Quasi-solid electrolyte diaphragm as well as preparation method and application thereof

By using electrospinning process in the lithium-ion battery separator, combined with high-temperature resistant polymer and lanthanum zirconate lithium electrolyte, the heat shrinkage and safety problems of traditional separators are solved, and the safety of lithium-ion batteries is significantly improved. and performance, achieving efficient electrolyte management.

CN119009077APending Publication Date: 2024-11-22DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES

Patent Information

Application Number
CN202411456784.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional lithium battery separators have large heat shrinkage, frequent safety accidents, poor lyophilicity of ceramic separators, low ionic conductivity, poor adhesion to the electrode sheet, easy to fall off, ceramic particles are prone to block holes, and low degree of production autonomy. High production costs affect the safety, usability and processability of lithium-ion batteries.

Method used

High-safe quasi-solid electrolyte separator composed of a base film and a composite functional layer grown in situ integrated electrospinning on the base film, including high-temperature resistant polymers, lanthanum zirconate lithium electrolyte and modified nanocellulose, through static electricity Prepared by spinning process, high porosity and high ion permeability are formed, and the safety and performance of the battery are improved.

Benefits of technology

It significantly improves the safety and performance of lithium-ion batteries, extends service life, reduces the amount of electrolyte, improves the ion conductivity and mechanical properties of the separator, avoids electrolyte leakage, and achieves the stability of lithium batteries at high temperatures. run.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention belongs to the field of quasi-solid-state batteries, and discloses a quasi-solid-state electrolyte diaphragm as well as a preparation method and application thereof, and the diaphragm comprises a base membrane and a composite functional layer which is integrally grown on the base membrane in an electrospinning in-situ manner. The functional layer is formed by crosslinking a high-temperature-resistant polymer, a lanthanum lithium zirconate electrolyte and modified nano cellulose on the base membrane through an electrostatic spinning process. The lithium lanthanum zirconate powder is adopted, so that ultrahigh lithium ion conductivity is realized; the high-temperature-resistant polymer has a strong-polarity functional group, can effectively improve the dynamic repair skill of the SEI membrane, improve the lithium ion transport kinetics, improve the rate discharge performance of the battery and the cycle performance under high rate, has ultrahigh thermal stability, and can tolerate the high temperature of 240 DEG C or above; the modified nanocellulose effectively enhances the mechanical properties and electrolyte absorption / retention rate of the material. The three materials are cross-linked to form a membrane on a base membrane by using an electrostatic spinning technology, so that high porosity and high ion permeability are formed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of quasi-solid-state batteries, and in particular relates to a quasi-solid-state electrolyte membrane and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries are widely used as power sources for various mobile devices due to their high energy density, high operating voltage, no memory effect and long cycle life. From 2017 to 2022, global lithium battery shipments increased from 160 GWh to 1080 GWh, and China's share increased from 33% to 83%. It is estimated that global lithium battery shipments will reach 2347 GWh in 2025, of which China will account for about 89%. Correspondingly, global lithium battery separator shipments have increased year by year. It is estimated that by 2025, global separator usage will reach 36.5 billion square meters, with a huge market demand. However, traditional separators have large thermal shrinkage, resulting in battery short circuits and frequent lithium battery safety accidents. Ceramic separators have problems such as poor lyophilicity, low ionic conductivity, poor adhesion to pole pieces, easy detachment of ceramic layers, easy pore blocking of ceramic particles, low degree of production autonomy, and high production costs. Therefore, how to improve the safety, usability and processability of lithium-ion batteries by improving the performance of the diaphragm, improve battery performance, extend service life and enhance market competitiveness is a problem that needs to be solved urgently. Summary of the invention

[0003] In view of the shortcomings of the prior art, one of the purposes of the present invention is to provide a highly safe quasi-solid electrolyte membrane. It is composed of a base membrane and a composite functional layer grown in situ by electrospinning on the base membrane. The composite functional layer is prepared by an electrostatic spinning process. The base membrane includes a PP film, a PE film or a PP and PE multilayer composite base membrane with a thickness of 5-12µm.

