Method for producing negative electrode material for lithium ion secondary battery and method for producing lithium ion secondary battery
By adopting a specific negative electrode material manufacturing method in lithium-ion secondary batteries and utilizing graphitization processing and crushing technology, the problem of poor cycle characteristics of lithium-ion secondary batteries is solved, and higher battery life and rapid charging performance are achieved.
Patent Information
- Application Number
- CN201980098990.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-07-31
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-07-31
AI Technical Summary
Existing lithium-ion secondary batteries have poor cycle characteristics in electrical products, electric vehicles, and storage power supplies, making it difficult to meet demand.
A method for manufacturing negative electrode materials for lithium ion secondary batteries is adopted, which includes obtaining a graphitizable aggregate and a binder mixture, forming and graphitizing the product, and then pulverizing the formed product to obtain pulverized products with a small specific surface area, for Reduce the contact area between the negative electrode material and the electrolyte to extend battery life.
The negative electrode material manufactured by this method can significantly improve the cycle characteristics and rapid charging performance of lithium-ion secondary batteries, extend the battery life, and provide lithium-ion secondary batteries with excellent cycle characteristics.
Smart Images

Figure BDA0003494807810000171
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a negative electrode material for a lithium ion secondary battery and a method for producing a lithium ion secondary battery. Background Art
[0002] Lithium-ion secondary batteries have a higher energy density than other secondary batteries such as nickel-cadmium batteries, nickel-hydrogen batteries, and lead-acid batteries, and are therefore widely used as power sources for portable electrical appliances such as notebook computers and mobile phones. In addition, lithium-ion secondary batteries can be expected to be used not only in smaller electrical appliances, but also in electric vehicles, power sources for power storage, and the like.
[0003] Graphite is widely used as a negative electrode material (negative electrode material) of a lithium ion secondary battery. As a method for manufacturing a negative electrode material using graphite, for example, Patent Document 1 describes the following method: a mixture obtained by mixing a carbon material and a binder, etc., is crushed, the crushed product is formed using a mold, graphitized in this state, and the obtained graphitized product is further crushed.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2015 / 147012 Summary of the invention
[0007] Technical problem to be solved by the invention
[0008] The demand for lithium ion secondary batteries in electrical appliances, electric vehicles, power supplies for power storage, and the like has increased, and along with this, lithium ion secondary batteries having excellent cycle characteristics have been desired.
[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for producing a negative electrode material for a lithium ion secondary battery capable of producing a lithium ion secondary battery having excellent cycle characteristics, and a method for producing a lithium ion secondary battery having excellent cycle characteristics.
[0010] Means for solving technical problems
[0011] Specific means for solving the technical problem include the following implementation methods.
[0012] <1> A method for producing a negative electrode material for a lithium-ion secondary battery, comprising the following steps:
[0013] (a) a process of obtaining a mixture comprising a graphitizable aggregate and a graphitizable binder;
[0014] (b) forming the mixture to obtain a density of 1.3 g / cm 3The following forming process:
[0015] (c) a step of graphitizing the formed product to obtain a graphitized product; and
[0016] (d) A step of pulverizing the graphitized material to obtain a pulverized material.
[0017] <2> according to <1> In the method for producing a negative electrode material for a lithium-ion secondary battery, the standard deviation of the particle size distribution of the aggregate is less than 0.20.
[0018] <3> according to <1> or <2> In the method for producing a negative electrode material for a lithium-ion secondary battery, the mixture contains a dispersant.
[0019] <4> According to the claim <3> In the method for producing a negative electrode material for a lithium ion secondary battery, the dispersant comprises a fatty acid.
[0020] <5> according to <1> ~ <4> The method for producing a negative electrode material for a lithium ion secondary battery according to any one of the above aspects, wherein the amount of the binder blended is 25% by mass or less relative to the mixture.
[0021] <6> A method for manufacturing a lithium ion secondary battery, comprising: <1> ~ <5> A step of producing a negative electrode using the negative electrode material obtained by the method for producing a negative electrode material for a lithium ion secondary battery according to any one of the above aspects.
[0022] <7> A method for manufacturing a lithium-ion secondary battery comprises the following steps:
[0023] pass <1> ~ <5> A step of manufacturing a negative electrode material for a lithium ion secondary battery according to any one of the methods for manufacturing a negative electrode material for a lithium ion secondary battery; and
[0024] A step of manufacturing a negative electrode using the negative electrode material for a lithium ion secondary battery.
[0025] Effects of the Invention
[0026] According to the present invention, a method for producing a negative electrode material for a lithium ion secondary battery capable of producing a lithium ion secondary battery having excellent cycle characteristics and a method for producing a lithium ion secondary battery having excellent cycle characteristics can be provided. DETAILED DESCRIPTION
[0027] Hereinafter, the mode for implementing the present invention will be described in detail. However, the present invention is not limited to the following embodiments. In the following embodiments, its constituent elements (including element steps, etc.) are not necessarily required unless they are considered to be obviously required in principle. The same is true for numerical values and their ranges, and the present invention is not limited thereto.
[0028] In the present disclosure, the term "process" includes not only a process that is independent of other processes, but also a process that cannot be clearly distinguished from other processes as long as the purpose of the process is achieved.
[0029] In the present disclosure, a numerical range expressed using "to" includes the numerical values described before and after "to" as the minimum value and the maximum value, respectively.
[0030] In the numerical range recorded in stages in the present disclosure, the upper limit or lower limit recorded in one numerical range can also be replaced by the upper limit or lower limit of the numerical range recorded in other stages. In addition, in the numerical range recorded in the present disclosure, the upper limit or lower limit of the numerical range can also be replaced by the value shown in the embodiment.
