Fluorescent component, manufacturing method thereof, and light-emitting device
By using water-impregnation pressurized sintering method of magnesium oxide and magnesium hydroxide matrix, high thermal conductivity fluorescent components were prepared, which solved the problem of deterioration of phosphor particles and insufficient thermal conductivity in high-temperature sintering. It is suitable for high-power LED and laser excitation illumination.
Patent Information
- Application Number
- CN202080005111.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-07-22
- Filing Date
- 2020-07-22
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-07-22
AI Technical Summary
The existing fluorescent components deteriorate during high-temperature sintering, and the thermal conductivity is insufficient, making it difficult to apply to high-power LED and laser excitation illumination.
A matrix containing magnesium oxide and magnesium hydroxide as the main components is used, and a fluorescent component with a thermal conductivity higher than 5W/(m·K) is prepared by water immersion and pressurized sintering method to avoid high temperature processes.
Fluorescent components that do not require high-temperature sintering processes but have good thermal conductivity and fluorescent characteristics have been realized, which significantly increases the scope of application of phosphor particles and solves the problems of deterioration of phosphor particles and insufficient thermal conductivity.
Smart Images

Figure CN114144497B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a fluorescent component and a method for manufacturing the same. In addition, the present invention also relates to a semiconductor light emitting element and a light emitting device including the fluorescent component. Background Art
[0002] Light-emitting devices equipped with semiconductor light-emitting elements such as light-emitting diodes (LEDs) or laser diodes (LDs) have excellent characteristics of low power consumption and long life, and are used in lighting equipment, backlights of liquid crystal display devices, or light sources of laser devices. Among these LEDs, white light LEDs have been widely and increasingly used as alternative lighting elements to fluorescent lamps.
[0003] As is known to all, white light LED emits white light by combining a light-emitting diode as the main light source with a fluorescent component. As the fluorescent component, a molding material in which phosphor particles are dispersed in a resin is developed. The use of resin as the matrix of the fluorescent component has excellent moldability. However, the heat generated by the light-emitting diode as the main light source and the heat generated by the energy conversion loss of the fluorescent component during the excitation-emission process can easily cause high temperatures, leading to the problem of degradation of the resin (matrix) with low thermal conductivity and low heat resistance. This problem is particularly serious when using high-power LEDs or high-power lasers.
[0004] Therefore, as a matrix for dispersing phosphor particles, phosphor dispersed glass in which phosphor particles are dispersed in glass with excellent heat resistance instead of resin, and phosphor dispersed YAG ceramic in which yellow phosphor Ce:YAG phosphor particles are dispersed in transparent YAG ceramic have been reported. In addition, phosphor dispersed Sialon ceramic in which phosphor particles are dispersed in a matrix composed of Sialon compounds has been proposed (Patent Document 1). In addition, a wavelength conversion component in which inorganic phosphor particles are dispersed in magnesium oxide has been proposed (Patent Document 2). In addition, attempts have been made to fluoresce the entire plate.
[0005] Although not an example of application to fluorescent components, a method of sintering ceramics using a “low temperature sintering” method has been reported, and this method will be described in the “Solution to the Problem” section below (Non-Patent Documents 1 to 5).
[0006] Citation List
[0007] Patent Literature
[0008] Patent Document 1: International Patent Publication WO2018 / 38259
[0009] Patent Document 2: Japanese Unexamined Patent Application Publication No. 2018-180271
[0010] Non-patent literature
[0011] Non-patent literature 1: Journal of the American Ceramic Society - Shnjer and Koy, MWSHAFER et al., Vol. 42, No. 11, November 1959
[0012] Non-patent document 2: J. Am. Ceram. Soc., Clive A. Randall et al., 99
[11] 3489-3507, 2016
[0013] Non-patent literature 3: J. Am. Ceram. Soc., Clive A. Randall et al., 100: 546-553, 2017.
[0014] Non-patent document 4: J. Am. Ceram. Soc., Clive A. Randall et al., 100: 669-677, 2017
[0015] Non-patent literature 5: Journal of Power Source, Sun Xueliang et al., 393:193-203, 2018 Summary of the invention
[0016] Technical issues
[0017] The above-mentioned method of fluorescing the entire board requires high-temperature sintering, so there is a problem that the types that can be densified are limited. According to the method disclosed in Patent Document 2, a temperature of 1000 to 1400°C is cited as the sintering temperature. In addition, the fluorescent component using Sialon as the matrix requires a high-temperature sintering process of, for example, 1000 to 1500°C to densify the matrix. The problem is that the dispersed phosphor particles are easily degraded in such a high-temperature process. In addition, it is necessary to exclude the combination of the matrix and the phosphor particles reacting at high temperatures, which limits the scope of application of the phosphor particles. At the same time, fluorescent components with glass as the matrix can be made at relatively low temperatures. However, due to the low thermal conductivity of glass itself, such fluorescent components are difficult to use in the above-mentioned high-power LED and laser excitation lighting.
[0018] Nowadays, there are many demands for light-emitting devices for high-power applications. As mentioned above, it is hoped that fluorescent components with excellent thermal conductivity can be developed to effectively dissipate the heat generated by the temperature rise of the light-emitting diode or laser diode itself, as well as the heat generated by the energy conversion loss during the excitation-emission process.
[0019] It should be noted that although the above describes the problems with white light LEDs, the same problems may also occur with general fluorescent components.
[0020] The present invention is proposed in view of the above situation, and its purpose is to provide a fluorescent component that does not require a high-temperature sintering process (a high-temperature process with a temperature higher than 250°C) while having satisfactory thermal conductivity and fluorescent properties, and to provide a method for manufacturing such a fluorescent component and a light-emitting device using such a fluorescent component.
[0021] Solutions to the problem
[0022] [1]: A fluorescent component, which is composed of a sintered body for wavelength conversion, the sintered body containing: a matrix containing magnesium oxide and magnesium hydroxide as main components; and fluorescent powder particles dispersed in the matrix.
[0023] [2]: The fluorescent component described in item [1] has a thermal conductivity of 5 W / (m·K) or more.
[0024] [3]: The fluorescent component described in item [1] or [2], wherein the mass ratio of magnesium hydroxide to magnesium oxide in the matrix is less than 0.4.
[0025] [4]: The fluorescent component according to any one of items [1] to [3], wherein the fluorescent powder particles contain nitride fluorescent powder particles.
[0026] [5]: The fluorescent component according to any one of items [1] to [4], wherein the relative density of the fluorescent component is 85% or more.
[0027] [6]: The fluorescent component described in any one of items [1] to [5], wherein the sintered body is obtained by the following method:
[0028] A preform is obtained which is made of at least a mixture of matrix raw material powder and phosphor particles; the preform is impregnated with water and then sintered under pressure. For the preform impregnated with water, a high temperature process higher than 250°C is not required to obtain a sintered body.
[0029] [7]: The fluorescent component according to item [6], wherein the average particle size of magnesium oxide in the matrix obtained by the intercept method of ISO 13383-1:2012 is 0.1 μm to 10 μm.
