Thermoplastic elastomer composition, and joint member and method for producing the same

By using a specific proportion of styrene-butadiene hydrogenated block copolymer and polypropylene resin in the thermoplastic elastomer composition and dynamic crosslinking, the sliding, welding and high-temperature compression in the prior art are solved. The problem of insufficient permanent deformation performance has achieved the performance improvement of the composite molded bodies for automobiles.

CN114144457BActive Publication Date: 2024-11-05MITSUBISHI CHEM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080052657.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-08-26
Filing Date
2020-05-11
Publication Date
2024-11-05
Estimated Expiration
2040-05-11

AI Technical Summary

Technical Problem

The conventional thermoplastic elastomer composition has insufficient performance in terms of sliding properties, welding properties and compression permanent deformation (degradability) at high temperatures, and it is difficult to meet the requirements of composite molded bodies for automobiles.

Method used

The thermoplastic elastomer composition formed by adopting a specific proportion of styrene-butadiene hydrogenated block copolymer and polypropylene resin and dynamically crosslinked by crosslinking agent is optimized to improve the component ratio and crosslinking reaction, and improve the It has smoothness and welding properties, while maintaining good compression permanent deformation performance at high temperatures.

Benefits of technology

It achieves excellent sliding properties, welding properties and compression permanent deformation performance at high temperatures, meets the needs of composite molded bodies for automobiles, and provides better forming processability and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114144457B_ABST
    Figure CN114144457B_ABST
Patent Text Reader

Abstract

A joining member, comprising a thermoplastic elastomer composition comprising the following (A), (B) and (C), wherein the composition comprises 100 to 140 parts by mass of the component (B) and 60 to 140 parts by mass of the component (C) relative to 100 parts by mass of the component (A), and is crosslinked by the following component (D), wherein the compression set measured under the conditions of 70°C, 22 hours, and 25% compression is 60% or less in accordance with JIS K6262. Component (A): a hydrogenated product of a block copolymer having at least two polymer blocks mainly composed of a vinyl aromatic compound and at least one polymer block containing butadiene, wherein the proportion of the hydrogenated product of the block copolymer (A1) having a weight average molecular weight of 300,000 or more in the hydrogenated product of the block copolymer is 30 to 100% by mass; Component (B): a hydrocarbon rubber softener; Component (C): a polypropylene resin; Component (D): a crosslinking agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a thermoplastic elastomer composition, a joining member formed from the thermoplastic elastomer composition, a method for producing the same, and a composite molded body for automobiles using the joining member. Specifically, the present invention relates to a thermoplastic elastomer composition having excellent sliding properties, weldability with extrusion materials, and compression set (deterioration) at high temperatures and having fluidity suitable for injection molding, a joining member formed from the thermoplastic elastomer composition, a method for producing the same, and a composite molded body for automobiles using the joining member. Background Art

[0002] The thermoplastic elastomer composition obtained by subjecting a polypropylene resin and a styrene-butadiene block copolymer to dynamic heat treatment exhibits the characteristics of a rubbery soft material, and does not require a vulcanization process, and has the same molding processability as a thermoplastic resin. Therefore, from the perspectives of rationalization of the manufacturing process and recyclability, such a thermoplastic elastomer composition has attracted attention and is widely used in the fields of automobile parts, home appliances, medical equipment parts, wires, and sundries. In particular, the thermoplastic elastomer composition is often used as a sealing material for automobiles and sealing materials for building materials.

[0003] Since automobile sealing materials and building material sealing materials have complicated structures, the target members are usually manufactured by joining members composed of thermoplastic elastomer compositions. In this case, as a technique for joining molded bodies composed of thermoplastic elastomer compositions without using an adhesive or the like, for example, as described in Patent Document 1, there is known a technique for heat-welding the joined members by mixing olefin copolymer rubber, mineral oil-based rubber softener and polypropylene-based resin at a certain ratio and dynamically crosslinking the resulting joined members.

[0004] Patent Document 2 discloses a technique for mixing olefin copolymer rubber, crystalline ethylene copolymer and polypropylene resin at a certain ratio and performing dynamic crosslinking as a technique for obtaining a thermoplastic elastomer for joint corner members for composite molded bodies for automobiles that allow vulcanized rubber molded bodies to be fully welded to each other.

[0005] Patent Document 3 discloses a technique for obtaining a joining member for a composite molded body having excellent sliding properties, welding properties, and compression set (deterioration resistance) at high temperatures, using a thermoplastic elastomer composition obtained by mixing a styrene-butadiene non-hydrogenated block copolymer of a specific viscosity, a styrene-butadiene hydrogenated block copolymer, a hydrocarbon rubber softener, and a polypropylene resin at a certain ratio and subjecting them to dynamic crosslinking.

[0006] Patent Document 1: Japanese Patent Application Publication No. 2008-266615

[0007] Patent Document 2: Japanese Patent Application Publication No. 2003-155386

[0008] Patent Document 3: Japanese Patent Application Publication No. 2019-131722

[0009] In recent years, automotive composite molded bodies composed of thermoplastic elastomer compositions have been required to have excellent sliding properties, weldability with extruded materials, and compression set (deterioration) at high temperatures, as well as good moldability (flowability) as joining members.

[0010] The joining member composed of the thermoplastic elastomer composition described in Patent Document 1 has good adhesion to the elastomer molded body, but Patent Document 1 does not mention the sliding property required for the joining member of the composite molded body for automobiles.

[0011] Generally, if a lubricant such as silicone oil or oleic acid amide is added, high sliding properties can be obtained. However, the surface tension of the lubricant is low and it is exposed on the bonding surface with the molded body, resulting in reduced weldability.

[0012] In Patent Document 1, since a low-fluidity propylene homopolymer (MFR: 0.7 g / 10 min (230° C., 21.18 N)) is used as the polypropylene-based resin, the fluidity is low and the injection moldability is insufficient.

[0013] The joining member composed of the thermoplastic elastomer composition described in Patent Document 2 has good adhesion to the vulcanized rubber molded body, but Patent Document 2 does not mention the sliding property required for the joining member of the composite molded body for automobiles. In addition, Patent Document 2 describes the compression set (deterioration) at 70°C for 22 hours, but it is also more than 60% and is not sufficient, and the compression set at high temperature (100°C for 22 hours) may be further deteriorated.

[0014] The joining member composed of the thermoplastic elastomer composition described in Patent Document 3 has good weldability with the extruded material and compression set (deterioration resistance) at high temperatures. However, since the molecular weight of the low-viscosity block copolymer is relatively low, the elastomer composition sometimes has poor tensile properties required as a joining member, and there is still room for improvement.

[0015] As described above, there has been no thermoplastic elastomer composition suitable as a joining member of a composite molded body for automobiles, which has all of the sliding properties and welding properties, compression set (deterioration properties) at high temperatures, and moldability in a well-balanced manner. Summary of the invention

[0016] Problems to be solved by the invention

[0017] An object of the present invention is to provide a thermoplastic elastomer composition having excellent slidability and weldability as well as excellent compression set (deterioration resistance) at high temperatures, a joined member formed from the thermoplastic elastomer composition, a method for producing the same, and a composite molded body for an automobile using the joined member.

[0018] Technical solutions to solve problems

[0019] The present inventors have found that the above-mentioned problems can be solved by using a styrene-butadiene hydrogenated block copolymer and a polypropylene resin having a specific molecular weight in a specific ratio, thereby improving not only the compression set at high temperature but also the sliding property. The inventors have thus completed the present invention.

[0020] That is, the gist of the present invention is as follows.

[0021] [1] A joining member comprising a thermoplastic elastomer composition,

[0022] The thermoplastic elastomer composition comprises the following (A), (B) and (C), wherein the composition comprises 100 to 140 parts by mass of the component (B) and 60 to 140 parts by mass of the component (C) based on 100 parts by mass of the component (A).