[0031] In the present disclosure, each component may include a plurality of corresponding substances. When there are a plurality of substances corresponding to each component in the composition, the content rate or content of each component refers to the total content rate or total content of the plurality of substances present in the composition unless otherwise specified.
[0032] In the present disclosure, particles belonging to each component may include multiple types. When multiple types of particles belonging to each component exist in the composition, the particle size of each component refers to a value for a mixture of the multiple types of particles present in the composition unless otherwise specified.
[0033] In the present disclosure, the term "layer" includes a case where the layer is formed on only a part of the region in addition to the case where the layer is formed on the entire region when observing the region where the layer exists.
[0034] <Method for producing negative electrode material for lithium ion secondary battery>
[0035] The method for producing a negative electrode material for a lithium ion secondary battery (hereinafter also simply referred to as a negative electrode material) disclosed in the present invention comprises the following steps:
[0036] (a) a process of obtaining a mixture comprising a graphitizable aggregate and a graphitizable binder;
[0037] (b) forming the mixture to obtain a density of 1.3 g / cm 3 The following forming process:
[0038] (c) a step of graphitizing the formed product to obtain a graphitized product; and
[0039] (d) A step of pulverizing the graphitized material to obtain a pulverized material.
[0040] In the above method, after obtaining a mixture comprising a graphitizable aggregate and a graphitizable binder, the mixture is formed to obtain a density of 1.3 g / cm 3 The following molded product. In this method, after obtaining a molded product with a relatively low density, the molded product is graphitized, and then the graphitized product is crushed. As a result, the graphitized product can be easily crushed compared to when a graphitized product obtained using a molded product with a relatively high density is crushed, and as a result, a crushed product with a small specific surface area can be obtained. By using a negative electrode material containing a crushed product with a small specific surface area for the production of a lithium-ion secondary battery, the contact area between the negative electrode material and the electrolyte can be reduced, thereby suppressing the decomposition reaction of the electrolyte, extending the life of the battery, and manufacturing a lithium-ion secondary battery with excellent cycle characteristics.
[0041] Each step of the above method can be carried out continuously or discontinuously. In addition, each step of the above method can be carried out in the same place or in different places.
[0042] In step (a), a mixture containing a graphitizable aggregate and a graphitizable binder is obtained. The method for obtaining the mixture is not particularly limited, and a kneader or the like can be used. The mixing is preferably performed at a temperature at which the graphitizable binder softens. Specifically, when the graphitizable binder is asphalt, tar, etc., the temperature may be 50°C to 300°C, and when it is a thermosetting resin, the temperature may be 20°C to 100°C.
[0043] The graphitizable aggregate is not particularly limited as long as it is graphitized by graphitization treatment. Specifically, cokes such as fluidized coke, needle coke, and mosaic coke are exemplified, and needle coke is preferably used. The graphitizable aggregate is preferably in a particle form.
[0044] The average particle size of the graphitizable aggregate is, for example, preferably 5 to 40 μm, more preferably 10 to 30 μm, and even more preferably 10 to 25 μm. The average particle size is, for example, a volume average particle size (D50) measured by a laser diffraction-scattering method described below.
[0045] The standard deviation of the particle size distribution of the graphitizable aggregate is, for example, preferably less than 0.20, more preferably less than 0.18, and further preferably less than 0.16. By having the standard deviation of the particle size distribution of the aggregate being less than 0.20, the unevenness of the particle size of the aggregate can be reduced, and the unevenness of the particle size of the obtained pulverized material can also be suppressed. By using the negative electrode material of the pulverized material containing the uneven small particle size for the production of a lithium ion secondary battery, the resistance distribution in the negative electrode can be uniformized, and as a result, there is a tendency that the rapid charging performance of the lithium ion secondary battery is improved. Furthermore, by reducing the unevenness of the particle size of the aggregate, even if the content or content of the graphitizable binder is reduced, the function as a binder can also be appropriately ensured. The standard deviation of the particle size distribution is, for example, a value (volume standard) measured by the laser diffraction-scattering method described later.
[0046] The lower limit of the standard deviation of the particle size distribution of the graphitizable aggregate is not particularly limited, and may be, for example, 0.05 or more, or 0.10 or more.
[0047] Examples of a method for adjusting the average particle size of the graphitizable aggregate and the standard deviation of the particle size distribution of the graphitizable aggregate to within the above ranges include classification using a sieve, wind classification, and wet classification.
[0048] The graphitizable binder is not particularly limited as long as it can be graphitized by a graphitization treatment, and specific examples thereof include coal-based, petroleum-based, and artificial pitch and tar, thermoplastic resins, and thermosetting resins.
[0049] The ratio of each material in the mixture is not particularly limited. For example, the content of the graphitizable binder can be 10 to 30 parts by mass, 12 to 25 parts by mass, or 14 to 20 parts by mass relative to 100 parts by mass of the graphitizable aggregate. When the amount of the binder is 10 parts by mass or more, it has a tendency to function appropriately as a binder for the graphitizable aggregate. When the amount of the binder is 30 parts by mass or less, it has a tendency to fully ensure the amount of fixed carbon in the mixture and excellent yield.
[0050] The content of the graphitizable binder is preferably 25% by mass or less, more preferably 20% by mass or less, further preferably 10% to 19% by mass, and particularly preferably 12% to 18% by mass, based on 100% by mass of the mixture.
[0051] The graphitizable aggregate and the graphitizable binder contained in the mixture may be only one kind, or may be two or more kinds. In addition, the mixture may also contain components other than these. As components other than the graphitizable aggregate and the graphitizable binder, graphite, a dispersant, a graphitization catalyst, etc. may be cited.
