Fertilizer compositions and improvements therein

The NBPT is coated on fertilizer particles through aqueous wax dispersion and protected with MgO outer layer, which solves the problem of NBPT degradation caused by acidic fertilizers, and achieves stable suspension and effective coating of NBPT, significantly reduces ammonia volatility loss and improves the Nitrogen utilization efficiency.

CN114206809BActive Publication Date: 2024-11-26GLAZE PAINT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080045474.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-24
Filing Date
2020-08-10
Publication Date
2024-11-26
Estimated Expiration
2040-08-10

AI Technical Summary

Technical Problem

The prior art is difficult to effectively apply nitration inhibitors and urease inhibitors to land in need, especially the contact of acid fertilizers with NBPT causes the problem of NBPT degradation, resulting in the inability of urea and other acid fertilizers to provide necessary nutrients in a single application step. , and there is a lack of aqueous formulations that can be used to suspend and maintain suspension.

Method used

An aqueous wax dispersion containing high melting point emulsification wax, dispersed clay, inhibitor actives and xanthan gum or guar gum for coating NBPT or other urease/nitration inhibitors onto fertilizer particles and through MgO outer layer protects NBPT from acidic fertilizer degradation.

Benefits of technology

The stable suspension and effective coating of NBPT are achieved, which prevents reaction with acid fertilizers, improves the mixing stability of urea and phosphate fertilizers, significantly reduces ammonia volatility loss, and improves nitrogen utilization efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003423205220000181
    Figure BDA0003423205220000181
  • Figure BDA0003423205220000191
    Figure BDA0003423205220000191
  • Figure BDA0003423205220000201
    Figure BDA0003423205220000201
Patent Text Reader

Abstract

An aqueous urease inhibitor and / or nitrification inhibitor formulation, comprising: i) an aqueous wax dispersion, comprising: essentially 10-50 wt% of a high melting point emulsified wax; water to 100%; ii) at least one inhibitor active; wherein the amount of the inhibitor active is: i) 1 wt%-30 wt% of the aqueous wax dispersion; iii) dispersed clay; wherein the amount of the dispersed clay is i) 5 wt%-50 wt% of the aqueous wax dispersion.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Statement of related application

[0002] This application is based upon specifications related to New Zealand Patent Application No. 756188 and New Zealand Patent Application No. 760305, the entire contents of each of which are incorporated herein by reference. Technical Field

[0003] The present invention relates to fertilizer compositions and improvements therein. In particular, the present invention relates to improvements in fertilizer compositions and improvements therein relating to urease inhibitors and / or nitrification inhibitors. Background Art

[0004] As the human population grows from 7.7 billion to 9.8 billion by 2050, large-scale farming of animals for fiber, leather, meat and dairy production, as well as the use of nitrogen-based fertilizers in agriculture, will increase significantly 1 .

[0005] The above-mentioned intensification of agriculture will have serious negative environmental impacts unless solutions are found to address nitrogen losses: through nitrogen oxide (NO2) greenhouse gas emissions; and (NO3) leaching into waterways from nitrogen-based fertilizers and animal urine through nitrification.

[0006] NBPT and DMPP are urease inhibitors and nitrification inhibitors, respectively, which are useful against the above-mentioned NO2 emissions (volatilization) and NO3 losses, respectively.

[0007] It remains imperative to find better ways to utilize inhibitor actives in agricultural practices - including NBPT and DMPP (or other urease / nitrification inhibitors, including the urease inhibitor N-(n-propyl)thiophosphoric triamide (NPPT) and the nitrification inhibitor 2-(3,4-dimethyl-1H-pyrazol-1-yl)succinic acid (DMPSA)) - to address the above problems.

[0008] There is a need to prevent environmental N losses and / or improve N utilization efficiency.

[0009] One problem that currently exists is how to effectively apply nitrification inhibitors and urease inhibitors to the land in need.

[0010] Ideally, it would be nice if an aqueous nitrification inhibitor and / or urease inhibitor formulation could be provided that would coat nitrogen or phosphate-containing fertilizer granules.

[0011] Indeed, another problem that needs to be solved is that currently acidic fertilizers such as phosphate fertilizers degrade NBPT when in contact with it. This makes it impossible to co-apply urea with other acidic fertilizers to provide the necessary nutrients in a single application step.

[0012] It would therefore be desirable for a coating of urea granules / flakes or a coating of phosphate fertilizer granules or flakes to not only:

[0013] - allows urea and phosphorus to mix without adverse reactions, and

[0014] - The NBPT coated urea granules can also be mixed with phosphate fertilizer granules without NBPT degradation due to the low pH of the phosphate fertilizer.

[0015] It would also be useful to be able to provide an aqueous formulation that could be used to suspend and keep NBPT suspended, rather than organic solvents that are flammable or reactive with fertilizers.