[0023] And cross-linked by the following component (D),

[0024] According to JIS K6262, the compression set measured at 70°C, 22 hours, and 25% compression is 60% or less.

[0025] Component (A): a hydrogenated product of a block copolymer having at least two polymer blocks mainly composed of a vinyl aromatic compound and at least one polymer block containing butadiene, wherein the proportion of the hydrogenated product of the block copolymer (A1) having a weight average molecular weight of 300,000 or more in the hydrogenated product of the block copolymer is 30 to 100% by mass;

[0026] Component (B): a hydrocarbon rubber softener;

[0027] Component (C): polypropylene resin;

[0028] Component (D): a cross-linking agent.

[0029] [2] The joined member according to [1], wherein the component (C) contains a propylene-based random copolymer having a melting peak temperature of 100°C or higher and lower than 157°C.

[0030] [3] The joined member according to [1] or [2], wherein the thermoplastic elastomer composition contains 0.5 parts by mass or more and 10.0 parts by mass or less of the component (D) relative to 100 parts by mass of the component (A).

[0031] [4] A composite molded body for an automobile, comprising the joining member according to any one of [1] to [3].

[0032] [5] A method for producing a joined member, the method comprising melt-kneading a thermoplastic elastomer composition and injection molding the kneaded product, wherein the thermoplastic elastomer composition comprises the following (A), (B), (C) and (D), wherein the composition comprises 100 to 140 parts by mass of the component (B) and 60 to 140 parts by mass of the component (C) per 100 parts by mass of the component (A);

[0033] Component (A): a hydrogenated product of a block copolymer having at least two polymer blocks mainly composed of a vinyl aromatic compound and at least one polymer block containing butadiene, wherein the proportion of the hydrogenated product of the block copolymer (A1) having a weight average molecular weight of 300,000 or more in the hydrogenated product of the block copolymer is 30 to 100% by mass;

[0034] Component (B): a hydrocarbon rubber softener;

[0035] Component (C): polypropylene resin;

[0036] Component (D): a cross-linking agent.

[0037] [6] A thermoplastic elastomer composition comprising the following (A), (B) and (C), wherein the composition comprises 100 to 140 parts by mass of the component (B) and 60 to 140 parts by mass of the component (C) per 100 parts by mass of the component (A);

[0038] And cross-linked by the following component (D),

[0039] According to JIS K6262, the compression set measured at 70°C, 22 hours, and 25% compression is 60% or less.

[0040] Component (A): a hydrogenated product of a block copolymer having at least two polymer blocks mainly composed of a vinyl aromatic compound and at least one polymer block containing butadiene, wherein the proportion of the hydrogenated product of the block copolymer (A1) having a weight average molecular weight of 300,000 or more in the hydrogenated product of the block copolymer is 30 to 100% by mass;

[0041] Component (B): a hydrocarbon rubber softener;

[0042] Component (C): polypropylene resin;

[0043] Component (D): a cross-linking agent.

[0044] [7] The thermoplastic elastomer composition according to [6], wherein the density of the thermoplastic elastomer composition is 0.90 to 0.95 g / cm 3 .

[0045] [8] The thermoplastic elastomer composition according to [6] or [7], wherein the melt flow rate of the thermoplastic elastomer composition measured at a measurement temperature of 230° C. and a measurement load of 21.2 N in accordance with JIS K7210 is 10 to 80 g / 10 min.

[0046] Effects of the Invention

[0047] The thermoplastic elastomer composition of the present invention has excellent molding processability, and also has good slidability, weldability, and compression set (degradation) at high temperatures. Using the thermoplastic elastomer composition of the present invention, a composite molded body joint member having excellent slidability, weldability, and compression set (degradation) at high temperatures can be obtained based on good molding processability.

[0048] The joining member formed from the thermoplastic elastomer composition of the present invention is useful as a sealing material for automobiles and a sealing material for building materials due to its excellent sliding property and weldability, compression set (deterioration property) at high temperature and moldability. The joining member formed from the thermoplastic elastomer composition of the present invention is particularly useful as a joining member for a composite molded body for automobiles such as an automobile glass run channel. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 This is a perspective view showing an example of a glass run channel for an automobile to which the present invention is applied.

[0050] Description of Reference Numerals

[0051] 1A, 1B: Extrusion molding parts

[0052] 2: Joining components

[0053] 3: Composite molding DETAILED DESCRIPTION

[0054] The present invention will be described in detail below. The present invention is not limited to the following description, and can be implemented in any modified manner without departing from the gist of the present invention.

[0055] In the present specification, when a numerical value or a physical property value is expressed by inserting "to" before or after it, it is used as including the values ​​before and after it.

[0056] [Thermoplastic elastomer composition]

[0057] The thermoplastic elastomer composition of the present invention contains at least the following components (A) to (C) in a predetermined ratio and is crosslinked by the following component (D). The compression set measured under the conditions of 70°C, 22 hours, and 25% compression according to JIS K6262 is 60% or less.

[0058] Component (A): a hydrogenated product of a block copolymer having at least two polymer blocks mainly composed of a vinyl aromatic compound and at least one polymer block containing butadiene, wherein the proportion of the hydrogenated product of the block copolymer (A1) having a weight average molecular weight of 300,000 or more in the hydrogenated product of the block copolymer is 30 to 100% by mass;

[0059] Component (B): a hydrocarbon rubber softener;

[0060] Component (C): polypropylene resin;

[0061] Component (D): a cross-linking agent.

[0062] [mechanism]

[0063] The thermoplastic elastomer composition of the present invention has the effects of being excellent in sliding property, weldability, and compression set (deterioration property) at high temperature, and also having good molding processability.

[0064] The details of why the thermoplastic elastomer composition of the present invention achieves such effects are not known, but it is presumed as follows:

[0065] 1) In the hydrogenated product (A1) of the block copolymer having a weight average molecular weight of 300,000 or more in an amount of 30 parts by mass or more and 100 parts by mass or less out of 100 parts by mass of the component (A), double bonds between carbon atoms present in a small amount serve as connecting crosslinking points with the crosslinking agent or crosslinking aid of the component (D) added during dynamic crosslinking, thereby forming loose bonds between molecular chains, thereby improving rubber elasticity at high temperatures, that is, compression set (degradation resistance).

[0066] 2) By kneading the hydrogenated product (A1) of the block copolymer having a weight average molecular weight of 300,000 or more with the crosslinking agent and the crosslinking aid of the component (D), the rubber component is dispersed in a fine dispersion diameter during kneading, which also contributes to the smoothness of the surface of the molded body, thereby obtaining good sliding properties.

[0067] 3) As a result of the good sliding properties brought about by the rubber component (A), the amount of lubricant added, such as silicone oil, which has the effect of reducing the surface tension (welding properties with the adherend), can be controlled, thereby improving the welding properties.

[0068] 4) Component (A) as a rubber component is mainly composed of vinyl aromatic compound units, so it can contain more rubber softener than olefin rubber, thereby showing moderate fluidity of 10 to 80 / 10 minutes (230°C, 21.2N) suitable for injection molding, and the molding processability is also improved.

[0069] 5) The thermoplastic elastomer composition of the present invention contains the crosslinking agent as component (D). Therefore, when heat-welded to the olefin rubber as an adherend by injection molding, it becomes a crosslinking point connecting the molecular chains of the elastomer and the adherend, thereby improving the weldability.

[0070] [Ingredients (A)]

[0071] The component (A) used in the thermoplastic elastomer of the present invention is a hydrogenated product (hydrogenated block copolymer) of a block copolymer having at least two polymer blocks mainly composed of a vinyl aromatic compound (hereinafter sometimes referred to as "block P") and at least one polymer block containing butadiene (hereinafter sometimes referred to as "block Q"), wherein the proportion of the hydrogenated block copolymer (A1) having a weight average molecular weight of 300,000 or more in 100 parts by mass of the hydrogenated block copolymer of the component (A) is 30 parts by mass or more and 100 parts by mass or less.