[0030] [8]: A light emitting device comprising:
[0031] A semiconductor light emitting element capable of emitting a first light; and a fluorescent component according to any one of items [1] to [7], which is arranged on the light emitting side of the semiconductor light emitting element and emits a second light by using the first light as excitation light.
[0032] [9]: A method for manufacturing a fluorescent component, comprising:
[0033] The raw material powder of at least one matrix and phosphor particles are mixed to obtain a mixture; the mixture is preformed to obtain a preform; a sintered body is obtained by impregnating the preform with water and then sintering the preform under pressure, wherein the method does not require sintering the preform at a high temperature exceeding 250°C, and the matrix has magnesium oxide and magnesium hydroxide as main components.
[0034]
[10] : The method for producing a fluorescent component according to item [9], wherein the average particle size of magnesium oxide as a raw material powder is greater than or equal to 20 nm, and the average particle size is obtained from the specific surface area and the density.
[0035] Advantageous Effects of the Invention
[0036] According to the present invention, a fluorescent component that does not require a high-temperature sintering process (a high-temperature process with a temperature higher than 250°C) but has satisfactory thermal conductivity and satisfactory fluorescent properties can be provided, and a method for manufacturing such a fluorescent component and a light-emitting device using such a fluorescent component can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 is a cross-sectional schematic diagram of a light emitting device according to an embodiment of the present invention;
[0038] Figure 2 is a cross-sectional schematic diagram of a light emitting device according to an improved embodiment of the present invention;
[0039] Figure 3A is a SEM image of the preform of Experimental Example A;
[0040] Figure 3B is a SEM image of the sintered body of Experimental Example A;
[0041] Figure 3C is a SEM image of the sintered body of Comparative Example 1;
[0042] Figure 4 is a SEM image of the fluorescent component of Experimental Example 1b;
[0043] Figure 5 is the X-ray analysis result of the sintered body of Experimental Example A;
[0044] Figure 6 are the fluorescence spectra of the fluorescent components of Example 1a and Comparative Example 2;
[0045] Figure 7 is the fluorescence spectrum of the fluorescent component of Example 2b;
[0046] Figure 8 is the fluorescence spectrum of the fluorescent component of Example 3b;
[0047] Fig. 9is a scanning transmission electron microscope (STEM) image of Example 1b;
[0048] Fig.10 is the oxygen spectrum of Example 1b. DETAILED DESCRIPTION
[0049] Embodiments of the present invention will be described below. It should be noted that other embodiments are also included in the scope of the present invention as long as they meet the purpose of the present invention. In addition, the numerical values specified in this specification are determined by the methods disclosed in the embodiments or embodiments. In order to make the description clear, the following description and drawings are appropriately simplified. In addition, for matters necessary for the implementation of the present invention but not particularly described in this specification, those skilled in the art can understand based on the relevant technology in the art.
[0050] [Fluorescent parts]
[0051] The fluorescent component of this embodiment includes a sintered body for wavelength conversion, which contains a matrix with magnesium oxide and magnesium hydroxide as main components, and phosphor particles dispersed in the matrix. The shape of the fluorescent component can be disc-shaped, flat, convex lens-shaped, concave lens-shaped, spherical, hemispherical, cube-shaped, rectangular, columnar such as square column or cylinder, or tubular such as square cylinder or cylinder. When the present invention is applied to white light LED, the fluorescent component of the present invention can be set on the emission light side of the blue light LED as the excitation light source for use.
[0052] In the fluorescent component, the fluorescent powder particles absorb at least a part of the first light emitted from the semiconductor light-emitting element as the excitation light and emit the second light. The fluorescent powder particles in this specification include not only particles that generate fluorescence, but also particles that generate phosphorescence. The first light refers to light with a specific wavelength or light of a specific wavelength band, and the first light can be composed of one type of light or multiple types of light. An example of the first light being composed of multiple types of light is that the light-emitting device includes a semiconductor light-emitting element that emits blue light as the first light and a semiconductor light-emitting element that emits ultraviolet light as the first light. The second light refers to the light emitted from the fluorescent powder particles because at least a part of the first light becomes the excitation light of the fluorescent powder particles. The second light can also be composed of one type of light or multiple types of light. An example of the second light being composed of multiple types of light is that multiple types of fluorescent powder particles with different emission wavelength bands are dispersed in the same fluorescent component. In addition, another example is that the fluorescent powder particles with different emission wavelength bands are dispersed in different fluorescent components respectively.
[0053] For example, when a fluorescent component is used to obtain white light, the fluorescent component contains fluorescent powder particles that emit red light by using blue light as excitation light and fluorescent powder particles that emit green light by using blue light as excitation light. In addition, the fluorescent component should have transmissivity, that is, transmit blue light that is not used as excitation light. In this way, the blue light transmitted by the fluorescent component is mixed with the red light and green light emitted from the fluorescent component to obtain white light.
[0054] In another example, the fluorescent component contains fluorescent powder particles that emit blue light when ultraviolet or purple light is used as excitation light, fluorescent powder particles that emit red light when ultraviolet or purple light is used as excitation light, and fluorescent powder particles that emit green light when ultraviolet or purple light is used as excitation light. In this way, the blue light, red light, and green light emitted from the fluorescent component are mixed with each other, and according to this embodiment, white light can be obtained through the fluorescent component. In this case, in addition to the case where a part of the excitation light is transmitted through the fluorescent component, it can also be designed that all the excitation light is absorbed by the fluorescent component.
[0055] In the fluorescent component of this embodiment, it is preferred that the phosphor particles are evenly dispersed throughout the fluorescent component so that the generated fluorescence is uniform and the total transmittance of the excitation light is uniform. In this way, the excitation light transmitted through the fluorescent component and the fluorescence generated from the fluorescent component are mixed with each other, and the color of the emitted light of the fluorescent component can be easily adjusted. In addition, the distribution of the phosphor particles can have a concentration gradient, or a fluorescent component with different phosphor particles in different regions can be used, and such a fluorescent component can be easily obtained by changing the process during the manufacturing process. Different types of fluorescent components can also be connected to each other.
[0056] A preferred example of the thickness of the fluorescent member may vary depending on its application, and may be, for example, 100 μm or more. An optical film may be provided on at least one of the incident surface side and the emission surface side of the fluorescent member. For example, an antireflection film may be provided as the optical film.
[0057] According to the fluorescent component of this embodiment, a fluorescent component as described below can be obtained without a high temperature sintering process (a high temperature process exceeding 250° C.). Therefore, the degradation problem of fluorescent powder particles can be fundamentally solved, and the types of fluorescent powder particles that can be used can be significantly increased. A fluorescent component for wavelength conversion with excellent fluorescent characteristics can be provided.
