Epoxy resin composition, cured product, and electrical / electronic component

By adjusting the composition and processing methods of epoxy resin, an epoxy resin composition with excellent electrical and optical properties is generated, which solves the problems of insufficient transparency, curability and heat resistance of epoxy resin in the existing technology, and achieves High-performance electrical/electronic components and optical materials.

CN114222789BActive Publication Date: 2024-10-22MITSUBISHI CHEM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080052013.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-08-22
Filing Date
2020-08-07
Publication Date
2024-10-22
Estimated Expiration
2040-08-07

AI Technical Summary

Technical Problem

Existing hydrogenated bisphenol epoxy resins are still insufficient to meet the increasingly stringent requirements of the electronics industry in terms of transparency, curability, crack resistance and heat resistance in the optical field.

Method used

Using an epoxy resin composition of a specific composition, by adding connecting groups such as isopropylene to the aromatic epoxy resin, controlling the proportion and chlorine content of the epoxy resin, combined with appropriate hydrogenation reaction and distillation treatment, the product has excellent properties. An epoxy resin composition with electrical and optical properties and mixed with a curing agent to improve curability and heat resistance.

Benefits of technology

It has achieved an epoxy resin composition with excellent electrical properties, optical properties, curability and heat resistance, which is suitable for high-performance electrical/electronic components and optical materials and meets the strict requirements of the modern electronics industry for material performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114222789B_ABST
    Figure CN114222789B_ABST
Patent Text Reader

Abstract

An epoxy resin composition, comprising an epoxy resin (1) having a structure represented by the following formula (1), an epoxy resin (2) having a structure represented by the following formula (2), and / or an epoxy resin (3) having a structure represented by the following formula (3). In the total of 100% by mass of the epoxy resin (1) and the epoxy resin (2) and / or the epoxy resin (3), the epoxy resin (1) is contained in an amount of 89.0 to 99.9% by mass, and the epoxy resin (2) and / or the epoxy resin (3) is contained in an amount of 0.1 to 11.0% by mass. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an epoxy resin composition, a cured product, and an electrical / electronic component. Specifically, the present invention relates to an epoxy resin composition (A) having excellent electrical and optical properties; an epoxy resin composition (B) having excellent curability obtained by mixing a curing agent into the epoxy resin composition (A); and a cured product and an electrical / electronic component having excellent crack resistance and heat resistance obtained by curing the epoxy resin composition (B). Background Art

[0002] Epoxy resins are generally cured with various curing agents to form cured products with excellent mechanical properties, heat resistance, electrical properties, etc., and are therefore used in a wide range of fields such as adhesives, coatings, and electrical / electronic materials. In particular, hydrogenated bisphenol epoxy resins obtained by hydrogenating aromatic epoxy resins are widely used in the optical field.

[0003] Patent Document 1 describes a method for producing a glycidyl group-containing alicyclic compound having a low chlorine content in the presence of an ether group-containing alcohol, and an epoxy resin composition containing the glycidyl group-containing alicyclic compound having excellent electrical insulation and weather resistance and low viscosity.

[0004] Patent Document 2 discloses a method for producing a hydrogenated bisphenol epoxy resin by cyclohydrogenating a bisphenol A epoxy resin and a bisphenol F epoxy resin in the presence of a specific heterogeneous ruthenium catalyst supported on silica.

[0005] Patent Document 3 describes a method for producing an alicyclic epoxy compound having improved color tone by selectively hydrogenating the aromatic ring of an aromatic epoxy compound in the presence of a hydrogenation catalyst and then reacting the compound in the presence of a reaction solvent containing an ester solvent at a content of 50% by mass.

[0006] Patent Document 1: Japanese Patent Application Publication No. 2002-97251

[0007] Patent Document 2: Japanese Patent Application No. 2007-515276

[0008] Patent Document 3: Japanese Patent Application Publication No. 2003-212955

[0009] In recent years, with the remarkable development of the electronics industry, the requirements for electrical properties, optical properties, curability, crack resistance, and heat resistance required of optical materials have become increasingly stringent.

[0010] The hydrogenated bisphenol epoxy resins described in Patent Documents 1 to 3 are still insufficient in optical properties such as transparency, curability when a cured product is prepared, crack resistance of the cured product, heat resistance, etc. Summary of the invention

[0011] The object of the present invention is to provide: an epoxy resin composition (A) having excellent electrical and optical properties; an epoxy resin composition (B) comprising the epoxy resin composition (A) and having excellent curing properties; and a cured product and electrical / electronic components having excellent crack resistance and heat resistance obtained by curing the epoxy resin composition (B).

[0012] The present inventors have found that an epoxy resin composition (A) having a specific composition and an epoxy resin composition (B) comprising the epoxy resin composition (A) and a curing agent can solve the above-mentioned problems, thereby completing the present invention.

[0013] That is, the gist of the present invention lies in the following [1] to [9].

[0014] [1] An epoxy resin composition (A), comprising an epoxy resin having a structure represented by the following formula (1) (hereinafter referred to as “epoxy resin (1)”), an epoxy resin having a structure represented by the following formula (2) (hereinafter referred to as “epoxy resin (2)”), and / or an epoxy resin having a structure represented by the following formula (3) (hereinafter referred to as “epoxy resin (3)”), wherein the epoxy resin (1) is contained in an amount of 89.0 to 99.9% by mass and the epoxy resin (2) and / or the epoxy resin (3) is contained in an amount of 0.1 to 11.0% by mass based on 100% by mass of the total of the epoxy resin (1), the epoxy resin (2), and / or the epoxy resin (3).

[0015] [Chemistry 1]

[0016]

[0017] In the above formulae (1), (2) and (3), X is a divalent linking group selected from a direct bond, -SO2-, -O-, -CO-, -C(CF3)2-, -S- or a hydrocarbon group having 1 to 20 carbon atoms. 1 is a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, or a halogen element, which may be the same or different from each other. The two R atoms bonded to adjacent carbon atoms on the cyclohexane ring are 1 They may be bonded to each other to form a ring structure having 4 to 20 carbon atoms. n is an integer of 0 to 2.

[0018] [2] The epoxy resin composition (A) as described in [1], wherein in the above formulas (1) to (3), X is an isopropylidene group, and R 1 is a hydrogen atom, and n is 0.

[0019] [3] The epoxy resin composition (A) according to [1] or [2], wherein the total chlorine content (based on JIS K7043-3) is 1000 ppm or less.

[0020] [4] The epoxy resin composition (A) according to any one of [1] to [3], wherein the epoxy equivalent is 176 to 186 g / equivalent.

[0021] [5] The epoxy resin composition (A) according to any one of [1] to [4], wherein the Hazen color value (APHA value: in accordance with ISO 6271-2:2004) is 12 or less.

[0022] [6] An epoxy resin composition (B) comprising 0.01 to 1000 parts by mass of a curing agent based on 100 parts by mass of the epoxy resin composition (A) according to any one of [1] to [5].

[0023] [7] A cured product obtained by curing the epoxy resin composition (B) described in [6].

[0024] [8] An electric / electronic component obtained by curing the epoxy resin composition (B) described in [6].

[0025] [9] An optical component obtained by curing the epoxy resin composition (B) described in [6].

[0026] Effects of the Invention

[0027] According to the present invention, there can be provided an epoxy resin composition (A) having excellent electrical and optical properties; an epoxy resin composition (B) comprising the epoxy resin composition (A) and having excellent curing properties; and a cured product and electrical / electronic components having excellent crack resistance and heat resistance obtained by curing the epoxy resin composition (B). DETAILED DESCRIPTION

[0028] The following is an example of an embodiment of the present invention, and the present invention is not limited to the following contents unless it exceeds the gist thereof.

[0029] When the expression "to" is used in this specification, it is used as an expression including numerical values ​​or physical property values ​​before and after it.

[0030] [Epoxy resin composition (A)]

[0031] The epoxy resin composition (A) of the present invention is characterized in that it is an epoxy resin composition comprising an epoxy resin having a structure represented by the following formula (1) (hereinafter sometimes referred to as "epoxy resin (1)"), an epoxy resin having a structure represented by the following formula (2) (hereinafter sometimes referred to as "epoxy resin (2)"), and / or an epoxy resin having a structure represented by the following formula (3) (hereinafter sometimes referred to as "epoxy resin (3)"), wherein the epoxy resin (1) is contained in an amount of 89.0 to 99.9% by mass and the epoxy resin (2) and / or the epoxy resin (3) is contained in an amount of 0.1 to 11.0% by mass based on 100% by mass of the total of the epoxy resin (1) and the epoxy resin (2) and / or the epoxy resin (3).

[0032] Hereinafter, the proportion of epoxy resin (1) in the total 100 mass % of epoxy resin (1) and epoxy resin (2) and / or epoxy resin (3) is sometimes referred to as the "epoxy resin (1) content", and the proportion of epoxy resin (2) and / or epoxy resin (3) in the total 100 mass % of epoxy resin (1) and epoxy resin (2) and / or epoxy resin (3) is sometimes referred to as the "epoxy resin (2) / (3) content".

