alkyl esters are straight chain C 12-14 (Meth)acrylate of alcohol mixture ((meth)acrylate C 12-14 alkyl esters).
[0107] The term "(meth)acrylic acid C 16-40"Alkyl ester" refers to an ester formed from (meth)acrylic acid and a straight chain or branched alcohol having 16 to 40 carbon atoms. The term includes a single (meth)acrylic acid ester formed with an alcohol of a specific length, and also includes a mixture of (meth)acrylic acid esters formed with alcohols of different lengths.
[0108] According to the present invention, the one or more monomers according to formula (III) (ie (meth) acrylic acid C 16-40 Each of the alkyl esters) can also be independently selected from hexadecyl (meth)acrylate, 2-methylhexadecyl (meth)acrylate, heptadecyl (meth)acrylate, 5-isopropylheptadecyl (meth)acrylate, 4-tert-butyloctadecyl (meth)acrylate, 5-ethyloctadecyl (meth)acrylate, 3-isopropyloctadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, cetyl eicosyl (meth)acrylate, stearyl eicosyl (meth)acrylate, behenyl (meth)acrylate, eicosyl tetratriadecyl (meth)acrylate; cycloalkyl (meth)acrylate, 2,4,5-tri-tert-butyl-3-vinylcyclohexyl (meth)acrylate and 2,3,4,5-tetra-tert-butylcyclohexyl (meth)acrylate.
[0109] Preferably, the (meth)acrylic acid C 1-40 Alkyl esters include (meth) acrylic acid C 1-8 Alkyl esters and (meth) acrylic acid C 9-15 A mixture of alkyl esters, more preferably (meth) acrylic acid C 1-4 Alkyl esters and (meth) acrylic acid C 12-15 A mixture of alkyl esters.
[0110] Macromonomer component (c)
[0111] According to the invention, the monomer composition defined above comprises as component c) one or more (meth)acrylic acid and one or more monomers having a number average molecular weight (M) of 500 to 10,000 g / mol. n) is an ester formed by a hydroxylated hydrogenated polybutadiene. In this regard, the polymer compound (B) of the present invention comprises a first polymer, also referred to as a backbone or main chain, and a plurality of additional polymers, referred to as side chains, covalently bonded to the main chain. In this context, the main chain of the polymer is formed by the unsaturated groups of the mentioned (meth)acrylates connected to each other. The alkyl groups of the (meth)acrylates and the hydrogenated polybutadiene chains form the side chains of the polymer. The reaction product formed by one or more additional (meth)acrylic acid esters and one or more hydroxylated hydrogenated polybutadienes having a number average molecular weight of 500 to 10,000 g / mol is also referred to as a macromonomer in the present invention.
[0112] The number average molecular weight M of the macromonomer n It is determined by gel permeation chromatography (GPC) using polybutadiene calibration standards according to DIN 55672-1 with tetrahydrofuran (THF) as eluent.
[0113] The one or more polymer compounds (B) prepared with the monomer composition comprising components a), b) and c) may be selected based on their molar degree of branching (“f 支化 The molar branching degree refers to the percentage expressed in mole % of the macromonomer (component (c)) used based on the total molar amount of all monomers in the monomer composition. The molar amount of the macromonomer used is based on the number average molecular weight (M) of the macromonomer. n The calculation of the molar degree of branching is described in detail in WO 2007 / 003238 A1, in particular on pages 13 and 14, to which explicit reference is made here.
[0114] Preferably, the one or more polymer compounds (B) have a molar branching degree f of 0.1 to 6 mol %, more preferably 1 to 4 mol % and most preferably 1.5 to 3 mol %. 支化 .
[0115] According to the present invention, by using a plurality of n ) as component c) in combination with the one or more functional monomers a) and the one or more (meth) alkyl acrylate monomers b) to obtain a polymer (B) which, when combined with the nanoparticle compound (A), provides a stable, well-dispersed nanoparticle composition.
[0116] The one or more hydroxylated hydrogenated polybutadienes used as component c) according to the present invention have a number average molecular weight (M) of 500 g / mol to 10,000 g / mol. nDue to their high molecular weight, the hydroxylated hydrogenated polybutadienes may also be referred to as macroalcohols in the context of the present invention. In the context of the present invention, the corresponding (meth)acrylic acid esters may also be referred to as macromonomers.
[0117] Component c) may comprise a single type of macromonomer or may comprise a mixture of different macromonomers based on different macroalcohols.
[0118] The hydroxylated hydrogenated polybutadiene may be a polybutadiene having a single number average molecular weight (M n ) or it may be a single polybutadiene having different number average molecular weights (M n ) of a mixture of different polybutadienes.
[0119] Preferably, the monomer composition comprises as component c) 20 to 80 wt %, more preferably 20 to 70 wt %, even more preferably 20 to 60 wt %, most preferably 20 to 50 wt %, based on the total weight of the monomer composition, of one or more (meth)acrylic acid and one or more having a number average molecular weight (M) of 500 to 10,000 g / mol. n ) is an ester formed by hydroxylated hydrogenated polybutadiene.
[0120] In a preferred embodiment, the one or more hydroxylated hydrogenated polybutadienes used as component c) according to the invention have a number average molecular weight (M) of from 1,500 to 7,500 g / mol. n ).
[0121] Preferably, the one or more hydroxylated hydrogenated polybutadienes of component c) have a number average molecular weight (M) of 1,500 to 2,100 g / mol, more preferably 1,800 to 2,100 g / mol, most preferably 1,900 to 2,100 g / mol. n ).
[0122] In another preferred embodiment, component c) can be a macromonomer prepared using one or more macroalcohols having different molecular weights, the first macroalcohol having a number average molecular weight of 1,500 to 2,100 g / mol, more preferably 1,800 to 2,100 g / mol, most preferably 1,900 to 2,100 g / mol, and the second macroalcohol having a number average molecular weight of 3,500 to 7,000 g / mol, preferably 4,000 to 6,000 g / mol, more preferably 4,500 to 5,000 g / mol. Component c) may also comprise a mixture of two macromonomers, the first macromonomer being prepared with a macroalcohol having a number average molecular weight of 1,500 to 2,100 g / mol, more preferably 1,800 to 2,100 g / mol, most preferably 1,900 to 2,100 g / mol, and the second macromonomer being prepared with a macroalcohol having a number average molecular weight of 3,500 to 7,000 g / mol, preferably 4,000 to 6,000 g / mol, more preferably 4,500 to 5,000 g / mol.
[0123] According to a preferred embodiment of the present invention, by combining two macromonomers with different number average molecular weights, the weight ratio of the lower molecular weight macromonomer to the higher molecular weight macromonomer is preferably 1 or more, more preferably 1.5 to 15, even more preferably 2 to 7, and most preferably 3 to 6.
[0124] In a preferred embodiment, the hydroxylated hydrogenated polybutadiene is a monohydroxylated hydrogenated polybutadiene, preferably a hydroxyethyl-terminated or hydroxypropyl-terminated hydrogenated polybutadiene.
[0125] In another preferred embodiment of the present invention, the one or more (meth)acrylic acid esters used to prepare component c) of the polymer compound (B) are methyl (meth)acrylate or ethyl (meth)acrylate.
[0126] Preferably, the one or more hydroxylated hydrogenated polybutadienes have a hydrogenation level of at least 99%. An alternative measure of the hydrogenation level that can be determined for the polymers of the present invention is the iodine value. The iodine value refers to the grams of iodine that can be added to 100 grams of polymer. Preferably, the polymers of the present invention have an iodine value of no more than 5 g of iodine per 100 g of polymer. The iodine value is determined by the Wijs method according to DIN 53241-1: 1995-05.
[0127] Preferred hydroxylated hydrogenated polybutadienes are obtainable according to GB 2270317.
[0128] As used herein, the term "hydroxylated hydrogenated polybutadiene" refers to a hydrogenated polybutadiene comprising one or more hydroxyl groups. The hydroxylated hydrogenated polybutadiene may further comprise additional structural units, such as polyether groups derived from the addition of alkylene oxides to polybutadiene or maleic anhydride groups derived from the addition of maleic anhydride to polybutadiene. These additional structural units may be introduced into the polybutadiene when the polybutadiene is functionalized with hydroxyl groups.
[0129] Monohydroxylated hydrogenated polybutadiene is preferred. More preferably, the hydroxylated hydrogenated polybutadiene is hydroxyethyl or hydroxypropyl terminated hydrogenated polybutadiene. Hydroxypropyl terminated polybutadiene is preferred.
