Solar cell and preparation method thereof, photovoltaic module and photovoltaic system

By designing substrates, tunneling dielectric layers, doping layers, isolation structures and transparent conductive layers in solar cells, the problem of insufficient performance of existing solar cells is solved, and higher light utilization and carrier recombination rate are achieved , simplifies the structure and reduces costs.

CN119050169APending Publication Date: 2024-11-29TRINA SOLAR CO LTD
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202411105828.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing solar cells have not yet reached the best level of performance and need to improve performance while simplifying the structure.

Method used

A solar cell is designed, including a substrate, a tunneling dielectric layer, a doping layer, an isolation structure, a passivation layer and a transparent conductive layer. The first and second gate lines are arranged on the backlight side and come into contact with the transparent conductive layer. The gate line occlusion of the light-receiving surface is reduced, the light utilization rate is improved, and the interface recombination of the substrate surface is reduced through the tunneling dielectric layer and the passivation layer, reducing the concentric circle effect generated by the TOPCon high-temperature preparation process.

Benefits of technology

Achieve higher light absorption and carrier recombination rates, improving the performance and power output of solar cells, while simplifying the structure and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050169A_ABST
    Figure CN119050169A_ABST
Patent Text Reader

Abstract

The invention relates to a solar cell and a preparation method thereof, a photovoltaic module and a photovoltaic system, and the solar cell comprises a substrate which comprises a light receiving surface and a backlight surface which are opposite to each other; the tunneling dielectric layer is positioned in the first region of the backlight surface; the first doping layer is positioned on one side, far away from the substrate, of the tunneling dielectric layer; the isolation structure is positioned on one side, far away from the substrate, of the tunneling dielectric layer; the first passivation layer is located in the second region of the backlight surface, and the isolation structure is located between the first passivation layer and the isolation structure; the second doping layer is located on the side, away from the substrate, of the first passivation layer; the transparent conducting layers are located on the sides, away from the substrate, of the first doping layer and the second doping layer respectively, isolation grooves are formed in the transparent conducting layers, and the isolation structures are exposed out of the groove bottoms of the isolation grooves; and the first grid line and the second grid line are arranged in an insulated manner and are in contact with the transparent conductive layer, so that the performance of the solar cell can be improved while the structure of the solar cell is simplified.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of photovoltaic technology, and in particular to a solar cell and a preparation method thereof, a photovoltaic module and a photovoltaic system. Background Art

[0002] At present, solar cells, a new energy technology, are experiencing an unprecedented development trend. Among them, crystalline silicon solar cells have been dominating the photovoltaic industry with a market share of more than 90%. With such a huge volume and broad market prospects, crystalline silicon solar cells are also developing continuously.

[0003] However, the performance of existing solar cells needs to be further improved. Summary of the invention

[0004] Based on this, it is necessary to provide a solar cell that can simplify the structure of the solar cell and improve the performance in order to solve the above technical problems.

[0005] In a first aspect, the present application provides a solar cell, comprising:

[0006] A substrate, the substrate comprising a light-receiving surface and a backlight surface that are arranged opposite to each other;

[0007] A tunneling dielectric layer, located in the first area of ​​the backlight surface;

[0008] A first doped layer, located on a side of the tunnel dielectric layer away from the substrate;

[0009] An isolation structure, located on a side of the tunnel dielectric layer away from the substrate;

[0010] A first passivation layer is located in the second area of ​​the backlight surface, and the isolation structure is located between the first passivation layer and the isolation structure;

[0011] A second doping layer is located on a side of the first passivation layer away from the substrate;

[0012] A transparent conductive layer, located on the first doped layer and the second doped layer at a side away from the substrate, and an isolation groove is provided on the transparent conductive layer, and the isolation structure is exposed at the bottom of the isolation groove;

[0013] A first gate line, located at a side of the transparent conductive layer in the first region away from the first doping layer;

[0014] The second gate line is located at a side of the transparent conductive layer in the second region away from the second doping layer.

[0015] In one embodiment, a portion of the first passivation layer covers a sidewall of the isolation structure away from the first doping layer.

[0016] In one of the embodiments, a size of a portion of the first passivation layer covering a side wall of the isolation structure in a thickness direction of the solar cell is larger than a size of the isolation structure in the thickness direction.

[0017] In one embodiment, the material of the isolation structure includes intrinsic polysilicon.

[0018] In one embodiment, the materials of the first gate line and the second gate line include low-temperature metal paste respectively.

[0019] In one embodiment, the first doped layer is a phosphorus-doped polysilicon layer; the second doped layer includes boron-doped hydrogenated microcrystals, a boron-doped polysilicon layer, a boron-doped silicon oxide, and a boron-doped silicon oxycarbide.

[0020] In one embodiment, the solar cell further comprises:

[0021] A second passivation layer is located on the light-receiving surface of the substrate;

[0022] The anti-reflection layer is located on a side of the second passivation layer away from the substrate.

[0023] In a first aspect, the present application provides a method for preparing a solar cell, comprising:

[0024] Providing a substrate; wherein the substrate comprises a light-receiving surface and a backlight surface disposed opposite to each other;

[0025] Forming a tunnel dielectric layer, an isolation structure and a first doped layer in a first area of ​​the backlight surface of the substrate; wherein the isolation structure and the first doped layer are respectively formed on a side of the tunnel dielectric layer away from the substrate;

[0026] forming a first passivation layer and a second doping layer in a second region of the backlight surface of the substrate; wherein the second doping layer is located on a side of the first passivation layer away from the substrate, and the isolation structure is located between the first passivation layer and the isolation structure;

[0027] A transparent conductive layer is formed on the first doped layer and the second doped layer at a side away from the substrate; wherein an isolation groove is formed in the transparent conductive layer, and the isolation structure is exposed at the bottom of the isolation groove;

[0028] A first gate line and a second gate line are formed, wherein the first gate line is disposed in contact with the transparent conductive layer located in the first region, and the second gate line is disposed in contact with the transparent conductive layer located in the second region.

[0029] In one embodiment, forming a tunnel dielectric layer, an isolation structure and a first doping layer in a first region of the backlight surface of the substrate includes:

[0030] forming a tunneling material layer on the backlight surface of the substrate;

[0031] forming an intrinsic polysilicon material layer on a side of the tunneling material layer away from the substrate;

[0032] Doping the intrinsic polysilicon material layer located in the first region and annealing the resulting structure to form a first doping layer located in the first region and an isolation layer located in the second region;

[0033] Part of the isolation layer and part of the tunneling material layer are removed to correspondingly form the isolation structure and the tunneling dielectric layer.

[0034] In one embodiment, the removing part of the isolation layer and part of the tunneling material layer to correspondingly form the isolation structure and the tunneling dielectric layer includes:

[0035] forming a blocking sacrificial layer on a side of the first doped layer and the isolation layer away from the tunnel dielectric layer;

[0036] Opening the blocking sacrificial layer, the isolation layer, and the tunneling material layer located in the first region; the openings expose the backlight surface of the substrate;

[0037] The remaining blocking sacrificial layer is removed to form the isolation structure and the tunneling dielectric layer.

[0038] In one embodiment, forming a first passivation layer and a second doping layer in a second region of the backlight surface of the substrate includes:

[0039] forming a passivation material layer on the second area of ​​the backlight surface, the first side surface of the isolation structure, and the isolation structure and the first doped layer on a side away from the substrate;

[0040] forming a doping material layer on a side of the passivation material layer away from the substrate;

[0041] The passivation material layer and the doping material layer located in the second region are removed to form the first passivation layer and the second doping layer.

[0042] In one embodiment, the method further comprises:

[0043] forming a second passivation layer on the light-receiving surface of the substrate;

[0044] An anti-reflection layer is formed on a side of the second passivation layer away from the substrate.