[0033] [Chemistry 2]

[0034]

[0035] In the above formulae (1), (2) and (3), X is a divalent linking group selected from a direct bond, -SO2-, -O-, -CO-, -C(CF3)2-, -S- or a hydrocarbon group having 1 to 20 carbon atoms. 1 is a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, or a halogen element, which may be the same or different from each other. The two R atoms bonded to adjacent carbon atoms on the cyclohexane ring are 1 They may be bonded to each other to form a ring structure having 4 to 20 carbon atoms. n is an integer of 0 to 2.

[0036] The epoxy resin composition (A) of the present invention is defined as an "epoxy resin composition" because it contains multiple components such as epoxy resin (1) and epoxy resin (2) and / or epoxy resin (3). However, in the technical field of epoxy resins, "epoxy resins" are sometimes obtained in the form of "compositions" composed of multiple components in addition to epoxy resins composed of a single component. Therefore, the epoxy resin composition (A) of the present invention is sometimes also described as "epoxy resin" or sold as "epoxy resin" in the industry or on the market. In addition, "epoxy compounds (uncured materials)" are referred to as "epoxy resins" in the industry.

[0037] In the above formulae (1) to (3), X is preferably a direct bond or a hydrocarbon group having 1 to 10 carbon atoms, more preferably a direct bond, a methylene group, or an isopropylene group, and most preferably X is an isopropylene group.

[0038] R 1 It is preferably a hydrogen atom or a methyl group, and most preferably a hydrogen atom.

[0039] In the above formulae (1) to (3), n is preferably 0 to 1, and most preferably 0. As n increases, the molecular weight increases, and thus the viscosity and softening temperature increase, and the handling properties may deteriorate.

[0040] Regarding the multiple R in formula (1) 1 When n is 1 or more, all of the multiple Xs present may be the same or different. However, when the epoxy resin (1) is distilled, the different compounds may have different boiling points, which makes the distillation difficult. Therefore, they are preferably the same. 1 The same goes for X.

[0041] X and R in formulas (1) to (3) 1 , n may be the same or different in formula (1) to formula (3), but from the perspective of ease of adjusting the content of each component in the epoxy resin composition (A) and ease of production, it is preferred that X, R in each structural formula be 1 , n is the same in formula (1) to formula (3).

[0042] [Composition of epoxy resin composition (A)]

[0043] The epoxy resin composition (A) of the present invention has the following characteristics from the viewpoint of obtaining excellent electrical properties, optical properties, and excellent curability, crack resistance, and heat resistance of the epoxy resin composition (B) described later containing a curing agent: the epoxy resin (1) and the epoxy resin (2) and / or the epoxy resin (3), wherein 89.0 to 99.9% by mass of the epoxy resin (1) and 0.1 to 11.0% by mass of the epoxy resin (2) and / or the epoxy resin (3) are contained in 100% by mass of the total of the epoxy resin (1) and the epoxy resin (2) and / or the epoxy resin (3). When the content of the epoxy resin (1) increases and the content of the epoxy resin (2) and / or the epoxy resin (3) decreases, the Hazen color value of the epoxy resin composition (A) tends to decrease, but the crack resistance is improved due to the increase in crosslinking density and the decrease in linear expansion coefficient when the epoxy resin composition (B) is prepared, and the heat resistance is improved due to the increase in glass transition temperature. On the other hand, when the content of the epoxy resin (1) is reduced and the content of the epoxy resin (2) and / or the epoxy resin (3) is increased, the crack resistance and heat resistance of the epoxy resin composition (B) tend to be deteriorated.

[0044] From the perspective of more effectively obtaining the effects of the present invention brought about by the epoxy resin (1) and the epoxy resin (2) and / or the epoxy resin (3), it is preferred that the epoxy resin (1) content is 90.0 to 99.0 mass % and the epoxy resin (2) and / or the epoxy resin (3) content is 1.0 to 10.0 mass %, more preferably the epoxy resin (1) content is 92.0 to 98.0 mass % and the epoxy resin (2) and / or the epoxy resin (3) content is 2.0 to 8.0 mass %, and particularly preferably the epoxy resin (1) content is 95.0 to 98.0 mass % and the epoxy resin (2) and / or the epoxy resin (3) content is 2.0 to 5.0 mass %.

[0045] In the epoxy resin composition (A) of the present invention, the ratio of the epoxy resin (2) and / or the epoxy resin (3) to the epoxy resin (1) is preferably 0.1 to 13% by mass, more preferably 1 to 12% by mass.

[0046] Epoxy resin (2) and epoxy resin (3) have the same molecular weight and number of hydroxyl groups, and it is difficult to distinguish them and analyze their contents, so they are described as "epoxy resin (2) and / or epoxy resin (3)" in the present invention. The epoxy resin composition (A) of the present invention may contain only one of epoxy resin (2) and epoxy resin (3), or may contain both of epoxy resin (2) and epoxy resin (3). According to the method for producing the epoxy resin composition (A) of the present invention described later, an epoxy resin composition (A) containing both epoxy resin (2) and epoxy resin (3) is generated. Since it is difficult to separate epoxy resin (2) and epoxy resin (3) by purification, when producing epoxy resin composition (A) on an industrial scale, it is easier to analyze the content in the form of "epoxy resin (2) and / or epoxy resin (3)" than to analyze the contents of each of epoxy resin (2) and epoxy resin (3) in epoxy resin composition (A).

[0047] The epoxy resin composition (A) of the present invention may generally contain other components in addition to the epoxy resins (1) to (3).

[0048] Other components refer to chlorine impurities produced as by-products during the reaction process in the above formulas (1) to (3) generated during the production process of the epoxy resin composition (A) of the present invention. Chlorine impurities are a general term for organic substances and compounds containing chlorine atoms (Cl), for example, compounds containing chlorine atoms in the structural formula produced as by-products during the production of the epoxy resin composition (A).

[0049] The content of other components in the epoxy resin composition (A) of the present invention is preferably 3% by mass or less, more preferably 2% by mass or less, and further preferably 1% by mass or less. The greater the content of other components, the less it is possible to ensure the necessary content of epoxy resins (1) to (3), and the electrical properties, optical properties, curability, crack resistance, and heat resistance of the epoxy resin composition (B) cannot be fully improved.

[0050] When the epoxy resin composition (A) of the present invention contains other components, the total of the epoxy resins (1) to (3) and other components is 100% by mass.

[0051] The contents of the epoxy resins (1) to (3) and other components in the epoxy resin composition (A) of the present invention can be measured, for example, using gel permeation chromatography analysis (hereinafter referred to as GPC analysis) under the following conditions.

[0052] Device: Tosoh HLC-8220L GPC

[0053] Detector: RI

[0054] Mobile phase: Tetrahydrofuran (containing BHT)

[0055] Flow rate: 0.8 mL / min

[0056] Column: Tosoh TSKgel G2000Hxl+G1000Hxl×2

[0057] Column temperature: 40°C

[0058] [Epoxy equivalent]

[0059] In the epoxy resin composition (A) of the present invention, the epoxy equivalent is preferably 178 to 186 g / equivalent from the perspective of obtaining excellent curability, crack resistance, and heat resistance as the epoxy resin composition (B) containing a curing agent, and is more preferably 178 to 181 g / equivalent from the perspective of further improving the above characteristics. It is known that by making the epoxy equivalent within the above specific range, excellent above characteristics can be obtained.

[0060] The "epoxy equivalent" in the present invention is defined as "the mass of an epoxy resin containing 1 equivalent of epoxy groups", and can be measured in accordance with JIS K7236-1955.

[0061] [Hazen color value]

[0062] In the epoxy resin composition (A) of the present invention, the Hazen color value is preferably 12 or less from the perspective of obtaining excellent optical properties as an epoxy resin, and is more preferably 9 or less, and particularly preferably 8 or less from the perspective of further improving the optical properties. It is believed that by making the Hazen color value below the above upper limit, excellent optical properties can be obtained. The lower the Hazen color value, the more preferred, and there is no particular restriction on the lower limit.

[0063] The "Hazen color value" in the present invention can be measured according to ISO 6271-2:2004.

[0064] [Total chlorine content]

[0065] In the epoxy resin composition (A) of the present invention, from the aspect of obtaining excellent electrical reliability as epoxy resin, the total chlorine content is preferably 1000ppm (mass ppm) or less, and from the aspect of further improving electrical reliability, the total chlorine content is more preferably 750ppm or less, particularly preferably 700ppm or less. By making the total chlorine content below the above upper limit, electrical properties, optical properties, and cured products with excellent curing properties, crack resistance, and heat resistance when the epoxy resin composition (B) containing a curing agent is prepared can be provided. The lower the total chlorine content, the more preferred it is, and there is no particular restriction on its lower limit.

[0066] The "total chlorine content" is the content of chlorine atoms (Cl) contained in the epoxy resin composition (A).

[0067] The "total chlorine content" in the present invention can be measured in accordance with JIS K7243-3.