[0130] These monohydroxylated hydrogenated polybutadienes can be prepared by first converting butadiene monomers into polybutadiene by anionic polymerization. Subsequently, hydroxyl-functionalized polybutadiene can be prepared by reacting the polybutadiene monomers with an alkylene oxide such as ethylene oxide or propylene oxide. The polybutadiene can also be reacted with more than one alkylene oxide unit to result in a polyether-polybutadiene block copolymer having terminal hydroxyl groups. The hydroxylated polybutadiene can be hydrogenated in the presence of a suitable transition metal catalyst.
[0131] These monohydroxylated hydrogenated polybutadienes may also be selected from products obtained by hydroboration of (co)polymers having terminal double bonds (e.g., as described in U.S. Pat. No. 4,316,973); maleic anhydride-ene-amino alcohol adducts obtained by ene reaction between (co)polymers having terminal double bonds and maleic anhydride and amino alcohols; and products obtained by hydroformylation of (co)polymers having terminal double bonds and subsequent hydrogenation (e.g., as described in JP Publication S63-175096).
[0132] The macromonomers used according to the invention can be prepared by transesterification of alkyl (meth)acrylates. The reaction of the alkyl (meth)acrylates with the hydroxylated hydrogenated polybutadiene forms the esters according to the invention. Methyl (meth)acrylate or ethyl (meth)acrylate is preferably used as reactant.
[0133] Such transesterification is widely known. For example, heterogeneous catalyst systems such as lithium hydroxide / calcium oxide mixtures (LiOH / CaO), pure lithium hydroxide (LiOH), lithium methoxide (LiOMe) or sodium methoxide (NaOMe), or homogeneous catalyst systems such as isopropyl titanate (Ti(OiPr) 4 ) or dioctyltin oxide (Sn(OCt) 2 O). The reaction is an equilibrium reaction. Therefore, the low molecular weight alcohols released are usually removed, for example, by distillation.
[0134] Furthermore, the macromonomers are obtainable by direct esterification, for example, preferably under acidic catalysis with p-toluenesulfonic acid or methanesulfonic acid, starting from (meth)acrylic acid or (meth)acrylic anhydride, or by the DCC process (dicyclohexylcarbodiimide) starting from free methacrylic acid.
[0135] Additionally, the hydroxylated hydrogenated polybutadiene of the present invention can be converted into an ester by reaction with an acid chloride (eg, (meth)acryloyl chloride).
[0136] Preferably, in the preparation of the esters of the invention as detailed above, a polymerization inhibitor is used, for example 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl free radical and / or hydroquinone monomethyl ether.
[0137] Preferred monomer compositions
[0138] According to a preferred aspect of the present invention, the one or more polymer compounds (B) can be obtained by polymerizing the following monomer composition, wherein the monomer composition comprises:
[0139] a) 1 to 30 wt %, preferably 5 to 30 wt %, more preferably 10 to 20 wt % of the one or more functional monomers as component a), based on the total weight of the monomer composition; and
[0140] b1) 30 to 60 wt %, preferably 30 to 50 wt %, more preferably 35 to 50 wt %, based on the total weight of the monomer composition, of the one or more alkyl (meth)acrylate monomers of formula (I) as first component b); and
[0141] b2) 0 to 20 wt. %, preferably 1 to 15 wt. %, more preferably 1 to 10 wt. %, based on the total weight of the monomer composition, of the one or more alkyl (meth)acrylate monomers of formula (II) as second component b); and,
[0142] b3) 0 to 20 wt %, preferably 0 to 15 wt %, more preferably 0 to 10 wt % of the one or more alkyl (meth)acrylate monomers of formula (III) as third component b), based on the total weight of the monomer composition; and,
[0143] c) 20 to 60 wt %, more preferably 25 to 55 wt %, more preferably 30 to 50 wt %, based on the total weight of the monomer composition, of one or more (meth)acrylic acid esters and one or more monomers having a number average molecular weight (M) of 500 to 10,000 g / mol. n ) is a hydroxylated hydrogenated polybutadiene;
[0144] The amounts of all monomers in the monomer composition add up to 100% by weight.
[0145] In a particularly preferred embodiment of the present invention, the one or more polymer compounds (B) are obtainable by polymerizing the following monomer composition, the monomer composition comprising:
[0146] a1) as first component a) 0.5 to 5 wt. % of aminoalkyl(meth)acrylamide (most preferably N-(3-dimethylaminopropyl)methacrylamide), based on the total weight of the monomer composition; and
[0147] a9) 5 to 15 wt % of a vinyl monomer containing an aromatic group (most preferably styrene) as second component a), based on the total weight of the monomer composition; and
[0148] b1) 35 to 50 wt. % of an alkyl (meth)acrylate monomer of formula (I), most preferably methyl methacrylate and / or butyl methacrylate, as a first component b), based on the total weight of the monomer composition; and
[0149] b2) 1 to 10 wt. % of an alkyl (meth)acrylate monomer of formula (II), most preferably lauryl methacrylate, as a second component b), based on the total weight of the monomer composition; and
[0150] c) 30 to 50% by weight of the following as component c), based on the total weight of the monomer composition: (meth)acrylic acid and a monomer having a number average molecular weight (M) of 500 to 10,000 g / mol. n ) is formed from a hydroxylated hydrogenated polybutadiene, most preferably a macromonomer derived from an ester of (meth)acrylic acid and having a number average molecular weight (M) of 1,500-5,000 g / mol. n ) between hydroxylated hydrogenated polybutadiene;
[0151] The amounts of all monomers in the monomer composition add up to 100% by weight.
[0152] Preparation of polymer compound (B)
[0153] According to the present invention, the above polymer can be prepared according to a method comprising the following steps:
[0154] (x) providing a monomer composition as described above; and
[0155] (y) initiating free radical polymerization in the monomer composition.
[0156] Standard free-radical polymerization is described in detail in particular in Ullmann's Encyclopedia of Industrial Chemistry, 6th edition. In general, for this purpose, polymerization initiators and optionally chain transfer agents are used.
[0157] The polymerization can be carried out at standard pressure, reduced pressure or elevated pressure. The polymerization temperature is also not critical. However, in general, it is in the range of -20 to 200°C, preferably 50 to 150°C and more preferably 80 to 130°C.
[0158] The polymerization step (y) can be carried out with or without dilution in oil. If dilution is carried out, the amount of the monomer composition, i.e. the total amount of monomers, is preferably 20 to 90% by weight, more preferably 40 to 80% by weight, most preferably 50 to 70% by weight relative to the total weight of the reaction mixture.
[0159] Preferably, the oil used to dilute the monomer mixture is an API Group I, II, III, IV or V oil or a mixture thereof. Preferably, a Group III oil or a mixture thereof is used to dilute the monomer mixture.
[0160] Preferably, step (y) comprises adding a free radical initiator.
[0161] Suitable free radical initiators are, for example, azo initiators, such as azobisisobutyronitrile (AIBN), 2,2′-azobis(2-methylbutyronitrile) (AMBN) and 1,1-azobiscyclohexanecarbonitrile, and peroxide compounds, such as methyl ethyl ketone peroxide, acetylacetone peroxide, dilauroyl peroxide, tert-butyl per-2-ethylhexanoate, ketone peroxide, tert-butyl peroctoate, methyl isobutyl ketone peroxide, cyclohexanone peroxide, dibenzoyl peroxide, tert-Butyl peroxybenzoate, tert-Butyl peroxyisopropyl carbonate, 2,5-bis(2-ethylhexanoylperoxy)-2,5-dimethylhexane, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxy-3,5,5-trimethylhexanoate, dicumyl peroxide, 1,1-bis(tert-butylperoxy)cyclohexane, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, cumyl hydroperoxide, tert-butyl hydroperoxide and bis(4-tert-butylcyclohexyl)peroxydicarbonate.
[0162] Preferably, the free radical initiator is selected from 2,2'-azobis(2-methylbutyronitrile), 2,2-bis(tert-butylperoxy)butane, tert-butyl peroxy-2-ethylhexanoate, 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane, tert-butyl peroxybenzoate and tert-butyl peroxy-3,5,5-trimethylhexanoate. Particularly preferred initiators are tert-butyl peroxy-2-ethylhexanoate and 2,2-bis(tert-butylperoxy)butane.
[0163] Preferably, the total amount of free radical initiator is 0.01 to 5 wt%, more preferably 0.02 to 0.8 wt%, relative to the total weight of the monomer mixture.
