A kind of thermoelectromagnetic refrigeration device and its preparation method

Through the preparation and particle processing of thermoelectromagnetic bulk materials, combined with the interface barrier layer and SPS sintering process, the problem of inapplicability of traditional thermoelectric devices has been solved, and efficient manufacturing and mass production of thermoelectromagnetic all-solid-state refrigeration devices have been achieved, improving refrigeration. performance and yield, and reduced thermal resistance.

CN114242883BActive Publication Date: 2024-10-22WUHAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111551645.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-17
Publication Date
2024-10-22
Estimated Expiration
2041-12-17

AI Technical Summary

Technical Problem

The processing methods and integration technologies of traditional thermoelectric devices are not suitable for the shape characteristics of new thermoelectromagnetic all-solid-state refrigeration devices, resulting in low refrigeration performance and yield, making it difficult to achieve mass manufacturing.

Method used

Thermoelectromagnetic refrigeration components suitable for Π-shaped structures are prepared by using the steps of preparation of thermomagnetic bulk materials, grain processing and cutting, interface barrier layer setting and device assembly integration, and through SPS sintering process and arc spraying process, using magnetocaloric materials. Gradient design reduces thermal resistance and improves heat dissipation effect.

Benefits of technology

It has realized efficient processing and manufacturing of thermoelectromagnetic all-solid-state refrigeration devices, improved yield and refrigeration performance, and is suitable for batch manufacturing. The gradient design of magnetocaloric materials has reduced thermal resistance and improved heat dissipation effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003417801280000011
    Figure HDA0003417801280000011
  • Figure HDA0003417801280000012
    Figure HDA0003417801280000012
  • Figure HDA0003417801280000021
    Figure HDA0003417801280000021
Patent Text Reader

Abstract

The present invention discloses a thermo-electromagnetic refrigeration component and a preparation method thereof, the preparation method comprising the steps of preparing thermo-electromagnetic block materials, processing and cutting of grains, surface treatment of grains and device assembly and integration, wherein the thermo-electromagnetic refrigeration component comprises an electrode block and an n-type thermo-electromagnetic refrigeration arm and a p-type thermo-electromagnetic refrigeration arm symmetrically connected to one side thereof. The present invention develops a Π-type thermo-electromagnetic component and an integrated manufacturing method thereof in view of the shape characteristics of the thermo-electromagnetic all-solid-state refrigeration component, the method can efficiently realize the processing and manufacturing of the thermo-electromagnetic all-solid-state refrigeration device, and has the advantages of high yield, simple operation, and batch manufacturing; by designing and optimizing the composition and structure of the thermo-electromagnetic block material, the heat dissipation speed of the magnetocaloric effect at the heat dissipation end of the obtained device can be effectively guaranteed, and the thermal resistance of the magnetocaloric effect can be effectively reduced; it can provide technical support for high-performance thermo-electromagnetic refrigeration components and their preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of functional devices and their manufacturing, and specifically relates to a thermoelectric refrigeration device and a preparation method thereof. Background Art

[0002] Thermo-electromagnetic all-solid-state refrigeration devices are electronic devices that can realize thermo-electromagnetic energy conversion. They have the advantages of no moving parts, easy maintenance and small size. They are widely used in the fields of thermo-electromagnetic energy conversion refrigeration, heating and two-way temperature control.

[0003] Thermo-electromagnetic all-solid-state refrigeration devices are new structural energy conversion devices that can realize thermoelectric refrigeration and magnetic refrigeration, and have higher refrigeration efficiency. Thermo-electromagnetic all-solid-state refrigeration devices have a complex structure, consisting of multiple thermo-electromagnetic refrigeration elements connected in series or in parallel through electrodes, where each thermo-electromagnetic refrigeration element is composed of one n-type and one p-type thermo-electromagnetic material connected in series through electrodes to form a Π-type structure.

[0004] However, the seeds used in conventional thermoelectric devices are rectangular, which are quite different in size and shape from the seeds in the new thermo-electromagnetic all-solid-state refrigeration device. Therefore, the processing methods and integration technologies of conventional thermoelectric devices are no longer applicable. In view of the shape characteristics of the new thermo-electromagnetic all-solid-state refrigeration device, the present invention has developed a thermo-electromagnetic energy conversion all-solid-state refrigeration device and an integrated manufacturing method thereof. The method can efficiently realize the processing, manufacturing and integration of the thermo-electromagnetic all-solid-state refrigeration device, while showing good refrigeration performance. Summary of the invention