[0072] Here, "polymer mainly containing vinyl aromatic compounds" refers to a polymer obtained by polymerizing monomers mainly containing vinyl aromatic compounds. "Polymer containing butadiene" refers to a polymer obtained by polymerizing monomers containing butadiene. "Polymer mainly containing vinyl aromatic compounds" means containing 50 mol% or more of vinyl aromatic compounds.

[0073] When the proportion of the hydrogenated block copolymer (A1) having a weight average molecular weight of 300,000 or more in 100 parts by mass of the component (A) is greater than the above lower limit, good compression set (degradation) and weldability can be obtained. When the proportion of the hydrogenated block copolymer (A1) having a weight average molecular weight of 300,000 or more is less within the above range, fluidity tends to become good.

[0074] The weight average molecular weight of the hydrogenated block copolymer (A1) is a value converted to polystyrene measured by gel permeation chromatography (hereinafter sometimes referred to as GPC). The weight average molecular weight of the hydrogenated block copolymer (A1) is 300,000 or more, preferably 320,000 or more, and more preferably 340,000 or more. The upper limit of the weight average molecular weight of the hydrogenated block copolymer (A1) is usually 600,000 or less, preferably 580,000 or less, more preferably 560,000 or less, and from the viewpoint of weld strength, it is further preferably 430,000 or less.

[0075] When the weight average molecular weight of the hydrogenated block copolymer (A1) is within the above range, it is possible to obtain good sliding properties while having sufficient compression set.

[0076] Component (A) contains 30 to 100 parts by mass of the hydrogenated block copolymer (A1) in 100 parts by mass of component (A). From the viewpoint of compression set (deterioration) and weldability, the content of the hydrogenated block copolymer (A1) in 100 parts by mass of component (A) is preferably 35 to 100 parts by mass, particularly preferably 40 to 100 parts by mass, and particularly preferably 45 to 100 parts by mass.

[0077] Component (A) is a hydrogenated product of a block copolymer, wherein the block copolymer comprises the above-mentioned hydrogenated block copolymer other than the hydrogenated block copolymer (A1), at least two polymer blocks P mainly composed of a vinyl aromatic compound, and at least one polymer block Q containing butadiene, and may also contain a hydrogenated block copolymer having a weight average molecular weight of less than 300,000 (hereinafter sometimes referred to as "hydrogenated block copolymer (A2)"). In this case, the weight average molecular weight of the hydrogenated block copolymer (A2) is preferably 220,000 to 290,000, and particularly preferably 230,000 to 280,000. The content of the hydrogenated block copolymer (A2) in the component (A) also depends on the weight average molecular weight of the hydrogenated block copolymer (A2), and is 70 parts by mass or less, preferably 65 parts by mass or less, relative to 100 parts by mass of the component (A). The weight average molecular weight of component (A), as an average value calculated from the weight average molecular weights and content ratios of the hydrogenated block copolymer (A1) and the hydrogenated block copolymer (A2) in component (A), is preferably 300,000 or more, particularly preferably 305,000 to 340,000, and particularly preferably 310,000 to 335,000.

[0078] Component (A) contains x parts by weight of a weight average molecular weight W a The hydrogenated block copolymer (A1) of y parts by mass has a weight average molecular weight W b When the hydrogenated block copolymer (A2) is contained (condition: x+y=100), the weight average molecular weight W calculated from the component (A) is calculated according to the following formula. The component (A) preferably contains the hydrogenated block copolymer (A1) and the hydrogenated block copolymer (A2) so that the value W is within the above range. When two or more hydrogenated block copolymers (A1) and hydrogenated block copolymers (A2) are contained respectively, the weight average molecular weight W calculated from the weight average molecular weight and the content ratio can also be calculated in the same manner.

[0079] W = {(W a×x)+(W b×y)} / 100

[0080] By using the hydrogenated block copolymer (A1) and the hydrogenated block copolymer (A2) in combination under such conditions, molding can be performed with good fluidity while maintaining compression set (deterioration resistance) and weldability.

[0081] When component (A) contains hydrogenated block copolymer (A1) and hydrogenated block copolymer (A2), in the elution curve measured by GPC, a peak from the hydrogenated block copolymer (A1) and a peak from the hydrogenated block copolymer (A2) are detected. Therefore, it can be known that it is a mixture of hydrogenated block copolymer (A1) and hydrogenated block copolymer (A2). In addition, based on the intensity ratio of the peak, the content ratio of the hydrogenated block copolymer (A1) and the hydrogenated block copolymer (A2) in component (A) can be calculated.

[0082] The monomer vinyl aromatic compound constituting the block P of the hydrogenated block copolymer of component (A) is not limited, but preferably a styrene derivative such as styrene and / or α-methylstyrene. Among them, styrene is preferably used as the main component. Block P may also contain monomers other than vinyl aromatic compounds as raw materials.

[0083] Block Q may contain a monomer other than butadiene as a raw material. In this case, isoprene is preferred as the monomer raw material other than butadiene. Block Q preferably contains butadiene or butadiene and isoprene as a main component.

[0084] Here, "mainly containing butadiene" means containing 50 mol% or more of butadiene. "Mainly containing butadiene and isoprene" means containing 50 mol% or more of butadiene and isoprene in total.

[0085] The weight ratio of the block P in the hydrogenated block copolymer of component (A) is not limited, but is preferably 5% by mass or more, more preferably 10% by mass or more, preferably 55% by mass or less, more preferably 50% by mass or less, and further preferably 45% by mass or less. When the weight ratio of the block P is within the above range, the ratio of the crosslinking reaction tends to be good.

[0086] The chemical structure of the hydrogenated block copolymer of component (A) may be linear, branched or radial, but is preferably a structure represented by the following formula (1) or (2). From the viewpoint of improving mechanical strength, the structure of the following formula (1) is more preferred.

[0087] P-(QP)m (1)

[0088] (PQ)n (2)

[0089] In the formula, P represents block P, Q represents block Q, m represents an integer of 1 to 5, and N represents an integer of 2 to 5.

[0090] In formula (1) or (2), m and n are preferably as large as possible from the viewpoint of lowering the order-disorder transition temperature of the rubber polymer, but are preferably as small as possible from the viewpoint of ease of production and cost.

[0091] As the hydrogenated block copolymer of component (A), a hydrogenated block copolymer represented by formula (1) is preferred over a hydrogenated block copolymer represented by formula (2) because of its excellent rubber elasticity. A block copolymer represented by formula (1) in which m is 3 or less is more preferred, and a hydrogenated block copolymer represented by formula (1) in which m is 2 or less is further preferred.

[0092] As the hydrogenated block copolymer of component (A), there can be mentioned: styrene-butadiene-styrene hydrogenated block copolymer, styrene-isoprene-butadiene-styrene hydrogenated block copolymer, etc. Among these, styrene-butadiene-styrene hydrogenated block copolymer is preferred because it is easy to obtain the fluidity required for the weldability with the olefin rubber as the adherend material in the use as a joining member.

[0093] The manufacturing method of the hydrogenated block copolymer of component (A) in the present invention can be any method as long as the above-mentioned structure and physical properties can be obtained, and is not particularly limited. For example, the block copolymer can be obtained by the method described in Japanese Unexamined Patent Publication No. 7-97493, using a lithium catalyst, etc. Block polymerization. The hydrogenation (hydrogenation) of the block copolymer can be carried out in the presence of a hydrogenation catalyst in an inert solvent, for example, by the method described in Japanese Unexamined Patent Publication No. 59-133203.

[0094] Examples of commercially available hydrogenated block copolymers of component (A) include "TAIPOL-6151" and "TAIPOL-6159" manufactured by Taiwan Synthetic Rubber Co., Ltd. (TSRC), "G1651" and "G1633" manufactured by Kraton Polymer Japan Co., Ltd., and "SEPTON 4099" manufactured by Kuraray Co., Ltd.