[0016] Additionally, it would be useful if the aqueous formulation could also be used to suspend and keep suspended other urease / nitrification inhibitors including DMPP, NPPT, and DMPSA.

[0017] It would also be useful to provide an aqueous formulation that could be used to suspend and maintain in suspension a urease / nitrification inhibitor made from a non-toxic / biodegradable renewable resource.

[0018] It would also be useful to have a ready-made premix of one or more of the major ingredients of the aqueous formulation suitable for storage and transport, prior to adding the inhibitor active.

[0019] There is a need for an aqueous coating composition comprising NBPT in suspension that can be used to coat fertilizer granules comprising urea.

[0020] Alternatively, there is a need for an aqueous coating composition including DMPP, NPPT or DMPSA therein which can be used to coat fertilizer granules.

[0021] It is an object of the present invention to address the above problems or at least to provide the public with a useful choice.

[0022] All references, including any patents or patent applications cited in this specification, are incorporated herein by reference. No admission is made that any reference constitutes prior art. The discussion of the references states what their authors assert, and the applicant reserves the right to challenge the accuracy and relevance of the references. It is to be clearly understood that although a number of prior art publications are cited herein, this citation does not constitute an admission that any of these documents forms part of the common general knowledge in the art, in New Zealand or in any other country.

[0023] In this specification, the word "comprise" or variations such as "comprises" or "comprising" will be understood to imply the inclusion of stated elements, integers or steps, or groups of elements, integers or steps, but not the exclusion of any other elements, integers or steps, or groups of elements, integers or steps.

[0024] Further aspects and advantages of the invention will become apparent from the ensuing description which is given by way of example only.

[0025] definition

[0026] As used herein, the term "inhibitor active" refers to a nitrification inhibitor or a urease inhibitor, including NBPT; DMPP; NPPT; or DMPSA.

[0027] The terms "granules" and "pieces" used herein are used interchangeably and refer to small dense particles of a substance. The size of the granules is generally on the order of 1 mm to 10 mm, and most preferably 2 mm to 5 mm. The granules / pieces may be naturally occurring or may be made by artificial manipulation.

[0028] The term "high melting point emulsified wax" as used herein generally refers to:

[0029] - first, high melting point waxes are generally malleable over a fairly wide range of room temperature (i.e., about 5°C-45°C), and are liquid at substantially at least 50°C (but preferably at 80°C or higher), and all waxes are insoluble in water but soluble in organic non-polar solvents; and

[0030] -Secondly, include an emulsifier in the high melting point wax. Summary of the invention

[0031] The present invention is generally directed to a novel aqueous wax dispersion including dispersed clay that can be used to hold NBPT or other urease inhibitors / nitrification inhibitors in suspension for coating onto fertilizer granules.

[0032] According to a first aspect of the present invention, there is provided a water-based urease inhibitor and / or nitrification inhibitor coating formulation, comprising:

[0033] i) an aqueous wax dispersion comprising:

[0034] - essentially 10 to 50% by weight of a high melting point emulsified wax;

[0035] - Make up to 100% water;

[0036] ii) at least one inhibitor active substance;

[0037] wherein the amount of inhibitor active present is substantially: 1 wt% to 30 wt% of the aqueous wax dispersion;

[0038] iii) dispersed clay;

[0039] The amount of dispersed clay is 5wt%-50wt% of the aqueous wax dispersion.

[0040] According to a second aspect of the present invention there is provided an aqueous urease inhibitor and / or nitrification inhibitor coating formulation substantially as described above, wherein the formulation further comprises:

[0041] iv) xanthan gum or guar gum;

[0042] The amount of xanthan gum or guar gum is 0.25wt%-1wt% of the total urease inhibitor and / or nitrification formulation.

[0043] According to a third aspect of the present invention there is provided an aqueous urease inhibitor and / or nitrification inhibitor coating formulation substantially as described above wherein the high melting point emulsifying wax is a mineral wax or a vegetable based wax.

[0044] According to a fourth aspect of the present invention there is provided an aqueous urease inhibitor and / or nitrification inhibitor coating formulation substantially as described above wherein the mineral wax is montan wax.

[0045] According to a fifth aspect of the present invention there is provided an aqueous urease inhibitor and / or nitrification inhibitor coating formulation substantially as described above wherein the clay is inert and has a particle size of substantially 20 microns or less.

[0046] According to a sixth aspect of the present invention, there is provided a water-based urease inhibitor and / or nitrification inhibitor coating formulation, comprising:

[0047] i) an aqueous wax dispersion comprising:

[0048] - 10% by weight of high melting point emulsified wax, about 70 kg;

[0049] -90% water, about 630kg;

[0050] ii) an inhibitor active selected from the group consisting of: 210 kg NBPT; 210 kg DMPP; 210 kg NPPT; 210 kg DMPSA; or a mixture of 210 kg NBPT and DMPP;

[0051] iii) 100 kg dispersed clay;

[0052] iv) 2.5 kg xanthan gum.