[0052] The mixture may further include graphite. Examples of graphite include natural graphite and artificial graphite. The graphite is preferably in the form of particles. The mixture may include only one type of graphite or may include two or more types.
[0053] In step (b), from the viewpoint of facilitating the dispersion of the components in the mixture, it is preferred that the mixture contains a dispersant. By including a dispersant in the mixture, the uneven particle size of the pulverized product obtained by pulverizing the graphitized product can be suppressed, and a pulverized product with a uniform particle size can be easily obtained. As a result, there is a tendency that the rapid charging performance of the lithium ion secondary battery is improved.
[0054] Furthermore, the inclusion of a dispersant in the mixture is related to the amount of the graphitizable binder being suppressed, and improvement in battery characteristics such as the initial charge and discharge efficiency of the negative electrode material can be expected.
[0055] The type of dispersant is not particularly limited. Specifically, hydrocarbons such as liquid paraffin, paraffin wax, polyethylene wax, stearic acid, oleic acid, erucic acid, 12-hydroxystearic acid, fatty acids such as zinc stearate, lead stearate, aluminum stearate, calcium stearate, magnesium stearate, fatty acid metal salts such as stearic acid amide, oleic acid amide, erucic acid amide, methylene bis stearic acid amide, ethylene bis stearic acid amide, fatty acid amides such as stearic acid monoglyceride, stearyl stearate, hydrogenated oil, and higher alcohols such as stearyl alcohol can be cited. Among them, fatty acids are preferred, and stearic acid is more preferred, because it is difficult to affect the performance of the negative electrode material, it is easy to handle because it is solid at room temperature, it is uniformly dispersed because it melts at the temperature of step (a), it disappears in the process before graphitization, and it is cheap.
[0056] When the mixture contains a dispersant, the amount thereof is not particularly limited. For example, the content of the dispersant relative to the entire mixture may be 0.1% to 20% by mass, 0.5% to 10% by mass, or 0.5% to 5% by mass.
[0057] From the viewpoint of promoting graphitization of the graphitizable aggregate or binder, it is preferred that the mixture contains a graphitization catalyst. The type of graphitization catalyst is not particularly limited. Specifically, materials having a graphitization catalytic effect such as silicon, iron, nickel, titanium, boron, and carbides, oxides, nitrides, etc. of these materials can be cited.
[0058] When the mixture contains a graphitization catalyst, the amount thereof is not particularly limited. For example, the content of the graphitization catalyst relative to the entire mixture may be 0.1% to 50% by mass, 0.5% to 40% by mass, or 0.5% to 30% by mass.
[0059] In step (b), the mixture obtained in step (a) is shaped to obtain a shaped article. Preferably, the shaped article is shaped into a predetermined shape by uniaxial pressing or the like. By performing the shaping in this way, the loading amount in the graphitization furnace can be increased when the mixture is graphitized to improve productivity, or the effect of the graphitization catalyst can be improved.
[0060] In step (b), the method for molding the mixture is not particularly limited. For example, there can be mentioned a mold molding method in which the mixture is placed in a container such as a mold and pressurized in a uniaxial direction, a vibration molding method in which the mixture is placed in a container such as a mold, a heavy object is placed on it, and a metal frame is vibrated and impacted to perform molding, and an extrusion molding method in which the mixture is horizontally pushed and extruded from a nozzle by pressing to perform molding.
[0061] In step (b), the density of the obtained molded product is only 1.3 g / cm 3 From the viewpoint of the productivity of the negative electrode material and the cycle characteristics of the lithium ion secondary battery, it is preferably 0.8 g / cm 3 ~1.2g / cm 3 , more preferably 0.9 g / cm 3 ~1.1g / cm 3 . Thus, after obtaining a molded product with a relatively low density, the molded product can be graphitized and then the graphitized product can be crushed. Compared with the case where the graphitized product obtained using a molded product with a relatively high density is crushed, the graphitized product can be crushed more easily. As a result, there is a tendency to obtain a crushed product with a small specific surface area. By using a negative electrode material containing a crushed product with a small specific surface area for the production of a lithium-ion secondary battery, since the contact area between the negative electrode material and the electrolyte can be reduced, the decomposition reaction of the electrolyte can be suppressed, the life of the battery can be extended, and there is a tendency to manufacture a lithium-ion secondary battery with excellent cycle characteristics.
[0062] The molded product obtained in step (b) is preferably subjected to heat treatment before graphitizing the molded product in step (c). By performing heat treatment, organic components contained in the mixture that do not contribute to graphitization are removed, which tends to suppress gas generation during graphitization.
[0063] The temperature of the heat treatment is not particularly limited, but is preferably a temperature lower than the heat treatment temperature in step (c). For example, the heat treatment can be performed in the range of 500°C to 1000°C.
[0064] In step (c), the molded product obtained in step (b) is graphitized. The method for graphitizing the molded product is not particularly limited as long as the conditions under which the graphitizable components contained in the mixture can be graphitized. For example, a method of heat treatment in an atmosphere in which the mixture is difficult to oxidize can be cited. The atmosphere in which the mixture is difficult to oxidize is not particularly limited, and examples thereof include inactive atmospheres such as nitrogen and argon, and vacuum.
[0065] The temperature of the heat treatment for graphitization can be, for example, above 1500°C, above 2000°C, above 2500°C, or above 2800°C. The upper limit of the temperature of the heat treatment is not particularly limited, and can be, for example, below 3200°C. When the temperature of the heat treatment is above 1500°C, there is a tendency that changes in crystallization occur and graphitization is easy to proceed. When the firing temperature is above 2000°C, there is a tendency that the crystallization of graphite develops better. On the other hand, when the temperature of the heat treatment for graphitization is below 3200°C, there is a tendency that sublimation of a portion of the graphite can be suppressed.