[0095] The hydrogenated block copolymer of the component (A) may be used alone or in combination of two or more copolymers having different compositions and properties. However, since it is easy to control the overall property balance, it is preferred to use two or more in combination. As a preferred example of this case, a hydrogenated block copolymer (A1) and a hydrogenated block copolymer (A2) may be used in combination so that the weight average molecular weight W of the component (A) is within the preferred range.

[0096] [Ingredient (B)]

[0097] The thermoplastic elastomer composition of the present invention contains 100 parts by mass or more and 140 parts by mass or less of a hydrocarbon rubber softener as component (B) based on 100 parts by mass of component (A) from the viewpoint of improving moldability.

[0098] The lower limit of the content of the component (B) in the thermoplastic elastomer composition of the present invention is usually 100 parts by mass or more, preferably 102 parts by mass or more, and more preferably 104 parts by mass or more, relative to 100 parts by mass of the component (A), from the viewpoint of moldability. The upper limit of the content of the component (B) in the thermoplastic elastomer composition of the present invention is usually 140 parts by mass or less, preferably 138 parts by mass or less, and more preferably 136 parts by mass or less, relative to 100 parts by mass of the component (A), from the viewpoint of flexibility.

[0099] As the hydrocarbon-based rubber softener of component (B), mineral oil-based softeners, synthetic resin-based softeners, etc. can be cited, but mineral oil-based softeners are preferred from the viewpoint of affinity with other components. Mineral oil-based softeners are usually a mixture of aromatic hydrocarbons, cycloparaffinic hydrocarbons and paraffinic hydrocarbons. Those containing 50% or more of all carbon atoms as paraffinic hydrocarbons are called paraffinic oils, those containing 30 to 45% of all carbon atoms as cycloparaffinic hydrocarbons are called cycloparaffinic oils, and those containing 35% or more of all carbon atoms as aromatic hydrocarbons are called aromatic oils. Among these, paraffinic oils are preferably used.

[0100] The kinematic viscosity of the hydrocarbon rubber softener of component (B) at 40°C is not particularly limited, but is preferably 20 cSt or more, more preferably 50 cSt or more, and preferably 800 cSt or less, more preferably 600 cSt or less. The flash point (COC method) of the hydrocarbon rubber softener is preferably 200°C or more, more preferably 250°C or more.

[0101] The hydrocarbon rubber softener of component (B) can be obtained as a commercial product. Examples of such commercial products include the "Nippon Polybutene (registered trademark) HV" series manufactured by JX Nippon Mining and Energy Co., Ltd. and the "DIANA (registered trademark) PROCESS OIL PW" series manufactured by Idemitsu Kosan Co., Ltd., and suitable products can be appropriately selected from these for use.

[0102] The hydrocarbon rubber softener of component (B) may be used alone or in any combination and ratio of two or more.

[0103] [Ingredient (C)]

[0104] The thermoplastic elastomer composition of the present invention contains 60 parts by mass or more and 140 parts by mass or less of the polypropylene resin as the component (C) based on 100 parts by mass of the component (A) from the viewpoint of improving moldability.

[0105] The lower limit of the content of the component (C) in the thermoplastic elastomer composition of the present invention is usually 60 parts by mass or more, preferably 70 parts by mass or more, and more preferably 80 parts by mass or more, relative to 100 parts by mass of the component (A), from the viewpoint of moldability. The upper limit of the content of the component (C) in the thermoplastic elastomer composition of the present invention is usually 140 parts by mass or less, preferably 130 parts by mass or less, and more preferably 120 parts by mass or less, relative to 100 parts by mass of the component (A), from the viewpoint of obtaining a hardness having sufficient flexibility as a molded product.

[0106] Component (C) preferably contains a propylene polymer having a melting peak temperature of 100° C. or higher and less than 157° C. (hereinafter sometimes referred to as “component (C1)”). If component (C1) is contained, component (C) may contain other polypropylene resins such as component (C2) described later. In the present invention, “polypropylene resin” refers to a resin having a propylene unit content of 50% by mass or more. Component (C1) mainly contributes to injection moldability.

[0107] When the melting peak temperature of the component (C1) contained in the component (C) is not less than the above lower limit, it is preferred from the viewpoint of heat resistance, and when it is less than the above upper limit, it is preferred from the viewpoint of compatibility with the component (A).

[0108] The melting peak temperatures of the component (C1) and the component (C2) described later can be measured by the following method in accordance with JIS K7121.

[0109] The melting behavior of the polypropylene resin was measured by sequentially performing the following steps (1) to (3) using a differential scanning calorimeter (DSC6220 manufactured by SSI Nanotech Corporation).

[0110] In each step, time is plotted on the horizontal axis and the heat of fusion is plotted on the vertical axis to obtain a melting curve, and the peak top observed in step (3) is taken as the melting peak temperature.

[0111] Step (1): 5 mg of a sample was heated from room temperature to 200°C at a rate of 100°C / min from 40°C. After the heating was completed, the temperature was maintained for 3 minutes.

[0112] Step (2): The temperature was lowered from 200°C to 40°C at a rate of 10°C / min. After the temperature was lowered, the temperature was maintained for 3 minutes.

[0113] Step (3): Raise the temperature from 40°C to 200°C at a rate of 10°C / min.

[0114] Component (C1) is preferably a propylene random copolymer. Relative to the total amount of the monomer units constituting component (C1), the content of propylene units in the propylene random copolymer of component (C1) is preferably 60 to 99% by mass, more preferably 80 to 98% by mass. When the content of propylene units in component (C1) is within the above range, it is easy to become the range of the aforementioned melting peak temperature, and thus preferred.

[0115] The content of each structural unit of the component (C1) can be determined by infrared spectroscopy. The same applies to the component (C2) described later.

[0116] The propylene-based random copolymer of component (C1) is a copolymer having propylene units and structural units other than propylene units. As structural units other than propylene units, specifically, α-olefin units other than ethylene units and propylene units can be mentioned. As structural units other than propylene units that component (C1) can contain, for example, ethylene units, 1-butene units, 1-pentene units, 1-hexene units, 1-heptene units, 1-octene units, 1-nonene units, 1-decene units, 1-undecene units, 1-dodecene units, 1-tridecene units, 1-tetradecene units, 1-pentadecene units, 1-hexadecene units, 1-heptadecene units, 1-octadecene units, 1-nonadecene units, 1-eicosene units, 3-methyl-1-butene units, 3-methyl-1-pentene units, 4-methyl-1-pentene units, 2-ethyl-1-hexene units, and 2,2,4-trimethyl-1-pentene units. Component (C1) may contain only one of these or two or more thereof. Preferred structural units other than propylene units contained in component (C1) include ethylene units and 1-butene units.

[0117] Examples of the polypropylene resin contained in component (C) other than component (C1) include propylene polymers having a melting peak temperature of 157° C. to 175° C. (hereinafter sometimes referred to as “component (C2)”). Component (C2) is mainly a component that imparts heat resistance to the thermoplastic elastomer composition.

[0118] By setting the melting peak temperature of component (C2) to 157° C. or higher, heat resistance is imparted. From this viewpoint, the melting peak temperature of component (C2) is preferably 160° C. or higher. From the viewpoint of weldability with an extruded member, the upper limit of the melting peak temperature of component (C2) is 175° C. or lower, preferably 170° C. or lower.

[0119] In the propylene polymer of component (C2), the content of propylene units is preferably 90% by mass or more, more preferably 98 to 100% by mass, relative to the total amount of monomer units constituting component (C2). When the content of propylene units of component (C2) is within the above range, it is easy to fall within the above-mentioned range of the melting peak temperature, which is preferred.