[0045] In a third aspect, the present application provides a photovoltaic module, comprising at least one cell string, wherein the cell string comprises at least two of the aforementioned solar cells, or the cell string comprises at least two solar cells manufactured by the aforementioned solar cell manufacturing method.

[0046] In a fourth aspect, the present application provides a photovoltaic system, comprising the aforementioned photovoltaic component.

[0047] The solar cell, the method for preparing the solar cell, the photovoltaic module and the photovoltaic system include a substrate, a tunnel dielectric layer, a first doped layer, an isolation structure, a first passivation layer and a second doped layer, a transparent conductive layer, a first grid line and a second grid line, wherein the first grid line and the second grid line are arranged on the backlight side of the solar cell, directly contacting the transparent conductive layer, and the light-receiving surface of the cell for receiving light is completely free of grid line shielding, so that the light incident on the cell is fully absorbed, thereby improving the light utilization rate of the cell. The first grid line and the second grid line can directly contact the transparent conductive layer, thereby improving the conductivity of the first grid line and the second grid line and the transparent conductive layer, and can simplify the structure of the solar cell and reduce costs.

[0048] In addition, on the back of the solar cell, the dangling bonds on the substrate surface can be chemically passivated by the tunneling dielectric layer located in the first area of ​​the backlight surface of the substrate and the first passivation layer in the second area, which greatly reduces the interface recombination on the substrate surface. In addition, the isolation structure and the first doping layer are both located on the side of the tunneling dielectric layer away from the substrate, and the isolation structure is located between the first doping layer and the second doping layer, which can achieve electrical isolation between the first doping layer and the second doping layer, thereby preventing leakage. The isolation structure also achieves interface passivation of the first doping layer, which can further reduce the carrier recombination rate at the corresponding position of the backlight surface of the substrate. In addition, only one doping layer is set in the first area and the second area, for example, the first doping layer in the first area and the second doping layer in the second area, which reduces the concentric circle effect produced by the TOPCon high-temperature preparation process, and can further improve the performance of the solar cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the conventional technology, the drawings required for use in the embodiments or the conventional technology descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0050] Figure 1 is a schematic diagram of a cross-sectional structure of a solar cell in one embodiment of the present application;

[0051] Figure 2is a schematic diagram of a cross-sectional structure of a solar cell in another embodiment of the present application;

[0052] Figure 3 is a flow chart of a method for preparing a solar cell in one embodiment of the present application;

[0053] Figure 4 It is a cross-sectional view of a structure obtained after a tunnel dielectric layer, an isolation structure and a first doping layer are formed in a first region of a backlight surface of a substrate in one embodiment of the present application;

[0054] Figure 5 It is a cross-sectional view of a structure obtained after forming a first passivation layer and a second doping layer in a second region of a backlight surface of a substrate in an embodiment of the present application;

[0055] Figure 6 It is a cross-sectional view of a structure obtained after a transparent conductive layer is formed on a side of the first doping layer and the second doping layer away from the substrate in one embodiment of the present application;

[0056] Figure 7 This is a flow chart of forming a tunnel dielectric layer, an isolation structure and a first doping layer in a first area of ​​a backlight surface of a substrate in one embodiment of the present application;

[0057] Figure 8 It is a cross-sectional view of a structure obtained after an intrinsic polysilicon material layer is formed on a side of the tunneling material layer away from the substrate in one embodiment of the present application;

[0058] Fig. 9 It is a cross-sectional view of a structure obtained after doping an intrinsic polysilicon material layer located in a first region and annealing the obtained structure to form a first doping layer located in the first region and an isolation layer located in the second region in one embodiment of the present application;

[0059] Fig.10 This is a flow chart of removing part of the isolation layer and part of the tunneling material layer to correspondingly form an isolation structure and a tunneling dielectric layer in one embodiment of the present application;

[0060] Fig.11 is a flow chart of a method for preparing a solar cell in one embodiment of the present application;

[0061] Fig.12 It is a cross-sectional view of a structure obtained after opening the blocking sacrificial layer, the isolation layer, and the tunneling material layer located in the first region in one embodiment of the present application;

[0062] Fig.13 It is a cross-sectional view of a structure obtained by texturing the second area of ​​the light-receiving surface of the substrate based on a blocking sacrificial layer in one embodiment of the present application;

[0063] Fig.14This is a flow chart of forming a first passivation layer and a second doping layer in a second area of ​​a backlight surface of a substrate in one embodiment of the present application;

[0064] Fig.15 It is a cross-sectional view of a structure obtained after a second doping material layer is formed on a side of the passivation material layer away from the substrate in one embodiment of the present application;

[0065] Fig.16 It is a cross-sectional view of a structure obtained after a second passivation layer is formed on a light-receiving surface of a substrate and an anti-reflection layer is formed on a side of the second passivation layer away from the substrate in one embodiment of the present application;

[0066] Fig.17 It is a schematic diagram of the structure of a photovoltaic module in one embodiment of the present application.

[0067] Description of reference numerals:

[0068] 100-solar cell; 110-substrate; 120-tunneling dielectric layer; 121-tunneling material layer; 131-intrinsic polysilicon material layer; 130-first doping layer; 140-isolation structure; 141-isolation layer; 102-blocking sacrificial layer; 150-first passivation layer; 160-second doping layer; 170-transparent conductive layer; 181-first gate line; 182-second gate line; 191-second passivation layer; 192-anti-reflection layer; 200-photovoltaic module; 210-cell string. DETAILED DESCRIPTION

[0069] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0070] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0071] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of this application, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0072] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0073] In the present application, unless otherwise clearly specified and limited, a first feature being “above” or “below” a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being “above”, “above”, and “above” a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being “below”, “below”, and “below” a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0074] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "upper", "lower", "left", "right" and similar expressions used herein are for illustrative purposes only and are not intended to be the only implementation method.

[0075] The solar cell and its manufacturing method, photovoltaic module and photovoltaic system according to the embodiments of the present application are described below with reference to the accompanying drawings.

[0076] Figure 1 This is one of the schematic diagrams of the structure of the solar cell provided in the embodiment of the present application. Figure 1In one embodiment of the present application, a solar cell is provided. In one embodiment of the present application, the solar cell may include a substrate 110, a tunnel dielectric layer 120, a first doping layer 130, an isolation structure 140, a first passivation layer 150, a second doping layer 160, a transparent conductive layer 170, a first gate line 181, and a second gate line 182.

[0077] The substrate 110 includes a light-receiving surface and a backlight surface that are arranged opposite to each other; wherein the backlight surface has a first area and a second area that are adjacent to each other in a first direction D1. It can be understood that the substrate 110 has a backlight surface and a light-receiving surface that are opposite to each other in a second direction D2 (i.e., the thickness direction of the solar cell). The light-receiving surface can be understood as the surface of the solar cell facing the sunlight, and the backlight surface can be understood as the surface of the solar cell facing away from the sunlight. In the embodiment of the present application, the first area and the second area can be arranged flush or not flush, and it can be understood that there is a step between the substrate 110 where the first area is located and the substrate 110 where the second area is located. Wherein, the thickness of the substrate 110 where the first area is located is greater than or equal to the thickness of the substrate 110 where the second area is located.