[0066] In step (d), the graphitized product obtained in step (c) is pulverized to obtain a pulverized product. The pulverization method is not particularly limited, and it can be performed using a jet mill, a vibration mill, a steel needle grinder, a hammer mill, etc. using a known method. The pulverized product can be adjusted in particle size to achieve a desired size. The method for adjusting the particle size is not particularly limited, and examples thereof include a method using the above-mentioned pulverization device, a method using a sieve, and the like.
[0067] If necessary, the pulverized product obtained in step (d) may be subjected to steps such as (e) disposing low-crystalline carbon on at least a portion of the surface of the pulverized product, (f) mixing the pulverized product with other negative electrode active materials, and the like.
[0068] In step (e), as a method for configuring low-crystalline carbon on at least a portion of the surface of the pulverized product, for example, a method of mixing a substance (resin, etc.) that can become low-crystalline carbon with the pulverized product by heat treatment and then heat treating the mixture can be cited. When low-crystalline carbon is configured on at least a portion of the surface of the pulverized product, the input-output characteristics such as the rapid charge-discharge characteristics of a lithium-ion secondary battery using the pulverized product as a negative electrode material are sometimes improved.
[0069] The method of mixing the pulverized material with other negative electrode active materials in step (f) is not particularly limited. By mixing the pulverized material with other negative electrode active materials, the desired properties of the lithium ion secondary battery can sometimes be improved compared to when only the pulverized material is used as the negative electrode active material. As other negative electrode active materials, graphite particles such as natural graphite and artificial graphite, particles containing elements capable of embedding and deintercalating lithium ions, etc. can be cited, but are not limited to these. As elements capable of embedding and deintercalating lithium ions, there are no particular limitations, for example, Si, Sn, Ge, In, etc. can be cited.
[0070] The pulverized material obtained in step (f) may also include particles in which a plurality of flat graphite particles are aggregated or combined, and may also include particles in which a plurality of flat graphite particles are aggregated or combined in a manner such that the main surfaces of the graphite particles become non-parallel to each other (hereinafter also referred to as graphite secondary particles).
[0071] When the pulverized product is in the form of graphite secondary particles, the phenomenon of the particles of the negative electrode material being oriented along the direction of the collector can be suppressed during pressing for high density of the negative electrode, and there is a tendency to ensure sufficient paths for lithium ions to enter and exit the negative electrode material.
[0072] Furthermore, by including particles in a state where a plurality of flat graphite particles are aggregated or combined, the presence of gaps between the plurality of flat graphite particles can reduce the effect of the pressure applied during pressing on the individual graphite particles, thereby tending to suppress the destruction of the graphite particles and the occurrence of cracks.
[0073] In the present disclosure, "flat graphite particles" refer to non-spherical graphite particles having anisotropic shapes. Examples of flat graphite particles include graphite particles having shapes such as scales, flakes, and partial blocks.
[0074] When the length of the flat graphite particles in the long axis direction is A and the length in the short axis direction is B, the aspect ratio represented by A / B is preferably 1.2 to 20, more preferably 1.3 to 10. When the aspect ratio is 1.2 or more, there is a tendency that the contact area between particles increases and the conductivity is further improved. When the aspect ratio is 20 or less, there is a tendency that the input and output characteristics such as the rapid charge and discharge characteristics of the lithium ion secondary battery are further improved.
[0075] The aspect ratio is obtained by observing graphite particles under a microscope, randomly selecting 100 graphite particles to measure their respective A / B, and taking the arithmetic mean of these measured values. In the observation of the aspect ratio, the length A in the major axis direction and the length B in the minor axis direction are measured as follows. That is, in the projected image of the graphite particles observed using a microscope, the tangent a1 and the tangent a2, which are 2 parallel tangents circumscribed to the periphery of the graphite particles and whose distance is the largest, are selected as the length A in the major axis direction. In addition, the tangent b1 and the tangent b2, which are 2 parallel tangents circumscribed to the periphery of the graphite particles and whose distance is the smallest, are selected as the length B in the minor axis direction.
[0076] In the present disclosure, "non-parallel principal surfaces" of graphite secondary particles means that the faces (principal surfaces) with the largest cross-sectional areas of a plurality of flat graphite particles are not aligned in a certain direction. Whether the principal surfaces of a plurality of flat graphite particles are non-parallel to each other can be confirmed by microscopic observation. A plurality of flat graphite particles are aggregated or combined in a state where the principal surfaces are non-parallel to each other, which has a tendency to suppress the orientation of the principal surfaces of the flat graphite particles in the negative electrode, suppress the expansion of the negative electrode accompanying charging, and further improve the cycle characteristics of the lithium-ion secondary battery.
[0077] Furthermore, the graphite secondary particles may partially include a structure in which a plurality of flat graphite particles are aggregated or bonded so that their main surfaces become parallel.
[0078] In the present disclosure, a plurality of flat graphite particles "are in a state of aggregation or combination" refers to a state in which two or more flat graphite particles are aggregated or combined. "Combination" refers to a state in which particles are chemically combined with each other directly or through a carbon substance. "Aggregation" is a state in which particles are not chemically combined with each other but maintain a shape as an aggregate due to their shape, etc. The flat graphite particles can also be aggregated or combined through a carbon substance. As the carbon substance, for example, a graphitized product of a graphitizable binder can be cited. From the viewpoint of mechanical strength, it is preferred that two or more flat graphite particles are combined through a carbon substance. Whether the flat graphite particles are aggregated or combined can be confirmed, for example, by observation using a scanning electron microscope.