[0164] The total amount of the free radical initiator can be added in a single step, or the free radical initiator can be added in multiple steps during the polymerization reaction. Preferably, the free radical initiator is added in multiple steps. For example, a portion of the free radical initiator can be added to initiate free radical polymerization and a second portion of the free radical initiator can be added 0.5 to 3.5 hours after the initial dose.
[0165] Preferably, step (y) further comprises adding a chain transfer agent. Suitable chain transfer agents are in particular oil-soluble mercaptans, such as n-dodecyl mercaptan or 2-mercaptoethanol, or chain transfer agents selected from terpenes, such as terpinolene. It is particularly preferred to add n-dodecyl mercaptan.
[0166] The monomer composition can also be divided into an initial part and a second part, and a portion of the free radical initiator can be added only to the initial part to initiate the polymerization reaction therein. Then, the second portion of the free radical initiator is added to the second portion of the monomer composition, which is then added to the polymerization mixture over a period of 0.5 to 5 hours, preferably 1.5 to 4 hours, and more preferably 2 to 3.5 hours. After the addition of the second monomer mixture, the third portion of the free radical initiator can be added to the polymerization reaction as described above.
[0167] Preferably, the total reaction time of the free radical polymerization is 2 to 10 hours, more preferably 3 to 9 hours.
[0168] After the free radical polymerization is completed, the obtained polymer is preferably further diluted with the above mentioned oil to the desired viscosity. Preferably, the polymer is diluted to a concentration of 5 to 60 wt % polymer, more preferably 10 to 50 wt %, most preferably 20 to 40 wt %.
[0169] Nanoparticle composition of the present invention
[0170] According to a preferred embodiment of the present invention, the nanoparticle composition comprising the one or more nanoparticles (A) and the one or more polymer compounds (B) as defined herein may further comprise a base fluid (C).
[0171] In a preferred embodiment, the base fluid (C) has a kinematic viscosity at 40°C of 3 to 30 cSt, more preferably 3 to 15 cSt according to ASTM D-445, and a flash point above 110°C according to ASTM D-93.
[0172] The base fluid (C) may be a base oil selected from the group consisting of API Group I base oil, API Group II base oil, API Group III, API Group IV base oil and API Group V base oil or a combination thereof.
[0173] The base oil may also be defined as specified by the American Petroleum Institute (API) (see the April 2008 version of "Appendix E—API Base Oil Interchangeability Guidelines for Passenger Car Motor Oils and Diesel Engine Oils," Section 1.3, Subheading 1.3, "Base Stock Categories").
[0174] The API currently defines five groups of lubricant base stocks (API 1509, Annex E—API Base Oil Interchangeability Guide for Passenger Car Motor Oils and Diesel Engine Oils, September 2011). Groups I, II, and III are mineral oils, which are classified by the amount of saturates and sulfur they contain and by their viscosity index; Group IV is polyalphaolefins; and Group V is all other materials, including, for example, ester oils. The following table illustrates these API classifications.
[0175] Table 1 - API Definitions of Lubricant Base Stocks
[0176]
[0177] In a preferred embodiment, the base fluid (C) having a kinematic viscosity at 40°C of 3 cSt to 30 cSt, more preferably 3 cSt to 15 cSt according to ASTM D-445 and a flash point above 110°C according to ASTM D-93 is selected from polyalphaolefins, tetrabutane, API Group III base oils or mixtures thereof; preferably selected from tetrabutane or API Group III base oils or mixtures thereof.
[0178] The base fluid (C) may be a fluorinated compound, such as polyhexafluoropropylene oxide, perfluoropolyether (PFPE), perfluoroalkyl ether (PFAE), perfluoropolyalkyl ether (PFPAE), hydrofluoroether or a mixture thereof.
[0179] If the base fluid (C) is selected from API Group V base oils, it is preferably selected from silicone oils, cycloparaffins, polyalkylene glycols, synthetic oils including liquid esters of phosphorus-containing acids or mixtures thereof.
[0180] The base fluid (C) may also be a mixture of any of the base oils listed above.
[0181] Preferably, the nanoparticle composition used as a heat transfer fluid comprises 85 to 99.9 wt% of the base fluid (C) and 0.1 to 15 wt% of (A) and (B), more preferably 90 to 99.9 wt% of the base fluid (C) and 0.1 to 10 wt% of (A) and (B), and most preferably 92 to 99.5 wt% of the base fluid (C) and 0.5 to 8 wt% of (A) and (B), based on the total weight of the nanoparticle composition. Preferably, the amount of (A), (B) and (C) totals 100 wt%, based on the total weight of the nanoparticle composition.
[0182] In a preferred embodiment of the method for producing the nanoparticle composition, the mixture of one or more nanoparticles (A), the one or more polymer compounds (B) and optionally the base fluid (C) is ground using an ultrasonic device having a power between 10 and 1000 W, preferably 50 to 800 W and more preferably 100 to 500 W. Preferably, the composition is ground for 1 to 240 minutes, more preferably 10 to 180 minutes, and even more preferably 30 to 150 minutes to obtain a stable nanoparticle composition.
[0183] In another preferred embodiment, the mixture of one or more nanoparticles (A), the one or more polymer compounds (B) and optionally the base fluid (C) is ground using ultrahigh pressure technology (e.g. jet milling device SuginoUltimaizer HJP-25050). With the help of a pump, preferably a high-pressure pump, at least two streams of this mixture are each sprayed through a nozzle (0.25 mm diameter) into a grinding chamber enclosed by a reactor housing to the collision point, characterized in that the grinding chamber is filled with the mixture and the last ground mixture is removed from the grinding chamber by the overpressure of the continuous flow flowing into the grinding chamber. The pump pressure is between 100 and 4000 bar, preferably between 400 and 3000 bar, more preferably between 1000 and 2500 bar.
[0184] According to another preferred embodiment, the nanoparticle composition comprising one or more nanoparticles (A), one or more polymer compounds (B) and optionally the base fluid (C) is ground via a ball milling process. Preferably, the ball milling process comprises introducing 0.1 to 10 kWh / kg, preferably 1 to 5 kWh / kg, more preferably 1.5 to 3.5 kWh / kg of energy into the mixture.
[0185] In another preferred embodiment, the method for making a nanoparticle composition, in particular a nanoparticle composition as described above, comprises the following steps:
[0186] (i) providing one or more nanoparticle compounds (A) as defined herein;
[0187] (ii) providing one or more polymer compounds (B) as defined herein;
[0188] (iii) preferably providing a base fluid (C) as defined herein;
[0189] (iv) combining at least the one or more nanoparticle compounds (A) and the one or more polymer compounds (B) to obtain a mixture, preferably combining at least the one or more nanoparticle compounds (A), the one or more polymer compounds (B) and the base fluid (C) to obtain a mixture; and
[0190] (v) grinding the mixture.
[0191] According to the present invention, the milling step (v) is defined by the change in the particle size distribution of the resulting nanoparticle composition measured using the dynamic light scattering technique (DLS).
[0192] The grinding technique according to the invention described in step (v) can be a dissolver, rotor-stator apparatus, homogenization, high pressure homogenization, high shear mixing, ultrasound, ball milling or ultra-high pressure technology (jet mill) or a combination thereof. In fact, using these grinding techniques reduces the particle size of the agglomerates.
[0193] The most preferred embodiment is to grind the mixture via a ball milling process.
[0194] The nanoparticle composition for use as a heat transfer fluid according to the present invention may optionally further contain as component (D) an additional additive selected from dispersants, defoamers, seal fixatives or seal compatibilizers, detergents, antioxidants, pour point depressants, antiwear additives, extreme pressure additives, corrosion inhibitors, metal passivators, rust inhibitors, electrostatic discharge inhibitors, demulsifiers, emulsifiers, friction modifiers, dyes and mixtures thereof, as discussed below.
[0195] Suitable dispersants include poly(isobutylene) derivatives, such as poly(isobutylene) succinimide (PIBSI), including borated PIBSI; and ethylene-propylene oligomers having N / O functional groups.
[0196] Dispersants, including borated dispersants, are preferably used in an amount of 0 to 10 wt % based on the total amount of the nanoparticle composition.
[0197] Suitable defoamers are silicone oils, fluorosilicone oils, fluoroalkyl ethers.
[0198] The defoaming agent is preferably used in an amount of 0.005 to 0.5 wt % based on the total amount of the nanoparticle composition.
[0199] Preferred detergents include metal-containing compounds, such as phenates; salicylates; thiophosphonates, especially thiopyrophosphonates, thiophosphonates and phosphonates; sulfonates and carbonates. As metals, these compounds may contain, inter alia, calcium, magnesium and barium. These compounds may preferably be used in neutral or overbased form.