[0058] (Matrix)
[0059] In this specification, the matrix refers to the components in the fluorescent component except the phosphor particles and the components with a very small content (i.e., less than 1% by mass), and may also include additives that can be added optionally. In addition, the main component refers to the component containing more than 90% by mass in the matrix. In the present embodiment, magnesium oxide and magnesium hydroxide are the main components of the matrix. Any proportion of magnesium oxide and magnesium hydroxide is acceptable. In addition to the main components, other components include sodium chloride (NaCl), zinc oxide (ZnO), barium titanate (BaTiO3) and calcium carbonate (CaCO3). In addition, a dispersant may also be added.
[0060] The mass ratio of magnesium hydroxide to magnesium oxide in the fluorescent component matrix of this embodiment ([magnesium hydroxide] / [magnesium oxide]) can be appropriately designed according to the application situation. However, in order to effectively improve the thermal conductivity, the mass ratio is preferably less than 0.4, more preferably less than 0.3, and more preferably less than 0.25. The lower limit of the mass ratio of magnesium hydroxide to magnesium oxide is not limited to any specific ratio, as long as the fluorescent component can be densified, but the lower limit of the ratio is preferably greater than 0.1, so that the densification process can be easily performed at low temperatures.
[0061] There is no particular restriction on the average particle size of magnesium oxide in the matrix, but from the perspective of thermal conductivity, the average particle size is preferably 0.1 μm to 10 μm. The average particle size of magnesium oxide in the matrix is obtained by measuring as described below by the linear intercept method or a similar method in accordance with the provisions of ISO13383-1:2012. That is, the observation surface is mirror polished and plasma etched to make the crystal particles on the observation surface clear, and then a microscopic structure photograph of the crystal particles is obtained by scanning electron microscopy. Draw a straight line on the obtained micrograph, and measure the distance between the intersection of the straight line and the particle interface as the particle diameter. Repeat this measurement of the particle diameter, and take the average value of the obtained values as the average particle size of magnesium oxide.
[0062] It should be noted that when resin is used as the matrix of the fluorescent component, its thermal conductivity is about 0.1 W / (m·K), while when glass is used, its thermal conductivity is about 1 W / (m·K). The fluorescent component of this embodiment, in which a matrix containing magnesium oxide and magnesium hydroxide as main components is used, can greatly improve its thermal conductivity. By optimizing the manufacturing process of the fluorescent component, it is easy to achieve a thermal conductivity of more than 5 W / (m·K).
[0063] The thermal conductivity of the fluorescent component of this embodiment is preferably 5W / (m·K) or more, more preferably 6W / (m·K) or more, and in order to further improve the thermal conductivity, it is more preferably 8W / (m·K) or more. Although the upper limit of the thermal conductivity is not limited, for a matrix with magnesium oxide and magnesium hydroxide as the main components, the thermal conductivity is theoretically below 50W / (m·K). By changing the process and thus controlling the heat conduction path, a higher thermal conductivity can be obtained. It should be noted that the thermal conductivity in this specification refers to the thermal conductivity of the fluorescent component measured according to JIS R1611, and in particular refers to the value measured by the method described in the embodiment.
[0064] (Phosphor particles)
[0065] According to the present embodiment, sintering can be performed at room temperature without heating as described later, so any type of phosphor particles can be used, such as β-SiAlON phosphor, KSF-based phosphor (K2SiF6:Mn), CASN, S-CASN, cerium-activated yttrium aluminum garnet (YAG)-based phosphor, cerium-activated lutetium aluminum garnet (LAG)-based phosphor, europium and / or chromium-activated nitrogen-containing calcium aluminum silicate (CaO-Al2O3-SiO2)-based phosphor, and europium-activated silicate ((Sr,Ba)2SiO4)-based phosphor. In order to suppress the decrease in luminous intensity caused by the temperature rise caused by laser excitation, etc., nitride phosphor particles are preferred. Examples of nitride phosphor particles include α-SiAlON phosphor, β-SiAlON phosphor, CASN, S-CASN, etc.
[0066] The phosphor particles are preferably nitride phosphor particles containing nitrogen in their phosphor components. Specific examples include nitride phosphors containing strontium and silicon in the crystal phase (such as SCASN and Sr2Si5N8), nitride phosphors containing calcium and silicon in the crystal phase (such as SCASN, CASN and CASON), nitride phosphors containing strontium, silicon and aluminum in the crystal phase (such as SCASN and Sr2Si5N8), nitride phosphors containing barium and silicon in the crystal phase (such as BSON), and nitride phosphors containing calcium, silicon and aluminum in the crystal phase (such as SCASN, CASN and CASON).
[0067] Another aspect of the classification of nitride phosphors includes lanthanum silicate nitride (such as LSN), alkaline earth metal nitride silicate (such as Sr2Si5N8), alkaline earth metal nitride silicate (CASN, SCASN, α-SiAlON and (Ca,Sr)AlSi4N7), etc.
[0068] More specifically, for example, the phosphor β-SiAlON can be represented by the following general formula:
[0069] Si 6-zAl z O z N 8-z :Eu(where 0 <z<4.2),α-SiAlON
[0070] LSN is represented by the following general formula: x Si6N y M z [1]
[0071] (In formula [1], Ln represents one or more elements selected from rare earth elements other than the activation element, and M represents one or more elements selected from the activation elements. In addition, x, y and z are values that independently satisfy the following formula:
[0072] 2.7≤x≤3.3,10≤y≤12,0 <z≤1.0)
[0073] CASN can be represented by the following general formula: CaAlSiN3:Eu;
[0074] SCASN can be represented by the following general formula: (Ca, Sr, Ba, Mg)AlSiN3:Eu and / or (Ca, Sr, Ba)AlSi(N, O)3:Eu;
[0075] CASON can be represented by the following general formula: (CaAlSiN3) 1-x (Si2N2O) x :Eu(0 <x<0.5);
[0076] CaAlSi4N7 can be represented by the following general formula: Euy(Sr,Ca,Ba)1-y:Al 1+x Si 4-x O x N 7-x (where 0≤x<4, 0≤y<0.2);
[0077] Sr2Si5N8 can be represented by the following general formula: (Sr,Ca,Ba)2Al x Si 5-x O x N 8-x :Eu(where 0≤x≤2);
[0078] BSON can be represented by the following general formula: x Ba y (Sr,Ca,Mg,Zn) z L6O 12N2 (wherein M represents an activating element selected from Cr, Mn, Fe and lanthanide elements (excluding La, Pm, Gd and Lu), L represents a metal element belonging to Group 4 or Group 14 of the periodic table and Si. In addition, x, y and z are values that independently satisfy the following formula:
[0079] 0.03≤x≤0.9,0.9≤y≤2.95,x+y+z=3)
[0080] Among these phosphors, in order to prevent the brightness from decreasing during sintering, it is best to use oxygen-free nitride phosphors (including the necessary oxygen), that is, nitride phosphors such as LSN, CaAlSiN3, SCASN, Sr2Si5N8, β-SiAlON, and BSON.
[0081] The type of phosphor particles to be added is not particularly limited, and various types of phosphor particles can be added according to the application.
[0082] The content of phosphor particles in the fluorescent component can be appropriately adjusted according to the shape (thickness, etc.), transparency (total transmittance of the excitation light), and fluorescence characteristics (fluorescence intensity, emission wavelength) required by the fluorescent component.