[0053] According to a seventh aspect of the present invention, there is provided a water-based urease inhibitor and / or nitrification inhibitor coating formulation,

[0054] i) an aqueous wax dispersion comprising:

[0055] -30% by weight of high melting point emulsified aqueous wax, about 210 kg;

[0056] -70% water, about 490kg;

[0057] ii) 200kg NBPT or 200kg DMPP;

[0058] iii)100kg clay;

[0059] iv) 2.5 kg guar gum.

[0060] According to an eighth aspect of the present invention, there is provided an aqueous wax dispersion comprising:

[0061] - 10-50% of high melting point emulsified mineral wax or vegetable based wax;

[0062] -Fill up to 100% with water.

[0063] According to a ninth aspect of the present invention there is provided an aqueous wax dispersion comprising 1 wt% to 30 wt% NBPT based on the aqueous wax substantially as described above.

[0064] According to a tenth aspect of the present invention, there is provided an aqueous wax dispersion comprising an inhibitor active or a combination of a nitrification inhibitor and a urease inhibitor.

[0065] According to an 11th aspect of the present invention there is provided a wax dispersion substantially as described above wherein the mineral wax is montan wax.

[0066] According to a 12th aspect of the present invention, there is provided a wax dispersion substantially as described above, wherein the plant-based wax is selected from:

[0067] -Carnauba wax;

[0068] -Rice bran wax.

[0069] According to a 13th aspect of the present invention there is provided a fertilizer composition comprising a nutrient source in the form of fertilizer granules or tablets coated with an aqueous urease and / or nitrification inhibitor coating formulation substantially as described above.

[0070] According to a 14th aspect of the present invention there is provided a fertilizer composition substantially as described above wherein the composition comprises a further outer layer of MgO.

[0071] According to a 15th aspect of the present invention there is provided a fertilizer composition substantially as described above, wherein the amount of MgO added is 2% by weight of the total fertilizer composition including the MgO.

[0072] According to a 16th aspect of the present invention there is provided a fertilizer composition substantially as described above wherein the particle size of the MgO is substantially 45 microns or less.

[0073] According to a seventeenth aspect of the present invention there is provided a fertiliser composition substantially as described above wherein the fertiliser tablets or granules are urea.

[0074] According to the 18th aspect of the present invention, there is provided a fertilizer blend comprising an amount of a fertilizer composition substantially as described above, together with an amount of a fertilizer in granular or flaky form selected from:

[0075] - Single superphosphate;

[0076] -diammonium phosphate

[0077] - monoammonium phosphate (monoammonium phosphate);

[0078] - ammonium polyphosphate;

[0079] - ammonium sulfate;

[0080] - Potassium chloride;

[0081] -potassium sulfate;

[0082] -potassium carbonate; or

[0083] -potassium hydrochloride.

[0084] According to the 19th aspect of the present invention, there is provided a method for preventing NBPT and / or DMPP from reacting with acidic fertilizer particles, comprising the steps of:

[0085] a) suspending at least one inhibitor active in an aqueous wax dispersion;

[0086] b) applying the resulting suspension from step a) as a first layer onto fertilizer granules or tablets;

[0087] c) Applying a second layer of MgO on the first layer.

[0088] According to a 20th aspect of the present invention, there is provided a method for protecting NBPT coated on fertilizer particles from degradation by acidic fertilizers, characterized by the step of encapsulating the NBPT layer beneath a further MgO layer.

[0089] According to the 21st aspect of the present invention, there is provided a method for protecting NBPT and / or DMPP coated on fertilizer particles from degradation by acidic fertilizers, characterized in that the coating formulation for coating NBPT and / or DMPP (or other urease inhibitors / nitrification inhibitors) on the fertilizer particles includes MgO.

[0090] According to the 22nd aspect of the present invention, there is provided an aqueous coating composition comprising:

[0091] i) an aqueous wax dispersion comprising:

[0092] - essentially 10 to 50% by weight of a high melting point emulsified wax;

[0093] - Make up to 100% water;

[0094] ii) dispersed clay;

[0095] The amount of dispersed clay is 5wt%-50wt% of the aqueous wax dispersion.

[0096] According to a twenty-third aspect of the present invention there is provided an aqueous coating composition substantially as described above, which in addition to the aqueous wax dispersion and dispersed clay further comprises guar gum or xanthan gum.

[0097] According to the 24th aspect of the present invention, there is provided an aqueous wax dispersion comprising:

[0098] - a high melting point wax, substantially constituting 25% of the aqueous wax dispersion; and

[0099] - Water, substantially 75% of the aqueous wax dispersion.

[0100] Preferably, the high melting point wax may be montan wax.