[0200] The detergent is preferably used in an amount of 0.2 to 5 wt % based on the total amount of the nanoparticle composition.
[0201] Suitable antioxidants include, for example, phenol-based antioxidants and amine-based antioxidants.
[0202] Phenol-based antioxidants include, for example, octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate; 4,4'-methylenebis(2,6-di-tert-butylphenol); 4,4'-bis(2,6-di-tert-butylphenol); 4,4'-bis(2-methyl-6-tert-butylphenol); 2,2'-methylenebis(4-ethyl-6-tert-butylphenol); 2,2'-methylenebis(4-methyl-6 -tert-butylphenol); 4,4'-butylidenebis(3-methyl-6-tert-butylphenol); 4,4'-isopropylidenebis(2,6-di-tert-butylphenol); 2,2'-methylenebis(4-methyl-6-nonylphenol); 2,2'-isobutylidenebis(4,6-dimethylphenol); 2,2'-methylenebis(4-methyl-6-cyclohexylphenol); 2,6-di-tert-butyl-4-methylphenol ; 2,6-di-tert-butyl-4-ethyl-phenol; 2,4-dimethyl-6-tert-butylphenol; 2,6-di-tert-amyl-p-cresol; 2,6-di-tert-butyl-4-(N,N'-dimethylaminomethylphenol); 4,4'-thiobis(2-methyl-6-tert-butylphenol); 4,4'-thiobis(3-methyl-6-tert-butylphenol); 2,2'-thiobis(4-methyl-6-tert-butylphenol); phenol); bis(3-methyl-4-hydroxy-5-tert-butylbenzyl) sulfide; bis(3,5-di-tert-butyl-4-hydroxybenzyl) sulfide; 3-(4-hydroxy-3,5-di-tert-butylphenyl) propionate; 3-(4-hydroxy-3,5-di-tert-butylphenyl) propionate; 2,2'-thio[diethyl-bis-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate]. Among them, bisphenol-based antioxidants and phenol-based antioxidants containing ester groups are particularly preferred.
[0203] The amine-based antioxidants include, for example, monoalkyldiphenylamines, such as monooctyldiphenylamine, monononyldiphenylamine; dialkyldiphenylamines, such as 4,4'-dibutyldiphenylamine, 4,4'-dipentyldiphenylamine, 4,4'-dihexyldiphenylamine, 4,4'-diheptyldiphenylamine, 4,4'-dioctyldiphenylamine, 4,4'-dinonyldiphenylamine; polyalkyldiphenylamines, such as tetrabutyldiphenylamine, tetrahexyldiphenylamine, tetraoctyldiphenylamine, tetranonyldiphenylamine; naphthylamines, specifically, α-naphthylamine, phenyl-α-naphthylamine and other alkyl-substituted phenyl-α-naphthylamines, such as butylphenyl-α-naphthylamine, pentylphenyl-α-naphthylamine, hexylphenyl-α-naphthylamine, heptylphenyl-α-naphthylamine, octylphenyl-α-naphthylamine, nonylphenyl-α-naphthylamine. Among them, diphenylamines are superior to naphthylamines from the viewpoint of their antioxidant effects.
[0204] Suitable antioxidants may further be selected from compounds containing sulfur and phosphorus, for example metal dithiophosphates, such as zinc dithiophosphate (ZnDTP), "OOS triesters" = reaction products of dithiophosphoric acids with activated double bonds from olefins, cyclopentadiene, norbornadiene, α-pinene, polybutene, acrylates, maleates (ashless on combustion); organic sulfur compounds, such as dialkyl sulfides, diaryl sulfides, polysulfides, modified mercaptans, thiophene derivatives, xanthates, thioglycols, thioaldehydes, sulfur-containing carboxylic acids; heterocyclic sulfur / nitrogen compounds, especially dialkyldimercaptothiadiazoles, 2-mercaptobenzimidazoles; zinc bis(dialkyldithiocarbamates) and methylenebis(dialkyldithiocarbamates); organic phosphorus compounds, such as triaryl and trialkyl phosphites; organic copper compounds and overbased calcium- and magnesium-based phenolates and salicylates.
[0205] The antioxidant is used in an amount of 0 to 15 wt %, preferably 0.1 to 10 wt %, more preferably 0.2 to 5 wt %, based on the total amount of the nanoparticle composition.
[0206] The pour point depressant includes ethylene-vinyl acetate copolymer, chlorinated paraffin-naphthalene condensate, chlorinated paraffin-phenol condensate, polymethacrylate, polyalkylstyrene. Preferably, the pour point depressant has a weight average molecular weight (MW) of 5,000 to 200,000 g / mol. w ) of polymethacrylate.
[0207] The amount of the pour point depressant is preferably 0.1 to 5 wt % based on the total amount of the nanoparticle composition.
[0208] Preferred antiwear and extreme pressure additives include sulfur-containing compounds such as zinc dithiophosphate, di-C 3-12 Zinc alkyl dithiophosphates (ZnDTP), zinc phosphate, zinc dithiocarbamate, molybdenum dithiocarbamate, molybdenum dithiophosphate, disulfides, sulfurized olefins, sulfurized oils and fats, sulfurized esters, thiocarbonates, thiocarbamates, polysulfides; phosphorus-containing compounds, such as phosphites, phosphates, such as trialkyl phosphates, triaryl phosphates, such as tricresyl phosphate, amine-neutralized mono- and dialkyl phosphates, ethoxylated mono- and dialkyl phosphates, phosphonates, phosphines, amine salts or metal salts of these compounds; sulfur- and phosphorus-containing antiwear agents, such as thiophosphites, thiophosphates, thiophosphonates, amine salts or metal salts of these compounds.
[0209] The antiwear agent may be present in an amount of 0 to 3 wt %, preferably 0.1 to 2 wt %, based on the total amount of the nanoparticle composition.
[0210] Preferred friction modifiers may include mechanically active compounds such as molybdenum disulfide, graphite (including graphite fluoride), poly(trifluoroethylene), polyamide, polyimide; compounds that form adsorption layers such as long-chain carboxylic acids, fatty acid esters, ethers, alcohols, amines, amides, imides; compounds that form layers by tribochemical reactions such as saturated fatty acids, phosphates; compounds that form polymeric layers such as ethoxylated dicarboxylic acid partial esters, functionalized poly(meth)acrylates, unsaturated fatty acids, sulfided olefins and organometallic compounds such as molybdenum compounds (molybdenum dithiophosphates and molybdenum dithiocarbamates MoDTC) and their combinations with ZnDTP, copper-containing organic compounds.
[0211] Some of the compounds listed above can fulfill multiple functions. For example, ZnDTP is primarily an antiwear additive and an extreme pressure additive, but also has the characteristics of an antioxidant and a corrosion inhibitor (here: metal passivator / deactivator).
[0212] The additives specified above are described in detail in particular in T. Mang, W. Dresel (eds.): “Lubricants and Lubrication”, Wiley-VCH, Weinheim 2001; RM Mortier, ST Orszulik (eds.): “Chemistry and Technology of Lubricants”.
[0213] Preferably, the total concentration of the one or more additives (D) is up to 20 wt%, more preferably 0.05 wt% to 15 wt%, based on the total weight of the nanoparticle composition.
[0214] Preferably, the amounts of (A) to (D) total 100 wt %, based on the total weight of the nanoparticle composition. DETAILED DESCRIPTION
[0215] Experimental Section
[0216] The present invention is hereinafter further illustrated in detail with reference to Examples and Comparative Examples, without any intention of limiting the scope of the present invention.