[0083] The average particle size of the phosphor particles in the matrix is not particularly limited, but in order to obtain good excitation light transmittance, good fluorescence characteristics and excellent dispersibility, the average particle size is preferably 500nm to 30μm, more preferably 1μm to 10μm. According to ISO13383-1:2012, the average particle size of the phosphor particles in the matrix is determined by the linear intercept method. The specific measurement method is the same as that of magnesium oxide.
[0084] [Method for producing fluorescent component]
[0085] Next, a method for manufacturing a fluorescent member will be described by way of example, but the method for manufacturing a fluorescent member of the present invention is not limited to the following.
[0086] The manufacturing method of the fluorescent component of this embodiment includes the following steps: mixing at least fluorescent powder particles and raw material powder of the matrix to obtain a mixture; preforming the mixture into a preform; impregnating the preform with water, and then sintering the preform under pressure to obtain a sintered body. The manufacturing method of this embodiment can manufacture a fluorescent component with excellent thermal conductivity and fluorescent properties without high-temperature processing at a temperature higher than 250°C.
[0087] Sintering in this specification refers to the phenomenon of reducing the surface area of the powder, and refers to a method of obtaining a preform, impregnating it with water, and then pressurizing and sintering it at a temperature below 250°C to fix it as a fluorescent component (hereinafter also referred to as "low-temperature sintering"). It is synonymous with the so-called cold sintering. By performing low-temperature sintering, as described later, the water (liquid phase) in which the preform is impregnated is introduced into the particle-particle interface, and the particles are uniformly expanded with an appropriate amount of water. Then, under pressure, the diffusion of the substance in the liquid phase is promoted, and part of the magnesium oxide reacts with water to form magnesium hydroxide, thereby obtaining a dense ceramic. Here, the lower limit of the sintering temperature is not limited to any specific temperature, but is preferably room temperature. The preform in this specification refers to a molding process from an amorphous state such as a granular state to a solid state with a fixed shape by pressurization or the like. For example, a solid form formed into a certain shape by pressurization should refer to a molded body before impregnation with water. It should be noted that the formation process of the preform can be carried out at a temperature higher than 250°C. In addition, in the process of obtaining the preform, the particles are in point contact, and the surface area does not change significantly. Therefore, the "sintering" mentioned in this specification refers to the process after impregnation with water, and does not include the process of forming a preform. The manufacturing method will be described in detail below.
[0088] First, weigh and mix the raw material powder and phosphor particles. The average particle size calculated from the specific surface area S and density ρ of the raw material powder magnesium oxide using the formula 6 / (S·ρ) is preferably 20 to 1000 nm, more preferably 30 to 800 nm, and more preferably 40 to 700 nm. The specific surface area is measured according to ISO9277. By adjusting the average particle size of the raw material powder magnesium oxide to within the range of 20 to 1000 nm, excellent thermal conductivity and mechanical properties can be obtained at the same time. The raw material powder of the matrix can use magnesium oxide of a variety of different average particle sizes in order to more effectively promote density. For example, the density can be improved by using second particles of relatively smaller size to fill the gaps formed between the first particles.
[0089] Although the average particle size of the phosphor particles is not particularly limited within the scope of the present invention, in order to obtain satisfactory light transmittance, dispersibility and fluorescence in a balanced manner, the average particle size is preferably 500nm to 30μm, more preferably 1μm to 10μm. The average particle size of the phosphor particles of this embodiment is calculated from the specific surface area and density.
[0090] The mixing ratio of the raw material powder forming the matrix and the phosphor particles is not particularly limited and is appropriately adjusted according to the required transparency and fluorescent characteristics of the fluorescent component. When the content of the raw material powder forming the matrix is 100 vol%, the content of the phosphor particles is 0.1 to 30 vol%, preferably 0.5 to 20 vol%, and more preferably 1 to 15 vol%, in consideration of compactness. The total transmittance of the excitation light of the fluorescent component in the optical path direction is preferably 10% or more.
[0091] The raw material powder of the matrix and the phosphor particles can be subjected to a pulverization process or / and a decomposition process independently before mixing. The raw material powder and at least one phosphor particle are weighed to obtain a predetermined molar ratio. Additives can be added within a range that does not affect the formation of the fluorescent component matrix. Additives include magnesium chloride, hydrochloric acid, acetic acid, ammonia water, etc. By using at least magnesium oxide as a raw material powder, and impregnating a preform containing magnesium oxide and phosphor particles with water, and then sintering at a low temperature, magnesium hydroxide is obtained by the reaction between magnesium oxide and water.
[0092] The method for obtaining the mixture is not particularly limited, and for example, the mixture may be obtained by a dry method or / and a wet method. Taking the dry process as an example, the raw materials are put into a mortar for mixing, and at this time, a dispersant may be added. In order to make the particle size of the powder of the mixture uniform, two or more sieves with different mesh sizes may be used in stages so that the mixture has a predetermined particle size.
[0093] The preform can be formed after obtaining the mixture, or it can be formed simultaneously with the step of obtaining the mixture. In the case of mixing by a wet process, a slurry can be prepared by mixing with a solvent (such as ethanol or the like) by a ball mill or similar equipment, and then the solvent is removed to obtain a mixture and a preform at the same time. In this case, further preforming can be performed by pressure or a similar method. For the preforming method, the existing methods can be used without restriction. For example, the mixture is filled into a mold and a preform is obtained by pressurization. The pressurization can be isotropic or anisotropic (for example, pressurization in a uniaxial direction). In addition, the mixture can be heated. In order to prevent degradation of the phosphor particles, when the mixture is heated, the heating temperature is preferably below 250°C. In order to simplify the equipment, the heating is more preferably carried out at room temperature by cold isostatic pressing or a similar method. In order to obtain high-quality fluorescent components, it is preferred to pressurize the preform so that its internal structure is uniform in the preforming stage. In order to make the internal structure uniform, the aggregation and cracking of the raw material powder and the process conditions of preforming (pressurization conditions, etc.) are important.
[0094] Taking the preform as an example, uniaxial pressure molding is performed at a pressure of 50 MPa for 30 seconds to obtain a preform; the preform is chamfered and then packed into a vacuum packaging bag; and then cold isostatic pressing (CIP: Cold Isostatic Pressing) is performed at a pressure of 200 MPa for 1 minute, once or multiple times. In order to make the internal structure of the preform uniform, the maximum pressure of the preform is preferably 5 to 1000 MPa, more preferably 200 to 1000 MPa, and more preferably 500 to 1000 MPa.
[0095] The preform is then impregnated with water. The water may contain additives without prejudice to the purpose of the present invention, and the additives may be neutral, acidic or alkaline. The water may be added under normal pressure, or under vacuum or reduced pressure. Adding water under vacuum or reduced pressure allows the water to be evenly distributed (or diffused) in a short period of time. This method is particularly effective when the preform is thick.