[0078] The substrate 110 is used to receive incident light and generate photogenerated carriers. The substrate 110 includes, but is not limited to, a doped semiconductor substrate made of silicon or germanium, or a doped compound semiconductor substrate made of silicon carbide, silicon germanium, gallium arsenide, indium phosphide, zinc oxide, or gallium oxide. For example, in the embodiment of the present application, the material of the substrate 110 can be a doped single crystal silicon material. Further, the doping element type of the substrate 110 can be N-type, and the N-type element can be, for example, any one of phosphorus, arsenic, or antimony; the doping element type of the substrate 110 can also be P-type, and the P-type element can be, for example, boron and gallium. For example, the doping element type of the substrate 110 is N-type. In the implementation of the present application, the light-receiving surface and the backlight surface of the substrate 110 will also have certain morphological changes based on the morphology of the battery film layer and other features. For example, the light-receiving surface can be a velvet structure; and the first area of ​​the backlight surface can be a planar structure, and the second area of ​​the backlight surface can also be a velvet structure.

[0079] The tunnel dielectric layer 120 is located in the first area of ​​the backlight surface. The tunnel dielectric layer 120 is used to achieve interface passivation on the backlight surface of the substrate 110, and has a chemical passivation effect. Specifically, by saturating the dangling bonds on the surface of the substrate 110, the interface defect state density on the backlight surface of the substrate 110 is reduced, thereby reducing the recombination center on the backlight surface of the substrate 110 to reduce the carrier recombination rate, thereby increasing the open circuit voltage of the solar cell and improving the photoelectric conversion efficiency of the solar cell. The material of the tunnel dielectric layer 120 can be a dielectric material, such as at least one of silicon oxide, amorphous silicon, polycrystalline silicon, silicon carbide, silicon nitride, silicon oxynitride, aluminum oxide or titanium oxide. Exemplarily, the dielectric material can contain doping elements of the same type as the doping elements of the substrate 110.

[0080] The material of the first doping layer 130 may be doped polysilicon, or doped polysilicon containing at least one of oxygen, carbon, and nitrogen. Optionally, the material of the first doping layer 130 may include heavily doped polysilicon. The first doping layer 130 is used to achieve interface passivation of the tunnel dielectric layer 120, and has the effect of field effect passivation. An electric field can be generated at the interface to prevent carriers of similar polarity from approaching by the same-order repulsion effect, thereby greatly reducing the recombination of photogenerated carriers. The doping type of the first doping layer 130 may be the same as the doping type of the substrate 110, or the opposite.

[0081] The isolation structure 140 is located on the side of the tunnel dielectric layer 120 away from the substrate 110, and is arranged in contact with the first passivation layer 150. It can be understood that the isolation structure 140 is located between the first doping layer 130 and the first passivation layer 150, which can achieve electrical isolation between the first doping layer 130 and the second doping layer 160, thereby preventing leakage. The isolation structure 140 also achieves interface passivation of the first doping layer 130, which can further increase the carrier recombination rate at the corresponding position of the backlight surface of the substrate 110. Optionally, the thickness dimension of the isolation structure 140 may be the same as the thickness dimension of the first doping layer 130. Optionally, the thickness dimension of the isolation structure 140 may be greater than the thickness dimension of the first doping layer 130. It should be noted that the thickness dimension refers to the dimension in the thickness direction of the solar cell.

[0082] The first passivation layer 150 is located in the second area of ​​the backlight surface. The material of the first passivation layer 150 may include intrinsic amorphous silicon and intrinsic hydrogenated amorphous silicon. Optionally, the material of the first passivation layer 150 is doped with at least one element of oxygen, carbon and nitrogen, for example, intrinsic amorphous silicon or intrinsic hydrogenated amorphous silicon containing at least one element of oxygen, carbon and nitrogen. The first passivation layer 150 chemically passivates the dangling bonds on the surface of the substrate 110, reduces the interface defect state density of the backlight surface of the substrate 110, thereby reducing the recombination center of the backlight surface of the substrate 110 to reduce the carrier recombination rate, thereby increasing the open circuit voltage of the solar cell and improving the photoelectric conversion efficiency of the solar cell.

[0083] The second doping layer 160 is located on the side of the first passivation layer 150 away from the substrate 110. The material of the second doping layer 160 may include doped amorphous silicon or microcrystalline silicon, or doped amorphous silicon or microcrystalline silicon containing at least one element of oxygen, carbon, and nitrogen. The conductivity type of the second doping layer 160 is opposite to the conductivity type of the first doping layer 130. Exemplarily, the conductivity type of the first doping layer 130 is one of P-type and N-type, and the conductivity type of the second doping layer 160 is the other of P-type and N-type.

[0084] The transparent conductive layer 170 is respectively located on the side of the first doped layer 130 and the second doped layer 160 away from the substrate 110. In the embodiment of the present application, the transparent conductive layer 170 extends from the space where the first area is located to the space where the second area is located. The material of the transparent conductive layer 170 can be one or more of zinc oxide ZnO, indium oxide InO and tin oxide SnO. The transparent conductive material can be doped with one or more of gallium Ga, tin Sn, molybdenum Mo, cerium Ce, fluorine F, tungsten W and aluminum Al.

[0085] The first gate line 181 is located on the side of the transparent conductive layer 170 in the first region away from the first doped layer 130. It can be understood that the projection of the first gate line 181 toward the substrate 110 is located in the first region. The second gate line 182 is located on the side of the transparent conductive layer 170 in the second region away from the second doped layer 160. It can be understood that the projection of the second gate line 182 toward the substrate 110 is located in the second region. Exemplarily, the materials of the first gate line 181 and the second gate line 182 include but are not limited to one or more of aluminum Al, titanium Ti, nickel Ni, cobalt Co, silver Ag, copper Cu and tin Sn. In the embodiment of the present application, the first gate line 181 and the second gate line 182 can be understood as metal gate lines, and the width and thickness of the metal gate lines are not limited. In this embodiment, the first gate line 181 and the second gate line 182 are both arranged on the back of the solar cell, so that the front of the cell for receiving light is completely shielded by no gate line, so that the light incident on the cell is fully absorbed, which improves the utilization rate of light and the short-circuit current of the solar cell.

[0086] In addition, an isolation groove 101 is provided on the transparent conductive layer 170, and the isolation groove 101 is located in the first region, and the isolation structure 140 is exposed at the bottom of the isolation groove 101. The isolation groove 101 is arranged between the first gate line 181 and the second gate line 182, and penetrates at least to the isolation structure 140, so that the first gate line 181 and the second gate line 182 are insulated, which can effectively prevent the two first gate lines 181 and the second gate line 182 from short-circuiting, thereby ensuring the battery performance. In addition, the isolation groove 101 can also prevent the occurrence of leakage between the first doping layer 130 and the second doping layer 160.

[0087] The solar cell provided in this embodiment includes a substrate, a tunneling dielectric layer, a first doped layer, an isolation structure, a first passivation layer, a second doped layer, a transparent conductive layer, a first grid line and a second grid line, wherein the first grid line and the second grid line are arranged on the backlight side of the solar cell, and the light-receiving surface of the cell for receiving light is completely free of grid lines, so that the light incident on the cell is fully absorbed, thereby improving the light utilization rate of the cell. The first grid line and the second grid line can directly contact the transparent conductive layer, thereby improving the conductivity of the first grid line and the second grid line and the transparent conductive layer, and simplifying the solar cell structure and reducing costs. In addition, on the back side of the solar cell, the dangling bonds on the substrate surface can be chemically passivated by the tunneling dielectric layer located in the first area of ​​the backlight surface of the substrate and the first passivation layer in the second area, thereby greatly reducing the interface recombination on the substrate surface. Moreover, the isolation structure and the first doped layer are both located on the side of the tunnel dielectric layer away from the substrate, and the isolation structure is located between the first doped layer and the second doped layer, which can achieve electrical isolation between the first doped layer and the second doped layer, thereby preventing leakage. The isolation structure also achieves interface passivation of the first doped layer, which can further reduce the carrier recombination rate at the corresponding position of the backlight surface of the substrate. In addition, only one doped layer is set in the first region and the second region, for example, the first doped layer in the first region and the second doped layer in the second region, which reduces the concentric circle effect produced by the TOPCon high-temperature preparation process, and can further improve the performance of the solar cell.