[0120] The propylene polymer of component (C2) may also have structural units other than propylene. Component (C) may contain, for example, α-olefin units other than ethylene units and propylene. In this case, the α-olefin units that may be contained in component (C2) include, for example, 1-butene units, 1-pentene units, 1-hexene units, 1-heptene units, 1-octene units, 1-nonene units, 1-decene units, 1-undecene units, 1-dodecene units, 1-tridecene units, 1-tetradecene units, 1-pentadecene units, 1-hexadecene units, 1-heptadecene units, 1-octadecene units, 1-nonadecene units, 1-eicosene units, 3-methyl-1-butene units, 3-methyl-1-pentene units, 4-methyl-1-pentene units, 2-ethyl-1-hexene units, and 2,2,4-trimethyl-1-pentene units. Component (C2) may contain only one structural unit other than these propylene units, or may contain two or more structural units. When component (C2) contains structural units other than propylene units, preferred other structural units include ethylene units and 1-butene units.

[0121] When component (C) contains component (C2), the content of component (C2) in component (C) is 50% by mass or less, for example, preferably 5 to 50% by mass. Component (C) contains component (C2), which imparts heat resistance, but when the content is too high, the weldability with the extruded member may be reduced.

[0122] As the method for producing the propylene-based polymer of component (C1) and component (C2), a known polymerization method using a known olefin polymerization catalyst can be used. For example, a polymerization method using a Ziegler-Natta catalyst can be used. In the polymerization method, a slurry polymerization method, a solution polymerization method, a bulk polymerization method, a gas phase polymerization method, etc. can be used, and these methods can be used in combination of two or more.

[0123] Component (C1) and component (C2) can be obtained as commercial products. Examples of the commercial products include Prime Polymer's Prim Polypro (registered trademark), Sumitomo NOBLEN (registered trademark) of Sumitomo Chemical Co., Ltd., polypropylene block copolymers of SunAllomer Co., Ltd., NOVATEC (registered trademark) PP of Japan Polypropylene Co., Ltd., Moplen (registered trademark) of LyondellBasell, ExxonMobil PP of ExxonMobil, Formolene (registered trademark) of Formosa Plastics, Borealis PP of Borealis, SEETEC PP of LG Chem, ASI POLYPROPYLENE of A. Schulman, INEOS PP of INEOS Olefins & Polymers, Braskem PP of Braskem, Sumsung Total of SAMSUNG TOTAL PETROCHEMICALS, Sabic (registered trademark) PP of Sabic, and TOTAL PETROCHEMICALS Polypropylene, SK's YUPLENE (registered trademark), etc., and suitable products can be appropriately selected from these and used in combination.

[0124] The component (C1) and the component (C2) may be used alone or in combination of two or more copolymers having different compositions and physical properties.

[0125] [Ingredient (D)]

[0126] The thermoplastic elastomer composition of the present invention contains a crosslinking agent as component (D). The thermoplastic elastomer composition of the present invention can improve rubber elasticity by crosslinking at least a portion of component (A) by dynamically heat treating in the presence of the crosslinking agent as component (D).

[0127] As the crosslinking agent, organic peroxides, phenolic resins, other crosslinking aids, etc. These crosslinking agents may be used alone or in combination of two or more.

[0128] As the organic peroxide that can be used as the crosslinking agent, any of aromatic organic peroxides and aliphatic organic peroxides can be used. Specific examples include: dialkyl peroxides such as di-tert-butyl peroxide, tert-butyl isopropyl peroxide, diisopropyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne, 1,3-bis(tert-butylperoxyisopropyl)benzene, and 1,1-di(tert-butylperoxy)-3,3,5-trimethylcyclohexane; peroxyesters such as tert-butyl peroxybenzoate, tert-butyl peroxyisopropyl carbonate, 2,5-dimethyl-2,5-di(benzoyl peroxide)hexane, and 2,5-dimethyl-2,5-di(benzoyl peroxide)-3-hexyne; and hydroperoxides such as acetyl peroxide, lauroyl peroxide, benzoyl peroxide, p-chlorobenzoyl peroxide, and 2,4-dichlorobenzoyl peroxide. Among these, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane is preferred. These organic peroxides may be used alone or in combination of two or more.

[0129] Examples of the phenolic resin that can be used as a crosslinking agent include alkylphenol formaldehyde, brominated alkylphenol formaldehyde, etc. These phenolic resins may be used alone or in combination of two or more.

[0130] Examples of crosslinking aids other than organic peroxides and phenolic resins include: peroxide aids such as sulfur, p-quinone dioxime, p-dinitrosobenzene, and 1,3-diphenylguanidine; crosslinking aids for phenolic resins such as anhydrous stannous chloride, dihydrated stannous chloride, and ferric chloride; polyfunctional vinyl compounds such as divinylbenzene, triallyl cyanurate, triallyl isocyanurate, and diallyl phthalate; and polyfunctional (meth)acrylate compounds such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and allyl (meth)acrylate. These may be used alone or in combination of two or more.

[0131] From the viewpoint of fully carrying out the crosslinking reaction, the amount of component (D) used is preferably 0.5 parts by mass or more, more preferably 1.0 parts by mass or more, and further preferably 1.5 parts by mass or more, relative to a total of 100 parts by mass of component (A). From the viewpoint of controlling the crosslinking reaction, the amount of component (D) used is preferably 10.0 parts by mass or less, more preferably 9.0 parts by mass or less, and further preferably 8.0 parts by mass or less, relative to a total of 100 parts by mass of component (A).

[0132] [Other ingredients]

[0133] In the production of the thermoplastic elastomer composition of the present invention, in addition to the components (A) to (D), other components may be used as raw materials as necessary within a range not impairing the effects of the present invention.

[0134] As other components, for example, various additives such as thermoplastic resins and elastomers other than component (A) and component (C), antioxidants, fillers, heat stabilizers, light stabilizers, ultraviolet absorbers, neutralizers, lubricants, antifogging agents, antiblocking agents, slip agents, dispersants, colorants, flame retardants, antistatic agents, conductivity imparting agents, metal deactivators, molecular weight modifiers, antibacterial agents, mildew inhibitors, fluorescent whitening agents, etc. can be mentioned. These arbitrary substances can be used alone or in combination.

[0135] Examples of thermoplastic resins other than component (A) and component (C) include: polyphenylene ether resins; polyamide resins such as nylon 6 and nylon 66; polyester resins such as polyethylene terephthalate and polybutylene terephthalate; polyoxymethylene resins such as polyoxymethylene homopolymers and polyoxymethylene copolymers; polymethyl methacrylate resins and polyolefin resins (excluding the resin belonging to component (C)).

[0136] Examples of the elastomer other than the component (A) and the component (C) include: styrene-based elastomers (excluding the resin belonging to the component (A)); polyester-based elastomers; and polybutadiene.

[0137] Examples of lubricants (hereinafter sometimes referred to as "component (E)") include silicone oil, silicone masterbatch, and liquid silicone wax. When a lubricant is used, it is usually used in an amount of 0.5 to 50 parts by mass, preferably 1 to 25 parts by mass, relative to 100 parts by mass of the total of component (A).

[0138] As described above, in the present invention, the effect of improving the sliding properties brought about by component (A) can suppress the amount of lubricant used. As described above, by adding a small amount of 20 parts by mass or less relative to a total of 100 parts by mass of component (A), a decrease in weldability can be suppressed and excellent sliding properties can be obtained.

[0139] As antioxidants (hereinafter sometimes referred to as "component (F)"), for example, phenolic antioxidants, phosphite antioxidants, and thioether antioxidants can be mentioned. In the case of antioxidants, the antioxidant is usually used in the range of 0.01 to 3.0 parts by mass, preferably 0.15 to 0.6 parts by mass, relative to 100 parts by mass of the total of component (A). When the content of the antioxidant is within the above range, good thermal stability is obtained.

[0140] Examples of fillers include glass fiber, hollow glass microspheres, carbon fiber, talc, calcium carbonate, mica, potassium titanate fiber, silica, metal soap, titanium dioxide, and carbon black. When a filler is used, 0.3 to 100 parts by mass of the filler is usually used relative to 100 parts by mass of the total of component (A).