[0096] The amount of water added should be enough to fill the voids in the preform, and the optimal amount of water may vary depending on the relative density of the preform. The material movement can also be promoted by adjusting the process temperature of the low-temperature sintering performed in the next step, so the optimal amount of water added may also vary according to the change of the process temperature. The amount of water required to achieve the densification of the fluorescent component can be defined as its upper limit. For example, when the preform is 100% by mass, the amount of water added can be 1 to 20% by mass.
[0097] After the preform is impregnated with water, it is sintered at low temperature under pressure to obtain a sintered body. The magnesium ions of magnesium oxide in the preform are dissolved by water immersion, and the material transfer of magnesium ions is promoted through the liquid phase under pressure, so that the dissolved ions are precipitated as magnesium hydroxide or magnesium oxide, which can achieve the densification of the fluorescent component. Therefore, there must be sufficient pressure to promote material transfer through the liquid phase. In order to achieve sufficient densification, the maximum pressure is preferably 200-1500MPa, more preferably 300-1200MPa, and more preferably 500-1000MPa. By adjusting the pressure to 200-1500MPa, it is possible to promote the dissolution and precipitation of particles constituting the matrix part into the liquid phase without high-temperature sintering, promote plastic deformation and produce high density. As a means of applying pressure, any known method can be used. The pressurization method by isostatic pressing is particularly preferred because it can achieve isotropic pressurization. The pressurization time depends on the chemical reaction mechanism and pressure that contribute to densification, but it is preferably 1-60min.
[0098] In the case of sintering at room temperature, there is a method for obtaining a sintered body, that is, after impregnating the preform with water, putting it into a vacuum packaging bag, and using a cold isostatic pressing device to perform CIP molding at a pressure of 1000 MPa for 60 minutes once or more, thereby obtaining a sintered body. In addition, when the preform is heated, a WIP hot isostatic pressing (WIP: Warm Isostatic Pressing) device can be used to mold the sintered body.
[0099] In consideration of thermal conductivity, it is preferred to adjust the ratio of magnesium oxide to magnesium hydroxide so that the amount of the former is greater than the latter. In addition, in consideration of the densification of the fluorescent component, it is preferred to add a large amount of water so that magnesium hydroxide is generated by the reaction of magnesium oxide and water. Since the densification of the fluorescent component can be promoted by heating, the densification can be promoted by high-temperature treatment at a temperature of 250° C. or less. In order to reduce energy consumption and simplify the device, it is preferred to perform low-temperature sintering at room temperature.
[0100] It should be noted that the above-mentioned manufacturing method is only an example, and the fluorescent component of this embodiment can be manufactured by various manufacturing methods. For example, the fluorescent component can be obtained by obtaining a mixture of fluorescent powder particles, raw material powder containing at least magnesium oxide, and ice particles, and then pre-forming at a temperature below the freezing point, and then performing the above-mentioned low-temperature sintering, or performing the above-mentioned low-temperature sintering without pre-forming. Furthermore, the fluorescent component can also be obtained by combining a freeze-drying method and a low-temperature sintering method. Specifically, a mixture of fluorescent powder particles, raw material powder containing at least magnesium oxide, water and a solvent with a sublimation point lower than that of water (such as methanol, etc.) can be obtained, and by freeze-drying, the mixture can be sprayed with a sprayer to form droplets, and particles with the solvent removed and residual water can be obtained, and the particles are subjected to the above-mentioned low-temperature sintering, thereby obtaining the fluorescent component.
[0101] In order to effectively improve the luminous efficiency, the relative density of the fluorescent component is preferably 85% or more. Here, the relative density refers to the value obtained by dividing the density of the fluorescent component measured by the Archimedean method specified in JIS Z2501:2000 by the true density of the raw material powder of the matrix (excluding the fluorescent powder particles) (expressed as a mass ratio). The relative density of the fluorescent component is more preferably 88% or more, and more preferably 90% or more.
[0102] According to this embodiment, it is possible to promote solid-liquid reaction by promoting material transfer in the solid without high-temperature sintering, thereby obtaining a highly dense fluorescent component containing phosphor particles. Due to the density, the pores can be reduced, so that a fluorescent component with excellent light transmittance can be provided. In addition, by using magnesium oxide as a matrix component, high thermal conductivity can be achieved. In addition, since this method does not require high-temperature sintering above 250°C, various types of phosphor particles can be used. It is possible to fundamentally solve traditional problems such as degradation and change of phosphor particles due to high-temperature sintering and undesirable reactions with the matrix part, and more flexible material design becomes possible. Therefore, a high-quality phosphor component can be provided. In addition, a fluorescent component having both high thermal conductivity and satisfactory fluorescent characteristics can be provided. The fluorescent component of this embodiment can be widely used not only in high-power LEDs, etc., but also in various other types of components.
[0103] [Light-emitting device]
[0104] The light emitting device of the present embodiment includes a semiconductor light emitting element that emits a first light and a fluorescent component of the present embodiment, the fluorescent component is located on the light emitting side of the semiconductor light emitting element and emits a second light by using the first light as an excitation light. In the light emitting device, at least one or more semiconductor light emitting elements and at least one or more fluorescent components are included.
[0105] Figure 1 1 is a schematic diagram of a light-emitting device of a white light LED of the present embodiment. In the white light LED 10, a blue light LED 2 as a main light source is arranged on a substrate 1, and a fluorescent component 5 is arranged on at least a part of the light emission path of the blue light LED 2. The fluorescent component 5 can be formed into any shape according to the shape of the blue light LED 2. A part of the emission light of the blue light LED 2 excites the fluorescent powder particles 4, such as yellow fluorescent powder particles, dispersed in the matrix 3 of the fluorescent component 5, and emits yellow light. In addition, a part of the light emitted by the blue light LED 2 that does not contribute to the excitation of the fluorescent powder particles in the fluorescent component passes through the fluorescent component 5 and is emitted from the white light LED 10 in the form of blue light. Since a plurality of emission lights are mixed with each other, white light is generated from the white light LED 10.
[0106] It should be noted that Figure 1 The example shown is only an example, and the fluorescent component can use red LED or / and green LED instead of blue LED or in combination with blue LED to improve the color quality of white light. In addition, yellow phosphor particles are only an example, and red phosphor particles or / and green phosphor particles can replace yellow phosphor particles or be used in combination with yellow phosphor particles. Of course, phosphor particles of other colors can also be used. In addition, it goes without saying that semiconductor light-emitting devices such as laser diodes can be used instead of LEDs.
[0107] In the case of the white light LED 10, in order to optimize the amount of blue light of the blue light LED 2 penetrating the fluorescent component 5 and the amount of light of another wavelength (green light, red light, etc.) absorbed by the phosphor particles of the fluorescent component 5, the thickness of the fluorescent component 5 and the concentration of the phosphor particles in the fluorescent component 5 can be designed accordingly. The excitation light of the blue light LED is, for example, light with a wavelength of 300nm to 500nm (light in the ultraviolet range to light in the blue range).
