Preparation method of strontium bismuth titanate / polyetherimide composite film material with ultralow dielectric loss

By adding strontium bismuth titanate two-dimensional sheet ceramics in polyetherimide materials, the contradiction between dielectric constant and dielectric loss is solved, and the dielectric constant is greatly improved and the dielectric loss is maintained. It is suitable for High-performance dielectric material.

CN118994906AInactive Publication Date: 2024-11-22SHANGHAI SECOND POLYTECHNIC UNIVERSITY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411343457.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

While increasing the dielectric constant, it is difficult to effectively reduce dielectric losses, and the large amount of addition of inorganic fillers will lead to a decrease in the mechanical properties of the material.

Method used

Strontium bismuth titanate is used as a two-dimensional sheet-shaped inorganic ceramic filler and polyetherimide polymer material to combine with polyetherimide polymer material. By adding inorganic filler in small amounts, good mechanical properties are maintained while significantly improving the dielectric constant.

Benefits of technology

While maintaining ultra-low dielectric loss, it significantly improves the dielectric constant, improves energy storage performance, and hinders breakdown current at low filler content. It is suitable for flexible ceramic nanofilms and high-power devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994906A_ABST
    Figure CN118994906A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a strontium bismuth titanate / polyetherimide composite film material with ultralow dielectric loss, and belongs to the field of dielectric materials. The preparation method of the bismuth strontium titanate / polyetherimide composite film material comprises the following steps: mixing a titanium source, a strontium source, a bismuth source, a fluxing agent and a solvent, and sintering to obtain bismuth strontium titanate powder; mixing the bismuth strontium titanate powder and polyetherimide in an organic solvent, then coating into a film shape, and stripping to obtain the bismuth strontium titanate / polyetherimide composite film material. According to the dielectric composite material designed by the invention, polyetherimide is used as a matrix, bismuth strontium titanate two-dimensional sheet-shaped inorganic ceramic is used as a filler, and a method of adding a trace amount of the inorganic filler is adopted, so that the technical effect of greatly increasing the dielectric constant on the premise of maintaining ultralow dielectric loss is achieved while good mechanical properties are maintained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of dielectric materials, and in particular to a method for preparing a bismuth strontium titanate / polyetherimide composite film material with ultra-low dielectric loss. Background Art

[0002] In recent years, dielectric energy storage capacitors have been widely used in many fields such as precision weapon systems, electronic power systems, and energy systems due to their advantages of ultra-high power density, low loss, and high operating voltage. Polymer nanocomposites are energy storage materials that have the characteristics of both polymers and nanofillers. They have better performance than conventional materials and have broad application prospects. However, most composite materials using inorganic fillers focus on high dielectric constants and ignore the dielectric loss problem of the material. Therefore, it is necessary to develop a new composite material to achieve low dielectric loss while achieving a significant increase in dielectric constant.

[0003] Polymers have the characteristics of easy processing, high breakdown strength, low dielectric constant and low energy density. Polyetherimide (PEI) is a heteroaromatic polymer and is currently a promising high-temperature dielectric material, but it has a very low dielectric constant, which will affect the energy storage performance of the composite material. At present, most methods to improve this problem are to add a large amount of inorganic fillers, but this will lead to the agglomeration of fillers and a sharp decline in the mechanical properties of the material. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a strontium bismuth titanate / polyetherimide composite film material with ultra-low dielectric loss to solve the above-mentioned problems in the background technology. The dielectric composite material designed by the present invention uses polyetherimide as a matrix and strontium bismuth titanate two-dimensional sheet inorganic ceramics as fillers. The method of adding a trace amount of inorganic fillers is adopted. While maintaining good mechanical properties, it also achieves the technical effect of greatly improving the dielectric constant under the premise of maintaining ultra-low dielectric loss.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] One of the technical solutions of the present invention is to provide a strontium bismuth titanate / polyetherimide composite film material, wherein the composite film material uses a polyetherimide film as a matrix and uses strontium bismuth titanate with a sheet structure as a filler.

[0007] Preferably, the proportion of strontium bismuth titanate in the composite film material is 0.1-2 vol%.

[0008] The second technical solution of the present invention is to provide a method for preparing the above-mentioned strontium bismuth titanate / polyetherimide composite film material, comprising the following steps:

[0009] A titanium source, a strontium source, a bismuth source, a flux and a solvent are mixed and sintered to obtain strontium bismuth titanate powder;

[0010] The strontium bismuth titanate powder and polyetherimide are mixed in an organic solvent, then coated into a film, and peeled off to obtain the strontium bismuth titanate / polyetherimide composite film material.