[0088] In an exemplary embodiment, the material of the isolation structure 140 includes intrinsic polysilicon. The isolation structure 140 formed by using intrinsic polysilicon has an insulating property, and the isolation structure 140 and the isolation trench 101 with good insulating isolation effect electrically isolate the first doped layer and the second doped layer with opposite conductivity types, thereby reducing the risk of leakage.

[0089] In an exemplary embodiment, the isolation structure 140 is disposed in the same layer as the first doping layer 130, and a portion of the first passivation layer 150 covers the sidewall of the isolation structure 140 away from the first doping layer 130. The isolation structure 140 may include a first sidewall and a second sidewall disposed opposite to each other, wherein the first sidewall is disposed in contact with a portion of the first passivation layer 150, and the second sidewall is disposed in contact with the first doping layer 130. In the embodiment of the present application, for ease of description, the portion of the first passivation layer covering the sidewall of the isolation structure 140 is referred to as a passivation structure. The passivation structure may cover the first sidewall of the isolation structure 140.

[0090] In this embodiment, the isolation structure is arranged on the same layer as the first doped layer, and the isolation structure is located between the first passivation layer and the first doped layer, and the isolation structure can cover the first side wall of the isolation structure, so that the first passivation layer protects the first side wall of the isolation structure, which can increase the passivation effect of the isolation structure. At the same time, the first passivation layer and the isolation structure are arranged between the first doped layer and the second doped layer, which can effectively avoid the occurrence of leakage on the edge surface of the second doped layer close to the first doped layer, thereby increasing the power output of the solar cell while improving the battery conversion efficiency.

[0091] Furthermore, the size of the portion of the first passivation layer 150 covering the side wall of the isolation structure 140 in the thickness direction of the solar cell is larger than the size of the isolation structure 140 in the thickness direction. Optionally, the passivation structure can also cover the side wall of the tunnel dielectric layer 120 close to the second region at the same time. Optionally, the passivation structure protrudes outward from the isolation structure 140 in the direction toward the transparent conductive layer 170 to further increase the passivation effect on the isolation structure, and can further effectively avoid the occurrence of leakage between the second doping layer 160 and the first doping layer 130.

[0092] In an exemplary embodiment, the materials of the first gate line 181 and the second gate line 182 are low temperature metal pastes, respectively. Exemplarily, the low temperature metal pastes include but are not limited to low temperature curing silver copper paste and low temperature silver paste.

[0093] In this embodiment, by using low-temperature metal slurry to form the first gate line and the second gate line, the high-temperature process of the metallization process can be avoided. A lower curing temperature can be used to form the first gate line and the second gate line, thereby simplifying the process flow. At the same time, the first gate line and the second gate line formed by the low-temperature metal slurry have better conductive properties.

[0094] In an exemplary embodiment, the conductivity type of the first doping layer 130 is N-type and the conductivity type of the second doping layer 160 is P-type. For example, the material of the first doping layer 130 includes phosphorus-doped polysilicon, which can be a phosphorus-doped polysilicon layer. The material of the second doping layer 160 includes one of boron-doped hydrogenated microcrystalline, boron-doped polysilicon layer, boron-doped silicon oxide, and boron-doped silicon oxycarbide. Exemplarily, the second doping layer 160 can be a boron-doped hydrogenated microcrystalline silicon layer.

[0095] In this embodiment, the first doping layer 130 and the second doping layer 160 have opposite conductivity types, and the first doping layer 130 and the second doping layer 160 are respectively located in the first area and the second area of ​​the backlight surface of the substrate 110. Compared with the TBC cell in the related art, when phosphorus-doped polysilicon and boron-doped polysilicon are deposited on the backlight surface, it is easy to form a concentric circle effect due to the superposition of high-temperature processes, which will affect the passivation and thus affect the performance of the cell. The solar cell (hybrid solar cell) provided in the embodiment of the present application has only one doping layer in the first area and the second area. For example, the first doping layer 130 in the first area is a phosphorus-doped polysilicon layer, and there is no boron-doped polysilicon layer, which reduces the concentric circle effect generated by the TOPCon high-temperature preparation process and can further improve the performance of the solar cell. In addition, compared with the HBC cell in the related art, a phosphorus-doped hydrogenated microcrystalline silicon layer is formed in the second area of ​​the backlight surface, and the structure of phosphorus-doped hydrogenated microcrystalline silicon is easily damaged by laser, but the second doping layer 160 in the second area of ​​the embodiment of the present application is a boron-doped hydrogenated microcrystalline or boron-doped polycrystalline silicon layer, which can avoid damage caused by laser.

[0096] like Figure 2 As shown, in an exemplary embodiment, the solar cell further includes a second passivation layer 191 and an anti-reflection layer 192. The second passivation layer 191 is located on the light-receiving surface of the substrate 110. The second passivation layer 191 may be a single-layer structure or a multi-layer structure, and the material of the second passivation layer 191 may be at least one of aluminum oxide, silicon oxide, silicon nitride and silicon oxynitride. Optionally, the material of the second passivation layer 191 may also be intrinsic amorphous silicon, or amorphous silicon containing at least one of oxygen, carbon and nitrogen. The second passivation layer 191 plays a surface passivation role in the solar cell, and can perform good chemical passivation on the dangling bonds on the surface of the substrate 110. The anti-reflection layer 192 is located on the side of the second passivation layer 191 away from the substrate 110. The anti-reflection layer 192 may be a single-layer structure or a multi-layer structure. In the anti-reflection layer 192 of the multi-layer structure, the material of each layer may be silicon oxide, silicon nitride or silicon oxynitride. The anti-reflection layer 192 is located on the light-receiving surface of the solar cell, and has an anti-reflection effect on the light-receiving surface of the solar cell.

[0097] Figure 3Schematic diagram of the process of manufacturing a solar cell provided in Example 4 of the present application. This embodiment provides a method for manufacturing a solar cell, which is used to manufacture the solar cell in any of the above embodiments. The structure, function, working principle, etc. of the solar cell have been described in detail in Example 1 and will not be repeated here. This embodiment of the present application also provides a method for manufacturing a solar cell. Figure 3 As shown, the method for preparing a solar cell includes steps 302 to 310.

[0098] Step 302, providing a substrate; wherein the substrate includes a light-receiving surface and a backlight surface disposed opposite to each other.

[0099] like Figure 4 As shown, the substrate 110 may include but is not limited to a doped semiconductor substrate made of silicon or germanium, or a doped compound semiconductor substrate made of silicon carbide, silicon germanium, gallium arsenide, indium phosphide, zinc oxide or gallium oxide. For example, in the embodiment of the present application, the material of the substrate 110 may be a doped single crystal silicon material. Further, the doping element type of the substrate 110 may be N-type, and the N-type element may be, for example, any one of phosphorus, arsenic or antimony; the doping element type of the substrate 110 may also be P-type, and the P-type element may be, for example, boron and gallium. In the embodiment of the present application, the substrate 110 is an N-type silicon substrate as an example for explanation. After providing the N-type silicon substrate, the N-type silicon substrate may be pre-cleaned to remove impurities on the surface of the N-type silicon substrate.