[0108] like Figure 2 As shown, in order to replace Figure 1 The fluorescent component 5 of the white light LED 10 can be formed by a fluorescent component 20 composed of a first fluorescent component 21 and a second fluorescent component 22. The first fluorescent component 21 contains first fluorescent powder particles 12 in the first matrix 11, and the first fluorescent powder particles 12 absorb the first light from the blue light LED 2 and emit light. At the same time, the second fluorescent component 22 contains second fluorescent powder particles 14 in the second matrix 13, and the second fluorescent powder particles 14 absorb the light emitted from the first fluorescent component 21 and emit light with a longer wavelength. By connecting the first fluorescent component 21 and the second fluorescent component 22 together, a part of the light emitted by the fluorescent component 20 can be used as the second excitation light to emit light with a longer wavelength. Through this configuration, the color of white can also be adjusted.
[0109] Example
[0110] The present invention will be described in more detail below by way of examples. However, the present invention is not limited to the examples described below.
[0111] [Experimental Example A] (Densification of the matrix)
[0112] DISPERMAG (registered trademark) TN-1 (average particle size 0.57 μm, manufactured by Tateho Chemical Industry Co., Ltd.) and PUREMAG (registered trademark) FNM-G (average particle size 0.54 μm, manufactured by Tateho Chemical Industry Co., Ltd.) were weighed as raw material MgO powders at a mass ratio of 7:3 and mixed using a mixer to obtain a mixture of base powders. 1 g of the base powder mixture was charged into a cylindrical stainless steel mold having a diameter of 15 mm, and primary molding was performed for 30 seconds at a pressure of 50 MPa using a uniaxial press molding machine (product name: hydraulic workshop press, manufactured by Woodward Fab Co., Ltd.) to obtain a preform.
[0113] Then, an isostatic pressure of 1000 MPa was applied at room temperature for 1 minute to obtain a preform. The relative density of the preform was 65%. The preform was impregnated with 10% by mass of water under reduced pressure (-0.05 MPa). After that, an isostatic pressure of 1000 MPa was applied at room temperature for 60 minutes using a cold isostatic pressing device (product name: Dr. CHEF, manufactured by Kobe Steel Co., Ltd.), and then a cylindrical sintered body was obtained by low temperature sintering, with a relative density of 96%.
[0114] [Comparative Example 1]
[0115] A sintered body was obtained in the same manner as in Experimental Example A, except that the preform was not impregnated with water. The relative density of the preform was 66%, and the relative density of the sintered body was 66%.
[0116] [Example 1a]
[0117] Red phosphor (Sialon Co., Ltd., CASN) was further added as phosphor particles to the mixture of the base powder of Experimental Example A, and the mixture was fully mixed in the mortar so that the volume ratio of the base raw material powder and the phosphor particles became 99:1, thereby obtaining a mixture containing phosphor particles. 1 g of the mixture containing phosphor particles was loaded into a mold in the same manner as in Experimental Example A, and a preform was formed under the same conditions as in Experimental Example A, and then a fluorescent component as a sintered body was obtained. The relative density of the preform was 65%, and the relative density of the fluorescent component was 92%.
[0118] [Example 1b]
[0119] The fluorescent component of Example 1b was obtained in the same manner as Example 1a, except that the volume ratio of [matrix]:[phosphor particles] was changed to 9: 1. The relative density of the preform was 65%, and the relative density of the fluorescent component was 88%.
[0120] [Example 1c]
[0121] The fluorescent component of Example 1c was obtained by the same method as Example 1a, except that the volume ratio of [matrix]:[phosphor particles] was changed to 8:2.
[0122] [Comparative Example 2]
[0123] The fluorescent component of Comparative Example 2 was obtained in the same manner as in Example 1b, except that the preform was sintered in air at 1300° C. for 1 hour without the process of impregnating the preform with water and the low-temperature sintering process. The relative density of the preform was 66%, and the relative density of the fluorescent component was 69%.
[0124] [Example 2b]
[0125] Orange phosphor (α-SiAlON manufactured by Sialon Co., Ltd.) was mixed with the mixture of Experimental Example A as phosphor particles in a mortar so that the volume ratio of [matrix]:[phosphor particles] was 9:1, thereby obtaining a mixture containing phosphor particles. 1 g of the mixture was loaded into a mold in the same manner as in Experimental Example A, and a preform was formed under the same conditions as in Experimental Example A, and then a fluorescent component as a sintered body was obtained. The relative density of the preform was 67%, and the relative density of the fluorescent component was 92%.
[0126] [Example 2a and Example 2c]
[0127] The fluorescent components of Examples 2a and 2c were obtained in the same manner as in Example 2b, except that the volume ratio of [matrix]:[phosphor particles] was changed to the values shown in Table 1.
[0128] [Example 3a]
[0129] Green phosphor (β-SiAlON manufactured by Sialon Co., Ltd.) was mixed as phosphor particles with the mixture of Experimental Example A in mortar so that the volume ratio of [matrix]:[phosphor particles] was 99:1, thereby obtaining a mixture containing phosphor particles. 1 g of the mixture was charged into a metal mold in the same manner as in Experimental Example A, and a preform was formed under the same conditions as in Experimental Example A, and then a phosphor component as a sintered body was obtained.
[0130] [Example 3b and Example 3c]
[0131] The fluorescent components of Examples 3b and 3c were obtained in the same manner as in Example 3a, except that the volume ratio of [matrix]:[phosphor particles] was changed to the values shown in Table 1.
[0132] [Experimental Example B] (Densification of the matrix)
[0133] RF-10CS (average particle size: 4-10 μm) and 500A (average particle size: 45-60 nm) produced by Ube Materials Co., Ltd. were weighed as MgO raw powders in a mass ratio of 7:3, and mixed thoroughly with a mixer to obtain a mixture of matrix powders. 1 g of the matrix powder mixture was charged into a mold, and a preform was obtained in the same manner as in Experimental Example A. Then, in order to make the internal structure uniform, an isostatic pressure of 200 MPa was applied at room temperature for 1 minute to obtain a preform. The relative density of the preform is 67%. The preform is then immersed in 10 mass % water in the same manner as in Experimental Example A. Thereafter, a cylindrical sintered body was obtained in the same manner as in Experimental Example A. The relative density of the sintered body of Experimental Example B is 91%.
[0134] [Example 4a]
[0135] Red phosphor (CASN manufactured by Sialon Co., Ltd.) was further added to the mixture of Experimental Example B as phosphor particles. The mixture containing the phosphor particles was fully stirred in a mortar so that the volume ratio of the matrix raw material powder and the phosphor particles was 99:1, thereby obtaining a mixture containing phosphor particles. 1 g of the mixture containing the phosphor particles was loaded into a mold in the same manner as in Experimental Example B, and a preform and a fluorescent component were obtained in the same manner as in Experimental Example B. The relative density of the preform was 66%, and the relative density of the fluorescent component was 87%.