[0011] Preferably, the titanium source includes one or more of titanium dioxide, titanium tetrachloride, titanium nitrate and titanium oxysulfate; the strontium source includes one or more of strontium carbonate, strontium acetate, strontium sulfate and strontium nitrate; the bismuth source includes one or more of bismuth acetate, bismuth acetate, bismuth sulfate and bismuth oxide.

[0012] Preferably, the molar ratio of the titanium source, the strontium source and the bismuth source is 4:1:4.

[0013] Preferably, the flux is potassium chloride.

[0014] Preferably, the sintering temperature is 600-1200° C. and the sintering time is 0.5-4 h.

[0015] Preferably, the volume ratio of the sum of the volumes of the strontium bismuth titanate powder and polyetherimide to the organic solvent is 1:5-10; the volume ratio of the strontium bismuth titanate powder and polyetherimide is (0.1-2):(98-99.9).

[0016] Preferably, the solvent is ethanol.

[0017] Preferably, the organic solvent is N-methylpyrrolidone.

[0018] The strontium bismuth titanate powder prepared according to the method of the present invention has a plane size of 0.5-5 μm.

[0019] Preferably, the stripping step further comprises a step of removing the organic solvent, wherein the organic solvent is removed by drying at 40-100° C. for 2-24 hours.

[0020] The third technical solution of the present invention is to provide an application of the above-mentioned strontium bismuth titanate / polyetherimide composite film material in the field of energy storage materials.

[0021] In the present invention, the potassium chloride serves as a reaction medium, which can melt and flow at high temperature to promote the reaction and combination of the titanium source, the bismuth source and the strontium source; the ethanol serves as a ball milling medium, which helps to fully mix the raw materials; and the N-methylpyrrolidone serves as a solvent for PEI, so that PEI can be evenly dispersed.

[0022] The technical principles of the present invention are as follows:

[0023] The invention discloses a method for preparing a strontium bismuth titanate / polyetherimide (SBT / PEI) composite film material. By mixing strontium bismuth titanate (SBT) with a sheet structure with polymer polyetherimide, a substantial increase in the dielectric constant at room temperature can be achieved while substantially maintaining ultra-low dielectric loss.

[0024] Strontium bismuth titanate (SrBi4Ti4O 15 , referred to as SBT) is an inorganic ceramic with a perovskite-like structure that can be grown into a two-dimensional sheet structure with a large aspect ratio. After the strontium bismuth titanate powder of the present invention is added to the raw material system, its high specific surface area can accumulate more charges on both sides of the filler sheet and enhance the interface polarization. At the same time, the two-dimensional sheet structure of the strontium bismuth titanate powder can effectively prevent charge migration and cut off the breakdown current path.

[0025] The present invention first mixes the raw materials by ball milling, then synthesizes SBT by molten salt method, and then removes Cl by washing. - Impurities such as PEI and PEI are removed to obtain the final two-dimensional sheet SBT material, and then the composite material is synthesized by scraping technology to obtain the final target product. The two-dimensional sheet SBT obtained by the method of the present invention has good crystallinity, has a large aspect ratio, forms a dense sheet material of micrometer level, and has a good surface morphology. The composite material can maintain good mechanical properties, and SBT can be evenly dispersed inside, while providing a higher dielectric constant for the composite material, it can hinder the formation of a breakdown circuit, thereby maintaining the excellent low-loss performance of PEI at a lower SBT content. Make it an ideal candidate material for flexible electronic products such as flexible ceramic nanofilms, high-power devices, and dielectric capacitors. The preparation method of the present invention is simple and easy to operate.

[0026] The beneficial technical effects of the present invention are as follows:

[0027] The dielectric composite material designed by the present invention uses polyetherimide as a matrix and strontium bismuth titanate two-dimensional flaky inorganic ceramics as a filler. The method of adding a trace amount of inorganic filler is adopted to maintain good mechanical properties while changing the addition amount, and achieves the technical effect of greatly improving the dielectric constant while maintaining ultra-low dielectric loss.

[0028] The present invention uses a two-dimensional filler and a matrix composite, and can use the high aspect ratio and high specific surface area of ​​the two-dimensional material to achieve higher interface polarization under the condition of trace filler content, thereby improving the dielectric constant and hindering the breakdown current path.