[0068] [Method for producing epoxy resin composition (A)]

[0069] <Raw material aromatic epoxy resin>

[0070] The method for producing the epoxy resin composition (A) of the present invention is not particularly limited, but it is preferred to produce the epoxy resin composition (A) of the present invention by hydrogenation reaction using an aromatic epoxy resin as a raw material because the epoxy resin composition (A) of the present invention can be obtained efficiently.

[0071] As the aromatic epoxy resin preferably used as the raw material, there can be mentioned an epoxy resin having a structure represented by the following formula (4) (hereinafter sometimes referred to as "aromatic epoxy resin (4)").

[0072] [Chemistry 3]

[0073]

[0074] In the above formula (4), R 1 , X, and n have the same meanings as in formula (1) to formula (3).

[0075] As specific examples of aromatic epoxy resins (4), the following can be cited as preferred: bisphenol-type epoxy resins such as bisphenol A epoxy resin, bisphenol F epoxy resin, 3,3',5,5'-tetramethyl-4,4'-biphenol epoxy resin, and 4,4'-biphenol epoxy resin; bisphenol A novolac epoxy resin; and naphthalene diol epoxy resin. Among them, bisphenol A epoxy resin is more preferred. These aromatic epoxy resins (4) can be used alone or in combination of two or more.

[0076] As the aromatic epoxy resin (4), it is preferred to use one having the following quality because it is suitable as a raw material before the hydrogenation reaction for efficiently obtaining the epoxy resin composition (A) of the present invention.

[0077] From the viewpoint of making the content of the epoxy resin (1) in the epoxy resin composition (A) within the above-mentioned preferred range, the epoxy equivalent of the aromatic epoxy resin (4) is preferably 165 to 194 g / equivalent.

[0078] From the viewpoint of making the total chlorine content of the epoxy resin composition (A) 1000 ppm or less, the total chlorine content of the aromatic epoxy resin (4) is preferably 2000 ppm or less, particularly preferably 1500 ppm or less.

[0079] <Distillation of Aromatic Epoxy Resins>

[0080] The epoxy resin composition (A) of the present invention is preferably produced by hydrogenating an aromatic epoxy resin (4). From the perspective of easily controlling the ratio and content of the epoxy resins (1) to (3) in the epoxy resin composition (A) and further facilitating the control of the total chlorine content, it is preferred that the aromatic epoxy resin (4) be distilled before subjecting the aromatic epoxy resin (4) to the hydrogenation reaction.

[0081] In this case, the distillation time is not particularly limited, but is preferably 5 to 30 hours, more preferably 6 to 15 hours.

[0082] The temperature and pressure during distillation are not particularly limited, but the temperature is preferably 130 to 240° C., more preferably 210 to 230° C. If the distillation temperature is too high, the aromatic epoxy resin (4) may decompose. If the distillation temperature is too low, the reduced pressure must be high vacuum, so it cannot be said to be an industrially advantageous method.

[0083] Regarding the distillation pressure, the degree of reduced pressure is preferably 0.001 to 1 Torr, more preferably 0.001 to 0.01 Torr.

[0084] The distillation is preferably carried out at a fraction of 70% or less, for example, 40 to 60%. When the distillation is carried out at a fraction exceeding 70%, the oligomer component of the aromatic epoxy resin (4) increases, and it tends to be difficult to control the content of each component of the epoxy resin composition (A) of the present invention within the above-mentioned preferred range.

[0085] The distillation method is not particularly limited, but distillation using a thin film distiller is preferred.

[0086] The physical properties of the aromatic epoxy resin (4) obtained by distillation are not particularly limited, but the epoxy equivalent is preferably 165 to 180 g / equivalent from the perspective of making it easy to adjust the content of the epoxy resin (1) in the epoxy resin composition (A) to the above-mentioned preferred range. The total chlorine content is preferably 1500 ppm or less, particularly preferably 1000 ppm or less.

[0087] <Hydrogenation reaction>

[0088] The hydrogenation catalyst used in the hydrogenation reaction is preferably a catalyst with a platinum group element as an active ingredient. Among them, a rhodium catalyst or a ruthenium catalyst is preferred. The hydrogenation catalyst is preferably a catalyst in which the active ingredient is supported on a carbon-based carrier. Examples of carbon-based carriers include activated carbon, graphite, carbon black, etc. Among them, activated carbon or graphite known as high surface area graphite is particularly preferred. The specific surface area of ​​the carbon-based carrier is generally 5 to 3000 m 2 / g, preferably 50 to 1500 m 2 / g, and the particle size is usually 5 to 500 μm.

[0089] The method for preparing the hydrogenation catalyst may be, for example, the method disclosed in Japanese Patent Application Laid-Open No. 11-217379. The amount of the catalyst metal component mixed in the obtained epoxy resin composition (A) varies depending on the method for preparing the hydrogenation catalyst, and the catalyst metal component may be removed by the purification step described below.

[0090] From the viewpoint of improving the color tone of the epoxy resin composition (A) obtained, the hydrogenation reaction is preferably performed in the presence of a reaction solvent containing an ester solvent in an amount of 50% by mass or more.

[0091] As the ester solvent, fatty acid esters, carbonates, lactones, etc. can be mentioned, and fatty acid esters are particularly preferred. From the perspective of handling, fatty acid esters with a boiling point in the range of 50 to 180° C. under normal pressure are preferred. As such fatty acid esters, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, pentyl acetate, methyl propionate, propyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, methyl isovalerate, etc. can be mentioned. Among these, acetates and propionates are preferred. Specifically, ethyl acetate, propyl acetate, butyl acetate, and methyl propionate are preferred, and ethyl acetate is particularly preferred.

[0092] The ester solvent can be mixed with an ether solvent, an alcohol solvent, or an alkane solvent widely used in the prior art. In this case, the proportion of the ester solvent is usually 50% by mass or more, preferably 90% by mass or more, relative to the mixed solvent. It is preferred that the ether solvent is not substantially contained, and specifically, the content of the ether solvent is preferably 1% by mass or less.

[0093] The amount of the reaction solvent used is usually 0.05 to 10, preferably 0.1 to 3, in terms of mass ratio relative to the raw material aromatic epoxy resin (4). When the amount of the reaction solvent is too small, the viscosity of the raw material is usually high, so the diffusion of hydrogen deteriorates, the reaction rate decreases, and the selectivity of the hydrogenation reaction decreases. When the amount of the reaction solvent is too large, the productivity decreases, which is economically disadvantageous.

[0094] The reaction temperature is usually 30 to 150° C., preferably 50 to 130° C. When the reaction temperature is too low, the reaction rate decreases, and a large amount of hydrogenation catalyst and a long time are required to complete the reaction. When the reaction temperature is too high, not only side reactions such as hydrogenation and decomposition of epoxy groups increase, but also the amount of elution of the catalyst metal component increases, and the quality of the epoxy resin composition (A) obtained is reduced.

[0095] The reaction pressure is usually 1 to 30 MPa, preferably 3 to 15 MPa. When the reaction pressure is too low, the reaction rate decreases, and a large amount of hydrogenation catalyst and a long time are required to complete the reaction. When the reaction pressure is too high, the necessary equipment becomes large-scale, which is economically disadvantageous.

[0096] The reaction method may be a liquid phase suspension reaction or a fixed bed reaction, and a liquid phase suspension reaction is particularly preferred.

[0097] Hydrogen can be introduced by circulation or only in the amount consumed. Hydrogen can also be introduced into the liquid and dispersed. Hydrogen can also be drawn from the gas phase into the liquid by stirring and other means and absorbed. The end point of the reaction can be determined by monitoring hydrogen absorption or by analysis based on sampling.

[0098] The hydrogenation rate of the aromatic ring of the aromatic epoxy resin (4) is preferably 85% or more, and may be even higher.

[0099] After the reaction is completed, the catalyst is separated from the reaction solution by filtration / centrifugation and the like when necessary, and the reaction solvent is then distilled off by distillation to obtain the target product. The reaction solvent is distilled off under reduced pressure at a temperature of usually 50 to 200° C., preferably 70 to 150° C. The residual amount of the reaction solvent is usually 1% by mass or less, preferably 0.2% by mass or less, from the perspective of the impact on the environment during use, especially the odor. The lower limit of the residual amount of the reaction solvent is usually 0.001% by mass. The distillation of the reaction solvent above this level requires long-term heating, and the stability of the epoxy resin composition (A) obtained may be reduced. In order to further reduce the residual amount of the reaction solvent, it is effective to introduce an inert gas such as nitrogen.

[0100] The concentration of the catalyst metal component in the epoxy resin composition (A) obtained by such a hydrogenation reaction is generally 0.01 to 50 ppm. By using an ester solvent as a solvent, the concentration of the catalyst metal component in the epoxy resin composition (A) can be made to reach such a low concentration by selecting the conditions for preparing the catalyst used in the hydrogenation reaction or the conditions for the hydrogenation reaction. Furthermore, in order to further reduce the concentration of the catalyst metal component in the epoxy resin composition (A) reliably, it is more preferable to perform a purification step using an adsorbent as shown below.