[0101] According to the 25th aspect of the present invention, there is provided an aqueous wax dispersion substantially as described in the 24th aspect, which additionally comprises:

[0102] - NBPT, accounting for 30 wt% of the aqueous wax dispersion;

[0103] - Kaolin, 5 wt% of the aqueous wax dispersion. BRIEF DESCRIPTION OF THE DRAWINGS

[0104] Further aspects of the present invention will become apparent from the ensuing description given by way of example only and with reference to the accompanying drawings, in which:

[0105] Figure 1 shows NBPT levels of urea over time comparing the present invention to current commercially available solvent-based NBPT formulations;

[0106] Figure 2 Showing aqueous emulsified wax emulsions of the present invention, including 30 wt% NBPT, with and without gum;

[0107] Figure 3 shows an enclosed chamber for collecting volatilized ammonia from urea fertilizer applied to pasture; and

[0108] Figure 4 Total ammonia volatilization losses of the fertilizers studied during the first 7 days are shown. Error bars represent standard error of the mean. DETAILED DESCRIPTION

[0109] Example 1 - Preparation Method Part 1

[0110] The method for preparing the aqueous wax dispersion of the present invention comprises the steps of:

[0111] - Heat water to 95°C;

[0112] - Add powdered high melting point emulsified wax to hot water in a 50:50 ratio;

[0113] - Slowly stir the wax / water mixture until it is evenly dispersed;

[0114] - While slowly stirring, add water to the dissolved wax / water mixture to obtain the desired water-to-wax ratio;

[0115] - If necessary, cool or allow the aqueous wax dispersion to cool down to room temperature (ie 15°C - 20°C).

[0116] The aqueous wax dispersion produced as described above may be prepared in advance for later use and / or shipment / transportation.

[0117] Once the dispersion has cooled to room temperature, an inhibitor additive such as NBPT can be added.

[0118] Example 2 - Preparation Method Part 2

[0119] The method of preparing the aqueous inhibitor formulation comprises the steps of:

[0120] - Add powdered xanthate or powdered guar gum to the dispersed clay and blend together;

[0121] - Add the gum / clay premix to the aqueous wax dispersion from Example 1 while stirring slowly.

[0122] The aqueous wax dispersion produced as described above may be prepared in advance for later use and / or shipment / transportation.

[0123] - Once the gum / clay / wax dispersion has cooled to room temperature (about 15°C-25°C), you can start adding the inhibitor active to it.

[0124] Example 3

[0125] An aqueous urease inhibitor formulation having the following composition:

[0126] 970 kg aqueous wax dispersion, containing:

[0127] 97 kg LICOCARE RBW made by Clariant TM , see https: / / www.clariant.com / en / Business-Units / Additives / Waxes / Licocare-RBW, about 10 wt % of the aqueous wax dispersion;

[0128] 873kg water, make up to 100%;

[0129] 19.4 kg NBPT, accounting for about 2 wt % of the aqueous wax dispersion;

[0130] 48.5 kg of kaolin, accounting for about 5 wt % of the aqueous wax dispersion, wherein the kaolin has a particle size of 20 microns or less.

[0131] Example 4

[0132] An aqueous urease inhibitor formulation having the following composition:

[0133] 700kg aqueous wax dispersion, containing:

[0134] - 70 kg LICOWAX KST made by Clariant TM , see https: / / www.clariant.com / en / Solutions / Products / 2014 / 03 / 18 / 16 / 33 / Licowax-KST , accounting for 10wt% of the aqueous wax dispersion;

[0135] - 630 kg water, accounting for 90 wt % of the aqueous wax dispersion;

[0136] 210 kg NBPT, substantially accounting for 30 wt % of the aqueous wax dispersion;

[0137] 98 kg calcium bentonite, substantially accounting for 14 wt % of the aqueous wax dispersion;

[0138] 2.1 kg xanthan gum, substantially accounting for 0.3 wt % of the aqueous wax dispersion.

[0139] Example 5

[0140] An aqueous urease inhibitor formulation having the following composition:

[0141] 970 kg aqueous wax dispersion, containing:

[0142] - 485 kg LICOWAX KST made by Clariant TM , see https: / / www.clariant.com / en / Solutions / Products / 2014 / 03 / 18 / 16 / 33 / Licowax-KST , accounting for 50% of the aqueous wax dispersion;

[0143] - 485 kg of water, substantially accounting for 50% of the aqueous wax dispersion;

[0144] 291 kg of a 50:50 mixture of NBPT and DMPP, substantially 30 wt % of the aqueous wax dispersion;

[0145] 48.5 kg kaolin, substantially accounting for 5 wt % of the aqueous wax dispersion;

[0146] 0.97 kg guar gum, substantially 1 wt % of the aqueous wax dispersion.

[0147] As a final step, a pink dye may be added to help coat the fertilizer granules using the formulation.