[0136] [Example 4b]
[0137] The fluorescent component of Example 4b was obtained in the same manner as Example 4a, except that the volume ratio of [matrix]:[phosphor particles] was changed to 9: 1. The relative density of the preform was 67%, and the relative density of the fluorescent component was 88%.
[0138] [Experimental Example C] (Densification of the matrix)
[0139] RF-10CS (average particle size 4 to 10 μm, manufactured by Ube Material Industries, Ltd.) and DISPERMAG (registered trademark) TN-1 (average particle size 0.57 μm, manufactured by Tateho Chemical Industries Co., Ltd.) were weighed as MgO raw material powders in a mass ratio of 5:5, and mixed thoroughly with a stirrer to obtain a mixture of matrix powders. 1 g of the matrix powder mixture was placed in a mold, and the same method as in Experimental Example A was performed to obtain a preform. Next, in order to make the internal structure uniform, isostatic pressing was applied at 1000 MPa for 1 minute at room temperature to obtain a preform. The relative density of the preform is 73%. The preform was immersed in 10% by mass of water in the same manner as in Experimental Example A, and then a cylindrical sintered body was obtained in the same manner as in Experimental Example A.
[0140] [Example 5a]
[0141] Red phosphor (CASN manufactured by Sialon Co., Ltd.) was further added to the mixture of Experimental Example C as phosphor particles, and the mixture containing the phosphor particles was fully stirred in a mortar so that the volume ratio of the base raw material powder to the phosphor particles was 9:1, thereby obtaining a mixture containing phosphor particles. 1 g of the mixture containing the phosphor particles was loaded into a mold in the same manner as in Experimental Example C, and a preform and a phosphor component as a sintered body were obtained in the same manner as in Experimental Example C.
[0142] [Experimental Example D] (Densification of the matrix)
[0143] 1 g of 500A (average particle diameter 45-60 nm) manufactured by Ube Material Industries, Ltd. was charged into a mold as MgO raw material powder, and a preform was obtained in the same manner as in Experimental Example A. Then, in order to make the internal structure uniform, an isostatic pressure of 200 MPa was applied at room temperature for 1 minute to obtain a preform. The relative density of the preform was 49%. Then, the preform was immersed in 10% by mass water in the same manner as in Experimental Example A. Thereafter, a cylindrical sintered body was obtained in the same manner as in Experimental Example A, and the relative density of the sintered body of Experimental Example D was 85%.
[0144] [Example 6a]
[0145] Red phosphor (CASN manufactured by Sialon) was further added to the mixture of Experimental Example D as phosphor particles. The mixture containing the phosphor particles was fully mixed in the mortar so that the volume ratio of the matrix raw material powder and the phosphor particles became 99:1, thereby obtaining a mixture containing phosphor particles. 1 g of the mixture containing the phosphor particles was loaded into a mold in the same manner as in Experimental Example D, and a preform and a fluorescent component were obtained in the same manner as in Experimental Example D. The relative density of the preform was 47%, and the relative density of the fluorescent component was 80%.
[0146] [Example 6b]
[0147] The fluorescent component of Example 6b was obtained in the same manner as Example 6a, except that the volume ratio of [matrix]:[phosphor particles] was changed to 9: 1. The relative density of the preform was 50%, and the relative density of the fluorescent component was 84%.
[0148] (Comparative Example 3)
[0149] Epoxy resin was used as the matrix instead of the MgO powder as the matrix raw material powder in Example 1a. The same amount of phosphor particles as in Example 1a (the amount of phosphor particles accounting for 1 vol% of the total amount of the mixture containing phosphor particles) was added to the epoxy resin and mixed thoroughly to obtain a mixture containing phosphor particles, which was then melt-kneaded to obtain a fluorescent component of Comparative Example 3 having the same shape as in Example 1a.
[0150] (Comparative Example 4)
[0151] The matrix material powder MgO powder in Example 1b was replaced by epoxy resin as the matrix. The same amount of phosphor particles as in Example 1b was added to the epoxy resin, and the fluorescent component of Comparative Example 4 with the same shape as in Example 1b was obtained by the same method as in Example 3.
[0152] (SEM image)
[0153] The observation surfaces of the preform of Experimental Example A, the sintered bodies of Experimental Example A and Comparative Example 1 (the same sintered bodies as the fluorescent components in the examples, but without phosphor particles) were mirror-polished and plasma-etched to clarify the crystal particles on the observation surface, thereby preparing samples for scanning electron microscope (SEM) observation. Then, the fracture surface was observed using a scanning electron microscope (SEM, product name: JSM-6390LV, manufactured by JEOL Co., Ltd.). Figure 3A is the SEM image of the preform. Figure 3B is the SEM image of the sintered body of Experimental Example A after the low temperature sintering step. Figure 3C This is a SEM image of Comparative Example 1 (a sintered body after low-temperature sintering without the water immersion step).
[0154] The SEM image of the preform without water impregnation process is as follows: Figure 3C As shown, it shows Figure 3A The structure of the preform was the same as that of the preform, and no change in the microstructure due to low-temperature sintering was observed. In addition, as described above, the relative density of the sample of Comparative Example 1 that was not impregnated with water was 66%, compared with the relative density of 65% of the preform, confirming that the relative density had almost no change. At the same time, the relative density of the sintered body of Experimental Example A that was subjected to the water impregnation step was 96%, as shown in FIG. Figure 3B As shown in the figure, it is confirmed that the structure of the preform is more compact. In addition, no particle growth is observed.
[0155] Figure 4 The SEM image of the fluorescent component of Example 1b is shown. Since the sintered body is formed using a mixture containing 10 vol% of phosphor fine particles, its relative density is lower than that of the sintered body of Experimental Example A (a sample manufactured under the same conditions as the fluorescent component of Experimental Example 1b except that the phosphor fine particles are not contained), but it is confirmed by visual inspection that the fluorescent component of Example 1b has a sintered body as dense as that of Experimental Example A.
[0156] (X-ray structural analysis)
[0157] The X-ray structural analysis results of the sintered body of Experimental Example A are as follows: Figure 5 As shown, the sample for X-ray structure analysis was measured using a sample-level multifunctional X-ray diffractometer Ultima IV manufactured by Rigaku Corporation in 2θ / θ mode. Figure 5 As shown, in Experimental Example A, the characteristic peak of magnesium oxide ( Figure 5 The peak in the figure is indicated by a black triangle) and the characteristic peak of magnesium hydroxide ( Figure 5 This peak in the graph is indicated by a black square mark), thus confirming that magnesium oxide and magnesium hydroxide are contained in the matrix of the fluorescent component.