[0005] The main purpose of the present invention is to provide a thermal electromagnetic energy conversion all-solid-state refrigeration device and a preparation method thereof in view of the problems and shortcomings of the prior art. The method has the advantages of high yield, simple operation, and batch production, and is suitable for promotion and application.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for preparing a thermoelectromagnetic cooling component comprises the steps of preparing a thermoelectromagnetic block material, processing and cutting a seed, treating the seed surface and assembling and integrating a device, wherein the thermoelectromagnetic cooling component comprises an electrode block and an n-type thermoelectromagnetic cooling arm and a p-type thermoelectromagnetic cooling arm connected to one side of the electrode block at intervals. The specific preparation steps include:

[0008] 1) Preparation of thermoelectromagnetic bulk materials

[0009] The n-type and p-type thermoelectric material powders are divided into several parts respectively, and the parts are mixed with magnetocaloric materials with increasing or decreasing contents respectively, and are laid layer by layer in a mold in sequence, and are pressed and sintered to obtain n-type thermoelectromagnetic bulk materials and p-type thermoelectromagnetic bulk materials respectively;

[0010] 2) Cutting the obtained n-type thermoelectromagnetic bulk material and p-type thermoelectromagnetic bulk material respectively to obtain thermoelectromagnetic material seeds;

[0011] 3) providing an interface barrier layer on the upper and lower surfaces of the obtained n-type and p-type thermoelectromagnetic material seeds to obtain an n-type thermoelectromagnetic cooling arm and a p-type thermoelectromagnetic cooling arm;

[0012] 4) Device assembly and integration; the upper surfaces of the n-type thermo-electromagnetic cooling arm and the p-type thermo-electromagnetic cooling arm which are spaced apart are welded and connected by electrode blocks to obtain the thermo-electromagnetic cooling component.

[0013] In the above scheme, the n-type or p-type thermoelectric material powder is obtained by crushing, grinding and sieving n-type or p-type bismuth telluride thermoelectric material crystal rods through 120 meshes.

[0014] In the above scheme, the n-type or p-type bismuth telluride thermoelectric material crystal rod is a commercially available product or a self-made crystal rod; the preparation method of the self-made crystal rod comprises: weighing the corresponding single substance powder according to the stoichiometric ratio of the n-type thermoelectric material and the p-type thermoelectric material, mixing them evenly, and then vacuum sealing, heating and melting, and zone melting growth to obtain n-type and p-type bismuth telluride thermoelectric material crystal rods respectively; and then crushing, grinding and sieving to obtain n-type and p-type thermoelectric material powders respectively.

[0015] In the above scheme, the n-type thermoelectric material is a Bi2(Te,Se)3-based alloy.

[0016] In the above solution, the p-type thermoelectric material is selected from (Bi, Sb)2Te3-based alloys.

[0017] In the above scheme, the temperature used in the zone melting growth process is 620-680°C, and the pulling speed is 10-20 mm / h.

[0018] In the above scheme, the magnetocaloric material is selected from Gd, YbAl3 or La(Fe,Si) 13 wait.

[0019] In the above scheme, the sieving step in step 1) is to sieve through a 120-mesh sieve.

[0020] In the above scheme, the content of the magnetocaloric material in the n-type thermoelectromagnetic bulk material and the p-type thermoelectromagnetic bulk material is 10-30wt%.

[0021] In the above scheme, the n-type or p-type thermoelectric material powder is respectively mixed with the magnetocaloric material by ball milling.

[0022] In the above scheme, in the preparation steps of the n-type thermoelectromagnetic bulk material and the p-type thermoelectromagnetic bulk material: the obtained n-type or p-type thermoelectric material powder is equally divided into N parts; the magnetocaloric material is divided into N parts in an arithmetic proportion starting from the amount 0 (in the mass ratio of 0:1:2:3:…:N-1, respectively).

[0023] In the above scheme, the sintering step in step 1) adopts the SPS sintering process, and the specific process parameters include: the sintering process is: the sintering step in step 1) adopts the SPS sintering process, and the specific process parameters include: first pre-pressurizing to 15-25MPa at room temperature, first heating to 320-340°C after 3-5min, continuing to heat to 340-350°C after 1-2min, and keeping warm to 350-360°C for 2-10min; then heating to 400-420°C at 45-60MPa for 5-10min, continuing to heat to 420-430°C after 1-3min, and finally keeping warm to 430-450°C after 3-5min, and cooling to room temperature with the furnace.

[0024] In the above scheme, the magnetocaloric material is distributed layer by layer in an equidistant proportion along the SPS sintering pressure direction.