[0101] <Refining process>

[0102] As adsorbents used in the refining process, activated carbon, activated clay, ion exchange resin, synthetic adsorbent, etc. can be cited. Among these, activated carbon is preferred. There is no particular limitation on the type of activated carbon, and various activated carbons made from various raw materials such as coconut shell raw materials, wood raw materials, and coal raw materials can be used. The specific surface area of ​​activated carbon is preferably 500 to 3000 m 2 / g range.

[0103] The active surface of the adsorbent may be acidic, neutral or alkaline, preferably alkaline. Examples of the alkaline adsorbent include solid alkaline compounds such as magnesium oxide, and alkaline ion exchange resins.

[0104] The purification step can be carried out by any of intermittent contact treatment using a powdered adsorbent and circulation treatment in a granular adsorbent filling layer. The powdered adsorbent is preferably an adsorbent having an average particle size of 1 to 1000 μm. The granular adsorbent is preferably an adsorbent having an average particle size of 1 to 10 mm.

[0105] The amount of the adsorbent used varies depending on the type of the adsorbent, but is generally 0.01 to 100% by mass, preferably 0.1 to 20% by mass, and more preferably 0.2 to 10% by mass, based on the epoxy resin composition to be purified.

[0106] The temperature during the adsorption treatment is usually 0 to 100° C., preferably 10 to 80° C. In addition, the state of the adsorption treatment is preferably a state containing a solvent from the perspectives of workability, recovery rate, adsorption efficiency, etc. There is no particular limitation on the type of solvent as long as it can dissolve the epoxy resin.

[0107] The above-mentioned refining step is usually carried out before the hydrogenation reaction liquid is concentrated, so it is suitable to directly use the reaction solvent as the solvent during the adsorption treatment. The content of the solvent is usually 5 to 80% by mass in terms of the concentration in the liquid provided for the adsorption treatment. When the amount of the solvent is too small, the viscosity of the treatment liquid increases and the adsorption efficiency decreases.

[0108] Alternatively, after the hydrogenation reaction, an adsorbent may be added to the reaction solution and mixed without separating the hydrogenation catalyst, and the catalyst and the adsorbent may be separated into a solid and a liquid to perform adsorption treatment. Such a method has the following advantages.

[0109] That is, when the solid-liquid separation of the catalyst is performed without adding an adsorbent to the reaction solution after the hydrogenation reaction, the solid-liquid separation property will be reduced due to the adhesion of organic matter attached to the catalyst surface. In contrast, according to the above method, when the solid-liquid separation of the catalyst is performed together with an adsorbent (particularly activated carbon), the solid-liquid separation property becomes very good. In this method, the removal efficiency of the catalyst also hardly changes. When the solid-liquid separation of the catalyst is performed together with an adsorbent, the amount of the adsorbent used is preferably 1 to 30 times the mass of the catalyst.

[0110] The content of each component of the epoxy resins (1) to (3) in the epoxy resin composition (A) of the present invention can be controlled by combining the various elements of the reaction conditions of the above-mentioned hydrogenation reaction and performing the reaction.

[0111] [Epoxy resin composition (B)]

[0112] The epoxy resin composition (B) of the present invention contains at least the epoxy resin composition (A) of the present invention and a curing agent.

[0113] The epoxy resin composition (B) of the present invention may contain other epoxy resins (hereinafter sometimes simply referred to as “other epoxy resins”) other than the epoxy resin composition (A) of the present invention, a curing accelerator, an inorganic filler, a coupling agent, etc. as needed.

[0114] The epoxy resin composition (B) of the present invention including the epoxy resin composition (A) of the present invention can provide a cured product having excellent curing properties such as curability and fully satisfying various physical properties required in various applications. As long as the epoxy resin composition (B) of the present invention has excellent curability, it is possible to achieve improved productivity in the application of various applications.

[0115] [Curing agent]

[0116] The curing agent in the present invention refers to a substance that contributes to the cross-linking reaction and / or chain extension reaction between epoxy groups of the epoxy resin.

[0117] In the present invention, even a substance generally called a "curing accelerator" can be regarded as a curing agent as long as it contributes to the cross-linking reaction and / or chain extension reaction between epoxy groups of the epoxy resin.

[0118] In the epoxy resin composition (B) of the present invention, the content of the curing agent is preferably 0.1 to 1000 parts by mass, more preferably 500 parts by mass or less, and even more preferably 300 parts by mass or less, based on 100 parts by mass of the total epoxy resin component as solid content.

[0119] In the present invention, the "solid content" refers to components other than the solvent, and includes not only solid epoxy resins but also semisolid or viscous liquid components.

[0120] The “total epoxy resin component” corresponds to the amount of the epoxy resin contained in the epoxy resin composition (B) of the present invention. When the epoxy resin composition (B) of the present invention contains only the epoxy resin composition (A), it corresponds to the amount of the epoxy resin in the epoxy resin composition (A). When it contains the epoxy resin composition (A) and other epoxy resins, it corresponds to the total of the epoxy resin in the epoxy resin composition (A) and other epoxy resins.

[0121] There are no particular restrictions on the curing agent, and all curing agents commonly known as epoxy resin curing agents can be used. Examples include phenolic curing agents, aliphatic amines, polyether amines, alicyclic amines, amine curing agents such as aromatic amines, acid anhydride curing agents, isocyanuric acid derivative curing agents, amide curing agents, tertiary amines, imidazoles, and the like.

[0122] Among them, by including an acid anhydride curing agent, an isocyanuric acid derivative curing agent, and a phenolic curing agent, the epoxy resin composition (B) of the present invention can obtain excellent curability, crack resistance, and heat resistance. Therefore, it is preferred to include an acid anhydride curing agent, an isocyanuric acid derivative curing agent, and a phenolic curing agent as a curing agent.

[0123] From the viewpoint of heat resistance and the like, it is preferred that an acid anhydride curing agent or an isocyanuric acid derivative curing agent be contained.

[0124] From the viewpoint of sufficiently advancing the curing reaction and improving the heat resistance, it is also preferable to use imidazoles.

[0125] The curing agent may be used alone or in combination of two or more. When two or more curing agents are used together, they may be pre-mixed to prepare a mixed curing agent and then used, or the curing agents may be separately added and mixed simultaneously when the components of the epoxy resin composition (B) are mixed.

[0126] <Anhydride Curing Agent>

[0127] Examples of the acid anhydride-based curing agent include acid anhydrides and modified products of acid anhydrides.

[0128] Examples of the acid anhydride include phthalic anhydride (phthalic anhydride), maleic anhydride, trimellitic anhydride (trimellitic anhydride), pyromellitic anhydride, benzophenonetetracarboxylic anhydride, dodecenylsuccinic anhydride, polyadipic anhydride, polyazelaic anhydride, polysebacic anhydride, poly(ethyloctadecane dioic acid) anhydride, poly(phenylhexadecanedioic acid) anhydride, tetrahydrophthalic anhydride (tetrahydrophthalic anhydride), methyltetrahydrophthalic anhydride (methyltetrahydrophthalic anhydride), methylhexahydrophthalic anhydride (methylhexahydrophthalic anhydride), hexahydrophthalic anhydride (hexahydrophthalic anhydride), methylhumic anhydride, trialkyltetrahydrophthalic anhydride, Phthalic anhydride, methylcyclohexene dicarboxylic anhydride, methylcyclohexene tetracarboxylic anhydride, ethylene glycol ditrimellitate dianhydride, chlorobridged anhydride, nadic anhydride, methylnadic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexane-1,2-dicarboxylic anhydride, 3,4-dicarboxy-1,2,3,4-tetrahydro-1-naphthalene succinic anhydride, 1-methyl-dicarboxy-1,2,3,4-tetrahydro-1-naphthalene succinic anhydride, glutaric anhydride, dimethylglutaric anhydride, diethylglutaric anhydride, succinic anhydride, etc.

[0129] Among these acid anhydride curing agents, phthalic anhydride, trimellitic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, glutaric anhydride, dimethylglutaric anhydride, and diethylglutaric anhydride are preferably used.

[0130] As modified products of acid anhydrides, for example, modified products obtained by modifying the above acid anhydrides with diols can be cited. Here, as examples of diols that can be used for modification, alkylene glycols such as ethylene glycol, propylene glycol, and neopentyl glycol, polyether diols such as polyethylene glycol, polypropylene glycol, and polytetramethylene ether glycol can be cited. Furthermore, copolymerized polyether diols of two or more of these diols and / or polyether diols can also be used.

[0131] The modified product of the acid anhydride is preferably modified with 0.4 mol or less of diol per mol of the acid anhydride. When the modification amount is below the upper limit, the viscosity of the epoxy resin composition will not be too high, the workability will tend to be good, and the curing reaction rate with the epoxy resin will also tend to be good.

[0132] The acid anhydride curing agents listed above may be used alone or in combination of two or more in any combination and in any blending amount.

[0133] When an acid anhydride curing agent is used, it is preferably used in a manner such that the equivalent ratio of the functional groups in the curing agent to the epoxy groups in all epoxy resin components in the epoxy resin composition (B) is in the range of 0.8 to 1.5. When it is in this range, unreacted epoxy groups and functional groups of the curing agent are less likely to remain, which is preferred.