[0100] Optionally, the solar energy preparation method provided in the embodiment of the present application can also perform a texturing treatment on part of the surface of the substrate 110. Exemplarily, the texturing treatment of the light-receiving surface of the substrate 110 is taken as an example for explanation. Specifically, a barrier layer of 300-500nm is plated on the backlight surface of the cleaned substrate 110. Among them, the material of the barrier layer includes but is not limited to silicon nitride material. Then, the substrate 110 with the barrier layer plated on the back is cleaned again. Next, the light-incident surface of the substrate 110 is texturized using the barrier layer as a mask to form a textured surface of uniform size on the light-incident surface of the substrate 110 (for example, anisotropic etching of the light-incident surface of the substrate 110 is performed using a low-concentration alkali solution to form a pyramid velvet surface). In addition, the organic matter and metal ions on the textured surface are cleaned through a cleaning solution (for example, RCA-1 and RCA-2), which can reduce the reflectivity and increase the absorption of sunlight by the silicon substrate 110. Finally, the surface of the pyramid velvet is smoothed, and finally the surface oxide layer and the barrier layer on the back are removed with hydrofluoric acid.

[0101] Step 304 , forming a tunnel dielectric layer, an isolation structure and a first doping layer in a first region of the backlight surface of the substrate.

[0102] Please continue to refer to Figure 4, the back side of the substrate 110 includes a first region and a second region adjacent to each other. Exemplarily, a tunnel dielectric layer 120 can be formed in the first region of the backlight side of the substrate 110 by plasma enhanced chemical vapor deposition (PECVD). The tunnel layer is used to achieve interface passivation of the backlight side of the substrate 110, and has a chemical passivation effect. Specifically, by saturating the dangling bonds on the backlight side of the substrate 110, the interface defect state density on the backlight side of the substrate 110 is reduced, thereby reducing the recombination center on the backlight side of the substrate 110 to reduce the carrier recombination rate.

[0103] After forming the tunnel dielectric layer 120, an isolation structure 140 and a first doped layer 130 may be formed on a surface of the tunnel dielectric layer 120 away from the substrate 110 by deposition. The isolation structure 140 and the first doped layer 130 are provided in the same layer. The isolation structure 140 and the first doped layer 130 are respectively formed on a side of the tunnel dielectric layer 120 away from the substrate 110.

[0104] Optionally, the material of the isolation structure 140 may include intrinsic polysilicon (poly-Si). By using intrinsic polysilicon to form the isolation structure 140, electrical isolation between the first doped layer and the second doped layer can be achieved, thereby preventing leakage. The isolation structure also achieves interface passivation of the first doped layer, which can further increase the carrier recombination rate at the corresponding position of the backlight surface of the substrate. The isolation structure 140 also achieves interface passivation of the first doped layer 130, which can further increase the carrier recombination rate at the corresponding position of the backlight surface of the substrate 110.

[0105] Step 306 , forming a first passivation layer and a second doping layer in a second region of the backlight surface of the substrate.

[0106] like Figure 5 As shown, the first passivation layer 150 is disposed in contact with the isolation structure 140 , and the second doping layer 160 is located on a side of the first passivation layer 150 away from the substrate 110 .

[0107] Exemplarily, a first passivation layer 150 can be formed in a first region of the backlight surface of the substrate 110 by plasma enhanced chemical vapor deposition (PECVD). The first passivation layer 150 is used to achieve interface passivation of the backlight surface of the substrate 110, and has a chemical passivation effect. After the first passivation layer 150 is formed, a second doping layer 160 can also be formed on a surface of the first passivation layer 150 away from the substrate 110 by deposition. The first doping layer 130 and the second doping layer 160 are respectively located in the first region and the second region of the backlight surface of the substrate 110, and the first doping layer 130 and the second doping layer 160 have opposite conductivity types. The conductivity type of the first doping layer 130 is one of P-type and N-type, and the conductivity type of the second doping layer 160 is the other of P-type and N-type.

[0108] Step 308 : forming a transparent conductive layer on a side of the first doped layer and the second doped layer away from the substrate.

[0109] like Figure 6 As shown, the material of the transparent conductive layer 170 includes a transparent conductive oxide, for example, one or more of zinc oxide ZnO, indium oxide InO and tin oxide SnO. Optionally, the transparent conductive oxide may also be doped with elements, for example, the doping elements include but are not limited to one or more of gallium element Ga, tin element Sn, molybdenum element Mo, cerium element Ce, fluorine element F, tungsten element W, aluminum element Al and manganese-doped indium oxide.

[0110] In the embodiment of the present application, a transparent conductive oxide may be deposited on the first doping layer 130 and the second doping layer 160 away from the substrate 110 by physical vapor deposition, chemical vapor deposition, or reactive plasma deposition (RPD) to form a transparent conductive layer 170. Please continue to refer to Figure 6 After forming the transparent conductive layer 170 , an isolation trench 101 may be formed in the transparent conductive layer 170 located in the first region, and the isolation structure 140 is exposed at the bottom of the isolation trench 101 .

[0111] Step 310: forming a first gate line and a second gate line.

[0112] Please continue to refer to Figure 1, wherein the first gate line 181 is disposed in contact with the transparent conductive layer 170 located in the first region, and is located on a side of the transparent conductive layer 170 in the first region away from the first doping layer 130. The second gate line 182 is disposed in contact with the transparent conductive layer 170 located in the second region, and is located on a side of the transparent conductive layer 170 in the second region away from the second doping layer 160. In the embodiment of the present application, the first gate line 181 and the second gate line 182 in contact with the transparent conductive layer 170 may be formed on the transparent conductive layer 170 by methods including but not limited to copper electroplating, evaporation, screen printing, steel plate printing, laser transfer, and the like.

[0113] The first grid line 181 and the second grid line 182 are arranged on the back of the solar cell. At this time, the front of the cell for receiving light is completely shielded by no grid lines, so that the light incident on the cell is fully absorbed, thereby improving the light utilization rate of the cell. In addition, the isolation groove 101 is arranged between the first grid line 181 and the second grid line 182, and penetrates at least to the isolation structure 140, so that the first grid line 181 and the second grid line 182 are insulated, which can effectively prevent the two first grid lines 181 and the second grid line 182 from short-circuiting, thereby ensuring the performance of the cell.

[0114] The preparation method of the solar cell provided by the embodiment of the present application, the first grid line and the second grid line of the solar cell prepared by the solar cell are arranged on the backlight side of the solar cell, directly contacted with the transparent conductive layer, and the light-receiving surface of the cell for receiving light is completely free of grid line shielding, so that the light incident on the cell is fully absorbed, and the light utilization rate of the cell is improved. The first grid line and the second grid line can directly contact the transparent conductive layer, improve the conductivity of the first grid line and the second grid line and the transparent conductive layer, and can simplify the process flow of the solar cell preparation method, and the cost is low. In addition, on the back of the solar cell, the dangling bonds on the surface of the substrate can be chemically passivated by the tunneling dielectric layer located in the first area of ​​the backlight surface of the substrate and the first passivation layer in the second area, which greatly reduces the interface recombination on the surface of the substrate. In addition, the isolation structure and the first doped layer are both located on the side of the tunneling dielectric layer away from the substrate, and the isolation structure is located between the first doped layer and the second doped layer, which can realize the electrical isolation between the first doped layer and the second doped layer, thereby preventing the occurrence of leakage, and the isolation structure also realizes the interface passivation of the first doped layer, which can further improve the carrier recombination rate at the corresponding position of the backlight surface of the substrate. In addition, only one doping layer is provided in the first region and the second region, for example, a first doping layer in the first region and a second doping layer in the second region, which reduces the concentric circle effect produced by the TOPCon high-temperature preparation process and can further improve the performance of the solar cell.

[0115] Optionally, the first gate line 181 and the second gate line 182 may be formed by printing a low-temperature conductive paste. Exemplarily, the low-temperature metal paste includes but is not limited to a low-temperature curing silver-copper paste and a low-temperature silver paste.

