Amorphous precious metal RuO x / Preparation method of ZnO MEMS hydrogen sensor
By synthesizing amorphous precious metal RuOx and ZnO nanosheet composite materials, a hydrogen sensor with high response value and low detection limit is prepared, which solves the problem of insufficient application of amorphous precious metals in the field of resistive gas sensors in the existing technology and realizes the detection of hydrogen. Highly sensitive detection, with application prospects for new high-efficiency gas sensors.
Patent Information
- Application Number
- CN202111394195.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-23
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-11-23
AI Technical Summary
There is a lack of application of amorphous precious metals in the field of resistive gas sensors in the existing technology, especially Ru-based amorphous precious metals that have not yet been studied. The scarcity and expense of traditional precious metal catalysts limit their wide application, and amorphous materials are widely used in gas sensors. Applications in the field are less common.
By synthesizing amorphous noble metal RuOx and ZnO nanosheet composite materials, and using RuOx to modify the ZnO surface through self-assembly, a hydrogen sensor with high response value and low detection limit was prepared. It was prepared by electromagnetic stirring, autoclave and ultrasonic treatment. RuOx/ZnO composite material and coating it on the MEMS chip.
It achieves high-sensitivity detection of hydrogen with a detection limit as low as 1 ppm. It has broad application prospects for new high-efficiency gas sensors and solves the problems of scarcity and application limitations of traditional precious metal catalysts.
Smart Images

Figure CN114166898B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of hydrogen sensors, and in particular to an amorphous noble metal RuO x / Preparation method of ZnO MEMS hydrogen sensor. Background Art
[0002] H2 is a colorless and odorless gas that is considered an attractive alternative energy source and sustainable energy carrier due to its relatively low impact on the environment. However, the leakage of H2 molecules can cause serious explosions and be extremely lethal when exceeding a certain critical concentration. The development of suitable sensors to determine and control the H2 content during production, transportation, storage and utilization is becoming increasingly important and urgent.
[0003] Traditional gas sensors are usually prepared by combining precious metals (such as Pd, Au, Rh and Ru, etc.) with MOS. Due to their specific chemical and electronic sensitization properties, they exhibit unique characteristics. However, the scarcity and high cost of precious metals greatly hinder their widespread application. Therefore, it is necessary to construct highly active precious metal catalysts by increasing the number of active sites or optimizing intrinsic activity. Since the adsorption / desorption kinetics of gas-sensitive reactions are highly dependent on the surface structure of the catalyst, constructing the catalyst surface structure, especially at the atomic level, has become an effective and successful strategy to further improve the catalytic performance of precious metals. Unlike crystalline materials with translational periodicity, the inherent disorder of amorphous materials can produce a large number of "dangling bonds" and defects in the loosely bound atomic free volume region, which can provide more active sites, thereby improving the catalytic activity. In addition, amorphous materials exhibit superior performance at the performance level. Amorphous precious metals have many applications in the field of catalysis, but their application as sensitizers in the field of gas sensors is very rare. In the prior art, there is only the synthesis of an amorphous Pd layer covering ZnO nanorods (am-Pd / ZnO NRs), am-Pd / ZnO NRs sensors exhibited significant sensing responses compared to ZnO nanorod sensors decorated with crystalline Pd nanoparticles (Sensor Actuators B: Chemical 2018, 262, 460-468). However, Ru-based amorphous noble metals as sensitizers have not been studied in the field of resistive gas sensors.
[0004] Therefore, it is necessary to design an amorphous noble metal RuO x / ZnO MEMS hydrogen sensor preparation method, the prepared RuO x / ZnO composite gas-sensitive materials have good sensitivity to hydrogen and have broad application prospects in the manufacture of new high-efficiency gas sensors. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide an amorphous noble metal RuO x / ZnO MEMS hydrogen sensor preparation method, the prepared RuO x / ZnO composite gas-sensitive materials have good sensitivity to hydrogen and have broad application prospects in the manufacture of new high-efficiency gas sensors.