[0134] <Isocyanuric acid derivative curing agent>

[0135] Examples of the isocyanuric acid derivative curing agent include 1,3,5-tris(1-carboxymethyl)isocyanurate, 1,3,5-tris(2-carboxyethyl)isocyanurate, 1,3,5-tris(3-carboxypropyl)isocyanurate, and 1,3-bis(2-carboxyethyl)isocyanurate.

[0136] Among these isocyanuric acid derivative-based curing agents, 1,3,5-tris(3-carboxypropyl)isocyanurate is preferably used.

[0137] The isocyanuric acid derivative curing agents listed above may be used alone or in combination of two or more in any combination and in any blending amount.

[0138] When an isocyanuric acid derivative curing agent is used, it is preferably used in a manner such that the equivalent ratio of the functional groups in the curing agent to the epoxy groups in all epoxy resin components in the epoxy resin composition (B) is in the range of 0.8 to 1.5. When it is in this range, unreacted epoxy groups and functional groups of the curing agent are less likely to remain, which is preferred.

[0139] <Phenol-based curing agent>

[0140] Examples of the phenolic curing agent include: novolac-type phenolic resins obtained by condensing or co-condensing phenols such as phenol, cresol, resorcinol, catechol, bisphenol A, bisphenol F, phenylphenol, and aminophenol and / or naphthols such as α-naphthol, β-naphthol, and dihydroxynaphthalene with a compound having an aldehyde group such as formaldehyde, benzaldehyde, and salicylaldehyde in the presence of an acidic catalyst; phenol-aralkyl resins synthesized from phenols and / or naphthols and dimethoxy-p-xylene or bis(methoxymethyl)biphenyl; and diphenylene. Aralkyl-type phenol resins such as aryl-type phenol-aralkyl resins and naphthol-aralkyl resins; dicyclopentadiene-type linear phenol-formaldehyde resins and dicyclopentadiene-type linear naphthol phenol-formaldehyde resins synthesized by copolymerization of phenols and / or naphthols with dicyclopentadiene; triphenylmethane-type phenol resins; terpene-modified phenol resins; p-xylene and / or m-xylene-modified phenol resins; melamine-modified phenol resins; cyclopentadiene-modified phenol resins; and phenol resins obtained by copolymerization of two or more of them, etc.

[0141] The amount of the phenolic curing agent is preferably 0.1 to 1000 parts by mass, more preferably 500 parts by mass or less, further preferably 300 parts by mass or less, particularly preferably 100 parts by mass or less, based on 100 parts by mass of the total epoxy resin components in the epoxy resin composition (B).

[0142] <Amine curing agent>

[0143] Examples of the amine-based curing agent (excluding tertiary amines) include aliphatic amines, polyether amines, alicyclic amines, and aromatic amines.

[0144] Examples of the aliphatic amines include ethylenediamine, 1,3-diaminopropane, 1,4-diaminopropane, hexamethylenediamine, 2,5-dimethylhexamethylenediamine, trimethylhexamethylenediamine, diethylenetriamine, iminobispropylamine, bis(hexamethylene)triamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, N-hydroxyethylethylenediamine, and tetrakis(hydroxyethyl)ethylenediamine.

[0145] Examples of the polyetheramines include triethylene glycol diamine, tetraethylene glycol diamine, diethylene glycol bis(propylamine), polyoxypropylene diamine, and polyoxypropylene triamine.

[0146] Examples of the alicyclic amines include isophoronediamine, menthyl diamine, N-aminoethylpiperazine, bis(4-amino-3-methyldicyclohexyl)methane, bis(aminomethyl)cyclohexane, 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxaspiro(5,5)undecane, and norbornene diamine.

[0147] Examples of the aromatic amines include tetrachloro-p-xylylenediamine, m-xylylenediamine, p-xylylenediamine, m-phenylenediamine, o-phenylenediamine, p-phenylenediamine, 2,4-diaminoanisole, 2,4-toluenediamine, 2,4-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 4,4'-diamino-1,2-diphenylethane, 2,4-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, m-aminophenol, m-aminobenzylamine, benzyldimethylamine, 2-(dimethylaminomethyl)phenol, triethanolamine, methylbenzylamine, α-(m-aminophenyl)ethylamine, α-(p-aminophenyl)ethylamine, diaminodiethyldimethyldiphenylmethane, and α,α'-bis(4-aminophenyl)-p-diisopropylbenzene.

[0148] The amine curing agents listed above may be used alone or in combination of two or more in any combination and mixing ratio.

[0149] The amine curing agent is preferably used in such a manner that the equivalent ratio of the functional groups in the curing agent to the epoxy groups in all epoxy resin components contained in the epoxy resin composition (B) is in the range of 0.8 to 1.5. When it is in this range, unreacted epoxy groups and functional groups of the curing agent are less likely to remain, which is preferred.

[0150] Examples of the tertiary amine include 1,8-diazabicyclo(5,4,0)triethylenediamine 7, triethylenediamine, benzyldimethylamine, triethanolamine, dimethylaminoethanol, tris(dimethylaminomethyl)phenol, and dimethylaminomethylphenol.

[0151] The tertiary amines listed above may be used alone or in combination of two or more in any combination and mixing ratio.

[0152] The tertiary amine is preferably used so that the equivalent ratio of the functional groups in the curing agent to the epoxy groups in all epoxy resin components contained in the epoxy resin composition (B) is in the range of 0.8 to 1.5. Within this range, unreacted epoxy groups and functional groups of the curing agent are less likely to remain, which is preferred.

[0153] <Amide curing agent>

[0154] Examples of the amide curing agent include dicyandiamide and its derivatives, and polyamide resins.

[0155] The amide curing agent may be used alone or in combination of two or more in any ratio.

[0156] When an amide curing agent is used, it is preferred to use the amide curing agent in an amount of 0.1 to 20% by mass based on the total amount of the entire epoxy resin component and the amide curing agent in the epoxy resin composition (B).

[0157] <Imidazoles>

[0158] Examples of imidazoles include 2-phenylimidazole, 2-ethyl-4(5)-methylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyano-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-( 1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and adducts of epoxy resins and the above imidazoles, etc.

[0159] Imidazoles have a catalytic ability and therefore are generally classified as curing accelerators, but are classified as curing agents in the present invention.

[0160] The above-mentioned imidazoles may be used alone or in combination of two or more in any ratio.

[0161] When using imidazoles, it is preferable to use imidazoles so that the total amount of imidazoles is 0.1 to 20 mass % based on the total amount of all epoxy resin components and imidazoles in the epoxy resin composition (B).

[0162] <Other curing agents>

[0163] In the epoxy resin composition (B) of the present invention, other curing agents may be used in addition to the above curing agents. The other curing agents that can be used in the epoxy resin composition (B) of the present invention are not particularly limited, and all components generally known as curing agents for epoxy resins can be used.

[0164] The other curing agents may be used alone or in combination of two or more.

[0165] [Other epoxy resins]

[0166] The epoxy resin composition (B) of the present invention may further contain other epoxy resins in addition to the epoxy resin composition (A). By containing other epoxy resins, the heat resistance, stress resistance, moisture absorption resistance, flame retardancy, etc. of the epoxy resin composition (B) of the present invention can be improved.

[0167] The other epoxy resins that can be used in the epoxy resin composition (B) of the present invention correspond to all epoxy resins other than the epoxy resin (mainly the epoxy resins (1) to (3)) contained in the above-mentioned epoxy resin composition (A).

[0168] Specific examples include bisphenol A type epoxy resins, trisphenol methane type epoxy resins, anthracene type epoxy resins, phenol-modified xylene resin type epoxy resins, bisphenol cyclododecyl type epoxy resins, bisphenol diisopropylresorcinol type epoxy resins, bisphenol F type epoxy resins, bisphenol AD ​​type epoxy resins, hydroquinone type epoxy resins, methylhydroquinone type epoxy resins, dibutylhydroquinone type epoxy resins, resorcinol type epoxy resins, methylresorcinol type epoxy resins, biphenol type epoxy resins, tetramethylbiphenol type epoxy resins other than the epoxy resins (1) and (2) in the epoxy resin composition (A), tetramethylbisphenol F type epoxy resins, dihydroxydiphenyl ether type epoxy resins, epoxy resins derived from thiodiphenols, dihydroxynaphthalene type epoxy resins, dihydroxyanthracene type epoxy resins, dihydroxydihydroanthracene type epoxy resins, dicyclopentadiene type epoxy resins, and epoxy resins derived from Epoxy resins from dihydroxystilbene, novolac epoxy resins, cresol-novolac epoxy resins, bisphenol A novolac epoxy resins, naphthol novolac epoxy resins, phenol aralkyl epoxy resins, naphthol aralkyl epoxy resins, biphenyl aralkyl epoxy resins, terpene phenol epoxy resins, dicyclopentadiene phenol epoxy resins, epoxy resins derived from condensates of phenol-hydroxybenzaldehyde, epoxy resins derived from condensates of phenol-crotonaldehyde, epoxy resins derived from condensates of phenol-glyoxal, epoxy resins derived from co-condensation resins of heavy oil or asphalt with phenols and formaldehyde, epoxy resins derived from diaminodiphenylmethane, epoxy resins derived from aminophenol, epoxy resins derived from xylenediamine, epoxy resins derived from methylhexahydrophthalic acid, epoxy resins derived from dimer acid, etc.