[0079] The average particle size of the flat graphite particles is preferably 1 μm to 50 μm, more preferably 1 μm to 25 μm, and further preferably 1 μm to 15 μm, from the viewpoint of easy aggregation or bonding. As a method for measuring the average particle size of the flat graphite particles, a method of measuring using a scanning electron microscope can be cited, and the average particle size of the flat graphite particles is, for example, the arithmetic mean of the particle sizes of 100 flat graphite particles.
[0080] The flat graphite particles and their raw materials are not particularly limited, and include artificial graphite, flaky natural graphite, flaky natural graphite, coke, resin, tar, asphalt, etc. Among them, since the graphite obtained from artificial graphite, natural graphite or coke has high crystallinity and is a soft particle, it has a tendency to facilitate the high density of the negative electrode.
[0081] The negative electrode material may further include spherical graphite particles. When the negative electrode material includes spherical graphite particles, since the spherical graphite particles themselves have a high density, there is a tendency that the pressing pressure required to obtain a desired electrode density can be reduced.
[0082] As spherical graphite particles, spherical artificial graphite, spherical natural graphite, etc. can be cited. From the viewpoint of high density of the negative electrode, the spherical graphite particles are preferably high-density graphite particles. Specifically, it is preferred that the spherical natural graphite produced by high tap density is implemented by sphericalization of particles. Furthermore, the negative electrode material layer containing spherical natural graphite has excellent peel strength, and there is a tendency that it is difficult to peel off from the collector even if it is pressed with strong force.
[0083] When the negative electrode material includes spherical graphite particles, it may also include the above-mentioned flat graphite particles and spherical graphite particles. When the negative electrode material includes the above-mentioned flat graphite particles and spherical graphite particles, the ratio of the two is not particularly limited and can be set according to the desired electrode density, the pressure conditions during pressing, the desired battery characteristics, etc.
[0084] When the negative electrode material includes flat graphite particles and spherical graphite particles, there can be cited a state in which flat graphite particles and spherical graphite particles are mixed, a state in which flat graphite particles and spherical graphite particles are combined (hereinafter also referred to as composite particles), etc. As composite particles, for example, there can be cited particles in which flat graphite particles and spherical graphite particles are combined via carbides of organic matter.
[0085] The composite particles can be produced, for example, by using a mixture containing flat graphite particles or a raw material thereof and spherical graphite particles as the mixture in step (a).
[0086] The average particle size of the negative electrode material produced by the above method is not particularly limited. For example, it is preferably 5 μm to 40 μm, more preferably 10 μm to 30 μm, and further preferably 10 μm to 25 μm. The average particle size can be measured by a scanning electron microscope in the same manner as the average particle size of the flat graphite particles, or can be a volume average particle size (D50) measured by a laser diffraction-scattering method.
[0087] As a method for measuring the average particle size when using a negative electrode material to manufacture an electrode (negative electrode), a method for making a sample electrode, mirror-polishing the electrode after embedding it in an epoxy resin, and observing the electrode cross section using a scanning electron microscope (e.g., Keyence Co., Ltd., "VE-7800"); a method for making an electrode cross section using an ion milling device (e.g., Hitachi High-Tech Co., Ltd., "E-3500"), and measuring the electrode cross section using a scanning electron microscope (e.g., Keyence Co., Ltd., "VE-7800"). The average particle size at this time is the median of 100 particle sizes arbitrarily selected from the observed particles.
[0088] The above-mentioned sample electrode can be produced, for example, as follows: a mixture of 98 parts by mass of negative electrode material, 1 part by mass of styrene butadiene resin as a binder and 1 part by mass of carboxymethyl cellulose as a thickening agent is used as a solid component, water is added to prepare a dispersion, the dispersion is applied on a copper foil with a thickness of 10 μm so that it reaches a thickness of about 70 μm (when coating), and then dried at 105°C for 1 hour to produce it.
[0089] The orientation of the negative electrode material when it is made into a negative electrode (when the negative electrode production is accompanied by a pressing step, it is the negative electrode after pressing) can be 40 or less, 20 or less, or 15 or less. In addition, the orientation can be 10 or more.
[0090] The orientation of the negative electrode material is an index indicating the degree of orientation of the particles of the negative electrode material contained in the negative electrode. Low orientation means that the negative electrode material particles are oriented in random directions. In other words, it means that the pressure during pressing has suppressed the orientation of the graphite particles along the surface of the collector.
[0091] In the present disclosure, the orientation of the negative electrode is obtained by measuring the surface of the sample electrode using an X-ray diffraction device using CuKα rays as an X-ray source. Specifically, the X-ray diffraction pattern of the surface of the sample electrode is measured, and the intensity of the carbon (004) plane diffraction peak detected near the diffraction angle 2θ = 53° to 56° and the carbon (110) plane diffraction peak detected near the diffraction angle 2θ = 70° to 80° is obtained using the following formula (1).
[0092] (004) plane diffraction peak intensity / (110) plane diffraction peak intensity formula (1)
[0093] The specific surface area of the negative electrode material is preferably 3.0 m 2 / g or less, more preferably 0.5m 2 / g~2.5m 2 / g, more preferably 0.7m 2 / g~2.0m2 / g.
[0094] The specific surface area of the negative electrode material can be calculated by using a specific surface area / pore distribution measuring device (e.g. FlowSorbIII 2310, manufactured by Shimadzu Corporation) and a mixed gas of nitrogen and helium (nitrogen:helium = 3:7) to measure nitrogen adsorption at liquid nitrogen temperature (77K) using a one-point method at a relative pressure of 0.3, and then calculating using the BET method.