[0025] In the above scheme, in step 2), the n-type thermoelectromagnetic bulk material and the p-type thermoelectromagnetic bulk material are cut into bulk materials with symmetrical structures.

[0026] In the above scheme, the n-type thermoelectromagnetic block material and the p-type thermoelectromagnetic block material are right-angled trapezoidal blocks or arc-shaped blocks; the dimensions of the right-angled trapezoidal blocks include: upper base length 10-15mm, lower base length 5-20mm, height 5-15mm, thickness 4-8mm; the dimensions of the arc-shaped blocks include: arc of 15-30°, outer diameter of the arc 80-100mm, inner diameter 60-80mm, thickness 4-8mm.

[0027] In the above scheme, the processing steps of the block material include: first, using an inner circle slicer to cut it into sheets with a thickness of 4 to 8 mm along the SPS ingot sintering pressure direction, and then using a precision dicing machine or wire cutting to cut the sheets into thermoelectromagnetic material particles according to the shape and size required by the thermoelectromagnetic energy conversion all-solid-state refrigeration device.

[0028] In the above solution, the interface barrier layer includes a nickel layer or a nickel alloy layer; wherein the nickel alloy layer can be selected from cobalt-nickel alloy or iron-nickel alloy.

[0029] In the above solution, the thickness of the interface barrier layer is 5 to 20 μm.

[0030] Preferably, in step 3), the surface of the n-type or p-type thermoelectromagnetic material seed to be provided with the interface barrier layer is first pretreated, specifically comprising: first polishing the surface of the seed with sandpaper, and then immersing the seed in acetone for degreasing, and the degreasing time is 10 to 30 seconds.

[0031] In the above scheme, the interface barrier layer is provided by arc spraying process, and the process parameters used include:

[0032] When spraying, the voltage is 40-50V, the current is 65-70A, and the speed is 10-20mm / s.

[0033] In the above scheme, the electrode block is a copper electrode, an aluminum electrode or a nickel electrode, etc.; its cross-section is bow-shaped or arc-shaped; the lower end surface of the electrode block matches the upper end surface of the n-type or p-type thermoelectromagnetic material particles, and the outer arc surface of the electrode is an arc of Φ100~110mm.

[0034] In the above scheme, in the assembly process described in step 4), first, the n-type and p-type thermoelectromagnetic material seeds are symmetrically and spaced apart in the grooves of the mold, the size of the grooves matches the shape of the seeds, wherein a side plate of one side of the grooves is positionally adjustable along the thickness direction of the seeds, and the position of the seeds can be adjusted during welding to ensure that the shape of the thermoelectromagnetic device is controllable; then, solder is set on the upper surface of the n-type and p-type thermoelectromagnetic material seeds, the lower surface of the electrode block is aligned with the upper surface of the n-type and p-type thermoelectromagnetic material seeds, and then the seeds are transferred to the welding workbench for welding.

[0035] In the above scheme, during the welding process, the hot end pressure head of the hot press welding machine used is an arc surface that matches the shape of the upper surface of the electrode block. The shape fits the copper electrode to ensure uniform pressure and heat transfer. During welding, the pressure head temperature is 300-400°C, the pressure head pressure is 0.1-0.3MPa, and the welding time is 20-40s. After the solder is completely melted, the power is turned off and cooled to complete the welding.

[0036] In the above solution, the solder may be tin paste or the like.

[0037] In the above scheme, after power-off cooling and demolding, the wires are welded on the lower surface to assemble a thermo-electromagnetic all-solid-state refrigeration device with a Π-shaped structure.

[0038] Based on the above contents, without departing from the basic technical concept of the present invention, according to the common knowledge and means in the field, the contents may be modified, replaced or changed in various forms.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] 1) The present invention develops an integrated manufacturing method for Π-type thermo-electromagnetic all-solid-state refrigeration components for the first time based on the shape characteristics of the thermo-electromagnetic all-solid-state refrigeration components. The method can efficiently realize the processing and manufacturing of thermo-electromagnetic all-solid-state refrigeration components, and has the advantages of high yield, simple operation, and batch production;

[0041] 2) During the sintering process of the thermo-electromagnetic block material of the present invention, the amount of the magnetocaloric material is divided into N parts according to the number of equal parts N of the thermoelectric material, starting from the condition of 0 amount according to an arithmetic difference ratio (0:1:2:3:…:N-1), and then the thermoelectric material is sequentially mixed with the magnetocaloric material and sintered, which can effectively ensure the heat dissipation speed of the magnetocaloric effect at the heat dissipation end of the obtained device and reduce the thermal resistance of the magnetocaloric effect;