[0148] Example 6

[0149] An aqueous wax dispersion having the following composition:

[0150] - 250 kg of LICOWAX KLE produced by Clariant, https: / / www.clariant.com / en / Solutions / Products / 2014 / 03 / 18 / 16 / 33 / Licowax-KLE-flakes , substantially 25% of said aqueous wax dispersion;

[0151] - 750 kg of water, substantially 75% of the aqueous wax dispersion.

[0152] Example 7

[0153] This is the aqueous emulsified wax dispersion of Example 6, but with the addition of:

[0154] - 300 kg NBPT, accounting for 30 wt% of the aqueous wax dispersion;

[0155] - 50 kg kaolin, representing 5 wt% of the aqueous wax dispersion.

[0156] Example 8

[0157] 1) Take 1000 kg of urea and place it in a rotating coating drum;

[0158] 2) adding 100 kg of the 0.3 urea aqueous formulation of Example 5 into urea, and starting the coating drum;

[0159] 3) Continue spinning the coating drum until all urea particles are coated with the 0.3 aqueous NBPT formulation, as evidenced once the coated particles change color to pink.

[0160] Example 9

[0161] Here, 980 kg of urea were first coated with the 0.3 NBPT aqueous formulation according to Example 8 and following the following additional steps:

[0162] 4) 20 kg of E45 powdered magnesium oxide was added to the coated urea having a 0.3 NBPT aqueous formulation layer thereon, and the coating drum was started again;

[0163] 5) When all urea particles are evenly coated with E45 magnesium oxide and flow freely, generally after about 2-3 minutes, the product can be taken out from the coating drum.

[0164] Example 10

[0165] Figure 1 Comparative results are shown when granular ammonium sulfate is mixed 50:50 with urea coated with:

[0166] - Commercially available solvent-based NBPT coatings; or

[0167] -0.3 NBPT aqueous wax dispersion of Example 7.

[0168] The amount of NBPT was assessed using HPLC at various time intervals from application to urea. It can be seen that the waterborne coating of the present invention (Southstar) retained NBPT on urea more effectively over a 24 hour period than the commercially available solvent-based NBPT coating.

[0169] Embodiment 11

[0170] Here, the coated urea according to Example 9 was mixed together with granular ammonium sulfate (GAS) in equal parts.

[0171] Example 12

[0172] Here, urea was coated with the aqueous wax dispersion of Example 7 in substantial accordance with the method of Example 8.

[0173] Importantly, since no gum is added to the wax dispersion, it is necessary to prepare the aqueous wax dispersion within 24 hours after production. Figure 2 The dispersion shown was coated with urea prior to isolation.

[0174] Example 13

[0175] An aqueous urease inhibitor formulation having the following composition:

[0176] 970 kg aqueous wax dispersion, containing:

[0177] -242.5kg LICOcare RBW TM , https: / / www.clariant.com / en / Business-Units / Additives / Waxes / Licocare-RBW , accounting for 50% of the aqueous wax dispersion;

[0178] - 727.5 kg of water, substantially accounting for 50% of the aqueous wax dispersion;

[0179] 58.2 kg NBPT, substantially 6 wt % of the aqueous wax dispersion;

[0180] 48.5 kg kaolin, substantially accounting for 5 wt % of the aqueous wax dispersion;

[0181] 0.97 kg guar gum, substantially 1 wt % of the aqueous wax dispersion.

[0182] Embodiment 14

[0183] A fertilizer composition comprising:

[0184] -Urea granules; coated with

[0185] - A layer of an aqueous urease inhibitor in the form of 0.3 NBPT on urea granules. For example, according to Example 5 above.

[0186] The application method for applying the aqueous NBPT layer to the urea granules was essentially the same as in Example 8, but with the 0.3 NBPT from Example 5 substituted appropriately.

[0187] Embodiment 15

[0188] A fertilizer composition according to Example 14, having a total weight of 1085 kg, and wherein the composition has undergone a further coating process to further include a further outer layer of E45 MgO covering the NBPT layer, wherein the amount of MgO used to coat the particles of Example 14 is 21.7 kg, accounting for 2% of the total weight of NBPT / MgO coated urea particles of 1106.7 kg.

[0189] The MgO coating was applied substantially as described in Example 9.

[0190] Example 16

[0191] Here, the coated urea of ​​Example 15 and single superphosphate (SSP) were mixed together in equal parts.

[0192] Embodiment 17

[0193] An aqueous urease inhibitor formulation having the following composition:

[0194] 970 kg aqueous wax dispersion, containing:

[0195] 485 kg carnauba wax, accounting for about 50 wt % of the aqueous wax dispersion;

[0196] 485kg water, replenished to 100%;

[0197] 19.4 kg NBPT, accounting for about 2 wt % of the aqueous wax dispersion;

[0198] 48.5 kg kaolin, accounting for about 5 wt % of the aqueous wax dispersion.