[0006] In order to achieve the above object, the present invention provides an amorphous noble metal RuO x A method for preparing a ZnO MEMS hydrogen sensor comprises the following steps:
[0007] S1: Mix the prepared composite gas-sensitive material and ethanol in an agate mortar and grind into a paste;
[0008] S2: Apply the paste on the Pt interdigital electrodes and dry naturally at room temperature to obtain a resistive sensor MEMS sensor;
[0009] S3: placing the resistive sensor MEMS sensor on a base with a heating electrode and a test electrode, and then setting the heating voltage of the sensor to 1.5V for 24 hours;
[0010] The preparation method of the composite gas-sensitive material comprises the following steps:
[0011] S10: Under electromagnetic stirring, 250 mg to 300 mg of RuCl3·xH2O hydrate was dissolved in 5 ml of deionized water, and then 4 to 5 g of LiOH·H2O was added to form a solution;
[0012] S20: heating the solution to 85-90° C. under stirring to evaporate water, and calcining the solid product obtained after evaporation at 350-410° C. in static air for 2 hours;
[0013] S30: The solid product was thoroughly washed with deionized water and ethanol and dried at 60 °C overnight to obtain the catalyst and was labeled as RuO x ;
[0014] S40: 8-15 mmol Zn(CH3COO)2·2H2O, 5-12 mmol hexamethyltetramine (HMT) and 5 mmol sodium dodecyl sulfate (SDS) were dissolved in 20 ml distilled water, and after vigorous stirring for 30 minutes, the solution was transferred to a 50 mL autoclave and maintained at 160-200°C for 9-12 hours;
[0015] S50: After the autoclave was cooled to room temperature, the white precipitate was centrifuged, washed several times with ethanol and distilled water, and dried at 60 °C overnight;
[0016] S60: calcining the precipitate at 500°C for 2 hours at a heating rate of 2°C / min in an air atmosphere to obtain ZnO nanosheets;
[0017] S70: RuO obtained in S30 x (0.5-2 mg) was dispersed in 20 mL of ethanol and mixed with ZnO (100 mg) to form a mixture;
[0018] S80: The mixture was treated with ultrasound for 1 hour and then dried at 60-80 °C for 8 hours to obtain RuO x Modified ZnO.
[0019] Compared with the prior art, the present invention has successfully synthesized Ru-based amorphous noble metal (RuO x ), ZnO is a typical n-type metal oxide semiconductor with a wide bandgap energy of 3.37 eV. It is also one of the most studied sensing materials. Then RuO x The ZnO surface was modified by self-assembly and a small amount of RuO x After modified ZnO, RuO x The ZnO / ZnO sensor shows a very high response value and an ultra-low detection limit (as low as 1 ppm) to hydrogen, and has broad application prospects in the manufacture of new high-efficiency gas sensors. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The amorphous noble metal RuO prepared by the present invention x XRD pattern of .
[0021] Figure 2 Scanning electron microscope and transmission electron microscope images of the microscopic morphology of the porous ZnO nanosheets prepared in the present invention.
[0022] Figure 3 The RuO of the present invention has a mass fraction of 0.5% of the amorphous noble metal Ru. x High-resolution display of / Zn-O nanocomposites.
[0023] Figure 4 The amorphous noble metal RuO of the present invention x 1% RuO x Sensitivity curve of ZnO nanocomposite to different hydrogen concentrations at 280℃.
[0024] Figure 5 The amorphous noble metal RuO of the present invention x RuO with a content of 1.2% x / ZnO nanocomposite sensitivity curve to 1 ppm hydrogen at 280°C. DETAILED DESCRIPTION
[0025] The present invention will now be further described with reference to the accompanying drawings.
[0026] See also Figure 1-5 The present invention provides an amorphous noble metal RuO x A method for preparing a ZnO MEMS hydrogen sensor comprises the following steps:
[0027] S1: Mix the prepared composite gas-sensitive material and ethanol in an agate mortar and grind into a paste;
[0028] S2: Apply the paste on the Pt interdigital electrodes and dry naturally at room temperature to obtain a resistive sensor MEMS sensor;
[0029] S3: placing the resistive sensor MEMS sensor on a base with a heating electrode and a test electrode, and then setting the heating voltage of the sensor to 1.5V for 24 hours;
[0030] The preparation method of the composite gas-sensitive material comprises the following steps:
[0031] S10: Under electromagnetic stirring, 250 mg to 300 mg of RuCl3·xH2O hydrate was dissolved in 5 ml of deionized water, and then 4 to 5 g of LiOH·H2O was added to form a solution;
[0032] S20: heating the solution to 85-90° C. under stirring to evaporate water, and calcining the solid product obtained after evaporation at 350-410° C. in static air for 2 hours;
[0033] S30: The solid product was thoroughly washed with deionized water and ethanol and dried at 60 °C overnight to obtain the catalyst and was labeled as RuO x ;
[0034] S40: 8-15 mmol Zn(CH3COO)2·2H2O, 5-12 mmol hexamethyltetramine (HMT) and 5 mmol sodium dodecyl sulfate (SDS) were dissolved in 20 ml distilled water, and after vigorous stirring for 30 minutes, the solution was transferred to a 50 mL autoclave and maintained at 160-200°C for 9-12 hours;
[0035] S50: After the autoclave was cooled to room temperature, the white precipitate was centrifuged, washed several times with ethanol and distilled water, and dried at 60 °C overnight;
[0036] S60: calcining the precipitate at 500°C for 2 hours at a heating rate of 2°C / min in an air atmosphere to obtain ZnO nanosheets;
[0037] S70: RuO obtained in S30 x (0.5-2 mg) was dispersed in 20 mL of ethanol and mixed with ZnO (100 mg) to form a mixture;
[0038] S80: The mixture was treated with ultrasound for 1 hour and then dried at 60-80 °C for 8 hours to obtain RuO x Modified ZnO.