[0141] [Method for producing thermoplastic elastomer composition]

[0142] The thermoplastic elastomer composition of the present invention is preferably obtained by subjecting a composition containing the component (A), the component (B), the component (C) and other components in predetermined amounts to dynamic heat treatment in the presence of the component (D) as a crosslinking agent.

[0143] The thermoplastic elastomer composition of the present invention can also be obtained by mixing a crosslinked product of the components (A) and (D) with the components (B), (C) and other components in advance and subjecting the mixture to dynamic heat treatment.

[0144] In the present invention, "dynamic heat treatment" refers to kneading in a molten state or a semi-molten state in the presence of a cross-linking agent. The dynamic heat treatment is preferably carried out by melt kneading. As a mixing and kneading device for melt kneading, for example, a non-open Banbury mixer, a mixing roll, a kneader, and a twin-screw extruder are used. Among these, a twin-screw extruder is preferably used. A preferred mode of the manufacturing method using a twin-screw extruder is to supply each component to a raw material supply port (hopper) of a twin-screw extruder having multiple raw material supply ports and perform dynamic heat treatment.

[0145] The temperature during the dynamic heat treatment is usually 80 to 300° C., preferably 100 to 250° C. The time for the dynamic heat treatment is usually 0.1 to 30 minutes.

[0146] When the thermoplastic elastomer composition of the present invention is produced by subjecting it to a dynamic heat treatment using a twin-screw extruder, it is preferred to extrude while maintaining the relationship of the following formula (I) among the barrel radius (R (mm)), the screw speed (N (rpm)) and the discharge amount (W (kg / hour)) of the twin-screw extruder, and more preferably, to extrude while maintaining the relationship of the following formula (II).

[0147] 2.6 <NW / R 3 <22.6(I)

[0148] 3.0 <NW / R 3 <20.0(II)

[0149] The above relationship among the barrel radius (R (mm)), the screw rotation speed (N (rpm)) and the discharge amount (W (kg / hour)) of the twin-screw extruder is preferably greater than the above lower limit because the thermoplastic elastomer composition can be efficiently produced. On the other hand, the above relationship is preferably less than the above upper limit because heat generation due to shearing can be suppressed and foreign matter causing poor appearance is unlikely to be generated.

[0150] [Physical properties of thermoplastic elastomer composition]

[0151] The thermoplastic elastomer composition of the present invention has a compression set of 60% or less measured under the conditions of 70°C, 22 hours, and 25% compression according to JIS K6262. Since the thermoplastic elastomer composition of the present invention has a compression set of 60% or less at 70°C, sufficient durability against compression can be obtained even when the thermoplastic elastomer composition of the present invention is used in a manner that the compression state is repeatedly placed by opening and closing window frames, door frames, etc., such as automobile sealing materials and building material sealing materials.

[0152] The thermoplastic elastomer composition of the present invention preferably has a compression set of less than 80% measured under the conditions of 100°C, 22 hours, and 25% compression according to JIS K6262. Since the thermoplastic elastomer composition of the present invention has a compression set of less than 80% at a high temperature of 100°C, it is possible to obtain more sufficient durability with respect to the compressed state even when the thermoplastic elastomer composition is used in a compressed state repeatedly by opening and closing such as window frames and door frames such as automobile sealing materials and building sealing materials. The compression set of the thermoplastic elastomer composition of the present invention at 100°C is more preferably less than 75%.

[0153] The thermoplastic elastomer composition of the present invention preferably has a melt flow rate (MFR) of 10 g / 10 min or more, more preferably 15 g / 10 min or more, and even more preferably 20 g / 10 min or more, as measured by a method based on JIS K7210 at a measurement temperature of 230° C. and a measurement load of 21.2 N, from the viewpoint of moldability. From the viewpoint of moldability, the melt flow rate (MFR) of the thermoplastic elastomer composition of the present invention is preferably 80 g / 10 min or less, more preferably 75 g / 10 min or less, and even more preferably 70 g / 10 min or less.

[0154] The thermoplastic elastomer composition of the present invention preferably has a density of 0.95 g / cm2 as measured by method A (water displacement method) in accordance with ISO 1183 from the viewpoint of weight reduction. 3 Below, the density is more preferably 0.93 g / cm 3 Below, more preferably 0.91 g / cm 3The lower limit of the density is usually 0.90 g / cm 3 above.

[0155] From the viewpoint of obtaining appropriate fit with a substrate when used as a bonding member, the lower limit of the tensile stress at break of the thermoplastic elastomer composition of the present invention measured according to the operating procedure of the measurement method based on JIS K6251 is preferably 8.5 MPa or more, and more preferably 9.0 MPa or more. From the viewpoint of preventing the once-fitted bonding member from detaching from the substrate, the upper limit of the tensile stress at break is preferably 15.0 MPa or less, and more preferably 14.5 MPa or less.

[0156] Based on the same viewpoint, the elongation at break measured according to the operating procedure of the measuring method based on JIS K6251 is preferably 650% or more, more preferably 700% or more. From the viewpoint of preventing the once-engaged joining member from detaching from the substrate, the upper limit of the elongation at break is preferably 1200% or less, more preferably 1100% or less.

[0157] 〔Moldings and Application〕

[0158] The thermoplastic elastomer composition of the present invention can be made into a molded body by various molding methods generally used for thermoplastic elastomer compositions, such as injection molding, extrusion molding, hollow molding, and compression molding. Among these, the molding method of the thermoplastic elastomer composition of the present invention is preferably injection molding. After these moldings, a molded body can be made by secondary processing such as lamination molding and thermoforming.

[0159] The molded article formed from the thermoplastic elastomer composition of the present invention can be applied to a wide range of fields, including: automotive parts such as skins, windshields, ceiling materials, interior sheets, bumper protection strips, body protection strips, air spoilers, air duct hoses, and sealing materials; civil engineering and building material parts such as waterproof materials, caulking materials, window frames, and sealing materials; sporting goods such as the grip of golf clubs and the grip of tennis rackets; industrial parts such as hoses and gaskets; home appliance parts such as hoses and gaskets; medical parts such as medical containers, gaskets, and gaskets; food parts such as containers and gaskets; medical machine parts; electric wires; sundries, etc.

[0160] The molded article composed of the thermoplastic elastomer composition of the present invention is suitable for use as a sealing material for automobiles and a sealing material for building materials among those listed above, and is suitable for use as a sealing material for automobiles, particularly as a glass run channel for automobiles.

[0161] 〔Joint components〕

[0162] The joining member of the present invention is composed of the thermoplastic elastomer composition of the present invention. The joining member of the present invention is manufactured by melt-kneading the thermoplastic elastomer composition of the present invention and injection molding the kneaded product to an extrusion-molded member as an adherend. As the adherend, an olefin-based rubber is preferred. As the olefin-based rubber, specifically, olefin-based thermoplastic elastomers and rubber vulcanized with sulfur can be cited. From the viewpoint of obtaining good weldability, the base resin is preferably an olefin-based thermoplastic elastomer that is the same as the thermoplastic elastomer composition of the present invention as a polypropylene-based resin.

[0163] In particular, the joining member of the present invention is suitable as a joining member used in a composite molded body for automobiles, such as a glass run channel for automobiles.

[0164] Figure 1 1 is a perspective view showing an example of an automobile glass run channel as an automobile composite molded body 3. The automobile composite molded body 3 is formed by integrating extrusion molded members 1A and 1B constituting a linear portion separately produced by extrusion molding of a thermoplastic elastomer composition by welding at a corner portion formed by a joining member 2 of the present invention.

[0165] Such a composite molded body 3 can be manufactured, for example, as follows: the joint end sides of the pre-made extruded molded components 1A, 1B are inserted into an injection molding mold, the thermoplastic elastomer composition of the present invention is injection molded in the mold to form the corner joint component 2, and at the same time, it is welded and integrated with the end faces of the extruded molded components 1A, 1B.