[0199] Embodiment 18

[0200] An aqueous urease inhibitor formulation having the following composition:

[0201] 970 kg aqueous wax dispersion, containing:

[0202] 97kg LICOCARE RBW TM , https: / / www.clariant.com / en / Business-Units / Additives / Waxes / Licocare-RBW , accounting for about 10 wt % of the aqueous wax dispersion;

[0203] 873kg water, make up to 100%;

[0204] 9.2 kg DMPP, accounting for about 1 wt % of the aqueous wax dispersion;

[0205] 485 kg of kaolin, accounting for about 50 wt % of the aqueous wax dispersion, wherein the kaolin has a particle size of 20 microns or less.

[0206] Embodiment 19

[0207] An aqueous urease inhibitor formulation having the following composition:

[0208] 970 kg of an aqueous wax dispersion comprising:

[0209] 485 kg of montan wax, accounting for about 50 wt % of the aqueous wax dispersion;

[0210] 485kg water, replenished to 100%;

[0211] 19.4 kg NPPT and NBPT (50:50 ratio), accounting for about 2 wt % of the aqueous wax dispersion;

[0212] 48.5 kg kaolin, accounting for about 5 wt % of the aqueous wax dispersion.

[0213] Embodiment 20

[0214] This example relates to independent research on the present invention conducted by Lincoln University.

[0215] The objective of this study was to determine ammonia volatilization losses from urea fertilizers containing different urease inhibitor formulations on soils with typical forage plant cover.

[0216] Experimental design and conditions

[0217] The standard gas capture system used in this study was similar to that used in previous ammonia volatilization studies conducted at Lincoln University. Briefly, soil blocks (20 cm diameter x 6 cm deep) were taken from pasture on the Lincoln University research dairy farm. The intact blocks contained a representative dairy pasture soil (Templeton Sandy Loam) with typical pasture cover (perennial ryegrass / white clover). The blocks were transferred to the Lincoln University outdoor research facility where they were placed in an area adjacent to the ammonia measurement facility. Stainless steel rings (20 cm diameter x 15 cm deep) were inserted 7.5 cm into the ground to surround each individual block. The area outside the fence was also pasture to simulate standard field conditions. A clear plexiglass lid was installed on the top of each fence. Each fence had inlet and outlet holes to allow air to pass through the chamber ( Figure 1 The outlet was connected to an acid gas capture system via PVC tubing to collect ammonia. The system was calibrated and tested before the start of the experiment.

[0218] Soil moisture in the pens was adjusted to field capacity with water before treatment application. Five treatments were applied in a completely randomized design, with four chambers assigned to each treatment (Table 1). Before application, fertilizer granules were sieved to the same diameter (1-2 mm) to prevent potential bias due to differences in surface area caused by granule size.

[0219] All fertilizer treatments were broadcast at a rate of 50 kg-N ha-1.

[0220]

[0221]

[0222] Ammonia gas from each chamber was collected continuously and 10% of the total flow was directed through a manifold to a gas trap where it was trapped in 0.05 M sulfuric acid.

[0223] Samples were collected between 3:00 PM and 5:00 AM each day and a fresh volume of 0.05 M sulfuric acid was placed in the acid trap. The collected samples were then taken to the Lincoln University Analytical Laboratory and analyzed for ammonium concentration using a flow injection analysis method. Daily air and soil temperatures were recorded during the trial.

[0224] result

[0225] Immediately after application to pasture, strong ammonia efflux was observed with standard urea fertilizer, reaching 4.4 kg NH3-N ha-1. Strong volatilization losses continued for about 4 days, after which daily emissions dropped to less than 1 kg NH3-N ha-1 day-1.

[0226] In contrast, the application of the two urease inhibitor fertilizers had no initial peak compared with standard urea, and the emissions occurred at a relatively steady rate, mostly not exceeding 1 kg NH3-N ha-1 day-1.

[0227] like Figure 4 As shown, the initial strong ammonia emission of standard urea resulted in significant cumulative losses within the first week after application. Specifically, the standard urea treatment lost 24.8% of the fertilizer N in the first week. The losses were smaller after the first week, which can be attributed to the partial immobilization and conversion of volatile ammonia to non-volatile forms. For urea + NBPT coating + 2% Mg and urea + NBPT coating, the total N losses as ammonia in the fertilizers treated with urease inhibitors were significantly reduced in the first 7 days. This corresponds to a 68% and 55% reduction in ammonia losses in the urease inhibitor products compared to standard urea.

[0228] The data from the week after application is the most important indicator of the value of urease inhibitor fertilizers compared to standard urea because it is very likely that rainfall will occur in most parts of New Zealand within or after the week. The probability of rainfall within 7 days is shown in Table 2.