[0039] Embodiment 1:
[0040] Under electromagnetic stirring, 250 mg of RuCl3·xH2O hydrate was dissolved in 5 ml of deionized water, and then 4.0 g of LiOH·H2O was added. The solution was heated to 85 °C under stirring to evaporate the distilled water, and the resulting solid was calcined at 350 °C in static air for 2 h. After that, the sample was thoroughly washed with deionized water and ethanol and dried at 60 °C overnight. The resulting sample was labeled as RuO x , its XRD spectrum is as follows Figure 1 As shown, XRD has no obvious diffraction peaks, proving the synthesis of amorphous materials. 10mmolZn(CH3COO)2·2H2O, 10mmolhexamethyltetramine (HMT) and 5mmolsodium dodecyl sulfate (SDS) were dissolved in 20mldistilled water. After vigorous stirring for 30 minutes, the solution was transferred to a 50mL autoclave and kept at 160-200℃ for 9h. After the autoclave was cooled to room temperature, the white precipitate was centrifuged, washed with ethanol and distilled water several times, and dried at 60℃ overnight. Finally, the precipitate was calcined at 500℃ for 2 hours in an air atmosphere at a heating rate of 2℃ / min to obtain ZnO nanosheets. Figure 2 The scanning electron microscope and transmission electron microscope images of the prepared porous ZnO nanosheets show that ZnO is a porous nanosheet. x The RuO was dispersed in 20 mL of ethanol and mixed with ZnO (100 mg). The mixture was treated with ultrasound for 1 h and then dried at 60 °C for 8 h to obtain RuO x / ZnO.
[0041] The prepared composite gas-sensitive material RuO x / ZnO and ethanol were mixed in an agate mortar, ground into a paste and applied to the Pt interdigital electrode. After natural drying at room temperature, a resistive sensor MEMS sensor was obtained. The sensor was placed on a base with a heating electrode and a test electrode, and then the heating voltage of the sensor was set to 1.5V. The aging process was completed after 24 hours. The gas-sensing test used a static gas distribution method. During the test, a micro-syringe was used to inject the required amount of target gas into the test chamber. The gas-sensing results are shown in Figure 1. Figure 4As shown, the gas sensing test results show that the response value of the sensor at 280°C increases with the increase of H2 gas concentration, indicating that the MEMS sensor we prepared can detect extremely low H2 and can quickly detect the presence of H2.
[0042] Embodiment 2:
[0043] Under electromagnetic stirring, 300 mg of RuCl3·xH2O hydrate was dissolved in 5 ml of deionized water, and then 5.0 g of LiOH·H2O was added. The solution was heated to 85 °C under stirring to evaporate the distilled water, and the resulting solid was calcined at 410 °C in static air for 2 h. The sample was thoroughly washed with deionized water and ethanol and dried at 60 °C overnight. The resulting sample was labeled as RuO x 8mmol Zn(CH3COO)2·2H2O, 5mmol hexamethyltetramine (HMT) and 5mmol sodium dodecyl sulfate (SDS) were dissolved in 20ml distilled water. After vigorous stirring for 30min, the solution was transferred to a 50mL autoclave and kept at 180℃ for 9h. After the autoclave was cooled to room temperature, the white precipitate was centrifuged, washed with ethanol and distilled water several times, dried at 60℃ overnight, and finally the precipitate was calcined at 500℃ for 2h in air atmosphere at a heating rate of 2℃ / min to obtain ZnO nanosheets. Finally, 1mg RuO x The RuO was dispersed in 20 mL of ethanol and mixed with ZnO (100 mg). The mixture was treated with ultrasound for 1 h and then dried at 60 °C for 8 h to obtain RuO x / ZnO.
[0044] The prepared composite gas-sensitive material RuO x / ZnO and ethanol are mixed in an agate mortar, ground into a paste and applied to the Pt interdigital electrode. After natural drying at room temperature, a resistive sensor MEMS sensor is obtained. The sensor is placed on a base with a heating electrode and a test electrode. The heating voltage of the sensor is then set to 1.5 V and continued for 24 hours to complete.
[0045] The prepared RuO was tested using the gas sensing performance test method in Example 1. x / ZnO nanocomposite gas-sensitive material, the results are as follows Figure 5 As shown, the sensitivity of this material to 1ppm hydrogen at 280℃ is 1.1. Figure 5 The response values shown are similar to those of Example 1.