[0217] abbreviation
[0218] C 1 AMA Methacrylic Acid C 1 -Alkyl esters (methyl methacrylate; MMA)
[0219] C 4 AMA Methacrylic Acid C 4 -Alkyl ester (n-butyl methacrylate)
[0220] C 12-14 AMA Methacrylic Acid C 12-14 -Alkyl ester
[0221] DMAPMA N-3-Dimethylaminopropyl methacrylamide
[0222] f 支化 Degree of branching expressed in mol%
[0223] CTA Chain Transfer Agent
[0224] MMA Methyl (meth)acrylate
[0225] MA-1 macroalcohol (hydroxylated hydrogenated polybutadiene, M n =2,000 g / mol)
[0226] MM-1 Macromonomer of hydrogenated polybutadiene MA-1 with methacrylate functional groups (M n =2,000 g / mol)
[0227] M n Number average molecular weight
[0228] M w Weight average molecular weight
[0229] NB3020 3020; Group III base oil from Neste with a KV of 7.7 cSt 40 (ASTM D-445) and flash point >150°C (ASTM D-93)
[0230] NB3043 3043; Group III base oil from Neste with a KV of 20 cSt 40 (ASTM D-445) and flash point > 220°C (ASTM D-92)
[0231] TetrabutaneTetrabutane (branched C 16 and C 20 Saturated hydrocarbon isomers), with a KV of 4.2 cSt 40 (ASTM D-445) and a flash point of 124°C (ASTM D-93)
[0232] PDI polydispersity index, via M w / M n Calculated molecular weight distribution
[0233] IF-WS 2 Inorganic Fullerene Tungsten Disulfide
[0234] hBN hexagonal boron nitride
[0235] Synthesis of Hydroxylated Hydrogenated Polybutadiene (Macroalcohol) MA-1
[0236] The macroalcohol is synthesized by anionic polymerization of 1,3-butadiene with butyl lithium at 20-45° C. When the desired degree of polymerization is reached, the reaction is terminated by adding propylene oxide and the lithium is removed by precipitation with methanol. Subsequently, the polymer is hydrogenated in a hydrogen atmosphere in the presence of a noble metal catalyst at up to 140° C. and a pressure of 200 bar. After the hydrogenation has ended, the noble metal catalyst is removed and the organic solvent is drawn off under reduced pressure to obtain 100% macroalcohol MA-1.
[0237] Table 2 summarizes the characterization data of MA-1.
[0238] Table 2 —Characterization data of the macroalcohols used.
[0239] <![CDATA[M n [g / mol]]]> Hydrogenation level [%] OH functionality [%] MA-1 2,000 >99 >98
[0240] Synthesis of Macromonomer MM-1
[0241] In a 2L stirred apparatus equipped with a saber stirrer, air inlet tube, thermocouple with controller, heating jacket, column with random packing of 3 mm spiral wire, vapor distributor, top thermometer, reflux condenser and bottom cooler, 1000 g of the above macroalcohol was dissolved in methyl methacrylate (MMA) by stirring at 60°C. 20 ppm of 2,2,6,6-tetramethylpiperidin-1-oxyl radical and 200 ppm of hydroquinone monomethyl ether were added to the solution. After heating to MMA reflux (bottom temperature about 110°C) while passing air through for stabilization, about 20 mL of MMA was distilled off for azeotropic drying. After cooling to 95°C, LiOCH was added. 3 , and the mixture was heated back to reflux. After a reaction time of about 1 hour, the top temperature had dropped to about 64° C. due to the formation of methanol. The methanol / MMA azeotrope formed was continuously distilled out until a constant top temperature of about 100° C. was established again. At this temperature, the mixture was reacted for another 1 hour. For further post-treatment, most of the MMA was extracted under reduced pressure. Insoluble catalyst residues were removed by pressure filtration (Seitz T1000 depth filter).
[0242] Table 3 summarizes the MMA or LiOCH used to synthesize the macromonomer MM-1. 3 The amount.
[0243] Table 3 - Amounts of macroalcohol, MMA and catalyst used for transesterification of the macromonomers.
[0244] Macromonomer Macroalcohol Amount of MMA [g] <![CDATA[LiOCH 3 Amount [g]]]> MM-1 MA-1 500 1.5
[0245] Preparation of polymer compound (B) according to the present invention:
[0246] As described above, the weight average molecular weight (M) of the polymer was measured by gel permeation chromatography (GPC) calibrated with polymethyl methacrylate (PMMA) standards. w ). Tetrahydrofuran (THF) was used as the eluent.
[0247] Polymer 1 (P1) as polymer compound (B):
[0248] 85 grams of Nexbase 3020, 85 grams of Berylane 230SPP, 140 grams of macromonomers, 107 grams of butyl methacrylate, 28 grams of styrene, 13 grams of lauryl methacrylate, 8 grams of dimethylaminopropyl methacrylamide and 1 gram of n-dodecyl mercaptan are fed into a 2-liter 4-necked round-bottom flask. The reaction mixture is stirred using a C stirring rod, protected by nitrogen inertia, and heated to 115°C. Once the reaction mixture reaches the set point temperature, 0.9 grams of tert-butyl 2-ethylperoxyhexanoate are fed into the reactor within 3 hours. Within 30 minutes and 3 hours after the previous feed, 0.5 grams of 2,2-di-(tert-butylperoxy) butane are added. The reaction is stirred for 1 hour, and then another 132 grams of Nexbase 3020 are added to the reactor and mixed for 1 hour. The polymer obtained has a weight average molecular weight (M ) of 260,000 g / mol. w )(PMMA standard).
[0249] For example P1, the monomer components total 100%. The amounts of initiator and chain transfer agent are given relative to the total amount of monomers. Table 4 below shows the monomer composition and reactants used to prepare polymer P1, as well as its final characterization.
[0250] Table 4 —Monomer composition and reactants used to prepare polymer P1, and its final characterization
[0251]
[0252] Preparation of the nanoparticle composition according to the present invention
[0253] Dispersion IE1 (using ball mill):
[0254] A ball mill apparatus (Netzsch laboratory mill micro series) was preloaded with 271.3 g NB3020 oil and 26.3 g P1, while the peristaltic pump was set to 90 rpm and the ball mill was set to 1000 rpm. Then, 52.5 g of hexagonal boron nitride particles (hBN; SLS d50: 2.7 μm) were added to the solution. The peristaltic pump was adjusted to 130 rpm and the ball mill was set to a rotation speed of 3900 rpm. The dispersion was processed for 120 minutes (introducing 0.8 kWh of energy). The particle size distribution (measured using a dynamic light scattering device, LA-950, Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d99 value of 430 nm.
[0255] Dispersion IE2 (Ball mill)
[0256] A ball mill apparatus (Netzsch laboratory mill micro series) was preloaded with 271.3 g tetrabutane and 26.3 g P1, while the peristaltic pump was set to 90 rpm and the ball mill was set to 1000 rpm. Then, 52.5 g of hexagonal boron nitride particles (hBN; SLS d50: 2.7 μm) were added to the solution. The peristaltic pump was adjusted to 130 rpm and the ball mill was set to a rotation speed of 3900 rpm. The dispersion was processed for 120 minutes (introducing 0.7 kWh of energy). The particle size distribution (measured using a dynamic light scattering device, LA-950, Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d99 value of 385 nm.
[0257] Dispersion IE3:
[0258] 10 g of carbon black particles (SLS d50: 17.6 μm) were added to a solution of 83 g of NB3020 including 7 g of P1, while the mixture was ground separately for 60 minutes using ultrasound (ultrasonic processor UP400S, using 400 watts, 24 kHz, using a Ti-ultrasonic generator). The particle size distribution (measured using a dynamic light scattering device, LA-950, Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d99 value of 96 nm.
[0259] Dispersion IE4 (using ball mill)
[0260] A ball mill apparatus (Netzsch laboratory mill micro series) was preloaded with 259 g NB3020 and 21 g P1, while the peristaltic pump was set to 90 rpm and the ball mill was set to 1000 rpm. Then, 70 g of inorganic fullerene tungsten disulfide particles (IF-WS2 ; SLS d50: 51.1 μm) was added to the solution. The peristaltic pump was adjusted to 130 rpm and the ball mill was set to a rotation speed of 3900 rpm. The dispersion was processed for 120 minutes (introduction of 0.7 kWh of energy). The particle size distribution (measured using a dynamic light scattering device, LA-950, Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d99 value of 123 nm.
[0261] Dispersion IE5:
[0262] 20 g of carbon black particles (SLS d50: 17.6 μm) were added to a solution of 166 g of NB3043 including 14 g of P1, while the mixture was ground separately for 60 minutes using ultrasound (ultrasonic processor UP400S, using 400 watts, 24 kHz, using a Ti-ultrasonic generator). The particle size distribution (measured using a dynamic light scattering device, LA-950, Horiba Ltd., Japan, in TegosoftDEC oil) showed a d99 value of 101 nm.
[0263] Preparation of Comparative Examples
[0264] Dispersion CE1:
[0265] 2 g of hexagonal boron nitride particles (hBN; SLS d50: 2.7 μm) were added to a solution of 18 g of NB3043, and the mixture was treated with ultrasound (ultrasonic processor UP400S, using 400 watts, 24 kHz, using a Ti-ultrasonic generator) for 120 minutes respectively. The particle size distribution (measured using a dynamic light scattering device, LA-950, Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d99 value of 1,144 nm.