[0229] Table 2 Average number of rainy days per month in New Zealand*

[0230]

[0231] *Data are monthly averages from 1981 to 2010

[0232] (Source: niwa.co.nz / sites / default / files / mean_monthly_wet-days.xlxs)

[0233] After 7 days, the ammonia losses of the different N fertilizers became similar.

[0234] in conclusion

[0235] This experiment showed that a urease inhibitor (NBPT) fertilizer formulation applied at a rate of 50 kg-N / ha significantly reduced ammonia volatilization losses compared to standard urea applied at the same rate. The efficacy of the four different formulations was similar. The benefits of the urease inhibitor were most evident in the first week after application, where NBPT reduced the rate of urea hydrolysis and prevented the strong ammonia efflux typical of standard urea.

[0236] Further Discussion of the Invention Including Non-Limiting Alternative Ways of Implementing the Invention

[0237] The high melting point waxes may generally be mineral waxes or vegetable based waxes.

[0238] The importance of high melting point waxes can be expressed as the need to ensure that the wax does not melt when exposed to direct sunlight and maintain the free-flowing integrity of the flakes / particles coated using the invention. If these characteristics are not important for a given application of the invention, waxes with a melting point of substantially 50°C can be used.

[0239] In a preferred embodiment, the mineral wax may be montan wax (also known as Lignite wax).

[0240] In other preferred embodiments, the high melting point wax may be selected from rice bran wax or carnauba wax.

[0241] In another embodiment, the mineral wax may be paraffin wax.

[0242] In some preferred embodiments, the high melting point emulsifying wax may be in powder form and is selected from:

[0243] LICOWAX KST TM (made from montan wax);

[0244] LICOCARE RBW TM (made from rice bran wax);

[0245] LICOWAX KLE TM (Made from montan wax).

[0246] All are manufactured and sold by Clariant, and more detailed information can be obtained from the web links mentioned in the Examples section above.

[0247] The present inventors have found that if the wax is present at substantially 60% and water at 40%, the resulting viscosity is similar to that of syrup and is therefore unsuitable as a suspension formulation for coating fertilizers.

[0248] While waxes are used herein, it should be understood that resins or hydrogenated oils having properties similar to the high melting point waxes used herein may also be used.

[0249] Many emulsifiers may be suitable for addition to the high melting point wax, such as those apparent to those skilled in the art, including anionic and nonionic emulsifiers or combinations thereof. A suitable emulsifier may be polysorbate 60 and / or PEG 150. Other examples of suitable emulsifiers that may be employed are described in McCutcheons, 2018 Emulsifiers Detergents, North American Edition.

[0250] The dispersed clay may be any clay having a particle size less than 20 microns and which is inert.

[0251] In one embodiment, the dispersed clay may be kaolin.

[0252] In one embodiment, 90% of the kaolin particles may be less than 10 microns in size.

[0253] In another embodiment, the dispersed clay is calcium bentonite, which may have a particle size of less than 20 microns.

[0254] Clays and waxes play an important role in the formulation because the inventors unexpectedly discovered that they can keep NBPT and other inhibitor actives stably suspended in water. This is because NBPT usually crystallizes in the presence of water.

[0255] The inventors have also discovered that guar gum or xanthan gum not only plays a key role as a thickener, providing a subtle increase in the viscosity of the formulation, but also enables NBPT or other inhibitor actives to remain suspended for a long period of time, for 3 to 6 months.

[0256] In particular, guar gum or xanthan gum holds the clay and NPBT in a uniform suspension with the wax. Without the gum, the NBPT and clay would separate from the wax to form a lower emulsion layer, while the wax forms an upper emulsion layer.

[0257] Generally speaking, when the formulation of the invention is to be used as a coating, it may also include a colored dye, which can serve as a visual indicator that the particles have been coated. Colored dyes may also be useful to show that a desired blend is present.

[0258] In a broad sense, the invention may also be said to consist in the parts, elements and features mentioned or indicated in the specification of the present application, individually or collectively, and in any or all combinations of two or more of the parts, elements or features, individually or collectively.

[0259] Aspects of the present invention have been described by way of example only, and it should be appreciated that modifications and additions may be made thereto without departing from the scope of the invention as defined in the appended claims.

Claims

1. A water-based urease inhibitor and / or nitrification inhibitor coating formulation, comprising: i) an aqueous wax dispersion comprising: 10-50% by weight of high melting point emulsified wax, Make up to 100% water; ii) at least one inhibitor active selected from NBPT, DMPP, NPPT and / or DMPSA, wherein the amount of the inhibitor active is: 1 wt% - 30 wt% of the aqueous wax dispersion in i); iii) Dispersed clay, wherein the amount of dispersed clay is 5wt%-50wt% of the aqueous wax dispersion in i); and iv) xanthan gum or guar gum, The amount of xanthan gum or guar gum is 0.25wt%-1wt% of the aqueous wax dispersion in i), And wherein the high melting point emulsified wax is: - montan wax or carnauba wax; or - Rice bran wax.