[0029] The composite film material obtained by the present invention can substantially improve the dielectric constant while basically maintaining the ultra-low dielectric loss of pure PEI film, effectively improving the energy storage performance of the composite film. The dielectric loss of the composite film material can be as low as 0.004 at a frequency of 1kHz, and the dielectric constant can reach 6.7.

[0030] The composite film material of the invention has good mechanical properties, high heat resistance and excellent processability, and can be widely used in the development of electronic components and other fields. The preparation method is simple, easy to operate and has no pollution to the environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0032] Figure 1 This is the SEM image of the strontium bismuth titanate powder in Example 1 (diameter).

[0033] Figure 2 This is the SEM image of the strontium bismuth titanate powder in Example 1 (thickness).

[0034] Figure 3 This is the XRD diagram of the strontium bismuth titanate powder in Example 1.

[0035] Figure 4 The dielectric constant diagram of the products of Examples 1-6.

[0036] Figure 5 The dielectric loss diagram of the products of Examples 1-6.

[0037] Figure 6 This is a physical picture of the product of Example 1.

[0038] Figure 7 The stress-strain curves of the products of Examples 1-6 are shown in FIG. DETAILED DESCRIPTION

[0039] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.

[0040] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0041] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.

[0042] The words “include,” “including,” “have,” “contain,” etc. used in the present invention are open-ended terms, meaning including but not limited to.

[0043] The present invention provides a method for preparing a strontium bismuth titanate / polyetherimide composite film material, comprising the following steps:

[0044] A titanium source, a strontium source, a bismuth source, a flux and a solvent are mixed, ground in a ball mill, sintered, and then centrifuged to obtain strontium bismuth titanate powder;

[0045] The strontium bismuth titanate powder and polyetherimide are mixed in an organic solvent, heated to obtain a precursor solution, and then coated into a film, peeled off, cured, and dried to obtain the strontium bismuth titanate / polyetherimide composite film material.

[0046] Furthermore, the rotation speed of the ball mill is 300-800r / min, and the grinding time is 8-48h.

[0047] Furthermore, the rotation speed of the centrifuge is 1000-5000 r / min, and the centrifugation time is 1-5 min.

[0048] Furthermore, the heating temperature is 40-150° C., the stirring speed is 100-800 r / min, and the stirring time is 1-12 h.

[0049] Furthermore, the curing temperature is 50-100° C. and the curing time is 10-60 min.

[0050] Furthermore, the drying temperature is 40-100° C., and the drying time is 2-24 hours.

[0051] Furthermore, the thickness of the strontium bismuth titanate / polyetherimide composite film material is 9-12 μm.

[0052] All raw materials used in the following examples and comparative examples of the present invention are commercially available products. Among them, bismuth oxide, strontium carbonate, titanium dioxide and potassium chloride were purchased from Shanghai Titan Technology Co., Ltd. (Adamas); polyetherimide and anhydrous ethanol were purchased from Shanghai Titan Technology Co., Ltd. (Greagent); N-methylpyrrolidone was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0053] Example 1

[0054] A method for preparing strontium bismuth titanate / polyetherimide composite film material:

[0055] (1) Preparation of strontium bismuth titanate powder: titanium source (titanium dioxide), strontium source (strontium carbonate), bismuth source (bismuth oxide) were weighed in a molar ratio of 4:1:4, and placed in a ball mill together, and potassium chloride (the molar ratio of the sum of the molar amounts of titanium source, strontium source and bismuth source to potassium chloride was 1:1) and 30 mL of anhydrous ethanol were added, and the mixture was ground at a speed of 300 r / min for 24 h. The slurry was then poured into a petri dish for drying, and after drying, it was hand-grinded until there was no agglomeration and placed in a crucible. The mixture was then sintered in a muffle furnace at a sintering temperature of 600°C for 4 h. The sample was taken out, soaked in hot water and stirred, and then poured into a centrifuge tube and centrifuged at a centrifugal speed of 1000 r / min for 5 min. The washing was repeated several times until no white precipitate appeared when the supernatant was dropped into a silver nitrate solution. The wet powder was then dried to obtain a two-dimensional strontium bismuth titanate powder (the powder plane size was about 5 μm).

[0056] (2) Preparation of strontium bismuth titanate / polyetherimide composite film material: Weigh strontium bismuth titanate powder and PEI particles at a volume ratio of 0.001:0.999 to obtain a solid component, and add N-methylpyrrolidone (NMP) solvent equivalent to 6 times the volume of the solid component. Stir for 12 hours at a temperature of 40°C and a speed of 500r / min to obtain a precursor solution of SBT / PEI composite film material. Absorb the precursor solution, use a doctor blade to apply it on a glass heating plate, and cure it at 50°C for 60 minutes. Then put it in an oven and dry it at 100°C for 2 hours, take out the glass plate and put it into deionized water for peeling, and put the peeled film into an oven to dry the moisture to obtain a strontium bismuth titanate / polyetherimide composite film material (thickness is about 10μm).