[0042] 3) According to the above-mentioned gradient design requirements, the present invention further optimizes the SPS sintering process, which can effectively ensure the molding effect and thermoelectromagnetic properties of the obtained thermoelectromagnetic block material. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a schematic diagram of cutting the SPS ingot seeds of thermo-electromagnetic materials;

[0044] Figure 2 Assemble and integrate the flow chart for the thermo-electromagnetic all-solid-state refrigeration device;

[0045] Figure 3 The XRD patterns of the p-type and n-type bismuth telluride-based thermoelectromagnetic materials obtained in the present invention are shown in FIG.

[0046] Figure 4 This is a refrigeration performance diagram of the thermo-electromagnetic energy conversion all-solid-state refrigeration device obtained in Example 1 of the present invention at an optimal current;

[0047] Figure 5 It is a schematic diagram of the distribution of magnetocaloric materials in the n-type thermoelectromagnetic cooling arm and the p-type thermoelectromagnetic cooling arm obtained by the present invention. DETAILED DESCRIPTION

[0048] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with specific embodiments, but the content of the present invention is not limited to the following embodiments.

[0049] In the following examples, the average particle size of the Gd spheres used was 100-150 μm, and they were provided by Baotou Rare Earth Research Institute.

[0050] Example 1

[0051] A thermal electromagnetic energy conversion all-solid-state refrigeration device, the preparation method of which comprises the following steps:

[0052] 1) Preparation of thermoelectromagnetic materials:

[0053] Bi powder, Te powder and Sb powder were used as raw materials respectively, and p-type bismuth telluride (Bi 0.5 T3S 1.5 ) and n-type bismuth telluride (Bi2Te 0.3 Se 2.7 )

[0054] The weighed raw material powders were mixed evenly, sealed in a vacuum tube, and placed in a rocking furnace for heat preservation at 650° C. for 2 h to obtain an n-type bismuth telluride solid solution alloy and a p-type bismuth telluride solid solution alloy, respectively;

[0055] The obtained n-type bismuth telluride solid solution alloy and p-type bismuth telluride solid solution alloy are placed in a pulling furnace for purification, wherein the set temperature is 630° C. and the pulling speed is 15 mm / h, to obtain n-type and p-type bismuth telluride based crystal rods, respectively;

[0056] 2) Seed processing and cutting:

[0057] 2-1; The p-type bismuth telluride-based crystal rods obtained in step 1) are crushed and ground and sieved through 120 mesh, 40g of the obtained p-type bismuth telluride-based powder is taken, and it is divided into 4 parts by mass, 4.4g of Gd balls are weighed according to a mass fraction of 10% (accounting for the total amount of bismuth telluride-based powder and Gd balls), and then the weighed Gd balls are divided into 4 parts according to a mass ratio of 0:1:2:3, and then respectively placed in a ball mill with the above 4 parts of bismuth telluride powder, and ball milled for 30 minutes under the conditions of a ball-to-material ratio of 10:1 and a rotation speed of 150rpm; the mixed 4 parts of thermo-electromagnetic composite powder are sieved according to the Gd ball content The amount of the alloy is gradually added into the mold and compacted, and SPS sintering is performed. The specific sintering process is: first, pre-pressurize to 20MPa at room temperature, heat to 330℃ after 5min, heat to 348℃ after 1min, and keep warm to 350℃ for 5min; then heat to 420℃ at 50MPa for 7min, heat to 428℃ after 1min, and keep warm to 430℃ for 5min, and cool to room temperature with the furnace to obtain a p-type bismuth telluride-based thermal electromagnetic composite ingot with an alloy doping amount of 10wt% and a gradient distribution of Gd elements. The obtained ingot has a diameter of 25mm and a thickness of 13mm.

[0058] 2-2; Referring to the step described in 2-1, 44.7 g of the obtained n-type bismuth telluride-based powder and 4.97 g of Gd balls with a doping amount of 10 wt% were weighed to prepare an n-type bismuth telluride-based thermo-electromagnetic composite ingot. The obtained ingot had a diameter of 25 mm and a thickness of 13 mm;

[0059] 2-3; The obtained p-type and n-type bismuth telluride-based thermo-electromagnetic composite ingots (XRD diagram see Figure 3) are first cut into sheets with a thickness of 5 mm along the axial direction using an inner circle slicer, and then the obtained sheets are cut into right-angled trapezoidal seeds using a precision dicing machine. The right-angled trapezoidal seeds obtained by cutting have the following dimensions: the upper and lower bases and heights are 14 mm, 18 mm and 10 mm respectively, and the thickness is 5 mm. At this time, the lower base of 18 mm is the side with the highest content of Gd balls;

[0060] 3) Surface treatment of seeds:

[0061] The obtained p-type and n-type seeds were first polished with 2000-grit sandpaper, then immersed in acetone for 20 seconds for degreasing, and finally a layer of metal Ni layer was sprayed on the upper and lower surfaces of the thermoelectromagnetic material seeds by arc spraying. The voltage was 50V, the current was 70A, the speed was 15mm / s, and the Ni layer thickness was 10μm.