[0169] These components may be used alone or in any combination and in any blending ratio.

[0170] [Curing accelerator]

[0171] The epoxy resin composition (B) of the present invention preferably contains a curing accelerator. By containing a curing accelerator, the curing time can be shortened, the curing temperature can be lowered, and a desired cured product can be easily obtained.

[0172] The curing accelerator is not particularly limited, and specific examples thereof include organic phosphines, phosphorus compounds such as phosphonium salts, tetraphenylborate salts, organic acid dihydrazides, and boron halide amine complexes.

[0173] Examples of phosphorus compounds that can be used as curing accelerators include organic phosphines such as triphenylphosphine, diphenyl (p-tolyl) phosphine, tri(alkylphenyl)phosphine, tri(alkoxyphenyl)phosphine, tri(alkyl-alkoxyphenyl)phosphine, tri(dialkylphenyl)phosphine, tri(trialkylphenyl)phosphine, tri(tetraalkylphenyl)phosphine, tri(dialkoxyphenyl)phosphine, tri(trialkoxyphenyl)phosphine, tri(tetraalkoxyphenyl)phosphine, trialkylphosphine, dialkylarylphosphine, and alkyldiarylphosphine, or complexes of these organic phosphines with organic boron, compounds obtained by adding these organic phosphines to quinone compounds such as maleic anhydride, 1,4-benzoquinone, 2,5-methylquinone, 1,4-naphthoquinone, 2,3-dimethylbenzoquinone, 2,6-dimethylbenzoquinone, 2,3-dimethoxy-5-methyl-1,4-benzoquinone, 2,3-dimethoxy-1,4-benzoquinone, and phenyl-1,4-benzoquinone, and compounds such as diazonophenylmethane.

[0174] Among the above-mentioned curing accelerators, organic phosphines and phosphonium salts are preferred, and organic phosphines are most preferred.

[0175] As the curing accelerator, only one of the above-mentioned components may be used, or two or more of them may be mixed and used in any combination and ratio.

[0176] The curing accelerator is preferably used in a range of 0.1 weight or more and 20 weight parts or less relative to 100 weight parts of all epoxy resin components in the epoxy resin composition (B), more preferably 0.5 weight parts or more, further preferably 1 weight parts or more, more preferably 15 weight parts or less, further preferably 10 weight parts or less. When the content of the curing accelerator is above the above lower limit, a good curing acceleration effect can be obtained. When the content of the curing accelerator is below the above upper limit, it is easy to obtain the desired cured physical properties.

[0177] [Inorganic filler]

[0178] The epoxy resin composition (B) of the present invention may be mixed with an inorganic filler. Examples of the inorganic filler include fused silica, crystalline silica, glass powder, aluminum oxide, calcium carbonate, calcium sulfate, talc, boron nitride, titanium oxide, and the like. These materials may be used alone or in any combination and in any blending ratio.

[0179] When an inorganic filler is used in the epoxy resin composition (B) of the present invention, the inorganic filler is preferably blended in an amount of 60 to 95% by mass of the entire epoxy resin composition (B).

[0180] [Release agent]

[0181] The epoxy resin composition (B) of the present invention may be mixed with a release agent. As the release agent, for example, natural waxes such as carnauba wax, synthetic waxes such as polyethylene wax, higher fatty acids such as stearic acid or zinc stearate and their metal salts, hydrocarbon-based release agents such as paraffins may be used. These release agents may be used alone or in combination of two or more in any combination and mixing ratio.

[0182] When a release agent is mixed in the epoxy resin composition (B) of the present invention, the amount of the release agent is preferably 0.1 to 5.0 parts by mass, more preferably 0.5 to 3.0 parts by mass, relative to 100 parts by mass of all epoxy resin components in the epoxy resin composition (B). When the amount of the release agent is within the above range, good release properties can be exhibited while maintaining the curing characteristics of the epoxy resin composition (B), and thus it is preferred.

[0183] [Coupling agent]

[0184] The epoxy resin composition (B) of the present invention preferably contains a coupling agent. The coupling agent is preferably used together with an inorganic filler. By adding the coupling agent, the adhesion between the epoxy resin as a matrix and the inorganic filler can be improved.

[0185] Examples of the coupling agent include silane coupling agents and titanate coupling agents.

[0186] Examples of the silane coupling agent include epoxy silanes such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, amino silanes such as γ-aminopropyltriethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, γ-aminopropyltrimethoxysilane, and γ-ureidopropyltriethoxysilane, mercaptosilanes such as 3-mercaptopropyltrimethoxysilane, p-phenylvinyltrimethoxysilane, vinyltrichlorosilane, vinyltri(β-methoxyethoxy)silane, vinyltrimethoxysilane, vinyltriethoxysilane, and vinyl silanes such as γ-methacryloxypropyltrimethoxysilane, and epoxy-based, amino-based, and vinyl-based polymer silanes.

[0187] Examples of the titanate coupling agent include isopropyl triisostearoyl titanate, isopropyl tri(N-aminoethyl-aminoethyl) titanate, diisopropyl bis(dioctyl phosphoyloxy) titanate, tetraisopropyl bis(dioctyl phosphite) titanate, tetraoctyl bis(ditridecyl) phosphite) titanate, tetra(2,2-diallyloxymethyl-1-butyl)bis(ditridecyl) phosphite titanate, bis(dioctyl pyrophosphate)oxyacetate titanate, and bis(dioctyl pyrophosphate)ethylene titanate.

[0188] These coupling agents may be used alone or in combination of two or more in any ratio.

[0189] When a coupling agent is used in the epoxy resin composition (B) of the present invention, the amount thereof is preferably 0.1 to 3.0 parts by mass relative to 100 parts by mass of the total epoxy resin component. When the amount of the coupling agent is greater than the above lower limit, there is a tendency to improve the adhesion between the epoxy resin as a matrix and the inorganic filler material brought about by the coupling agent. When the amount of the coupling agent is less than the above upper limit, the coupling agent is less likely to ooze out from the resulting cured product.

[0190] [Other mixed ingredients]

[0191] The epoxy resin composition (B) of the present invention may be mixed with components other than the above (sometimes referred to as "other mixed components" in the present invention). Examples of other mixed components include flame retardants, plasticizers, reactive diluents, pigments, etc., which may be mixed appropriately as needed. The epoxy resin composition (B) of the present invention may also be mixed with components other than the above without any hindrance.

[0192] Examples of the flame retardant used in the epoxy resin composition (B) of the present invention include halogen-based flame retardants such as brominated epoxy resins and brominated phenol resins, antimony compounds such as antimony trioxide, phosphorus-based flame retardants such as red phosphorus, phosphates, and phosphines, nitrogen-based flame retardants such as melamine derivatives, and inorganic flame retardants such as aluminum hydroxide and magnesium hydroxide.

[0193] [cured material]

[0194] The cured product of the present invention can be obtained by curing the epoxy resin composition (B) of the present invention. The cured product of the present invention obtained by curing the epoxy resin composition (B) of the present invention has excellent properties in terms of curability, crack resistance, and heat resistance.

[0195] There is no particular limitation on the method for curing the epoxy resin composition (B) of the present invention, and a cured product can usually be obtained by a heat-curing reaction based on heating. During the heat-curing reaction, it is preferred to appropriately select the curing temperature according to the type of curing agent used. For example, when an anhydride curing agent is used, the curing temperature is usually 80 to 250° C. By adding a curing accelerator to these curing agents, the curing temperature can also be reduced.

[0196] The reaction time of the thermal curing reaction is preferably 1 to 20 hours, more preferably 2 to 18 hours, and further preferably 3 to 15 hours. When the reaction time is above the lower limit, the curing reaction tends to proceed sufficiently, which is preferred. When the reaction time is below the upper limit, the deterioration due to heating and the energy loss during heating are easily reduced, which is preferred.

[0197] The cured product using the epoxy resin composition (B) of the present invention is excellent in curability, crack resistance and heat resistance.

[0198] The epoxy resin composition (B) of the present invention is preferably capable of providing a cured product, the gel time of which is measured at 120°C using a No. 153 gel time tester (magnetic type) manufactured by Yasuda Seiki Co., Ltd., and is within 34 minutes. The shorter the gel time of the cured product, the shorter the molding cycle for obtaining the cured product can be, and thus it is preferred.

[0199] The epoxy resin composition (B) of the present invention is preferably capable of providing a cured product, wherein when the second α2 (linear expansion coefficient after Tg) and Tg (glass transition temperature) are measured by a thermomechanical analyzer (TMA: TMA / SS6100 manufactured by Seiko Instruments) in a compression mode with the first temperature increase of 5°C / min (30°C to 200°C), the first temperature decrease of 10°C / min (200°C to 30°C), and the second temperature increase of 5°C / min (30°C to 200°C), α2 is 182 ppm or less and Tg is 125°C or more. The smaller the α2 of the cured product, the smaller the thermal expansion at high temperature, so that thermal stress and cracks are not easily generated, which is preferred. The higher the Tg, the smaller the change in physical properties at high temperature, which is preferred.