[0057] Figure 1 This is the SEM image of the strontium bismuth titanate powder in Example 1 (diameter).

[0058] Figure 2 This is the SEM image of the strontium bismuth titanate powder in Example 1 (thickness).

[0059] Figure 3 This is the XRD diagram of the strontium bismuth titanate powder in Example 1.

[0060] Figure 6This is a physical picture of the product of Example 1.

[0061] from Figure 1-2 It can be seen that the present invention successfully synthesized strontium bismuth titanate two-dimensional sheet material, and its sheet morphology can be clearly seen. Figure 3 It can be seen that the characteristic peaks of the prepared strontium bismuth titanate correspond one to one with the strontium bismuth titanate standard card. Figure 6 It can be seen that the prepared composite material can be bent at will and has good flexibility.

[0062] Example 2

[0063] The only difference from Example 1 is that the grinding operation in step (1) is modified to grinding at a rotation speed of 800 r / min for 8 hours, and the sintering operation is modified to sintering at a sintering temperature of 700° C. for 0.5 hours; the curing operation in step (2) is modified to curing at 100° C. for 10 minutes, and the volume ratio of strontium bismuth titanate powder to PEI particles is modified to 0.003:0.997.

[0064] The plane size of the strontium bismuth titanate powder is about 0.5 μm.

[0065] Example 3

[0066] The only difference from Example 1 is that the grinding operation in step (1) is modified to grinding at a rotation speed of 500 r / min for 12 h, and the sintering operation is modified to sintering at a sintering temperature of 800° C. for 2 h; the drying operation before stripping in step (2) is modified to curing at 40° C. for 24 h, and the volume ratio of strontium bismuth titanate powder to PEI particles is modified to 0.005:0.995.

[0067] The plane size of the strontium bismuth titanate powder is about 1 μm.

[0068] Example 4

[0069] The only difference from Example 1 is that the sintering operation in step (1) is modified to sintering at a sintering temperature of 900°C for 3 hours, and the centrifugation operation is modified to centrifugation at a centrifugal speed of 5000 r / min for 1 minute; the drying operation before stripping in step (2) is modified to curing at 80°C for 12 hours, the volume ratio of strontium bismuth titanate powder to PEI particles is modified to 0.01:0.99, and the volume ratio of the solid component to the organic solvent is modified to 1:10.

[0070] The plane size of the strontium bismuth titanate powder is about 2 μm.

[0071] Example 5

[0072] The only difference from Example 1 is that the volume ratio of strontium bismuth titanate powder to PEI particles in step (2) is changed to 0.015:0.985, the volume ratio of the solid component to the organic solvent is changed to 1:8.5, and the stirring operation is changed to stirring at a temperature of 150°C and a rotation speed of 800 r / min for 1 h.

[0073] The plane size of the strontium bismuth titanate powder is about 1.5 μm.

[0074] Example 6

[0075] The only difference from Example 1 is that the volume ratio of strontium bismuth titanate powder to PEI particles in step (2) is changed to 0.02:0.98, the volume ratio of the solid component to the organic solvent is changed to 1:5, and the stirring operation is changed to stirring at a temperature of 60°C and a rotation speed of 600 r / min for 3 h.

[0076] The plane size of the strontium bismuth titanate powder is about 3 μm.

[0077] Comparative Example 1

[0078] The only difference from Example 1 is that the addition of strontium bismuth titanate powder is omitted, and a pure polyetherimide film is finally obtained.

[0079] Comparative Example 2

[0080] Take a Ni-MOF two-dimensional sheet material with a plane size of about 0.5 μm and a thickness of about 3 nm, weighing 0.03 g, add it to 10 mL of N-methylpyrrolidone, then add 2.97 g of polyetherimide, mix thoroughly into a slurry, cast the slurry into a film, and dry it at 120°C for 12 hours to obtain a dry composite film.

[0081] Comparative Example 3

[0082] Take a Ni-MOF two-dimensional sheet material with a plane size of about 1.5 μm and a thickness of about 10 nm, weighing 0.03 g, add it to 10 mL of N-methylpyrrolidone, then add 2.97 g of polyetherimide, mix thoroughly into a slurry, cast the slurry into a film, and dry it at 120°C for 12 hours to obtain a dry composite film.