[0116] In this embodiment, low-temperature conductive paste is used to form the first gate line 181 and the second gate line 182. Compared with the related art that uses high-temperature conductive paste to form the first gate line 181 and the second gate line 182, the high-temperature process of the metallization process can be avoided. A lower curing temperature can be used to form the first gate line and the second gate line, which simplifies the process flow. At the same time, the first gate line and the second gate line formed by the low-temperature metal paste have better conductive performance.

[0117] Optionally, in the embodiment of the present application, the conductivity type of the first doping layer 130 is N-type and the conductivity type of the second doping layer 160 is P-type. For example, the first doping layer 130 can be formed by depositing phosphorus-doped polysilicon in the first area of ​​the backlight surface of the substrate 110. The second doping layer 160 can be formed by depositing one of boron-doped hydrogenated microcrystals, boron-doped polysilicon layer, boron-doped silicon oxide, and boron-doped silicon oxycarbide on the surface of the first passivation layer 150 away from the substrate 110.

[0118] In this embodiment, the first doping layer and the second doping layer have opposite conductivity types, and the first doping layer and the second doping layer are respectively located in the first area and the second area of ​​the backlight surface of the substrate. Compared with the TBC cell in the related art, when phosphorus-doped polysilicon and boron-doped polysilicon are deposited on the backlight surface, it is easy to form a concentric circle effect due to the superposition of high-temperature processes, which will affect the passivation and thus affect the performance of the cell. The solar cell (hybrid solar cell) provided in the embodiment of the present application has only one doping layer in the first area and the second area. For example, the first doping layer in the first area is a phosphorus-doped polysilicon layer, and there is no boron-doped polysilicon layer, which reduces the concentric circle effect generated by the TOPCon high-temperature preparation process and can further improve the performance of the solar cell. In addition, compared with the HBC cell in the related art, a phosphorus-doped hydrogenated microcrystalline silicon layer is formed in the second area of ​​the backlight surface, and the structure of phosphorus-doped hydrogenated microcrystalline silicon is easily damaged by laser, but the second doping layer in the second area of ​​the embodiment of the present application is a boron-doped hydrogenated microcrystalline or boron-doped polycrystalline silicon layer, which can avoid damage caused by laser.

[0119] like Figure 7 As shown, in an exemplary embodiment, a tunnel dielectric layer, an isolation structure and a first doping layer are formed in a first region of a backlight surface of a substrate, including steps 702 to 706.

[0120] Step 702, forming a tunneling material layer on the backlight surface of the substrate.

[0121] like Figure 8As shown, in an embodiment of the present application, a tunneling material can be deposited on the entire backlight surface of the substrate 110 to form a tunneling material layer 121. The tunneling material includes but is not limited to at least one of silicon oxide, amorphous silicon, polycrystalline silicon, silicon carbide, silicon nitride, silicon oxynitride, aluminum oxide or titanium oxide. The tunneling material layer 121 is made of the same material as the tunneling dielectric layer 120, which can achieve interface passivation on the backlight surface of the substrate 110 and achieve a chemical passivation effect. Specifically, by saturating the dangling bonds on the surface of the substrate 110, the interface defect state density on the backlight surface of the substrate 110 is reduced, thereby reducing the recombination center on the backlight surface of the substrate 110 to reduce the carrier recombination rate, thereby increasing the open circuit voltage of the solar cell and improving the photoelectric conversion efficiency of the solar cell.

[0122] Step 704 , forming an intrinsic polysilicon material layer on a side of the tunneling material layer away from the substrate.

[0123] Please continue to refer to Figure 8 After forming the tunnel material layer 121, illustratively, intrinsic amorphous silicon can be deposited on the side of the tunnel material layer 121 away from the substrate 110 to form an intrinsic polysilicon material layer 131. Optionally, the thickness of the intrinsic polysilicon material layer 131 can be about 100nm-500nm.

[0124] Step 706 , doping the intrinsic polysilicon material layer located in the first region and annealing the resulting structure to form a first doping layer located in the first region and an isolation layer located in the second region.

[0125] like Fig. 9 As shown, exemplarily, a mask can be set on the surface of the side of the intrinsic polysilicon material layer 131 away from the tunneling material layer 121, and based on the mask, a phosphorus paste or phosphorus ion implantation or laser phosphorus ion doping is applied to the surface of the side of the intrinsic polysilicon material layer 131 located in the first region away from the tunneling material layer 121, so as to phosphorus-dope the intrinsic polysilicon material layer 131 located in the first region. After phosphorus doping, the resulting structure is subjected to high-temperature annealing to form a first doped layer 130 located in the first region and an isolation layer 141 located in the second region. Exemplarily, when the high-temperature annealing treatment is performed, the annealing temperature can be 750°C-950°C, for example, 900°C. The annealing time can be 25 minutes-35 minutes, for example, 30 minutes. It should be noted that the first doped layer 130 located in the first region can be understood as the first region where the orthographic projection of the first doped layer 130 toward the substrate 110 falls on the backlight surface of the substrate 110. The isolation layer 141 located in the second region can be understood as a second region where the orthographic projection of the isolation layer 141 toward the substrate 110 falls into the backlight surface of the substrate 110 .

[0126] Step 707 , removing part of the isolation layer and part of the tunneling material layer to correspondingly form an isolation structure and a tunneling dielectric layer.

[0127] In the embodiment of the present application, a portion of the isolation layer 141 and a portion of the tunneling material layer 121 can be selectively etched by laser or wet mask to form an isolation structure 140 and a tunneling dielectric layer 120. Specifically, after removing a portion of the isolation layer 141, the remaining isolation layer 141 is the isolation structure 140; correspondingly, after removing a portion of the tunneling material layer 121, the remaining tunneling material layer 121 is the tunneling dielectric layer 120. Please continue to refer to Figure 4 .

[0128] For example, laser may be used to remove part of the isolation layer 141 and part of the tunneling material layer 121 to expose the second region of the backlight surface of the substrate 110. Furthermore, in the process of removing part of the isolation layer 141 and part of the tunneling material layer 121 by laser, if there is laser cutting damage to the substrate 110, wet etching may be used to remove the damaged part of the substrate 110, thereby reducing the reflectivity and increasing the absorption of sunlight by the silicon substrate 110.

[0129] Optionally, wet mask selective etching can be used to remove part of the isolation layer 141 and part of the tunneling material layer 121 to expose the second region of the backlight surface of the substrate 110. Furthermore, the structure obtained by wet etching can be cleaned to remove dirt from the second region of the backlight surface of the silicon substrate 110, thereby reducing the reflectivity and increasing the absorption of sunlight by the silicon substrate 110.

[0130] In this embodiment, in the process of forming the isolation structure and the first doping layer, both can be formed based on the intrinsic polysilicon material layer, without the need to additionally set up a film layer for forming the isolation structure. This can simplify the preparation process of the isolation structure, improve the preparation efficiency of solar cells, and reduce the preparation cost.

[0131] like Fig.10 As shown, in an exemplary embodiment, a portion of the isolation layer and a portion of the tunneling material layer are removed to correspondingly form an isolation structure and a tunneling dielectric layer, including steps 1002 to 1006.

[0132] Step 1002 : forming a blocking sacrificial layer on a side of the first doping layer and the isolation layer away from the tunnel dielectric layer.

[0133] like Fig.11 As shown, for example, a barrier material is deposited on the side of the first doping layer 130 and the isolation layer 141 away from the tunnel dielectric layer 120, and the resulting structure after the deposition of the barrier material is annealed to form a barrier sacrificial layer 102. The barrier material may include but is not limited to hydrogenated silicon nitride SiN X:H, silicon nitride and other materials. In the embodiment of the present application, the barrier material is hydrogenated silicon nitride as an example for explanation. In the process of annealing the structure obtained after depositing the barrier material, SiN X :H performs annealing treatment to form a blocking sacrificial layer 102.