[0004] The composite functional layer comprises a high temperature resistant polymer, a lanthanum lithium zirconate electrolyte and modified nanocellulose.

[0005] Preferably, the high temperature resistant polymer includes one or more of aramid, polyimide, polyaryletherketone and polyacrylonitrile.

[0006] Preferably, the lanthanum zirconate lithium electrolyte comprises lanthanum zirconate lithium Li7La3Zr2O 12 , zirconium-doped lanthanum lithium zirconate Li (7-x) Ln3Z (2-x) M x O (12) , where M represents tantalum, tantalum-aluminum, titanium or iron, respectively, tantalum-doped lithium lanthanum zirconate (Li (7-x) Ln3Z (2-x) Ta x O (12) ), titanium-doped lithium lanthanum zirconate (Li (7-x)Ln3Z (2-x) Ti x O (12) ), iron-doped lithium lanthanum zirconate (Li (7-x) Ln3Z (2-x) Fe x O (12) ), where x is between 0.05-0.6 (preferably 0.2-0.5).

[0007] Preferably, the grain size of the lanthanum zirconate lithium electrolyte is between 100-600 nm.

[0008] Preferably, the modified nanocellulose includes one or more of hydroxylated nanocellulose, carboxylated nanocellulose, cationically modified nanocellulose, anionically modified nanocellulose, acetate nanocellulose, and cyanylated nanocellulose, and the above samples are all from Xi'an North Huitian Chemical Industry Co., Ltd.

[0009] Preferably, the modified nanocellulose is 1-20 µm in length (preferably 5-15 µm) and 2-20 nm in diameter (preferably 5-15 nm).

[0010] In this application, lanthanum zirconate lithium powder can achieve ultra-high lithium ion conductivity; high temperature resistant polymers have strong polar functional groups, which can effectively improve the dynamic repair skills of SEI membrane, improve lithium ion transfer kinetics, improve battery rate discharge performance and high rate cycle performance, and have ultra-high thermal stability, which can withstand high temperatures above 240°C; modified nanocellulose effectively enhances the mechanical properties and electrolyte absorption / retention rate of the material. The above three materials are cross-linked on the base membrane using electrospinning technology to form a high porosity and high ion permeability. After the composite functional layer is activated by the electrolyte, it forms a gel state, which can significantly reduce the amount of electrolyte used, solve the problem of electrolyte leakage under extreme conditions of lithium batteries, and significantly improve battery safety.

[0011] The second object of the present invention is to provide a method for preparing a highly safe quasi-solid electrolyte membrane, the preparation method comprising the following steps: 1) Adding a high temperature resistant polymer into a polar solvent and stirring to dissolve; adding modified nanocellulose and lithium lanthanum zirconate into the polar solvent and dispersing them by ball milling; mixing the two liquids evenly to obtain an electrospinning solution; 2) Adding the electrospinning liquid into the syringe for electrospinning, with the receiving end being the base membrane; collecting a composite membrane with a spinning fiber layer attached to one side of the base membrane, and finally obtaining a diaphragm after a post-heat pressing treatment.

[0012] Preferably, the polar solvent in the above step 1) is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide and tetrahydrofuran.

[0013] Preferably, the concentration of the polymer in the polar solvent is 8-20wt%, wherein the amount of lanthanum zirconate lithium electrolyte added is 5-30wt% (preferably 10-22wt%) of the polymer, and the amount of modified nanocellulose added is 3-15wt% (preferably 5-13wt%) of the polymer.

[0014] Preferably, in the above step 2), the electrospinning voltage is set to 15-30 kV, the extrusion speed is 1.5-3 mL / h, and the receiving distance is 8-25 cm. The post-treatment method is: hot pressing the composite membrane at 80-120 ° C and 5-15 MPa for 3-15 min. The diameter of the spun fiber is 200-600 nm; the thickness of the composite functional layer is 1-10 µm.