[0046] Embodiment 3:
[0047] Under electromagnetic stirring, 300 mg of RuCl3·xH2O hydrate was dissolved in 5 ml of deionized water, and then 5.0 g of LiOH·H2O was added. The solution was heated to 90 °C under stirring to evaporate the distilled water, and the resulting solid was calcined at 400 °C in static air for 2 h. The sample was thoroughly washed with deionized water and ethanol and dried at 60 °C overnight. The resulting sample was labeled as RuO x 15mmol Zn(CH3COO)2·2H2O, 12mmol hexamethyltetramine (HMT) and 5mmol sodium dodecyl sulfate (SDS) were dissolved in 20ml distilled water. After vigorous stirring for 30min, the solution was transferred to a 50mL autoclave and kept at 160℃ for 9h. After the autoclave was cooled to room temperature, the white precipitate was centrifuged, washed with ethanol and distilled water several times, dried at 60℃ overnight, and the precipitate was calcined at 500℃ for 2h in air atmosphere at a heating rate of 2℃ / min to obtain ZnO nanosheets. Finally, 1mg RuO x The RuO was dispersed in 20 mL of ethanol and mixed with ZnO (100 mg). The mixture was treated with ultrasound for 1 h and then dried at 60 °C for 8 h to obtain RuO x / ZnO, Figure 3 RuO x / ZnO transmission image, which clearly shows the amorphous noble metal RuO x It was successfully loaded onto the surface of ZnO.
[0048] The prepared composite gas-sensitive material RuO x / ZnO and ethanol were mixed in an agate mortar, ground into a paste and applied on the Pt interdigital electrode. After natural drying at room temperature, a resistive MEMS sensor was obtained. The sensor was placed on a base with a heating electrode and a test electrode. The heating voltage of the sensor was then set to 1.5 V. The aging process was completed after 24 hours.
[0049] The above are only preferred embodiments of the present invention, which are only used to help understand the method and core ideas of the present application. The protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
[0050] The present invention solves the problem that the prior art does not use amorphous noble metals in the field of resistive gas sensors. x , and then composited it onto ZnO nanosheets by self-assembly.x The amount of RuO can be synthesized with different mass fractions of amorphous noble metals. x Gas sensing materials, by controlling amorphous noble metal RuO x The content of LiOH·H2O in the synthesis process can effectively control the synthesis of amorphous noble metals. Since there are a large number of coordination unsaturated points and dangling bonds on the surface of amorphous noble metal Ru, it has excellent sensitivity enhancement characteristics. Therefore, the prepared composite material is coated on a MEMS chip to prepare a highly sensitive and low-power hydrogen sensor, which has broad application prospects in the manufacture of new high-efficiency gas sensors.
Claims
1. A method for preparing a MEMS hydrogen sensor of amorphous noble metal RuOx composite ZnO, characterized in that The following steps are included: S1: Mix the prepared composite gas-sensitive material and ethanol in an agate mortar and grind into a paste; S2: applying the paste on the Pt interdigital electrodes and drying naturally at room temperature to obtain a resistive sensor MEMS sensor; S3: placing the resistive sensor MEMS sensor on a base with a heating electrode and a test electrode, and then setting the heating voltage of the sensor to 1.5V for 24 hours; The preparation method of the composite gas-sensitive material comprises the following steps: S10: Under electromagnetic stirring, 250 mg to 300 mg of RuCl3•xH2O hydrate was dissolved in 5 ml of deionized water, and then 4 to 5 g of LiOH•H2O was added to form a solution; S20: heating the solution to 85-90° C. under stirring to evaporate water, and calcining the solid product obtained after evaporation at 350-410° C. in static air for 2 hours; S30: The solid product was thoroughly washed with deionized water and ethanol and dried at 60 °C overnight to obtain the catalyst and was labeled as RuO x ; S40: 8-15 mmol Zn(CH3COO)2•2H2O, 5-12 mmol hexamethyltetramine (HMT) and 5 mmol sodium dodecyl sulfate (SDS) were dissolved in 20 ml distilled water. After vigorous stirring for 30 min, the solution was transferred to a 50 mL autoclave and kept at 160-200 °C for 9-12 h. S50: After the autoclave is cooled to room temperature, the white precipitate is centrifuged, washed with ethanol and distilled water for several times, and dried at 60° C. overnight; S60: calcining the precipitate at 500° C. for 2 hours at a heating rate of 2° C. / min in an air atmosphere to obtain ZnO nanosheets; S70: 0.5-2 mg of RuO obtained in S30 x dispersed in 20 mL of ethanol and mixed with the 100 mg of ZnO to form a mixture; S80: The mixture is treated with ultrasound for 1 hour, and then dried at 60-80°C for 8 hours to finally obtain RuO x Modified ZnO.