[0083] Effect verification

[0084] The dielectric constant data (room temperature) of the above-mentioned thin film materials were measured, and the test results are shown in Table 1.

[0085] Table 1

[0086]

[0087] It can be seen from Table 1 that at room temperature, the dielectric constant of the composite material after adding strontium bismuth titanate powder is significantly higher than that of the pure polyetherimide film, and compared with the composite material filled with Ni-MOF material, the composite material with strontium bismuth titanate is significantly higher, which effectively improves its dielectric constant, thereby further improving the energy storage performance of the material.

[0088] Figure 4 The dielectric constant diagram of the products of Examples 1-6.

[0089] Figure 5 The dielectric loss diagram of the products of Examples 1-6.

[0090] Figure 7 The stress-strain curves of the products of Examples 1-6 are shown in FIG.

[0091] Figure 4 By changing the content of strontium bismuth titanate filler (reference examples 1-6), it can be seen that as the filler content increases, the dielectric constant of the composite material can be greatly improved; it can be seen that the present invention can achieve a doubling effect for pure PEI material by adding trace fillers.

[0092] from Figure 5 It can be seen that the addition of a trace amount of strontium bismuth titanate filler does not have much effect on the dielectric loss of the composite material. At 1 kHz, the dielectric loss can basically be maintained below 0.01, and can even reach an ultra-low dielectric loss of 0.004.

[0093] Figure 7 It can be seen that adding a trace amount of strontium bismuth titanate filler does not change the tensile properties of the entire film much, indicating that the composite material can maintain good mechanical properties (maximum stress ≈ 56.68 MPa) while improving dielectric properties.

[0094] The composite material of the invention has a simple preparation process and is suitable for industrial production. The strontium bismuth titanate / polyetherimide (SBT / PEI) composite film material of the invention can be used alone or in combination with other substances as a low dielectric loss material.

[0095] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A strontium bismuth titanate / polyetherimide composite film material, characterized in that: The composite film material uses a polyetherimide film as a matrix and uses strontium bismuth titanate with a sheet structure as a filler.

2. The strontium bismuth titanate / polyetherimide composite film material according to claim 1, characterized in that: The proportion of strontium bismuth titanate in the composite film material is 0.1-2 vol%.

3. A method for preparing the strontium bismuth titanate / polyetherimide composite film material according to claim 1 or 2, characterized in that: The following steps are involved: A titanium source, a strontium source, a bismuth source, a flux and a solvent are mixed and sintered to obtain strontium bismuth titanate powder; The strontium bismuth titanate powder and polyetherimide are mixed in an organic solvent, then coated into a film, and peeled off to obtain the strontium bismuth titanate / polyetherimide composite film material.

4. The preparation method according to claim 3, characterized in that: The titanium source includes one or more of titanium dioxide, titanium tetrachloride, titanium nitrate and titanyl sulfate; the strontium source includes one or more of strontium carbonate, strontium acetate, strontium sulfate and strontium nitrate; the bismuth source includes one or more of bismuth acetate, bismuth acetate, bismuth sulfate and bismuth oxide.

5. The preparation method according to claim 4, characterized in that: The molar ratio of the titanium source, the strontium source and the bismuth source is 4:1:

4.

6. The preparation method according to claim 3, characterized in that: The flux is potassium chloride.

7. The preparation method according to claim 3, characterized in that: The sintering temperature is 600-1200° C. and the sintering time is 0.5-4 hours.

8. The preparation method according to claim 3, characterized in that: The volume ratio of the sum of the volumes of the strontium bismuth titanate powder and the polyetherimide to the organic solvent is 1:5-10; the volume ratio of the strontium bismuth titanate powder and the polyetherimide is (0.1-2):(98-99.9).

9. Use of the bismuth strontium titanate / polyetherimide composite film material according to claim 1 or 2 in the field of energy storage materials.

Citation Information

Patent Citations

  • Solid-phase firing method for synthesizing ceramic powder material

    CN101200378A

  • Method for preparing micro-wave dielectric adjustable strontium bismuth titanate film

    CN101205139A

  • High-energy-density strontium bismuth titanate based composite ceramic and preparation method thereof

    CN104710171A

  • Preparation method of strontium bismuth titanate dielectric ceramic powder by 3DP molding technology

    CN109095918A

  • Barium titanate / polyetherimide dielectric composite material and preparation method thereof

    CN112280297A