[0015] In this application, the electrospinning process adopts a high-throughput jet remote field control integrated array type electrospinning nozzle module and core components to realize batch manufacturing equipment of high uniformity diaphragms, and has a macro sensor detection system, 100% avoiding leakage and wrinkles, and realizing defect-free production of diaphragms. In addition, the present invention uses a base film as a support layer, a spinning layer as a composite layer, and a base film to provide mechanical strength for the solid electrolyte, so it can be continuously and quickly produced under the traction of the base film, and can be rolled up to form a coil, which is convenient for large-scale continuous production.

[0016] The third purpose of this application is to provide an application of a highly safe quasi-solid electrolyte membrane for use in lithium-ion batteries.

[0017] Compared with the prior art, the highly safe quasi-solid electrolyte membrane provided by the present invention has the following advantages: (1) In this application, garnet-type lanthanum lithium zirconate is used as a solid electrolyte to achieve ultra-high lithium ion conductivity; the high temperature resistant polymer has a strong polar functional group, which can effectively improve the dynamic repair function of the SEI film, improve the lithium ion transfer kinetics, improve the battery rate discharge performance and high rate cycle performance, and has ultra-high thermal stability and can withstand high temperatures above 240°C; the modified nanocellulose effectively enhances the mechanical properties of the material and the electrolyte absorption / retention rate.

[0018] (2) In the present application, the composite functional layer is grown in situ on the base membrane by electrospinning, and the functional layer-base membrane cross-section has good compatibility and strong adhesion; the nano-scale filamentous material is cross-linked to form a composite film, forming a high porosity and high ion permeability; after the composite functional layer is activated by the electrolyte, it forms a gel state, which can reduce the amount of electrolyte used, solve the problem of electrolyte leakage under extreme conditions of lithium batteries, and significantly improve battery safety.

[0019] (3) This application uses a high-throughput jet remote-field control integrated array electrospinning nozzle module and core components to achieve batch manufacturing equipment for high-uniformity diaphragms, and has a macro sensor detection system to 100% avoid leakage and wrinkles, and achieve defect-free production of diaphragms. In addition, the present invention uses a base film as a support layer and a spinning layer as a composite layer. The base film provides mechanical strength for the solid electrolyte, so continuous and rapid production can be carried out under the traction of the base film, and the coil can be rolled up to form a coil, which is convenient for large-scale continuous production.

[0020] (4) The high-safety quasi-solid functional layer diaphragm prepared in this application effectively overcomes the performance shortcomings of traditional ceramic diaphragms, greatly improves the ion conductivity and mechanical properties of the diaphragm, effectively improves the thermal shrinkage performance of the diaphragm, and significantly reduces the amount of electrolyte used, thereby improving battery safety. DETAILED DESCRIPTION

[0021] The present application is described in detail below in conjunction with embodiments, but the present application is not limited to the following embodiments.

[0022] Example 1

[0023] A quasi-solid electrolyte membrane and a preparation method and application thereof, comprising the following steps: 1) Add 10g of polyimide to 50g of polar solvent N,N-dimethylacetamide and stir to dissolve; add 1g of cyanated nanocellulose and 1.5g of lanthanum zirconate Li7La3Zr2O 12 Add 40g of polar solvent N,N-dimethylacetamide and disperse by ball milling; the above two liquids are mixed evenly to obtain electrospinning solution.

[0024] 2) The electrospinning solution was added to the syringe and electrospinning was performed under the conditions of 25 kV voltage, 15 cm receiving distance, and 2 mL / h extrusion speed, with the receiving end being the base membrane. The composite membrane with the spinning fiber layer attached to the surface of one side of the base membrane was collected and hot-pressed at 100 ° C and 10 MPa for 3 min to finally obtain a quasi-solid electrolyte separator.

[0025] The base film is PE film, 8µm thick; The diameter of the spun fibers in the spun fiber layer is 400 nm; the thickness of the composite functional layer is 5 µm.

[0026] The grain size of the lanthanum zirconate lithium electrolyte is 300nm; The cyanotyped nanocellulose is 10µm long and 15nm in diameter.