[0095] <Method for producing lithium-ion secondary battery>
[0096] A first embodiment of the method for producing a lithium ion secondary battery disclosed herein includes a step of producing a negative electrode using the negative electrode material obtained by the method for producing a negative electrode material described above.
[0097] A second embodiment of the method for producing a lithium ion secondary battery of the present disclosure includes a step of producing a negative electrode material by the method for producing a negative electrode material described above; and a step of producing a negative electrode using the negative electrode material.
[0098] The method for preparing the negative electrode using the negative electrode material is not particularly limited, and examples thereof include a method in which a negative electrode material layer is formed on a current collector using a composition containing a negative electrode material, a binder, and a solvent, and heat treatment or pressing is performed as necessary.
[0099] The adhesive contained in the composition is not particularly limited. For example, styrene-butadiene rubber, a polymer compound with ethylenically unsaturated carboxylic acid esters (methyl (meth) acrylate, ethyl (meth) acrylate, butyl (meth) acrylate, hydroxyethyl (meth) acrylate, etc.) as a polymerization component, a polymer compound with ethylenically unsaturated carboxylic acids (acrylic acid, methacrylic acid, itaconic acid, fumaric acid, maleic acid, etc.) as a polymerization component, polyvinylidene fluoride, polyethylene oxide, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polyimide, polyamide-imide and other polymer compounds can be cited. In the present disclosure, (meth) acrylate refers to either or both of methacrylate and acrylate.
[0100] The solvent contained in the composition is not particularly limited, and specifically, organic solvents such as N-methylpyrrolidone, dimethylacetamide, dimethylformamide, and γ-butyrolactone, and water can be used.
[0101] The composition may further contain a thickener for adjusting the viscosity as required. Examples of the thickener include carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, polyacrylic acid and its salts, oxidized starch, phosphorylated starch, casein, and the like.
[0102] The composition may further contain a conductive auxiliary agent as required. Examples of the conductive auxiliary agent include carbon black, graphite, acetylene black, conductive oxides, and conductive nitrides.
[0103] The material and shape of the current collector used in the preparation of the negative electrode are not particularly limited. For example, materials such as strip foil, strip perforated foil, strip screen formed by metals or alloys such as aluminum, copper, nickel, titanium, stainless steel, etc. can be used. In addition, porous materials such as porous metal (foamed metal) and carbon paper can also be used.
[0104] The method of using the composition to form a negative electrode material layer on a current collector is not particularly limited, and can be carried out by known methods such as metal mask printing, electrostatic coating, dip coating, spraying, roller coating, blade coating, gravure coating, screen printing, etc. When the above-mentioned negative electrode material layer and the current collector are integrated, it can be carried out by known methods such as rolling, pressing, and combinations thereof.
[0105] After the negative electrode material layer is formed on the current collector, heat treatment (drying) can also be performed. By performing heat treatment, the solvent contained in the negative electrode material layer is removed, and the solidification of the binder is utilized to promote high strength, which can improve the adhesion between particles and between particles and the current collector. In order to prevent oxidation of the current collector in the process, the heat treatment can be performed in an inactive gas environment such as helium, argon, nitrogen, or in a vacuum environment.
[0106] After the negative electrode material layer is formed on the current collector, a pressing process may be performed. By performing the pressing process, the electrode density of the negative electrode may be adjusted. The electrode density of the negative electrode is not particularly limited and may be 1.5 g / cm 3 ~1.9g / cm 3 , can also be 1.6g / cm 3 ~1.8g / cm 3 The higher the electrode density, the higher the volume capacity of the negative electrode, and the adhesion of the negative electrode material layer to the current collector tends to be improved, which in turn tends to improve the cycle characteristics. The pressing treatment is preferably performed before the heat treatment.
[0107] The lithium ion secondary battery manufactured by the above method may include a negative electrode, a positive electrode and an electrolyte manufactured by the above method. For example, the lithium ion secondary battery may be configured such that the negative electrode and the positive electrode are arranged facing each other with a separator interposed therebetween, and then an electrolyte solution containing an electrolyte is injected.
[0108] The positive electrode can be made by forming a positive electrode layer on the surface of a current collector in the same manner as the negative electrode. As the current collector, a strip-shaped foil, a strip-shaped perforated foil, a strip-shaped mesh, etc. made of a metal or alloy such as aluminum, titanium, stainless steel, etc. can be used.
[0109] The positive electrode material contained in the positive electrode layer is not particularly limited. For example, metal compounds, metal oxides, metal sulfides, and conductive polymer materials capable of doping or inserting lithium ions can be cited. Furthermore, lithium cobaltate (LiCoO2), lithium nickelate (LiNiO2), lithium manganate (LiMnO2), and their composite oxides (LiCo x Ni y Mn z O2, x + y + z = 1, 0 < x, 0 < y; LiNi 2-x Mn x O4, 0 < x ≤ 2), lithium manganese spinel (LiMn2O4), lithium vanadium compounds, V2O5, V6O 13 、VO2, MnO2, TiO2, MoV2O8, TiS2, V2S5, VS2, MoS2, MoS3, Cr3O8, Cr2O5, olivine-type LiMPO4 (M: Co, Ni, Mn, Fe), polyacetylene, polyaniline, polypyrrole, polythiophene, polyacene and other conductive polymers, porous carbon, etc. can be used alone or in combination of two or more of them. Among them, lithium nickelate (LiNiO2) and its composite oxides (LiCo x Ni y Mn z O2, x + y + z = 1, 0 < x, 0 < y; LiNi 2-x Mn x O4, 0 < x ≤ 2) are preferred as the positive electrode material due to their high capacity.