[0266] Dispersion CE2:
[0267] 2 g of hexagonal boron nitride particles (hBN; SLS d50: 2.7 μm) were added to a solution of 18 g of NB3020, and the mixture was treated with ultrasound (ultrasonic processor UP400S, using 400 watts, 24 kHz, using a Ti-ultrasonic generator) for 120 minutes respectively. The particle size distribution (measured using a dynamic light scattering device, LA-950, Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d99 value of 3,165 nm.
[0268] Dispersion CE3:
[0269] 2 g of hexagonal boron nitride particles (hBN; SLS d50: 2.7 μm) were added to a solution of 18 g of tetrabutane, and the mixture was treated with ultrasound (ultrasonic processor UP400S, using 400 watts, 24 kHz, using a Ti-ultrasonic generator) for 120 minutes respectively. The particle size distribution (measured using a dynamic light scattering device, LA-950, Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d99 value of 1,322 nm.
[0270] Dispersion CE4:
[0271] 2 g of hexagonal boron nitride particles (hBN; SLS d50: 2.7 μm) were mixed with 2 g of oleyl alcohol. After adding 16 g of NB3043, the mixture was treated with ultrasound (ultrasonic processor UP400S, using 400 watts, 24 kHz, using a Ti-ultrasound generator) for 120 minutes respectively. The particle size distribution (measured using a dynamic light scattering device, LA-950, Horiba Ltd., Japan, in TegosoftDEC oil) showed a d99 value of 1,470 nm.
[0272] Dispersion CE5:
[0273] 2 g of hexagonal boron nitride particles (hBN; SLS d50: 2.7 μm) were mixed with 2 g of Triton X-100. After adding 16 g of NB3043, the mixture was treated with ultrasound (ultrasonic processor UP400S, using 400 watts, 24 kHz, using a Ti-ultrasound generator) for 120 minutes respectively. The particle size distribution (measured using a dynamic light scattering device, LA-950, Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d99 value of 1,475 nm.
[0274] Dispersion CE6:
[0275] 2 g of hexagonal boron nitride particles (hBN; SLS d50: 2.7 μm) were mixed with 2 g of Triton X-100. After adding 16 g of NB3020, the mixture was treated with ultrasound (ultrasonic processor UP400S, using 400 watts, 24 kHz, using a Ti-ultrasound generator) for 120 minutes respectively. The particle size distribution (measured using a dynamic light scattering device, LA-950, Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d99 value of 4,357 nm.
[0276] Dynamic Light Scattering (DLS)
[0277] The particle size distribution was measured using a dynamic light scattering apparatus LB-500 manufactured by Horiba Ltd. in Tegosoft oil.
[0278] Dynamic light scattering (DLS) is a technique in physics that can be used to determine the size distribution curve of small particles in suspension or polymers in solution. This equipment can be used to measure the particle size of dispersed materials (such as nanoparticles or polymer spheres) in the range of 3nm to about 6μm. The measurement is based on the Brownian motion of particles in the medium and the scattering of incident laser light due to the difference in refractive index of liquid and solid materials.
[0279] The value obtained is the hydrodynamic diameter of the corresponding sphere of the particle. Values d50, d90 and d99 are common standards for discussion because they describe the following hydrodynamic diameter of the particle, and 50%, 90% or 99% of the particles in the particle size distribution are below the hydrodynamic diameter. The lower these values are, the better the particles are dispersed. Monitoring these values can give clues about particle dispersion stability. If the value increases significantly, the particles are not stabilized enough and may tend to agglomerate and settle over time, resulting in lack of stability. Depending on the viscosity of the medium, it can be illustrated that <500nm d99 values (e.g., for Nexbase base oils) are indications of stable dispersions when the particles remain suspended over time.
[0280] Dynamic viscosity
[0281] The dynamic viscosity is measured using a Physica MCR 300 from Anton Paar using the rotational viscometry method and a single-gap cylinder CC 27.
[0282] The motor of the viscometer drives a rotating unit (bob) in a fixed cup. The rotation speed of the rotating unit is preset, and it generates a specific motor torque required to rotate the measuring rotating unit. This torque must overcome the viscous forces of the material being measured and is therefore a measure of its viscosity. The data are in 100s -1 The shear rate was measured at 23 °C.
[0283] Visual inspection of appearance / stability
[0284] Each sample was tested for stability by diluting a small amount of concentrate to 1% by weight and 0.1% by weight solution of the nanoparticles (i.e., % by weight of the particles). The dilutions were prepared by blending the concentrate in a 50 mL glass beaker at room temperature for 1 hour. Each dilution was placed in a 5 mL glass vial and allowed to stand at room temperature. The vials were checked for signs of sedimentation after blending, one week thereafter, and four weeks later. The sedimentation was divided into 5 categories: no sedimentation (no particles settled at the bottom of the vial); slight sedimentation (some particles began to settle at the bottom of the vial); moderate sedimentation (thin layer at the bottom of the vial), almost complete sedimentation (almost all particles have settled, and the supernatant becomes clear).
[0285] For any type of dispersion containing particles, settling over time is a clear indicator of stability. Over time, the particles will settle to the bottom of the vial. Typically, this depends on their size, mass, and the viscosity of the base fluid. A stable dispersion is characterized in that the particles are uniformly dispersed in the medium and stabilized by known mechanisms.
[0286] Therefore, the stability of the nanoparticles in the dispersion is a clear prerequisite for the heat transfer performance of the nanofluid. Compared with the heat transfer nanofluids of the prior art, the embodiments of the present invention provided below show higher stability under different stability test conditions and show good thermal conductivity over a long period of time. Therefore, the stability tests below are not only carried out at room temperature, which is usually easier to achieve, but also at higher temperatures and for longer periods of time (e.g., 16 hours at 100° C.), which simulates the application of cooling electric motors with a maximum temperature of about 100° C.
[0287] Comparative Examples 1 to 3 are simple mixtures of non-chemically modified nanoparticles with any kind of surfactant or additive in a base fluid. Comparative Examples 4 to 6 are patent examples of US8850803B2.
[0288] Table 5 -Comparative ratio
[0289]
[0290] o: No settlement
[0291] Δ: Very slight settling
[0292] +: Slight settling
[0293] ++: Moderate settlement
[0294] +++: Almost completely settled.
[0295] Table 6 ——Embodiments of the present invention
[0296]
[0297] o: No settlement
[0298] Δ: Very slight settling
[0299] +: Slight settling
[0300] ++: Moderate settlement
[0301] +++: Almost completely settled.
[0302] Stability test at 100°C (viscosity change)
[0303] The corresponding dispersions were taken out and diluted to a concentration of 1 wt % and 5 wt % of nanoparticles in the dispersion (see Table 7). The dynamic viscosity and thermal conductivity of these samples were measured. Aliquots were filled into glass vials and stored in an oven at 100° C. for 16 hours (overnight). After the dispersions were cooled to room temperature, their dynamic viscosity and thermal conductivity were measured again.
[0304] During storage at 100°C, due to higher kinetic energy, dynamic processes between particles and fluid medium are enhanced, which may lead to reagglomeration and / or precipitation of nanoparticles in the dispersion. Therefore, a viscosity increase of more than 10% means that the stability of the dispersion is not satisfied.
[0305] As shown in Table 7 below, the inventors of the present invention were able to prepare nanoparticle dispersions for use as heat transfer fluids that not only have good thermal conductivity but also good stability given the requirements placed on heat transfer fluids.
[0306] In contrast, the comparative examples could not be measured because they were not stable even after one day of storage at room temperature. Therefore, it was not even possible to conduct stability tests at elevated temperatures (e.g. 100°C for 16 hours), which simulates the application of cooling an electric motor with a maximum temperature of about 100°C.
[0307] Table 7 - Viscosity of Examples of the Invention measured at room temperature (23°C) before and after storage of the dispersion at 100°C
[0308]
[0309] o: No change in viscosity (<5%)
[0310] Δ: Very small change in viscosity (>5%)
[0311] +: Slight change in viscosity (>10%)
[0312] ++: Moderate change in viscosity (>30%)
[0313] +++: Large change in viscosity (>50%)
[0314] *: Base fluid NB3020
[0315] **: Base fluid tetrabutane
[0316] Thermal conductivity was measured by LAMBDA apparatus (Flucon GmbH)
[0317] Thermal conductivity is determined by the hot wire method. The LAMBDA hot wire acts both as a heat source and as a sensor. To increase the temperature, the hot wire is subjected to a constant measuring current; as the surrounding medium heats up, the resistance of the hot wire changes according to the thermal viscosity of the surrounding medium. The voltage change in the hot wire therefore indicates the temperature change occurring in the surrounding medium. The measuring range is 10-2000 mW / m·K.