[0158] (Measurement of emission spectrum)
[0159] Figure 6 The emission spectrum of the fluorescent component of Example 1a was measured using a quantum efficiency measurement system QE-2000 (manufactured by Otsuka Electronics Co., Ltd.) in the reflection mode, and in particular, the emission spectrum of 500 nm to 800 nm was measured in the reflection mode using 455 nm excitation light. Figure 6 The emission spectrum of the preform of Example 1a and the emission spectrum of the fluorescent component of Comparative Example 2 are also shown. Figure 6 Compared with the emission spectrum of the preform in Example 1, the fluorescent component of Example 1a has an emission spectrum similar to that of the preform, and an emission spectrum derived from the addition of red phosphor is obtained, which increases the light emission intensity of the fluorescent component of Example 1a. Similar emission spectra are also obtained for the fluorescent components of other embodiments using CASN. At the same time, no emission spectrum is observed in the fluorescent component of Comparative Example 2, so it is confirmed that the phosphor particles therein are inactivated. The emission spectrum of the fluorescent component of Example 2b is as follows Figure 7 As shown, the emission spectrum of the fluorescent component of Example 3b is as follows Figure 8 The measurement method is the same as the above method. The emission spectra of the added phosphors are also shown in these figures. By comparing the emission spectra of each phosphor, it is confirmed that the emission spectra of the fluorescent components of Example 2b and Example 3b are the same.
[0160] (Scanning transmission electron microscopy-energy dispersive X-ray analysis (STEM-EDX))
[0161] In order to observe the cross-sectional structure of the fluorescent component of Example 1b, the large block sample after low temperature sintering was cut into small pieces, and then ground into thin slices using an ion milling device (Model 691 PIPS manufactured by Gatan Co., Ltd.) to prepare a measurement sample. Then, the cross section was observed using an EDX scanning transmission electron microscope (Multi-functional Analytical Transmission Electron Microscope JEM-F200 manufactured by JEOL Co., Ltd.) and oxygen mapping was performed. Fig. 9 For TEM images, Fig.10 is the oxygen spectrum result. Fig. 9 In the MgO samples, there are gaps at the grain boundaries between the MgO particles, and many needle-shaped or plate-shaped particles are observed in the gaps. Fig.10 The EDX surface analysis shown shows that the proportion of oxygen in these grain boundary phases is higher than that in the MgO particles. From these images, it can be confirmed that the gaps between the MgO particles are filled with Mg(OH)2.
[0162] Table 1 shows the results of relative density, average particle size, quantum efficiency and thermal conductivity of each experimental example, each embodiment and each comparative example. The relative density is obtained by dividing the density of the fluorescent component measured by the Archimedean method according to JIS Z2501:2000 by the true density of the raw material powder of the matrix (excluding the phosphor particles). The average particle size of the magnesium oxide in the fluorescent component is determined by the intercept method of ISO13383-1:2012. The quantum efficiency is measured in the reflection mode using the quantum efficiency measurement system QE-2000 (manufactured by Otsuka Electronics Co., Ltd.) with an excitation light wavelength of 455nm. The thermal conductivity is measured for each sample using the laser flash method thermal constant measuring instrument TC-9000 (manufactured by Advance Rico, Inc.) according to JIS R1611.
[0163] [Table 1]
[0164]
[0165] The internal quantum efficiency of Example 1a is 64%, and the internal quantum efficiency of Comparative Example 3 is 52%. In addition, the internal quantum efficiency of Example 1b is 86%, and the internal quantum efficiency of Comparative Example 4 is 81%. As shown in these examples, it is proved that the quantum efficiency of this embodiment is equal to or higher than the quantum efficiency of the related art.
[0166] In addition, the thermal conductivity of Comparative Examples 3 and 4 was measured according to ISO 22007-4 and was 0.1 W / (m·K).
[0167] This application is based on and claims the benefit of priority from Japanese application JP2019-134868 filed on July 22, 2019, and all disclosed contents of that application are incorporated herein in their entirety.
[0168] Industrial Applicability
[0169] The fluorescent component of the present invention can be used not only as a component of a light-emitting device such as a white light LED or a high-power LED, but also can be combined with components of displays such as a vacuum fluorescent display tube (VFD) or a PDP, and can be widely used for various purposes because the fluorescent component has high thermal conductivity and satisfactory fluorescent properties. In addition, the present invention can also be applied to purposes other than fluorescent components for wavelength conversion, such as stress light-emitting elements, electron beam irradiation light-emitting elements, and thermoluminescent elements.
[0170] Description of Reference Numerals
[0171] 1 substrate
[0172] 2 Blue LED
[0173] 3 Matrix
[0174] 4 Phosphor particles
[0175] 5 Fluorescent components
[0176] 10 White LED
[0177] 11. First Matrix
[0178] 12. First phosphor particles
[0179] 13 Second Matrix
[0180] 14 Second phosphor particles
[0181] 21 first fluorescent component
[0182] 22 second fluorescent member
Claims
1. A fluorescent component, comprising a sintered body for wavelength conversion, the sintered body comprising: a matrix with magnesium oxide and magnesium hydroxide as main components, the main components being components that account for 90% or more of the matrix; and fluorescent powder particles dispersed in the matrix; the sintered body is obtained by the following method: A preform is obtained which is made of at least a mixture of matrix raw material powder and phosphor particles, wherein the matrix raw material powder is magnesium oxide; the preform is impregnated with water, and then the preform is sintered under pressure to obtain a sintered body, wherein the sintering temperature is not higher than 250°C and the pressurizing pressure is 200 to 1500 MPa. 2 . The fluorescent component according to claim 1 , which has a thermal conductivity of 5 W / (m·K) or more. 3 . The fluorescent component according to claim 1 , wherein the mass ratio of magnesium hydroxide to magnesium oxide in the matrix is 0.4 or less. The fluorescent component according to claim 1 or 2, wherein the fluorescent powder particles contain nitride fluorescent powder particles.
5. The fluorescent component according to claim 1 or 2, wherein the relative density is 85% or more, wherein the relative density is a value expressed as a mass ratio obtained by dividing the density of the fluorescent component measured by the Archimedean method specified in JIS Z2501:2000 by the true density of the raw material powder of the matrix excluding the fluorescent powder particles. 6 . The fluorescent member according to claim 1 , wherein gaps between the magnesium oxide particles are filled with magnesium hydroxide. 7 . The fluorescent component according to claim 1 , wherein the average particle size of the magnesium oxide in the matrix is 0.1 μm to 10 μm according to the intercept method of ISO 13383-1:2012.
8. A light emitting device, comprising: a semiconductor light emitting element capable of emitting a first light; And the fluorescent member according to any one of claims 1 to 7, which is provided on the light emitting side of the semiconductor light emitting element, and emits the second light by using the first light as the excitation light.
9. A method for manufacturing a fluorescent component, comprising: mixing raw material powder of at least one matrix and phosphor particles to obtain a mixture; The mixture is preformed to obtain a preform, wherein the raw material powder of the matrix is magnesium oxide; the preform is impregnated with water, and then the preform is sintered under pressure at a high temperature not exceeding 250°C to obtain a sintered body, wherein the pressure of the pressurization is 200 to 1500 MPa, and the matrix has magnesium oxide and magnesium hydroxide as main components, and the main components refer to components that contain more than 90% by mass in the matrix.
10. The method for manufacturing a fluorescent component according to claim 9, wherein: The average particle size of magnesium oxide as the raw material powder is 20 nm or more, which is obtained from the specific surface area and the density.