[0110] As the separator, non-woven fabrics, fabrics, microporous membranes and combinations thereof mainly composed of polyolefins such as polyethylene and polypropylene can be cited. Among them, when the lithium ion secondary battery has a structure in which the positive electrode and the negative electrode do not contact, a separator is not required.
[0111] As the electrolyte, so-called organic electrolytes prepared by dissolving lithium salts such as LiClO4, LiPF6, LiAsF6, LiBF4, LiSO3CF3 in non-aqueous solvents which are single or mixtures of two or more components of ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, fluoroethylene carbonate, cyclopentanone, sulfolane, 3-methylsulfolane, 2,4-dimethylsulfolane, 3-methyl-1,3-oxazolidin-2-one, γ-butyrolactone, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, butyl methyl carbonate, ethyl propyl carbonate, butyl ethyl carbonate, dipropyl carbonate, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, methyl acetate, ethyl acetate, etc. can be used. Among them, the electrolyte containing fluoroethylene carbonate has a tendency to form a stable SEI (solid electrolyte interface) on the surface of the negative electrode material, and the cycle characteristics are significantly improved, so it is preferred.
[0112] The form of the lithium ion secondary battery is not particularly limited, and examples thereof include paper type batteries, button type batteries, coin type batteries, laminated type batteries, cylindrical type batteries, square type batteries, etc. In addition, the negative electrode material for lithium ion secondary batteries can also be applied to all electrochemical devices such as hybrid capacitors that use the insertion and removal of lithium ions as a charging and discharging mechanism, in addition to being applicable to lithium ion secondary batteries.
[0113] Example
[0114] Hereinafter, the above-mentioned embodiment will be described in more detail based on examples, but the above-mentioned embodiment is not limited to the following examples.
[0115] [Examples 1 to 3 and Comparative Example 1]
[0116] (1) Preparation of negative electrode materials
[0117] For the needle coke as raw material, after the coke is finely pulverized using a free pulverizer made by Nara Machinery Manufacturing Co., Ltd., TURBOPLEX (registered trademark) made by Hosokawa Micron Co., Ltd. is used for wind classification, thereby preparing the aggregate shown below, and then using the materials shown below as raw materials. In addition, the average particle size of the aggregate and the negative electrode material and the standard deviation of the particle size distribution of the aggregate are measured using a particle size distribution measuring device (Shimadzu Corporation, SALD-3000) using a laser diffraction-scattering method. The standard deviation of the particle size distribution of the aggregate is a standard deviation defined on a logarithmic scale.
[0118] Aggregate 1: Needle coke with an average particle size of 14 μm and a standard deviation of particle size distribution of 0.15
[0119] Adhesive tar asphalt
[0120] Dispersant: stearic acid
[0121] Aggregates, binders, etc. as raw materials shown in Table 1 are mixed in the amounts (parts by mass) described in Table 1 using a kneader to obtain a mixture. Then, the obtained mixture is molded by uniaxial pressing at room temperature to obtain a molded product. Then, the obtained molded product is heat treated at 800°C to 850°C in a nitrogen environment for 8 hours, and then graphitized at 2600°C to 3100°C for 30 hours to obtain a graphitized product. The obtained graphitized product is crushed to obtain graphite powders (negative electrode materials for lithium ion secondary batteries) of Examples 1 to 3 and Comparative Example 1.
[0122] The density (g / cm 3 ), density of graphite (g / cm 3) and the average particle size (μm) and specific surface area (m 2 / g), saturated tap density (g / cm 3 ) are shown in Table 1 respectively.
[0123] Furthermore, the pulverized product obtained in each example includes secondary particles of graphite as aggregates in a state where the graphite particles are aggregated or bonded so that the main surfaces thereof are not parallel to each other.
[0124] (2) Preparation of negative electrode and evaluation of its orientation
[0125] 96 parts by mass of the prepared negative electrode material, 1.5 parts by mass of styrene butadiene rubber (BM-400B, manufactured by Zeon Co., Ltd.), 1.5 parts by mass of carboxymethyl cellulose (CMC1380, manufactured by Daicel Co., Ltd.), and 1.0 parts by mass of carbon black (SuperP, manufactured by Imerys GC Co., Ltd.) were mixed, and water was added to adjust the viscosity to obtain a composition. The obtained composition was applied in an amount of 10 mg / cm 2 The composite layer was coated on the collector (copper foil with a thickness of 10 μm) to form a composite layer. The composite layer was pressurized to form an electrode, and then dried at 130°C for 8 hours in a vacuum dryer. The density after vacuum drying reached 1.60 g / cm 2 The orientation of the produced negative electrode was evaluated by the above method.
[0126] (3) Preparation of evaluation batteries
[0127] The negative electrode obtained above was punched into an electrode area of 1.54 cm 2 A 2016-type coin battery was prepared by using metallic lithium as the positive electrode, a mixed solution of ethylene carbonate / ethylmethyl carbonate (3 / 7 volume ratio) and vinylene carbonate (0.5 mass %) containing 1.0M LiPF6 as the electrolyte, a polyethylene microporous membrane with a thickness of 25 μm as the separator, and a copper plate with a thickness of 230 μm as the spacer. This battery was used as an evaluation battery.