[0134] Step 1004 , opening the blocking sacrificial layer, the isolation layer, and the tunneling material layer located in the first region to expose the backlight surface of the substrate.

[0135] like Fig.12 As shown, in the embodiment of the present application, laser or wet method with mask selective etching can be used to remove the blocking sacrificial layer 102, the isolation layer 141, and the tunneling material layer 121 located in the first region, and form an opening, the bottom of which is the backlight surface of the substrate 110. It can be understood that laser or wet method with mask selective etching can be used to remove the blocking sacrificial layer 102, the isolation layer 141, and the tunneling material layer 121 located in the first region, and the second region of the backlight surface of the substrate 110 can be exposed.

[0136] For example, after using laser to remove the blocking sacrificial layer 102, the isolation layer 141, and the tunneling material layer 121 located in the first area, KOH can be used to remove laser cutting damage in the laser opening area, and then the second area of ​​the backlight surface of the substrate 110 is cleaned. In this way, the reflectivity can be reduced and the absorption of sunlight by the silicon substrate 110 can be increased.

[0137] Step 1006 , removing the remaining blocking sacrificial layer to obtain an isolation structure and a tunneling dielectric layer.

[0138] For example, a wet etching process, such as using hydrofluoric acid, may be used to remove the remaining blocking sacrificial layer 102 (the blocking sacrificial layer 102 located in the first region). Please continue to refer to Figure 4 .

[0139] Optionally, before step 1002, the method for preparing a solar cell further includes texturing the second region of the light-receiving surface of the substrate 110 based on the blocking sacrificial layer 102. Fig.13 As shown, specifically, the second region of the light-receiving surface of the substrate 110 is textured using the sacrificial barrier layer as a mask, and a uniformly textured surface C is formed in the second region of the light-receiving surface of the substrate 110 (for example, a low-concentration alkali solution is used to anisotropically etch the light-incident surface of the substrate 110 to form a pyramid velvet surface C). In addition, organic matter and metal ions on the textured surface are cleaned by a cleaning solution (for example, RCA-1 and RCA-2), which can reduce the reflectivity and increase the absorption of sunlight by the silicon substrate 110. Finally, the surface of the pyramid velvet is smoothed using HNO3 / HF.

[0140] like Fig.14 As shown, in an exemplary embodiment, a first passivation layer and a second doping layer are formed in a second area of ​​a backlight surface of a substrate, including steps 1402 to 1406.

[0141] Step 1402 , forming a passivation material layer on the second region of the backlight surface, the first side surface of the isolation structure, and the side of the isolation structure and the first doped layer away from the substrate.

[0142] like Fig.15 As shown, in the embodiment of the present application, intrinsic amorphous silicon can be deposited using a deposition process such as plasma enhanced chemical vapor deposition (PECVD) or hot wire chemical vapor deposition (HWCVD) to form a passivation material layer 151. The passivation material layer 151 can be a single-layer structure or a stacked structure of multiple intrinsic polycrystalline silicon material layers.

[0143] Step 1404 , forming a second doping material layer on a side of the passivation material layer away from the substrate.

[0144] In the embodiment of the present application, a deposition process such as PECVD or HWCVD can be used to deposit a second doping material on the passivation material layer 151 to form a second doping material layer 161. Please continue to refer to Fig.15 . Among them, the second doping material may include a hydrogenated microcrystalline silicon layer doped with a P-type element, a microcrystalline silicon oxide layer (μc-SiOx:H layer) or a microcrystalline carbon oxide silicon layer (μc-SiCxOy:H layer), etc. Exemplarily, the second doping material may be boron-doped microcrystalline carbon oxide silicon or boron-doped microcrystalline silicon oxide or boron-doped hydrogenated microcrystalline silicon or boron-doped amorphous silicon, etc. It should be noted that in the implementation of the present application, the material of the passivation material layer is the same as the material of the first passivation layer, and the second doping material layer is the same as the material of the second doping layer 160.

[0145] Step 1406 , removing the passivation material layer and the second doping material layer located in the second region to form a first passivation layer and a second doping layer.

[0146] In the embodiment of the present application, the passivation material layer 151 and the second doping material layer 161 located in the second region can be selectively etched by laser or wet mask to form the first passivation layer 150 and the second doping layer 160. Specifically, after removing part of the passivation material layer 151, the remaining passivation material layer is the first passivation layer 150; correspondingly, after removing part of the second doping material layer 161, the remaining second doping material layer is the second doping layer 160. Please continue to refer to Figure 5 .

[0147] Exemplarily, after laser is used to remove the passivation material layer and the doping material layer located in the second region, KOH can also be used to remove the laser cutting damage to expose the isolation structure 140 and the first doping layer 130. Among them, the isolation structure 140 has a first side wall and a second side wall arranged opposite to each other, wherein the first side wall is arranged in contact with the first passivation layer 150 and is arranged to be insulated from the second doping layer 160, and the second side wall is arranged in contact with the second doping layer 160. It can be understood that a portion of the first passivation layer 150 and the isolation structure 140 are arranged between the first doping layer 130 and the second doping layer 160, which can effectively avoid the occurrence of leakage on the edge surface of the second doping layer close to the first doping layer, thereby increasing the power output of the solar cell while improving the battery conversion efficiency. In addition, the isolation structure can cover the first side wall of the isolation structure, so that the first passivation layer protects the first side wall of the isolation structure, which can increase the passivation effect on the isolation structure.

[0148] In an exemplary embodiment, the solar preparation method further includes the steps of forming a second passivation layer on the light-receiving surface of the substrate, and forming an anti-reflection layer on the side of the second passivation layer away from the substrate, such as Fig.16 As shown. Exemplarily, the steps of forming the second passivation layer 191 on the light-receiving surface of the substrate 110 and forming the anti-reflection layer 192 on the side of the second passivation layer 191 away from the substrate can be prepared before forming the blocking sacrificial layer.

[0149] Exemplarily, before forming the blocking sacrificial layer, a passivation material is deposited on the light-receiving surface of the substrate to form a second passivation layer 191. The passivation material includes but is not limited to intrinsic amorphous silicon or aluminum oxide or silicon oxide or hydrogenated silicon nitride. The second passivation layer 191 plays a surface passivation role in the solar cell and can perform good chemical passivation on the dangling bonds on the surface of the substrate 110.

[0150] After forming the second passivation layer 191, an anti-reflection material is deposited on the side of the second passivation layer 191 away from the substrate 110 to form an anti-reflection layer 192. The anti-reflection material includes but is not limited to silicon nitride, silicon oxide or silicon oxynitride. The anti-reflection layer 192 is located on the light-receiving surface of the solar cell, and the anti-reflection effect is achieved on the light-receiving surface of the solar cell.

[0151] Optionally, the thickness of the anti-reflection layer 192 is greater than that of the second passivation layer 191 to ensure that after the second area of ​​the light-receiving surface of the substrate 110 is subsequently textured based on the blocking sacrificial layer 102, sufficient thickness can be etched away by cleaning to ensure that the second passivation layer 191 remains at 80 nm or above on the textured surface.

[0152] Fig.17 This is a schematic diagram of the structure of a photovoltaic module provided in an embodiment of the present application. Fig.17This embodiment provides a photovoltaic module 200, including at least one battery string 210, the battery string 210 includes at least two solar cells 100 in any of the aforementioned embodiments, and the solar cells 100 can be connected together by serial welding.

[0153] For example, multiple solar cells can be connected in series by welding ribbons, so that the electricity generated by a single solar cell can be collected for subsequent transmission. Of course, the solar cells can be arranged at intervals or stacked in a shingled form.