[0027] Example 2

[0028] A quasi-solid electrolyte membrane and a preparation method and application thereof, comprising the following steps: 1) Add 20g aramid to 45g polar solvent N,N-dimethylformamide and stir to dissolve; add 0.6g anion-modified nanocellulose and 1g tantalum-doped lanthanum zirconate (Li 6.44 Ln3Z 1.44 Ta 0.56 O 12 ) was added into 35 g of polar solvent N,N-dimethylacetamide and dispersed by ball milling; the above two liquids were mixed evenly to obtain electrospinning solution.

[0029] 2) The electrospinning solution was added to the syringe and electrospinning was performed under the conditions of 15 kV voltage, receiving distance 25 cm, and extrusion speed 1.5 mL / h, with the receiving end being the base membrane. The composite membrane with the spinning fiber layer attached to the surface of one side of the base membrane was collected and hot-pressed at 120°C and 5 MPa for 5 min to finally obtain a highly safe quasi-solid electrolyte separator.

[0030] The base film is PE film, 5µm thick; The diameter of the spun fibers in the spun fiber layer is 200 nm; the thickness of the composite functional layer is 10 µm.

[0031] The grain size of the lanthanum zirconate lithium electrolyte is 200nm; The cyanotyped nanocellulose is 20µm long and 20nm in diameter.

[0032] Example 3

[0033] A quasi-solid electrolyte membrane and a preparation method and application thereof, comprising the following steps: 1) Add 8g of polyaryletherketone into 55g of polar solvent dimethyl sulfoxide and stir to dissolve; add 1.2g of carboxylated nanocellulose and 2.4g of titanium-doped lithium lanthanum zirconate (Li 6.95 Ln3Z 1.95 Ti 0.05 O 12 ) was added into 37 g of polar solvent tetrahydrofuran and dispersed by ball milling; the above two liquids were mixed evenly to obtain electrospinning solution.

[0034] 2) The electrospinning solution was added to the syringe and electrospinning was performed under the conditions of 30 kV voltage, 8 cm receiving distance, and 3 mL / h extrusion speed, with the receiving end being the base membrane. The composite membrane with the spinning fiber layer attached to the surface of one side of the base membrane was collected and hot-pressed at 80 ° C and 15 MPa for 15 min to finally obtain a highly safe quasi-solid electrolyte separator.

[0035] The base film is PE film, thickness 12µm; The diameter of the spun fibers in the spun fiber layer is 600 nm; the thickness of the composite functional layer is 1 µm.

[0036] The grain size of the lanthanum zirconate lithium electrolyte is 100 nm; The cyanotyped nanocellulose is 20µm long and 20nm in diameter.

[0037] Example 4

[0038] A quasi-solid electrolyte membrane and a preparation method and application thereof, comprising the following steps: 1) Add 8g polyacrylonitrile to 55g polar solvent dimethyl sulfoxide and stir to dissolve; add 1.2g acetate nanocellulose and 2.4g iron-doped lanthanum zirconate (Li 6.4 Ln3Z 1.4 Fe 0.6 O 12 ) was added into 37 g of polar solvent tetrahydrofuran and dispersed by ball milling; the above two liquids were mixed evenly to obtain electrospinning solution.

[0039] 2) The electrospinning solution was added to the syringe and electrospinning was performed under the conditions of 30 kV voltage, 8 cm receiving distance, and 3 mL / h extrusion speed, with the receiving end being the base membrane. The composite membrane with the spinning fiber layer attached to the surface of one side of the base membrane was collected and hot-pressed at 80 ° C and 15 MPa for 15 min to finally obtain a highly safe quasi-solid electrolyte separator.

[0040] The base film is PP film with a thickness of 7µm; The diameter of the spun fibers in the spun fiber layer is 600 nm; the thickness of the composite functional layer is 1 µm.

[0041] The grain size of the lanthanum zirconate lithium electrolyte is 600nm; The cyanotyped nanocellulose is 1µm long and 2nm in diameter.

[0042] Comparative Example 1 In the above-mentioned embodiment 1, only the PE base film is used.