[0200] [use]

[0201] The epoxy resin composition (A) of the present invention has excellent electrical and optical properties. The epoxy resin composition (B) of the present invention comprising the epoxy resin composition (A) of the present invention has excellent curability. The cured product of the epoxy resin composition (B) of the present invention has excellent crack resistance and heat resistance.

[0202] Therefore, as long as the application requires these physical properties, the epoxy resin composition (A), epoxy resin composition (B) and cured products of the present invention can be effectively used in any application. For example, in the field of coatings such as optical materials, electrodeposition coatings for automobiles, heavy anti-corrosion coatings for ships / bridges, and coatings for inner surface coatings of beverage cans; laminates, semiconductor packaging materials, insulating powder coatings, coil impregnation and other electrical and electronic fields; seismic reinforcement of bridges, concrete reinforcement, floor materials of buildings, linings of waterway facilities, drainage / permeable paving, and civil engineering / construction / adhesive fields of adhesives for vehicles / aircraft. Among these, it is particularly useful in the use of electrical / electronic components and optical materials.

[0203] The epoxy resin composition (B) of the present invention may be used after being cured when used for the above-mentioned applications, or may be used after being cured in the production process for the above-mentioned applications.

[0204] Example

[0205] The present invention is described in more detail below by way of examples. The present invention is not limited to the following examples unless the gist thereof is exceeded.

[0206] [Production and Evaluation of Epoxy Resin Composition (A)]

[0207] [Examples 1 to 3, Comparative Examples 1 to 7]

[0208] The analysis methods and physical property measurement methods of the epoxy resin compositions obtained in Examples 1 to 3 and Comparative Examples 1 to 7 are as follows.

[0209] (1) Composition analysis of epoxy resin composition:

[0210] The area % of "epoxy resin (1)", "epoxy resin (2 and / or epoxy resin (3)", and "other components" of the epoxy resin compositions produced in the Examples and Comparative Examples were analyzed under the following conditions, and the mass % was calculated from the area % thereof. Other components are epoxy resins other than the epoxy resins (1) to (3).

[0211] Device: Tosoh HLC-8220L GPC

[0212] Detector: RI

[0213] Mobile phase: Tetrahydrofuran (containing BHT)

[0214] Flow rate: 0.8 mL / min

[0215] Column: Tosoh TSKgel G2000Hxl+G1000Hxl×2

[0216] Column temperature: 40°C

[0217] (2)Total chlorine content:

[0218] The total chlorine content was analyzed in accordance with JIS K7243-3.

[0219] (3) Epoxy equivalent:

[0220] The epoxy equivalent was analyzed according to JIS K7236-1955.

[0221] (4) Hazen color value:

[0222] Hazen color analysis was performed using a UV-Vis spectrophotometer according to ISO 6271-2:2004.

[0223] [Example 1]

[0224] Regarding the bisphenol A epoxy resin "jER828EL" manufactured by Mitsubishi Chemical Corporation (in the above formula (4), X = isopropylidene, R 1 = hydrogen atom, n = 0, epoxy equivalent = 186g / equivalent, total chlorine content = 1300ppm) 1000g, using a centrifugal thin film distillation apparatus at a temperature of 220°C and a reduced pressure of 0.003Torr, 50% of the fraction (500g) was recovered in 6 hours to obtain a distilled bisphenol A type epoxy resin (epoxy equivalent = 171g / equivalent, total chlorine content = 800ppm).

[0225] Into a 1L induction stirring autoclave, 400g of the previously obtained distilled bisphenol A epoxy resin (epoxy equivalent = 171g / equivalent, total chlorine content = 800ppm), 100g of ethyl acetate, and 2.4g of a 5% by mass rhodium / graphite catalyst (NEChemcat Co., Ltd.) as a hydrogenation catalyst were placed, and the autoclave was purged with nitrogen and then purged with hydrogen. Thereafter, a hydrogenation reaction was carried out at 110°C and a hydrogen pressure of 8MPa until hydrogen absorption almost stopped. The reaction time was 180 minutes.

[0226] The hydrogenation catalyst was filtered out from the reaction liquid using 5C filter paper.

[0227] Next, the reaction solvent was distilled off at 100° C. under reduced pressure while blowing a small amount of nitrogen, thereby obtaining the epoxy resin composition (A) of Example 1.

[0228] [Example 2]

[0229] The epoxy resin composition (A) of Example 2 was obtained in the same manner as in Example 1 except that the amount of the hydrogenation catalyst used was 1.2 g and the hydrogenation reaction time was 360 minutes.

[0230] [Example 3]

[0231] The epoxy resin composition (A) of Example 3 was obtained in the same manner as in Example 1 except that the amount of the hydrogenation catalyst used was 4.8 g and the hydrogenation reaction time was 90 minutes.

[0232] In the following Comparative Example 1, the reaction was carried out according to Example 1 of JP-A-2002-97251.

[0233] [Comparative Example 1]

[0234] Into a 500 ml stainless steel autoclave equipped with an electromagnetic stirrer, 40 g of bisphenol A diglycidyl ether "Epotohto YD-8125" (epoxy equivalent = 172 g / equivalent) manufactured by Tohto Kasei Co., Ltd., 120 g of propylene glycol monomethyl ether and 1.0 g of a 5 mass % rhodium / graphite catalyst (NEChemcat Co., Ltd.) were placed, the system was replaced with hydrogen, and the mixture was stirred at 50° C. and a hydrogen pressure of 4.9 MPa (50 kg / cm 2 ) for 5 hours.

[0235] After the reaction, the catalyst was filtered off, and the solvent was distilled off at 150° C. and 266 Pa (20 Torr), thereby obtaining the epoxy resin composition of Comparative Example 1.

[0236] In the following Comparative Examples 2 to 4, the reaction was carried out according to Hydrogenation Examples 5, 6, and 7 using a catalyst produced according to the Examples of JP-A-2007-515276.

[0237] [Comparative Example 2]

[0238] In a 1.2-liter pressure-resistant autoclave equipped with a gas supply pipe (700 rpm) and a sample collection tube, 21 g of catalyst (catalyst D, Ru content 1.7% by mass) was filled into a catalyst cage, and heated to 50° C. together with 600 g of a 40% by mass solution of bisphenol A-bisglycidyl ether (distilled product, EEW=171 g / equivalent) with low oligomer content in THF having 4.5% by mass of water, and hydrogenated using a hydrogen pressure of 250 bar. After a reaction time of 24 hours, the autoclave was cooled to room temperature, depressurized, and the reaction batch (reaction batch) was taken out. The mechanical fine fragments of the catalyst were filtered using a filter. An aliquot of the colorless product was subjected to solvent removal using a rotary evaporator (conditions: oil bath temperature 130° C., vacuum 5-10 mbar, 15 minutes) to obtain the epoxy resin composition of Comparative Example 2.

[0239] [Comparative Example 3]

[0240] In a 1.2-liter pressure-resistant autoclave equipped with a gas supply tube (700 rpm) and a sample collection tube, 21 g of the catalyst (catalyst D, Ru content 2.0 mass %) was filled into a catalyst cage, and heated to 50° C. together with 600 g of a 40 mass % solution of bisphenol A-bisglycidyl ether (distilled product, EEW=171 g / equivalent) with low oligomer content in THF containing 4.5 mass % water, and hydrogenated at a hydrogen pressure of 250 bar. After a reaction time of 11 h, based on 1 The aromatic conversion rate of H-NMR was complete. The autoclave was cooled to room temperature, the pressure was released, and the reaction batch was taken out. The mechanical fine fragments of the catalyst were filtered using a filter. The solvent was removed from an aliquot of the colorless product using a rotary evaporator (conditions: oil bath temperature 130°C, vacuum 5-10 mbar, 15 minutes) to obtain the epoxy resin composition of Comparative Example 3.

[0241] [Comparative Example 4]

[0242] In a 1.2-liter pressure-resistant autoclave equipped with a gas supply pipe (700 rpm) and a sample collection tube, 17.9 g of the catalyst (catalyst D, Ru content 2.0 mass %) was filled into a catalyst cage, and heated to 50° C. together with 600 g of a 40 mass % solution of bisphenol A-bisglycidyl ether (distilled product, EEW=171 g / equivalent) with low oligomer content in THF containing 4.5 mass % water, and hydrogenated at a hydrogen pressure of 250 bar. After a reaction time of 14 h, based on 1 The aromatic conversion rate of H-NMR was complete. The autoclave was cooled to room temperature, depressurized, and the reaction batch was taken out. The mechanical fine fragments of the catalyst were filtered using a filter. The solvent was removed from an aliquot of the colorless product using a rotary evaporator (conditions: oil bath temperature 130°C, vacuum 5-10 mbar, 15 minutes) to obtain the epoxy resin composition of Comparative Example 4.