[0128] (4) Evaluation of battery characteristics
[0129] Using the prepared evaluation battery, the initial discharge capacity (Ah / kg) and the initial charge and discharge efficiency (%) were measured. Specifically, the evaluation battery was placed in a thermostatic chamber maintained at 25°C, and charged at a constant current of 0.53 mA until it reached 0 V. Then, it was further charged at a constant voltage of 0 V until the current decayed to a value equivalent to 0.026 mA, and the initial charge capacity was measured. After charging, the battery was discharged after a rest of 30 minutes. The initial discharge capacity was measured at 0.53 mA to 1.5 V. At this time, the capacity was converted to per unit mass of the negative electrode material used. The value obtained by dividing the initial discharge capacity by the initial charge capacity and multiplying it by 100 is the initial charge and discharge efficiency (%). The results are shown in Table 1.
[0130] (5) Evaluation of rapid charge capacity maintenance rate
[0131] The negative electrode obtained above was punched into an electrode area of 2.00 cm 2 A 2016-type coin cell was prepared by using a circular shape, an electrode coated with lithium cobalt oxide on aluminum foil as the positive electrode, a mixed solution of ethylene carbonate / ethylmethyl carbonate (3 / 7 volume ratio) containing 1.0M LiPF6 and vinylene carbonate (0.5 mass %) as the electrolyte, a polyethylene microporous film with a thickness of 25 μm as the separator, and a spring spacer as the spacer. The coin cell was used as an evaluation battery.
[0132] The evaluation battery was used to perform an aging treatment before the rapid charge test. Specifically, the evaluation battery was placed in a thermostatic chamber maintained at 25°C, and charged at a constant current of 0.92 mA until it reached 4.2 V. It was then further charged at a constant voltage of 4.2 V until the current decayed to a value equivalent to 0.046 mA. After charging, it was discharged at 0.92 mA until it reached 2.75 V after a 10-minute rest. This charging and discharging was repeated 5 times.
[0133] A rapid charging test was performed using an aged evaluation battery. Specifically, the evaluation battery was placed in a thermostatic chamber maintained at 25°C, and charged at a constant current of 0.92 mA until it reached 4.2 V, and the charge capacity was measured (1). After charging, the battery was discharged after a 10-minute break. The discharge was performed at 4.6 mA until it reached 2.75 V. Furthermore, the battery was charged at a constant current of 6.9 mA until it reached 4.2 V, and the charge capacity was measured (2). After charging, the battery was discharged at 4.6 mA until it reached 2.75 V after a 10-minute break.
[0134] The value obtained by dividing the charge capacity (2) by the charge capacity (1) and multiplying the value by 100 was taken as the rapid charge capacity maintenance rate (%). The results are shown in Table 1.
[0135] (6) Evaluation of battery life
[0136] The evaluation battery was prepared and aged in the same manner as in (5) above. The aged evaluation battery was used to perform a cycle test and evaluate the battery life. Specifically, the evaluation battery was placed in a thermostatic chamber maintained at 25°C, and charged at a constant current of 4.6 mA until it reached 4.2 V. It was then further charged at a constant voltage of 4.2 V until the current decayed to a value equivalent to 0.046 mA. After charging, the battery was rested for 10 minutes, and then discharged at 4.6 mA until it reached 2.75 V, and the initial discharge capacity was measured. The charge and discharge were further performed for 299 cycles, and the discharge capacity at the 300th cycle was measured.
[0137] The value obtained by dividing the discharge capacity at the 300th cycle by the initial discharge capacity and multiplying the result by 100 was defined as the battery life retention rate (%).
[0138] [Table 1]
[0139]
[0140] As shown in Table 1, the evaluation batteries made using the negative electrode material (Example) made by the method disclosed in the present invention have good rapid charge capacity maintenance rate and battery life maintenance rate compared with the evaluation batteries made using the negative electrode material (Comparative Example) made by the existing manufacturing method (the density of the molded product is high).
Claims
1. A method for producing a negative electrode material for a lithium ion secondary battery, comprising the following steps: (a) a process of obtaining a mixture comprising a graphitizable aggregate and a graphitizable binder; (b) forming the mixture to obtain a density of 1.3 g / cm 3 The following forming process: (c) a step of graphitizing the formed product to obtain a graphitized product; and (d) A step of pulverizing the graphitized material to obtain a pulverized material.
2. The method for producing a negative electrode material for a lithium ion secondary battery according to claim 1, wherein: The standard deviation of the particle size distribution of the aggregate is 0.20 or less.
3. The method for producing a negative electrode material for a lithium ion secondary battery according to claim 1 or 2, wherein: The mixture includes a dispersant.
4. The method for producing a negative electrode material for a lithium ion secondary battery according to claim 3, wherein: The dispersant comprises a fatty acid.
5. The method for producing a negative electrode material for a lithium ion secondary battery according to claim 1 or 2, wherein: The amount of the binder blended is 25% by mass or less based on the mixture. 6 . A method for producing a lithium ion secondary battery, comprising the step of producing a negative electrode using a negative electrode material obtained by the method for producing a negative electrode material for a lithium ion secondary battery according to claim 1 .
Citation Information
Patent Citations
Negative electrode material for lithium-ion secondary cell, method for manufacturing negative electrode material for lithium-ion secondary cell, negative electrode material slurry for lithium-ion secondary cell, negative electrode for lithium-ion secondary cell, and lithium-ion secondary cell
WO2015147012A1
Negative electrode material for lithium-ion secondary cell, method for manufacturing negative electrode material for lithium-ion secondary cell, negative electrode material slurry for lithium-ion secondary cell, negative electrode for lithium-ion secondary cell, and lithium-ion secondary cell
CN106104871A
Negative electrode material for lithium-ion secondary cell, method for manufacturing negative electrode material for lithium-ion secondary cell, negative electrode material slurry for lithium-ion secondary cell, negative electrode for lithium-ion secondary cell, and lithium-ion secondary cell
CN108565463A