[0043] Comparative Example 2 A quasi-solid electrolyte membrane and a preparation method and application thereof, comprising the following steps: 1) Add 10g of polyimide into 50g of polar solvent N,N-dimethylacetamide and stir to dissolve; add 1g of cyanated nanocellulose into 40g of polar solvent N,N-dimethylacetamide and disperse by ball milling; mix the two liquids evenly to obtain an electrospinning solution.

[0044] 2) The electrospinning solution was added to the syringe and electrospinning was performed under the conditions of 25 kV voltage, 15 cm receiving distance, and 2 mL / h extrusion speed, with the receiving end being the base membrane. The composite membrane with the spinning fiber layer attached to the surface of one side of the base membrane was collected and hot-pressed at 100 ° C and 10 MPa for 3 min to finally obtain a highly safe quasi-solid electrolyte separator.

[0045] The base film is PE film, 8µm thick; The diameter of the spun fibers in the spun fiber layer is 400 nm; the thickness of the composite functional layer is 5 µm.

[0046] The cyanotyped nanocellulose is 10µm long and 15nm in diameter.

[0047] Comparative Example 3 A quasi-solid electrolyte membrane and a preparation method and application thereof, comprising the following steps: 1) Add 10g of polyimide to 50g of polar solvent N,N-dimethylacetamide and stir to dissolve; add 1.5g of lanthanum zirconate Li7La3Zr2O 12 Add 40g of polar solvent N,N-dimethylacetamide and disperse by ball milling; the above two liquids are mixed evenly to obtain electrospinning solution.

[0048] 2) The electrospinning solution was added to the syringe and electrospinning was performed under the conditions of 25 kV voltage, 15 cm receiving distance, and 2 mL / h extrusion speed, with the receiving end being the base membrane. The composite membrane with the spinning fiber layer attached to the surface of one side of the base membrane was collected and hot-pressed at 100 ° C and 10 MPa for 3 min to finally obtain a highly safe quasi-solid electrolyte separator.

[0049] The base film is PE film, 8µm thick; The diameter of the spun fibers in the spun fiber layer is 400 nm; the thickness of the composite functional layer is 5 µm.

[0050] The grain size of the lanthanum zirconate lithium electrolyte is 300 nm.

[0051] Comparative Example 4 A highly safe quasi-solid electrolyte membrane and a preparation method and application thereof, comprising the following steps: 1) Add 10 g of polyimide into 90 g of polar solvent N,N-dimethylacetamide and stir to dissolve to obtain an electrospinning solution.

[0052] 2) The electrospinning solution was added to the syringe and electrospinning was performed under the conditions of 25 kV voltage, 15 cm receiving distance, and 2 mL / h extrusion speed, with the receiving end being the base membrane. The composite membrane with the spinning fiber layer attached to the surface of one side of the base membrane was collected and hot-pressed at 100 ° C and 10 MPa for 3 min to finally obtain a highly safe quasi-solid electrolyte separator.

[0053] The base film is PE film, 8µm thick; The diameter of the spun fibers in the spun fiber layer is 400 nm; the thickness of the composite functional layer is 5 µm.

[0054] Performance Test 1: The diaphragms obtained in Example 1 and Comparative Examples 1 to 4 were tested for heat shrinkage, peel strength, tensile strength, puncture strength, liquid absorption rate and room temperature conductivity. The specific test method is as follows. The test results are shown in Tables 1 and 2.

[0055] Thermal shrinkage rate: Cut the diaphragm into 100×100mm film samples, measure their longitudinal and transverse lengths, put them into a vacuum oven and bake them for 1h respectively, take out the diaphragm samples, cool them to room temperature, measure their longitudinal and transverse lengths again, calculate the thermal shrinkage rate, and characterize the heat resistance of the diaphragm. Test them at three temperatures of 105℃, 120℃ and 150℃ respectively.

[0056] Peel strength: Peel strength is tested with a universal tensile testing machine, and the standard adopted is "GB / T1040.32-2006 Test for tensile properties of plastics".

[0057] Tensile strength: The tensile strength is tested using a universal tensile testing machine, and the standard adopted is GB / T 1040.3-2006 "Test for tensile properties of plastics".

[0058] Puncture strength: The puncture strength is tested using a universal tensile testing machine, and the standard adopted is GB / T 37841-2019 "Test method for puncture resistance of plastic film and sheeting".