[0243] In the following Comparative Examples 5 and 6, the reaction was carried out according to Example 1 of Japanese Patent Application Laid-Open No. 11-269159.

[0244] [Comparative Example 5]

[0245] Into a four-necked flask equipped with a rotary stirring device, a decanter, a thermometer and a gas introduction tube, 1215 g (5 mol) of hydrogenated bisphenol A, 580 g of xylene and 15 g of tin chloride pentahydrate were added, and 1110 g (12 mol) of epichlorohydrin was added dropwise at 100°C for 60 minutes, and then stirring was continued for 30 minutes to terminate the addition reaction. Then, 35 g of benzyltrimethylammonium chloride and 1130 g of a 50% aqueous sodium hydroxide solution were added, and then stirring was continued at 80°C for 5 hours to terminate the ring-closure reaction. After removing the by-product sodium chloride and unreacted sodium hydroxide by washing with water, dehydration / desolvation was carried out at 120°C and 3 Torr for 1 hour to obtain 1860 g of a crude product (reaction crude product-A). Thereafter, 2 g of 2,6-di-tert-butyl-4-methylphenol as an antioxidant was dissolved in the above-mentioned crude reaction product, and a centrifugal molecular distillation apparatus (MS-150 molecular distillation apparatus manufactured by Nippon Shaft Corporation) having an evaporation surface diameter of 150 mm and a residence time of the treatment liquid of less than 1 second was used. The liquid was circulated at a liquid supply rate of 3 liters / hour for 1 hour at a temperature of 70°C, and then the operating conditions were adjusted to a liquid supply rate of 1.5 liters / hour and an evaporation surface temperature of 135°C at a vacuum degree of 0.005 Torr, thereby constantly distilling off a fore fraction of 5% by mass relative to the liquid supply amount to obtain an epoxy resin composition of Comparative Example 5.

[0246] [Comparative Example 6]

[0247] In Comparative Example 5, the epoxy resin composition of Comparative Example 6 was obtained in the same manner except that the distillation conditions using a centrifugal molecular distillation apparatus (MS-150 molecular distillation apparatus manufactured by Nippon Shaft Corporation) were changed from 5% by mass to 1% by mass in terms of the amount of the feed liquid.

[0248] In the following Comparative Example 7, the reaction was carried out according to Example 1 of JP-A-2003-212955.

[0249] [Comparative Example 7]

[0250] 400 g of bisphenol A epoxy resin "jER828EL" (epoxy equivalent = 186 g / equivalent) manufactured by Mitsubishi Chemical Corporation, 100 g of ethyl acetate, and 2.4 g of 5 mass% rhodium / graphite catalyst (NEChemcat Co., Ltd.) as a hydrogenation catalyst were placed in a 1L induction stirring autoclave, and the autoclave was purged with nitrogen and then purged with hydrogen. Thereafter, a hydrogenation reaction was carried out at 110°C and a hydrogen pressure of 8 MPa until hydrogen absorption was substantially stopped. The reaction time was 180 minutes.

[0251] The hydrogenation catalyst was filtered from the reaction solution using 5C filter paper. Then, the reaction solvent was distilled off at 100° C. under reduced pressure while blowing a small amount of nitrogen, thereby obtaining an epoxy resin composition of Comparative Example 7.

[0252] The analysis results of the epoxy resin compositions obtained in Examples 1 to 3 and Comparative Examples 1 to 7 are shown in Table 1 (Table 1A and Table 1B).

[0253]

[0254] [Production of epoxy resin composition (B) and evaluation of cured product]

[0255] [Examples 4 to 6, Comparative Examples 8 to 14]

[0256] The evaluation methods of the epoxy resin compositions obtained in Examples 4 to 6 and Comparative Examples 8 to 14 and their cured products are as follows.

[0257] (1) Gel time at 120℃:

[0258] The gel time was measured using a No. 153 gel time tester (magnetic type) manufactured by Yasuda Seiki Co., Ltd., on epoxy resin compositions uniformly blended in the proportions shown in Table 2 (Table 2A, Table 2B).

[0259] The following components were used as a curing agent and a curing accelerator.

[0260] Curing agent: "RIKACID MH-700" manufactured by Shin Nippon Chemical Co., Ltd. (4-methylhexahydrophthalic anhydride / hexahydrophthalic anhydride = 70 / 30)

[0261] Curing accelerator: "Hishicolin PX-4MP" (methyl tributylphosphonium dimethyl phosphate) manufactured by Nippon Chemical Industry Co., Ltd.

[0262] (2) α2 (linear expansion coefficient after Tg), Tg (glass transition temperature) (TMA):

[0263] Two glass plates with release PET films attached thereto were prepared so that both release PET films were facing inward and the interval between the glass plates was adjusted to 4 mm to prepare a mold.

[0264] The epoxy resin composition uniformly blended in the ratio shown in Table 2 (Table 2A, Table 2B) was poured into the mold, and heated at 100° C. for 3 hours and then at 130° C. for 3 hours to obtain a cured product.

[0265] The obtained cured product was cut into a cylindrical shape having a diameter of 1 cm and a thickness of 4 mm to obtain a test piece.

[0266] For this test piece, a thermomechanical analyzer (TMA: TMA / SS6100 manufactured by Seiko Instruments) was used. In compression mode, the first temperature increase was 5°C / min (30°C to 200°C), the first temperature decrease was 10°C / min (200°C to 30°C), and the second temperature increase was 5°C / min (30°C to 200°C). The second α2 and Tg were measured.

[0267] The evaluation results are shown in Table 2 (Table 2A, Table 2B).

[0268]

[0269] [Result evaluation]

[0270] As can be seen from Table 1, compared with the epoxy resin compositions of Comparative Examples 1 to 7, the epoxy resin compositions (A) of Examples 1 to 3 in which the compositions of epoxy resins (1) to (3) are within the specified range of the present invention have low total chlorine content, excellent electrical reliability, and small Hazen color values, and are excellent as optical materials.

[0271] As shown in Table 2, the cured products of the epoxy resin compositions (B) of Examples 4 to 6 using the epoxy resin compositions (A) of Examples 1 to 3 have excellent curability, low linear expansion, and heat resistance compared to the epoxy resin cured products of Comparative Examples 8 to 14.

[0272] Based on the above, it can be seen that the epoxy resin compositions (A) of Examples 1 to 3 and the epoxy resin compositions (B) of Examples 4 to 6 are superior to the epoxy resin compositions of Comparative Examples 1 to 7 and the epoxy resin compositions of Comparative Examples 8 to 14.

[0273] Although the present invention has been described in detail using specific embodiments, it will be apparent to one skilled in the art that various modifications can be made without departing from the spirit and scope of the present invention.

[0274] This application is based on Japanese Patent Application No. 2019-152125 filed on August 22, 2019, the entire contents of which are incorporated herein by reference.

Claims

1. An epoxy resin composition (A), comprising an epoxy resin having a structure represented by the following formula (1) (hereinafter referred to as epoxy resin (1), an epoxy resin having a structure represented by the following formula (2) (hereinafter referred to as epoxy resin (2) and / or an epoxy resin having a structure represented by the following formula (3) (hereinafter referred to as epoxy resin (3), wherein: The epoxy resin (1) and the epoxy resin (2) and / or the epoxy resin (3) account for 89.0% to 99.9% by mass of the epoxy resin (1) and 0.1% to 11.0% by mass of the epoxy resin (2) and / or the epoxy resin (3) in a total of 100% by mass. [Chemistry 1] In the formulae (1), (2) and (3), X is a divalent linking group selected from a direct bond, -SO2-, -O-, -CO-, -C(CF3)2-, -S- or a hydrocarbon group having 1 to 20 carbon atoms; R 1 is a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, or a halogen element, which may be the same or different from each other, and the two R atoms bonded to adjacent carbon atoms on the cyclohexane ring are 1 They are not bonded to each other, or they are bonded to each other to form a ring structure having 4 to 20 carbon atoms; n is an integer of 0 to 2.

2. The epoxy resin composition (A) according to claim 1, wherein In the formulas (1) to (3), X is an isopropylidene group, R 1 is a hydrogen atom, and n is 0.

3. The epoxy resin composition (A) according to claim 1 or 2, wherein The total chlorine content in accordance with JIS K7043-3 is 1000 ppm or less.

4. The epoxy resin composition (A) according to claim 1 or 2, wherein The epoxy equivalent is 176 g / equivalent to 186 g / equivalent.

5. The epoxy resin composition (A) according to claim 1 or 2, wherein The Hazen color value according to ISO 6271-2:2004, i.e., the APHA value, is 12 or less.

6. An epoxy resin composition (B), wherein The epoxy resin composition (A) according to any one of claims 1 to 5 contains 0.01 to 1000 parts by mass of a curing agent, based on 100 parts by mass of the epoxy resin composition (A).

7. A cured product obtained by curing the epoxy resin composition (B) according to claim 6.

8. An electric / electronic component obtained by curing the epoxy resin composition (B) according to claim 6. 9 . An optical component obtained by curing the epoxy resin composition (B) according to claim 6 .