[0318] The data were measured after calorimetry (thematicization) of the measuring device via a PT 100 platinum thermometer in a metal block thermostat at 40° C. and 100° C. These temperatures were chosen because they are of interest for important applications.
[0319] As shown in Table 8 below, the use of the nanoparticle composition according to the present invention as a heat transfer fluid is advantageous because not only is the stability of the nanoparticles in the dispersion maintained over time as shown in Table 6, but the nanoparticle composition of the present invention provides improved thermal conductivity when used as a heat transfer fluid compared to the prior art heat transfer base oil reference. Furthermore, as shown in Table 7, the addition of nanoparticles does not have a significant effect on viscosity change, which is unexpected and advantageous.
[0320]
[0321] As shown in the experimental section above, it can be concluded that the comparative dispersions cannot be used as heat transfer nanofluids since they do not even meet the stability standard test.
[0322] In contrast, nanoparticle compositions of the present invention comprising nanoparticles based on hierarchical structures such as hexagonal boron nitride, carbon black, and inorganic fullerene-tungsten disulfide have been shown to be long-term stable as heat transfer fluids under conditions close to application (16 hours at 100° C.) without losing dispersion stability (viscosity) and thermal conductivity.
[0323] Friction reduction rate measured by micro-traction tester
[0324] The coefficient of friction was measured using a microtraction tester named MTM2 from PCS Instruments according to the test method described in Table 9 below. SRR refers to the slide-to-roll ratio. This parameter was kept constant during the 2-hour test and is defined as (U 球 -U 盘 ) / U, where (U 球 -U 盘 ) represents the sliding velocity and U represents the entrainment velocity, which is given by U = (U 球 +U 盘 The Stribeck curve of each sample was measured according to the scheme in Table 9.
[0325] Table 9 : A scheme for measuring the Stribeck curve
[0326]
[0327] According to MTM Method 1, the coefficient of friction of each blend over the entire speed range was recorded and a Stribeck curve was obtained. For the formulations listed in Table 10, friction tests were conducted according to these conditions and the results are disclosed in Table 11 below. The weight percentages listed are based on the total weight of the different formulations.
[0328] Table 10: Formulations according to the invention
[0329]
[0330] In order to express the friction reduction in %, a quantifiable result can be expressed as a number and is obtained by integrating the friction value curve using the corresponding Stribeck curve obtained in the sliding speed range of 5 mm / s-60 mm / s using the trapezoidal rule. The area corresponds to the "total friction" in the selected speed range. The smaller the area, the greater the friction reduction effect of the product examined. By using the reference base oil 3043 value to calculate the percentage of friction reduction, the reference base oil 3043 produced a friction area of 6.32 mm / s. A positive value indicates a reduction in the coefficient of friction. The values for the reference oils are summarized in Table 11.
[0331] Table 11: Friction reduction of the formulation according to the invention in comparison with the base oil at the boundary conditions
[0332]
[0333] The experimental results show very good friction reduction performance compared to the base oil reference. In fact, the results of the total friction calculated in the sliding speed range of 5 mm / s-60 mm / s clearly show that Example IE5 of the present invention is superior to the reference in terms of friction reduction. 3043 oil has much better effect. 3043 is a reference base oil. It has been shown that the use of the nanoparticle composition of the present invention not only enhances heat capacity, but also provides friction reduction in electrical systems with metallic moving parts.
Claims
1. Use of a nanoparticle composition as a heat transfer fluid in a battery or other electrical device system, wherein the nanoparticle composition is obtained by grinding a mixture comprising one or more nanoparticle compounds (A) and one or more polymer compounds (B), (A) wherein the one or more nanoparticle compounds (A) are selected from: - Metal or metalloid nitride nanoparticles; -Multi-walled or single-walled carbon nanotubes; - carbon black; - a metal chalcogenide having the molecular formula MX2, wherein M is selected from titanium (Ti), vanadium (V), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), zirconium (Zr), niobium (Nb), molybdenum (Mo), Metal elements of tantalum (Ta), tungsten (W), osmium (Os) and combinations thereof, and X is a chalcogen selected from sulfur (S), oxygen (O), and combinations thereof; - or a mixture thereof, and (B) wherein the one or more polymer compounds (B) are obtained by polymerizing the following monomer composition, the monomer composition comprising: a) 1 to 30 wt % of one or more functional monomers, based on the total weight of the monomer composition, selected from: a1) Aminoalkyl (meth)acrylates and aminoalkyl (meth)acrylamides; a2) alkyl(meth)acrylic nitriles and other nitrogen-containing alkyl(meth)acrylates; a3) (meth)acrylates of ether alcohols; a4) epoxyalkyl alkyl (meth)acrylate; a5) phosphorus-, boron- and / or silicon-containing alkyl (meth)acrylates; a6) Heterocycloalkyl (meth)acrylate; a7) vinyl halides; a8) vinyl esters; a9) vinyl monomers containing aromatic groups; a10) heterocyclic vinyl compounds; a11) vinyl and prenyl ethers; a12) methacrylic acid and acrylic acid, and b) 30 to 80 weight percent, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylate monomers, wherein each of the alkyl groups of the one or more alkyl (meth)acrylate monomers is independently linear, cyclic or branched and contains 1 to 40 carbon atoms; and c) 20 to 60 wt. %, based on the total weight of the monomer composition, of one or more (meth)acrylic acid esters and one or more monomers having a number average molecular weight M of 500 to 10,000 g / mol. n A hydroxylated hydrogenated polybutadiene formed into an ester exchange reaction product; The sum of the weight percentages of the components in the monomer composition is 100 weight %; and wherein the weight ratio of the one or more nanoparticle compounds (A) to the one or more polymer compounds (B) is 9:1 to 1:
5.
2. The method according to claim 1, wherein the one or more hydroxylated hydrogenated polybutadienes of component c) have a number average molecular weight M of 1,500 to 2,100 g / mol. n , which is determined according to DIN 55672-1 using tetrahydrofuran as eluent by gel permeation chromatography using polybutadiene calibration standards.
3. The method according to claim 2, wherein the one or more hydroxylated hydrogenated polybutadienes of component c) have a number average molecular weight M of 1,800 to 2,100 g / mol. n , which is determined according to DIN 55672-1 using tetrahydrofuran as eluent by gel permeation chromatography using polybutadiene calibration standards.
4. The method according to claim 2, wherein the one or more hydroxylated hydrogenated polybutadienes of component c) have a number average molecular weight M of 1,900 to 2,100 g / mol. n , which is determined according to DIN 55672-1 using tetrahydrofuran as eluent by gel permeation chromatography using polybutadiene calibration standards.
5. The method according to claim 1 or 2, wherein the one or more polymer compounds (B) have a weight average molecular weight M of 10,000 to 1,000,000 g / mol. w , which was determined by gel permeation chromatography using polymethyl methacrylate calibration standards and tetrahydrofuran as eluent.
6. The method according to claim 5, wherein the one or more polymer compounds (B) have a weight average molecular weight M of 50,000 to 800,000 g / mol. w , which was determined by gel permeation chromatography using polymethyl methacrylate calibration standards and tetrahydrofuran as eluent.
7. The method according to claim 5, wherein the one or more polymer compounds (B) have a weight average molecular weight M of 100,000 to 500,000 g / mol. w, which was determined by gel permeation chromatography using polymethyl methacrylate calibration standards and tetrahydrofuran as eluent.
8. The method according to claim 5, wherein the one or more polymer compounds (B) have a weight average molecular weight M of 150,000 to 350,000 g / mol. w , which was determined by gel permeation chromatography using polymethyl methacrylate calibration standards and tetrahydrofuran as eluent.
9. The method according to claim 1 or 2, wherein the one or more polymer compounds (B) are obtained by polymerizing a monomer composition comprising: a) 1 to 30 wt. % of the one or more functional monomers as component a), based on the total weight of the monomer composition; and b1) 30 to 60% by weight, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylates of the formula (I) as first component b): Where R is hydrogen or methyl, R 1 refers to a straight-chain, branched or cyclic alkyl group having 1 to 8 carbon atoms; and b2) from 0 to 20% by weight, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylates of the formula (II) as second component b): Where R is hydrogen or methyl, R 2 refers to a straight-chain, branched or cyclic alkyl group having 9 to 15 carbon atoms; and b3) from 0 to 20% by weight, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylates of the formula (III) as third component b): Where R is hydrogen or methyl, R 3 refers to a straight-chain, branched or cyclic alkyl group having 16 to 40 carbon atoms; and c) 20 to 60 wt. %, based on the total weight of the monomer composition, of one or more (meth)acrylic acid esters and one or more monomers having a number average molecular weight M of 500 to 10,000 g / mol. n The hydroxylated hydrogenated polybutadiene forms a transesterification product.