[0166] The thermoplastic elastomer composition constituting the extrusion-molded members 1A and 1B is not particularly limited, but olefin-based thermoplastic elastomers and styrene-based thermoplastic elastomers are preferred because they have excellent weldability with the thermoplastic elastomer composition of the present invention and also have excellent mechanical strength and compression set (deterioration resistance) as a glass run channel frame for an automobile.

[0167] Example

[0168] Below, use embodiment to further specifically illustrate the content of the present invention.The present invention is not limited by the following examples as long as it does not exceed its gist.The values ​​of various manufacturing conditions and evaluation results in the following examples have the meaning of the preferred values ​​as the upper or lower limits in the embodiments of the present invention, and the preferred range can also be the range specified by the combination of the value of the above-mentioned upper or lower limit and the value of the following examples or the values ​​of the examples each other.

[0169] [raw materials]

[0170] The raw materials used in the following examples and comparative examples are as follows.

[0171] [Ingredients (A)]

[0172] {Hydrogenated block copolymer (A1)}

[0173] <a1-1>

[0174] Styrene-butadiene-styrene hydrogenated block copolymer (having the structure of the above formula (1). Styrene (block P) content: 32% by mass, weight average molecular weight: 390,000) / "TAIPOL-6159" manufactured by Taiwan Synthetic Rubber (TSRC) Co., Ltd.

[0175] <a1-2>

[0176] Styrene-isoprene-butadiene-styrene hydrogenated block copolymer (having the structure of the above formula (1). Styrene (block P) content: 30% by mass, weight average molecular weight: 452,000 / "SEPTON 4099" manufactured by Kuraray Co., Ltd.

[0177] {Hydrogenated block copolymer (A2)}

[0178] <a2-1>

[0179] Styrene-butadiene-styrene hydrogenated block copolymer (having the structure of the above formula (1). Styrene (block P) content: 32% by mass, weight average molecular weight: 260,000) / "TAIPOL-6151" manufactured by Taiwan Synthetic Rubber (TSRC) Co., Ltd.

[0180] [Ingredient (B)]

[0181] <b-1>

[0182] Paraffin-based rubber softener (kinematic viscosity at 40°C: 95.5 cSt, pour point: -15°C, flash point: 272°C) / "DIANA (registered trademark) PROCESS OIL PW90" manufactured by Idemitsu Kosan Co., Ltd.

[0183] [Ingredient (C)]

[0184] <c-1>

[0185] Propylene-ethylene random copolymer (MFR (JIS K7210): 30 g / 10 min (230°C, 21.2 N), melting peak temperature: 155°C, propylene unit content: 98% by mass) / "NOVATEC (registered trademark) PP MG03BD" manufactured by Japan Polypropylene Co., Ltd.

[0186] [Ingredient (D)]

[0187] <d-1>

[0188] A mixture of 40 parts by mass of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and 60 parts by mass of calcium carbonate / "Kayahexa AD40C" manufactured by Akzo Chemicals Corporation

[0189] <d-2>

[0190] A mixture of 55 parts by mass of divinylbenzene and 45 parts by mass of ethylvinylbenzene / "Divinylbenzene" manufactured by Wako Pure Chemical Industries, Ltd.

[0191] [Ingredient (E)]

[0192] <e-1>

[0193] Silicone oil / "KF96-100CS" manufactured by Shin-Etsu Chemical Co., Ltd.

[0194] [Ingredients (F)]

[0195] <f-1>

[0196] Phenolic antioxidant / "Irganox (registered trademark) 1010" manufactured by BASF Japan Ltd.

[0197] [Evaluation method]

[0198] The evaluation methods of the thermoplastic elastomer compositions in the following Examples and Comparative Examples are as follows.

[0199] In the following measurements (1) to (6), a sheet (120 mm in width, 80 mm in length, 2 mm in wall thickness) was used, which was obtained by injection molding each thermoplastic elastomer composition using a coaxial reciprocating screw injection molding machine ("IS130" manufactured by Toshiba Machine Co., Ltd.) under the conditions of an injection pressure of 50 MPa, a barrel temperature of 220°C, and a mold temperature of 40°C.

[0200] (1) Hardness DURO A: According to JIS K6253 (JIS-A), the value 15 seconds after a needle is pressed into a test piece is measured.

[0201] The hardness DURO A is preferably in the range of 35-95, particularly preferably 40-98.

[0202] (2) Tensile stress at break: As a strength index of the thermoplastic elastomer composition, the tensile stress at break was measured according to the tensile stress at break measurement method according to JIS K6251. The larger the value of the tensile stress at break, the more excellent the tensile properties required of the thermoplastic elastomer composition are evaluated to be.

[0203] (3) Elongation at break: As a strength index of the thermoplastic elastomer composition, the elongation at break was measured according to the elongation at break measurement method according to JIS K6251. The larger the elongation at break value, the more excellent the tensile properties required of the thermoplastic elastomer composition are evaluated to be.

[0204] (4) Compression set: measured under the conditions of 70°C, 22 hours, and 25% compression in accordance with JIS K6262.

[0205] The compression set measured under the conditions of 70°C, 22 hours, and 25% compression is preferably 60% or less.

[0206] (5) Compression set at high temperature: measured under the conditions of 100°C, 22 hours and 25% compression in accordance with JIS K6262.

[0207] Evaluation was performed based on the measured value of compression set (deterioration) (CS) according to the following criteria:

[0208] A: CS is less than 75%;

[0209] B: CS is 75% or more and less than 80%;

[0210] C: CS is 80% or more.

[0211] (6) Static friction coefficient and dynamic friction coefficient

[0212] The sheet obtained by injection molding (120 mm in width, 80 mm in length, 2 mm in thickness) was cut into a size of 60 cm × 45 cm, and a 200 g weight bonded to a glass plate (110 mm in length × 110 mm in width × 3 mm in thickness) was moved 6 cm on the test piece to measure the static friction coefficient and the dynamic friction coefficient. The measurement was repeated 3 times and the average value was calculated.

[0213] The static friction coefficient was evaluated according to the following criteria.

[0214] A: Static friction coefficient is less than 1.55

[0215] B: Static friction coefficient is 1.55 or more and less than 1.65

[0216] C: Static friction coefficient is 1.65 or more

[0217] (7) Weld strength and elongation with TPV (dynamically cross-linked thermoplastic elastomer)

[0218] An injection sheet of olefin-based dynamically crosslinked thermoplastic elastomer ("TREXPRENE (registered trademark) 3855N" manufactured by Mitsubishi Chemical Corporation) with a thickness of 2 mm was cut into a size of 10 cm × 5 cm and loaded into the mold of a 110-ton injection molding machine. Each thermoplastic elastomer composition was injected into the above mold at a barrel temperature of 210°C and a mold temperature of 40°C, and a composite molded body was obtained by insert molding. The composite molded body was punched with a JIS No. 3 dumbbell cutter and stretched at a tensile speed of 200 mm / min to measure the weld strength and weld elongation.

[0219] The weld strength was evaluated according to the following criteria:

[0220] A: Welding strength is 3.5MPa or more

[0221] B: Welding strength is 3.0 MPa or more and less than 3.5 MPa

[0222] C: Welding strength is less than 3.0MPa

[0223] This evaluation is an evaluation of the weldability of the injection sheet, but based on the evaluation results, it is also possible to evaluate the weldability of the injection sheet. Figure 1 Is the weldability of the composite molded body good?