[0154] Exemplarily, the photovoltaic module 200 also includes an encapsulation layer and a cover plate (not shown), the encapsulation layer is used to cover the surface of the battery string 210, and the cover plate is used to cover the surface of the encapsulation layer away from the battery string 210. The solar cells are electrically connected in the form of a whole piece or multiple pieces to form a plurality of battery strings 210, and the plurality of battery strings 210 are electrically connected in series and / or in parallel. Specifically, in some embodiments, the plurality of battery strings 210 can be electrically connected by a conductive tape. The encapsulation layer covers the surface of the solar cell. For example, the encapsulation layer can be an organic encapsulation film such as an ethylene-vinyl acetate copolymer film, a polyethylene octene co-elastic film, or a polyethylene terephthalate film. The cover plate can be a cover plate with a light-transmitting function such as a glass cover plate, a plastic cover plate, etc.

[0155] This embodiment provides a photovoltaic system (not shown), including the aforementioned photovoltaic components. The photovoltaic system can be used in photovoltaic power stations, such as ground power stations, rooftop power stations, water surface power stations, etc., and can also be used in equipment or devices that use solar energy to generate electricity, such as user solar power supplies, solar street lights, solar cars, solar buildings, etc. Of course, it can be understood that the application scenarios of the photovoltaic system are not limited to this, that is, the photovoltaic system can be used in all fields that require solar energy to generate electricity. Taking the photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a junction box and an inverter. The photovoltaic array may be an array combination of multiple photovoltaic components. For example, multiple photovoltaic components can form multiple photovoltaic arrays. The photovoltaic array is connected to the junction box. The junction box can converge the current generated by the photovoltaic array. The converged current flows through the inverter and is converted into the alternating current required by the mains power grid, and then connected to the mains network to realize solar power supply.

[0156] In the description of this specification, the description with reference to the terms "one embodiment", "other embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic description of the above terms does not necessarily refer to the same embodiment or example.

[0157] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0158] The above embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.

Claims

1. A solar cell, It is characterized in that include: A substrate, the substrate comprising a light-receiving surface and a backlight surface that are arranged opposite to each other; A tunneling dielectric layer, located in the first area of ​​the backlight surface; A first doped layer, located on a side of the tunnel dielectric layer away from the substrate; An isolation structure, located on a side of the tunnel dielectric layer away from the substrate; A first passivation layer is located in the second area of ​​the backlight surface, and the isolation structure is located between the first passivation layer and the isolation structure; A second doping layer is located on a side of the first passivation layer away from the substrate; A transparent conductive layer, located on the first doped layer and the second doped layer at a side away from the substrate, and an isolation groove is provided on the transparent conductive layer, and the isolation structure is exposed at the bottom of the isolation groove; A first gate line, located at a side of the transparent conductive layer in the first region away from the first doping layer; The second gate line is located at a side of the transparent conductive layer in the second region away from the second doping layer.

2. The solar cell according to claim 1, It is characterized in that A portion of the first passivation layer covers a sidewall of the isolation structure away from the first doping layer.

3. The solar cell according to claim 2, It is characterized in that A size of a portion of the first passivation layer covering the sidewall of the isolation structure in a thickness direction of the solar cell is larger than a size of the isolation structure in the thickness direction.

4. The solar cell according to claim 1, It is characterized in that The material of the isolation structure includes intrinsic polysilicon.

5. The solar cell according to claim 1, It is characterized in that The materials of the first gate line and the second gate line include low-temperature metal paste respectively.

6. The solar cell according to claim 1, It is characterized in that The material of the first doping layer includes a phosphorus-doped polysilicon layer; the material of the second doping layer includes one of boron-doped hydrogenated microcrystals, boron-doped polysilicon layer, boron-doped silicon oxide, and boron-doped silicon oxycarbide.

7. The solar cell according to claim 1, It is characterized in that The solar cell further comprises: A second passivation layer is located on the light-receiving surface of the substrate; The anti-reflection layer is located on a side of the second passivation layer away from the substrate.

8. A method for preparing a solar cell, It is characterized in that include: Providing a substrate; wherein the substrate comprises a light-receiving surface and a backlight surface disposed opposite to each other; Forming a tunnel dielectric layer, an isolation structure and a first doped layer in a first area of ​​the backlight surface of the substrate; wherein the isolation structure and the first doped layer are respectively formed on a side of the tunnel dielectric layer away from the substrate; forming a first passivation layer and a second doping layer in a second region of the backlight surface of the substrate; wherein the second doping layer is located on a side of the first passivation layer away from the substrate, and the isolation structure is located between the first passivation layer and the isolation structure; A transparent conductive layer is formed on the first doped layer and the second doped layer at a side away from the substrate; wherein an isolation groove is formed in the transparent conductive layer, and the isolation structure is exposed at the bottom of the isolation groove; A first gate line and a second gate line are formed, wherein the first gate line is disposed in contact with the transparent conductive layer located in the first region, and the second gate line is disposed in contact with the transparent conductive layer located in the second region.

9. The method for preparing a solar cell according to claim 8, It is characterized in that The step of forming a tunnel dielectric layer, an isolation structure and a first doping layer in a first region of the backlight surface of the substrate comprises: forming a tunneling material layer on the backlight surface of the substrate; forming an intrinsic polysilicon material layer on a side of the tunneling material layer away from the substrate; Doping the intrinsic polysilicon material layer located in the first region and annealing the resulting structure to form a first doping layer located in the first region and an isolation layer located in the second region; Part of the isolation layer and part of the tunneling material layer are removed to correspondingly form the isolation structure and the tunneling dielectric layer.

10. The method for preparing a solar cell according to claim 9, It is characterized in that The removing part of the isolation layer and part of the tunneling material layer to correspondingly form the isolation structure and the tunneling dielectric layer comprises: forming a blocking sacrificial layer on a side of the first doped layer and the isolation layer away from the tunnel dielectric layer; Opening the blocking sacrificial layer, the isolation layer, and the tunneling material layer located in the first region to expose the backlight surface of the substrate; The remaining blocking sacrificial layer is removed to form the isolation structure and the tunneling dielectric layer.

11. The method for preparing a solar cell according to claim 8, It is characterized in that The forming of a first passivation layer and a second doping layer in a second area of ​​the backlight surface of the substrate comprises: forming a passivation material layer on the second area of ​​the backlight surface, the first side surface of the isolation structure, and the isolation structure and the first doped layer on a side away from the substrate; forming a doping material layer on a side of the passivation material layer away from the substrate; The passivation material layer and the doping material layer located in the second region are removed to form the first passivation layer and the second doping layer.

12. The method for preparing a solar cell according to claim 8, It is characterized in that The method further comprises: forming a second passivation layer on the light-receiving surface of the substrate; An anti-reflection layer is formed on a side of the second passivation layer away from the substrate.

13. A photovoltaic module, It is characterized in that The invention comprises at least one battery string, wherein the battery string comprises at least two solar cells according to any one of claims 1 to 7, or the battery string comprises at least two solar cells manufactured by the method for manufacturing a solar cell according to any one of claims 8 to 12.

14. A photovoltaic system, It is characterized in that Comprising the photovoltaic module as claimed in claim 13.

Citation Information

Cited By

  • Back contact BC solar cell structure and preparation method thereof

    CN119767854A

  • Back contact bc solar cell structure and method of manufacturing the same

    CN119767854B

  • Solar cell, photovoltaic module and preparation method of solar cell

    CN119836054A

  • Back contact cell, photovoltaic module and preparation method

    CN120835619A

  • Back contact cells, photovoltaic modules and methods of manufacture

    CN120835619B