10. The use according to claim 9, wherein the monomer composition comprises: a) 5 to 30 wt. %, based on the total weight of the monomer composition, of the one or more functional monomers as component a).
11. The use according to claim 9, wherein the monomer composition comprises: a) 10 to 20 wt. % of the one or more functional monomers as component a), based on the total weight of the monomer composition.
12. The use according to claim 9, wherein the monomer composition comprises: b1) as first component b) 30 to 50% by weight, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylates of the formula (I).
13. The use according to claim 9, wherein the monomer composition comprises: b1) as first component b) 35 to 50% by weight, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylates of the formula (I).
14. The use according to claim 9, wherein in formula (I), R 1 It refers to a straight-chain, branched or cyclic alkyl group having 1 to 5 carbon atoms.
15. The use according to claim 9, wherein in formula (I), R 1 It refers to a straight-chain, branched or cyclic alkyl group having 1 to 4 carbon atoms.
16. The use according to claim 9, wherein the monomer composition comprises: b2) 1 to 15% by weight, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylates of the formula (II) as second component b).
17. The use according to claim 9, wherein the monomer composition comprises: b2) 1 to 10% by weight, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylates of the formula (II) as second component b).
18. The use according to claim 9, wherein in formula (II), R 2 It refers to a straight-chain, branched or cyclic alkyl group having 12 to 15 carbon atoms.
19. The use according to claim 9, wherein in formula (II), R 2 It refers to a straight-chain, branched or cyclic alkyl group having 12 to 14 carbon atoms.
20. The use according to claim 9, wherein the monomer composition comprises: b3) 0 to 15% by weight, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylates of the formula (III) as third component b).
21. The use according to claim 9, wherein the monomer composition comprises: b3) 0 to 10% by weight, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylates of the formula (III) as third component b).
22. The use according to claim 9, wherein in formula (III), R 3 It refers to a straight-chain, branched or cyclic alkyl group having 16 to 30 carbon atoms.
23. The use according to claim 9, wherein in formula (III), R 3 It refers to a straight-chain, branched or cyclic alkyl group having 16 to 20 carbon atoms.
24. The use according to claim 9, wherein the monomer composition comprises: c) 25 to 55 wt. %, based on the total weight of the monomer composition, of one or more (meth)acrylic acid esters and one or more monomers having a number average molecular weight M of 500 to 10,000 g / mol. n The hydroxylated hydrogenated polybutadiene forms a transesterification product.
25. The use according to claim 9, wherein the monomer composition comprises: c) 30 to 50 wt. %, based on the total weight of the monomer composition, of one or more (meth)acrylic acid esters and one or more monomers having a number average molecular weight M of 500 to 10,000 g / mol. n The hydroxylated hydrogenated polybutadiene forms a transesterification product.
26. The use according to claim 1 or 2, wherein the weight ratio of the one or more nanoparticle compounds (A) to the one or more polymer compounds (B) is from 5:1 to 1:
2.
27. The use according to claim 26, wherein the weight ratio of the one or more nanoparticle compounds (A) to the one or more polymer compounds (B) is from 3:1 to 1:
2.
28. The use according to claim 1 or 2, wherein the one or more polymer compounds (B) are obtained by polymerizing the following monomer composition, the monomer composition comprising: a1) as first component a) 0.5 to 5% by weight of aminoalkyl(meth)acrylamide, based on the total weight of the monomer composition; a9) 5 to 15% by weight, based on the total weight of the monomer composition, of a vinyl monomer containing an aromatic group as the second component a); b1) 35 to 50% by weight, based on the total weight of the monomer composition, of an alkyl (meth)acrylate monomer of the formula (I) as a first component b); b2) 1 to 10% by weight, based on the total weight of the monomer composition, of an alkyl (meth)acrylate monomer of the formula (II) as a second component b); c) 30 to 50% by weight of the following as component c), based on the total weight of the monomer composition: (meth)acrylic acid and a monomer having a number average molecular weight M of 500 to 10,000 g / mol. n Esters formed from hydroxylated hydrogenated polybutadiene.
29. The use according to claim 28, wherein the aminoalkyl(meth)acrylamide is N-(3-dimethylaminopropyl)methacrylamide.
30. The use according to claim 28, wherein the vinyl monomer containing an aromatic group is styrene.
31. The use according to claim 28, wherein the alkyl (meth)acrylate monomer of formula (I) is methyl methacrylate and / or butyl methacrylate.
32. The use according to claim 28, wherein the alkyl (meth)acrylate monomer of formula (II) is lauryl methacrylate.
33. The use according to claim 28, wherein the component c) is a macromonomer derived from an ester of (meth)acrylic acid and having a number average molecular weight M of 1,500 to 5,000 g / mol. n The ester exchange reaction is carried out between the hydroxylated hydrogenated polybutadiene.
34. The use according to claim 1 or 2, wherein the weight contents of the monomers a), b) and c) of the monomer composition add up to 100% by weight, based on the total weight of the monomer composition.
35. The use according to claim 1 or 2, wherein the nanoparticle compound (A) is selected from hexagonal boron nitride (hBN) nanoparticles; carbon black; a metal chalcogenide having a molecular formula MX2, wherein the metal element M is molybdenum (Mo) or tungsten (W), and the chalcogen element X is sulfur (S); or a mixture thereof.
36. Use according to claim 1 or 2, wherein the nanoparticle composition further comprises a base fluid (C) having a kinematic viscosity at 40°C of 3 cSt to 30 cSt according to ASTM D-445, and a flash point above 110°C according to ASTM D-93.
37. Use according to claim 36, wherein the base fluid (C) has a kinematic viscosity at 40°C according to ASTM D-445 of 3 to 15 cSt.
38. Use according to claim 36, wherein the base fluid is selected from the group consisting of API Group I base oils, API Group II base oils, API Group III base oils, API Group IV base oils, API Group V base oils or mixtures thereof.
39. The use according to claim 36, wherein the nanoparticle composition comprises 85 to 99.9 wt% of base fluid (C) and 0.1 to 15 wt% of (A) and (B), based on the total weight of the nanoparticle composition.
40. Use according to claim 39, wherein the nanoparticle composition comprises 90 to 99.9 wt% of base fluid (C) and 0.1 to 10 wt% of (A) and (B), based on the total weight of the nanoparticle composition.
41. The use according to claim 39, wherein the nanoparticle composition comprises 92 to 99.5 wt% of base fluid (C) and 0.5 to 8 wt% of (A) and (B), based on the total weight of the nanoparticle composition.
42. The use according to claim 36, wherein the amounts of (A), (B) and (C) add up to 100 wt.-%, based on the total weight of the nanoparticle composition.
43. The use according to claim 1 or 2, wherein the nanoparticle composition comprising one or more nanoparticles (A) and one or more polymer compounds (B) is milled via a ball milling process.
44. Use according to claim 36, wherein the nanoparticle composition comprising one or more nanoparticles (A), one or more polymer compounds (B) and the base fluid (C) is milled via a ball milling process.
45. The use according to claim 1 or 2, wherein the nanoparticle composition further comprises one or more additive components (D) selected from antioxidants, antiwear additives, pour point depressants, corrosion inhibitors, metal passivators, electrostatic discharge inhibitors, defoamers, seal fixatives or seal compatibilizers, rust inhibitors, demulsifiers, emulsifiers, friction modifiers, extreme pressure additives, dyes or mixtures thereof.
46. The use according to claim 1 or 2, wherein the other electrical equipment system is selected from the group consisting of electric motors, electric vehicle transmissions, power transformers, capacitors, fluid-filled transmission lines, and computers.
47. Use according to claim 1 or 2, wherein the other electrical equipment system is selected from fluid-filled power cables.
48. Use according to claim 1 or 2, wherein the other electrical equipment systems are selected from power electronic components.
Citation Information
Patent Citations
Butadiene polymers having terminal functional groups
GB2270317A
Composition for enhancing thermal conductivity of a heat transfer medium and method of use thereof
US20040069454A1
Nanofluids for heat transfer applications
US20150048272A1
Novel telechelic polymers and processes for the preparation thereof
US4316973A
Auxiliary power and emission-control system using vented gaseous fuel recovery and method
US8850803B2