2. The waterborne urease inhibitor and / or nitrification inhibitor coating formulation according to claim 1, wherein the dispersed clay is inert and has a particle size of 20 microns or less.

3. A water-based urease inhibitor and / or nitrification inhibitor coating formulation comprising: i) an aqueous wax dispersion comprising: 10 wt% high melting point emulsified wax, 70 kg, 90% water, 630 kg; ii) an inhibitor active selected from one of the following: 210 kg NBPT, 210 kg DMPP, 210 kg NPPT, 210 kg DMPSA, or 210 kg of a 50:50 mixture of NBPT and DMPP; iii) 100 kg dispersed clay; and iv) 2.5kg xanthan gum, Wherein the high melting point emulsified wax is: - montan wax or carnauba wax; or - Rice bran wax.

4. A water-based urease inhibitor and / or nitrification inhibitor coating formulation comprising: i) an aqueous wax dispersion comprising: 30 wt% high melting point emulsified wax, 210 kg, 70% water, 490 kg; ii) 200kg NBPT or 200kg DMPP; iii) 100 kg dispersed clay; and iv) 2.5 kg guar gum, Wherein the high melting point emulsified wax is: - montan wax or carnauba wax; or - Rice bran wax.

5. A fertilizer composition comprising a nutrient source in the form of fertilizer granules or tablets coated with the aqueous urease inhibitor and / or nitrification inhibitor coating formulation of any one of the preceding claims.

6. The fertilizer composition of claim 5, wherein the fertilizer composition comprises an outer layer of MgO.

7. The fertilizer composition according to claim 6, wherein the amount of MgO added is 2% of the total weight of the fertilizer composition including MgO.

8. The fertilizer composition of claim 6, wherein the particle size of MgO is 45 microns or less.

9. A fertilizer composition according to any one of claims 5 to 8, wherein the fertilizer granules or flakes are urea.

10. A fertilizer blend comprising the fertilizer composition of claim 8 and a fertilizer in the form of granules or tablets selected from the following: - Single superphosphate; - Diammonium phosphate; - Monoammonium phosphate; - ammonium polyphosphate; - Ammonium sulfate; - Potassium chloride; - Potassium sulfate; - Potassium carbonate; or - Potassium hydrochloride.

11. A method for preventing NBPT and / or DMPP from reacting with acidic fertilizer particles, comprising the steps of: a) applying the aqueous urease inhibitor and / or nitrification inhibitor coating formulation of claim 1 as a first layer onto fertilizer or mineral granules or flakes; and b) Applying a second layer of MgO on the first layer.

12. A water-based urease inhibitor and / or nitrification inhibitor coating formulation comprising: i) an aqueous wax dispersion comprising: 10-50% by weight of high melting point emulsified wax, Make up to 100% water; ii) at least one inhibitor active selected from NBPT, DMPP, NPPT and / or DMPSA, wherein the amount of the inhibitor active is: 1 wt% - 30 wt% of the aqueous wax dispersion in i); iii) Dispersed clay, wherein the amount of dispersed clay is 5wt%-50wt% of the aqueous wax dispersion in i); and iv) xanthan gum or guar gum, The amount of xanthan gum or guar gum is 0.25wt%-1wt% of the aqueous wax dispersion in i), And wherein the high melting point emulsified wax is: A wax that is ductile at 5°C - 45°C and liquid at at least 50°C, and all waxes are insoluble in water but soluble in organic non-polar solvents, and emulsifiers are added to high melting point waxes.

13. A water-based urease inhibitor and / or nitrification inhibitor coating formulation comprising: i) an aqueous wax dispersion comprising: 10 wt% high melting point emulsified wax, 70 kg, 90% water, 630 kg; ii) an inhibitor active selected from one of the following: 210 kg NBPT, 210 kg DMPP, 210 kg NPPT, 210 kg DMPSA, or 210 kg of a 50:50 mixture of NBPT and DMPP; iii) 100 kg dispersed clay; and iv) 2.5kg xanthan gum, Wherein the high melting point emulsified wax is: A wax that is ductile at 5°C - 45°C and liquid at at least 50°C, and all waxes are insoluble in water but soluble in organic non-polar solvents, and emulsifiers are added to high melting point waxes.

14. A water-based urease inhibitor and / or nitrification inhibitor coating formulation comprising: i) an aqueous wax dispersion comprising: 30 wt% high melting point emulsified wax, 210 kg, 70% water, 490 kg; ii) 200kg NBPT or 200kg DMPP; iii) 100 kg dispersed clay; and iv) 2.5 kg guar gum, Wherein the high melting point emulsified wax is: A wax that is ductile at 5°C - 45°C and liquid at at least 50°C, and all waxes are insoluble in water but soluble in organic non-polar solvents, and emulsifiers are added to high melting point waxes.