[0224] [Example / Comparative Example]

[0225] <Example 1>

[0226] 100 parts by mass of (A1-1), 133 parts by mass of (B-1), 100 parts by mass of (C-1), 2.5 parts by mass of (D-1) (a mixture of 40 parts by mass of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and 60 parts by mass of calcium carbonate), 2.5 parts by mass of (D-2) (a mixture of 55 parts by mass of divinylbenzene and 45 parts by mass of ethylvinylbenzene), 10 parts by mass of (E-1), and 0.3 parts by mass of (F-1) were mixed in a Henschel mixer for 1 minute to obtain a mixture. The mixture was fed into the supply section of a co-rotating twin-screw extruder ("TEX30α" manufactured by The Nippon Steel Works, Ltd., L / D=46, number of barrels: 13) at a total speed of 15 kg / h, melt-kneaded at a temperature within a range of 110 to 220°C, and pelletized to produce a thermoplastic elastomer composition.

[0227] The obtained thermoplastic elastomer composition was measured for melt flow rate (MFR) at a measurement temperature of 230° C. and a measurement load of 21.2 N according to a method based on JIS K7210. In addition, the obtained thermoplastic elastomer composition was measured for density according to method A (substitution in water method) of ISO 1183. In addition, the obtained thermoplastic elastomer composition was evaluated according to the above (1) to (7). The evaluation results are shown in Table 1.

[0228] <Examples 2 to 10 and Comparative Examples 1 to 3>

[0229] The same procedure as in Example 1 was carried out except that the blending composition shown in Table 1 was changed to obtain pellets of a thermoplastic elastomer composition. The obtained thermoplastic elastomer composition was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0230] In Table 1, regarding component (D-1), only the amount of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane added in component (D-1) (40% of the actual amount added) is shown, rather than the actual amount added. Regarding component (D-2), only the amount of divinylbenzene added in component (D-2) (55% of the actual amount added) is shown, rather than the actual amount added.

[0231] ※1 to ※3 in Table 1 represent the following:

[0232] ※1: "-" in each ingredient means that the ingredient is not used;

[0233] ※2: The amount of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane in component (D-1) only.

[0234] *3: The amount of divinylbenzene contained in the component (D-2) alone.

[0235] [Table 1]

[0236]

[0237] <Evaluation Results>

[0238] As shown in Table 1, Examples 1 to 10 are excellent in the evaluation of "sliding property (static friction coefficient)", "welding property with extruded material" and "compression set at high temperature (100°C)". In addition, Examples 1 to 10 are advantageous for weight reduction due to their low density, and also satisfy the flowability of 10 to 80 g / 10 minutes (230°C, 21N) suitable for injection molding in terms of moldability.

[0239] Comparative Examples 1 to 3 are examples in which (A1-1) used in Example 1 is replaced with the full amount of (A2-1). Among them, Comparative Examples 1 and 2 are examples in which the component (D) is reduced. However, the evaluations of "sliding properties (static friction coefficient)", "welding properties with extruded materials", and "compression set (deterioration) at high temperatures" are poor.

[0240] Industrial Applicability

[0241] The thermoplastic elastomer composition of the present invention can be used in a wide range of fields, including: automotive parts such as skins, windshield strips, ceiling materials, interior sheets, bumper protection strips, body protection strips, air spoilers, air duct hoses, and sealing materials; civil engineering and building materials such as waterproof materials, caulking materials, window frames, and sealing materials; sporting goods such as golf club grips and tennis racket grips; industrial parts such as hoses and gaskets; home appliance parts such as hoses and gaskets; medical parts such as medical containers, gaskets, and gaskets; food parts such as containers and gaskets; medical machine parts; electric wires; sundries, etc. Among the above-listed fields, the thermoplastic elastomer composition of the present invention is suitable for use as automotive sealing materials and building material sealing materials, and is suitable for use as automotive sealing materials, especially automotive glass run channels.

[0242] Although the present invention has been described in detail using specific embodiments, it will be apparent to one skilled in the art that various modifications can be made without departing from the spirit and scope of the invention.

[0243] This application is based on Japanese Patent Application No. 2019-015860 filed on January 31, 2019 and Japanese Patent Application No. 2019-153972 filed on August 26, 2019, which are incorporated herein in their entirety by reference.

Claims

1. A joining member, comprising a thermoplastic elastomer composition, the thermoplastic elastomer composition comprising the following (A), (B) and (C), wherein the composition comprises 100 to 140 parts by mass of the component (B) and 60 to 140 parts by mass of the component (C) per 100 parts by mass of the component (A); The crosslinking is performed by 1.4 parts by mass or more and 10.0 parts by mass or less of the following component (D) relative to 100 parts by mass of the component (A), The compression set measured under the conditions of 70°C, 22 hours, and 25% compression according to JIS K6262 is 60% or less, and the tensile stress at break measured according to the measurement method of JIS K6251 is 8.5 MPa or more and 15.0 MPa or less. Component (A): a hydrogenated product of a block copolymer having at least two polymer blocks mainly composed of a vinyl aromatic compound and at least one polymer block containing butadiene, wherein the proportion of the hydrogenated product of the block copolymer (A1) having a weight average molecular weight of 300,000 or more and 600,000 or less in the hydrogenated product of the block copolymer is 30 to 100% by mass; Component (B): a hydrocarbon rubber softener; Component (C): polypropylene resin; Component (D): a cross-linking agent.

2. The joining member according to claim 1, wherein The component (C) contains a propylene-based random copolymer having a melting peak temperature of 100°C or higher and lower than 157°C.

3. The joining member according to claim 1 or 2, wherein: The thermoplastic elastomer composition contains 1.7 parts by mass or more and 10.0 parts by mass or less of the component (D) based on 100 parts by mass of the component (A). 4 . A composite molded body for automobiles, comprising the joining member according to claim 1 .

5. A method for producing a joint member, the method comprising melt-kneading a thermoplastic elastomer composition and injection molding the kneaded product, wherein: The thermoplastic elastomer composition comprises the following (A), (B), (C) and (D), wherein the composition comprises 100 to 140 parts by mass of the component (B), 60 to 140 parts by mass of the component (C) and 1.4 to 10.0 parts by mass of the component (D) based on 100 parts by mass of the component (A). The tensile stress at break measured by the measuring method according to JIS K6251 is 8.5 MPa or more and 15.0 MPa or less, Component (A): a hydrogenated product of a block copolymer having at least two polymer blocks mainly composed of a vinyl aromatic compound and at least one polymer block containing butadiene, wherein the proportion of the hydrogenated product of the block copolymer (A1) having a weight average molecular weight of 300,000 or more and 600,000 or less in the hydrogenated product of the block copolymer is 30 to 100% by mass; Component (B): a hydrocarbon rubber softener; Component (C): polypropylene resin; Component (D): a cross-linking agent.

6. A thermoplastic elastomer composition comprising the following (A), (B) and (C), wherein the composition comprises 100 to 140 parts by mass of the component (B) and 60 to 140 parts by mass of the component (C) per 100 parts by mass of the component (A); The crosslinking is performed by 1.4 parts by mass or more and 10.0 parts by mass or less of the following component (D) relative to 100 parts by mass of the component (A), The compression set measured under the conditions of 70°C, 22 hours, and 25% compression according to JIS K6262 is 60% or less, and the tensile stress at break measured according to the measurement method of JIS K6251 is 8.5 MPa or more and 15.0 MPa or less. Component (A): a hydrogenated product of a block copolymer having at least two polymer blocks mainly composed of a vinyl aromatic compound and at least one polymer block containing butadiene, wherein the proportion of the hydrogenated product of the block copolymer (A1) having a weight average molecular weight of 300,000 or more and 600,000 or less in the hydrogenated product of the block copolymer is 30 to 100% by mass; Component (B): a hydrocarbon rubber softener; Component (C): polypropylene resin; Component (D): a cross-linking agent.

7. The thermoplastic elastomer composition according to claim 6, wherein The density of the thermoplastic elastomer composition is 0.90 to 0.95 g / cm 3 .

8. The thermoplastic elastomer composition according to claim 6 or 7, wherein The melt flow rate of the thermoplastic elastomer composition measured at a measurement temperature of 230° C. and a measurement load of 21.2 N in accordance with JIS K7210 is 10 to 80 g / 10 minutes.