[0059] Liquid absorption rate: The liquid absorption rate uses electrolyte solvent (ethylene carbonate and dimethyl carbonate, with a mass ratio of 1:1) as the test object, and the standard adopted is QB / T 2303.11-2008 "Pulp paper for batteries Part 11: Determination of liquid absorption rate", which characterizes the wettability of aramid coated diaphragm to electrolyte.

[0060] Room temperature conductivity: The room temperature conductivity is tested using a multi-channel ion conductivity test system.

[0061] As can be seen from Table 1, the heat resistance of the diaphragm provided in Example 1 is much higher than that of Comparative Example 1, indicating that the introduction of the composite functional layer significantly increases the thermal stability of the diaphragm. And due to the strong mechanical strength of the base film, the diaphragm provided in Example 1 has high tensile strength and puncture strength. At the same time, in this application, the composite functional layer is electrospun in situ on the base film and grows in an integrated manner, the functional layer-base film cross-section has good compatibility and strong adhesion, and the composite functional layer and the base film have good peel strength.

[0062] Table 1

[0063] Performance Test 2: The diaphragms obtained in Example 1 and Comparative Examples 1 to 4 were subjected to soft pack rate performance tests, including a positive electrode, a negative electrode, a shell and the above-obtained diaphragm, and the lithium battery diaphragm was filled with an electrolyte. The electrolyte solution was 1 mol / L LiPF6 (ethyl carbonate: dimethyl carbonate = 1:1 (V / V)), the positive electrode material was 811 nickel cobalt manganese (NCM) ternary positive electrode, and the negative electrode was a graphite pole piece. The test results are shown in Table 2.

[0064] As can be seen from Table 2, compared with Comparative Examples 1 to 4, the diaphragm provided in Example 1 has extremely high liquid absorption rate, room temperature conductivity, and significantly reduces the amount of electrolyte used. This is because garnet-type lithium lanthanum zirconate is used as a solid electrolyte in this application, which can achieve ultra-high lithium ion conductivity. And the high temperature resistant polymer has a strong polar functional group, which can effectively improve the dynamic repair function of the SEI membrane, improve the lithium ion transfer kinetics, and improve the battery rate discharge performance and high rate cycle performance. Modified nanocellulose effectively enhances the mechanical properties and liquid absorption rate of the material. After the composite functional layer is activated by the electrolyte, a gel state is formed, which can reduce the amount of electrolyte used, solve the problem of electrolyte leakage under extreme conditions of lithium batteries, and significantly improve battery safety.

[0065] Table 2

[0066] The above are only some embodiments of the invention, and are not intended to limit the present invention in any form. All raw material ratios, upper and lower limits of working conditions and interval values ​​in the preparation process of the present invention can realize the present invention, and the embodiments are not listed one by one here. Any person familiar with this profession, without departing from the technical solution of the present invention, can make some changes or modifications to equivalent embodiments of equivalent changes using the above technical content. However, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A quasi-solid electrolyte membrane, characterized in that: The diaphragm consists of a base film and a composite functional layer that is in-situ integratedly grown or modified or attached by electrospinning on the surface of one side of the base film; the base film is a PP and / or PE film; the composite functional layer includes a high-temperature resistant polymer, a lanthanum zirconate lithium electrolyte and modified nanocellulose; the composite functional layer is a spun fiber layer prepared by an electrospinning process.

2. The quasi-solid electrolyte membrane according to claim 1, characterized in that: The base film comprises a PP film, or a PE film, or a multi-layer composite base film composed of PP and PE laminated together, and the thickness of the base film is 5-12 μm.

3. The quasi-solid electrolyte membrane according to claim 1, characterized in that: The high temperature resistant polymer includes one or more of aramid, polyimide, polyaryletherketone and polyacrylonitrile; The lanthanum zirconate lithium electrolyte comprises lanthanum zirconate lithium Li7La3Zr2O 12 , zirconium-doped lanthanum lithium zirconate Li (7-x) Ln3Z (2-x) M x O (12) , where M represents one or more of tantalum, tantalum-aluminum, titanium or iron, respectively, tantalum-doped lanthanum zirconate lithium Li (7-x) Ln3Z (2-x) Ta x O (12) , titanium-doped lanthanum zirconate Li (7-x) Ln3Z (2-x) Ti x O (12) , Iron-doped lanthanum zirconate Li (7-x) Ln3Z (2-x) Fe x O (12) One or more of the following, wherein x is between 0.05 and 0.6; The modified nanocellulose includes one or more of hydroxylated nanocellulose, carboxylated nanocellulose, cation-modified nanocellulose, anion-modified nanocellulose, acetate-modified nanocellulose, and cyanated nanocellulose.

4. The quasi-solid electrolyte membrane according to claim 3, characterized in that: The lanthanum zirconate lithium electrolyte has a grain size of 100-600 nm; The modified nanocellulose is 1-20 μm in length and 2-20 nm in diameter.

5. The quasi-solid electrolyte membrane according to claim 1, characterized in that: In the composite functional layer, the addition amount of lanthanum lithium zirconate is 5-30wt% of the high temperature resistant polymer, and the addition amount of modified nanocellulose is 3-15wt% of the high temperature resistant polymer.

6. A method for preparing the quasi-solid electrolyte membrane according to any one of claims 1 to 5, characterized in that: The steps include: 1) Adding a high temperature resistant polymer into a polar solvent and stirring to dissolve; adding modified nanocellulose and lithium lanthanum zirconate into the polar solvent and dispersing them by ball milling; mixing the two liquids evenly to obtain an electrospinning solution; 2) Adding the electrospinning liquid into the syringe for electrospinning, with the receiving end being the base membrane; collecting a composite membrane with a spinning fiber layer attached to one side of the base membrane, and finally obtaining a diaphragm after a post-heat pressing treatment.

7. The method for preparing the quasi-solid electrolyte membrane according to claim 6, characterized in that: The polar solvent is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and tetrahydrofuran; The concentration of the polymer in the polar solvent is 8-20wt%, wherein the amount of lanthanum zirconate lithium electrolyte added is 5-30wt% of the polymer, and the amount of modified nanocellulose added is 3-15wt% of the polymer.

8. The method for preparing the quasi-solid electrolyte membrane according to claim 6, characterized in that: In step (2), the electrospinning voltage is set to 15-30 kV, the extrusion speed is 1.5-3 mL / h, and the receiving distance is 8-25 cm; The post-treatment method is: hot pressing the composite film at 80~120℃ and 5~15 MPa for 3~15min.

9. The method for preparing the quasi-solid electrolyte membrane according to claim 6, characterized in that: The diameter of the spun fibers in the spun fiber layer is 200-600 nm; the thickness of the composite functional layer is 1-10 µm.

10. Use of the quasi-solid electrolyte membrane according to any one of claims 1 to 5 or the quasi-solid electrolyte membrane obtained by the preparation method according to claim 6, characterized in that: It can be used as a separator in lithium-ion batteries.

Citation Information

Patent Citations

  • Organic / inorganic composite separator having morphology gradient, manufacturing method thereof and electrochemical device containing the same

    CN101326658A

  • Lithium ion battery composite membrane and preparation method thereof

    CN105958000A

  • Preparation method of lithium ion battery diaphragm

    CN106129310A

  • Preparation method of lithium lanthanum zirconium oxide nanometer fiber, preparation method of composite film and solid battery application

    CN107316965A

  • Composite diaphragm for lithium ion batteries, production method thereof, and lithium ion battery

    CN107437603A

Cited By

  • A composite diaphragm based on solid electrolyte coating and preparation method thereof

    CN119742538A

  • Solid electrolyte composite material and preparation method thereof

    CN120461967A

  • Solid-state electrolyte membrane layer, pole piece, preparation method of pole piece and solid-state battery

    CN120854659A

  • Composite diaphragm, preparation method thereof and secondary battery

    CN120933602A

  • Composite solid electrolyte diaphragm, preparation method and all-solid-state battery

    CN121054967A