[0062] 4) Device assembly and integration

[0063] Place the right-angled trapezoidal p-type seeds and n-type seeds that have been surface treated in step 3) in the mold, wherein the p-type seeds and the n-type seeds are aligned with each other along the right-angled sides in the height direction, and dip the solder paste in the mold and evenly apply it on the upper surface of the seeds;

[0064] The arcuate copper electrode block is placed on the surface of the p-type seed and the n-type seed along its plane bottom surface, and the copper electrode and the thermo-electromagnetic material are welded using a hot pressing welding machine, wherein the hot end pressure head temperature during welding is 350°C, the welding pressure is 0.2MPa, and the time is 20s;

[0065] After power-off, cooling and demolding, wires are welded to the lower surface of the thermo-electromagnetic material seeds, and power is turned on to test whether the circuit is open, thereby assembling a Π-shaped thermo-electromagnetic all-solid-state refrigeration device.

[0066] The refrigeration performance of the thermo-electromagnetic all-solid-state refrigeration device obtained in this embodiment at the optimal current is shown in FIG. Figure 4 The results show that at the optimal device current of 2A, the cooling temperature difference is 3.6K for p-type and 1.2K for n-type.

[0067] Example 2

[0068] A thermal electromagnetic energy conversion all-solid-state refrigeration device, the preparation method of which comprises the following steps:

[0069] 1) Preparation of thermoelectromagnetic materials:

[0070] Bi powder, Te powder and Sb powder were used as raw materials respectively, and p-type bismuth telluride (Bi 0.5 T3S 1.5 ) and n-type bismuth telluride (Bi2Te 0.3 Se 2.7 )

[0071] The weighed raw material powders were mixed evenly, sealed in a vacuum tube, and placed in a rocking furnace for heat preservation at 650° C. for 2 h to obtain an n-type bismuth telluride solid solution alloy and a p-type bismuth telluride solid solution alloy, respectively;

[0072] The obtained n-type bismuth telluride solid solution alloy and p-type bismuth telluride solid solution alloy are placed in a pulling furnace for purification, wherein the temperature is set to 630° C. and the pulling speed is 15 mm / h, to obtain n-type and p-type bismuth telluride based crystal rods, respectively;

[0073] 2) Seed processing and cutting:

[0074] 2-1; The p-type bismuth telluride-based crystal rods obtained in step 1) are crushed and ground and sieved through 120 mesh, 36.06g of the obtained p-type bismuth telluride-based powder is taken, and it is divided into 4 parts by mass, 9.02g of Gd balls are weighed according to a mass fraction of 20% (accounting for the total amount of bismuth telluride-based powder and Gd balls), and then the weighed Gd balls are divided into 4 parts according to a mass ratio of 0:1:2:3, and then respectively placed in a ball mill with the above 4 parts of bismuth telluride powder, and ball milled for 30 minutes under the conditions of a ball-to-material ratio of 10:1 and a rotation speed of 150rpm; the mixed 4 parts of thermal electromagnetic composite powder are mixed according to the Gd ball The content gradient is sequentially added into the mold and compacted, and SPS sintering is performed. The specific sintering process is: first, pre-pressurize to 20MPa at room temperature, heat to 330℃ after 5min, heat to 348℃ after 1min, keep warm to 350℃ for 5min, then heat to 420℃ at 50MPa for 7min, heat to 428℃ after 1min, and keep warm to 430℃ for 5min, and cool to room temperature with the furnace to obtain a p-type bismuth telluride-based thermo-electromagnetic composite ingot with an alloy doping amount of 20wt% and a gradient distribution of Gd elements. The obtained ingot has a diameter of 25mm and a thickness of 13mm;

[0075] 2-2; Referring to the step described in 2-1, 39.83 g of the obtained n-type bismuth telluride-based powder and 9.96 g of Gd balls with a doping amount of 20 wt% were weighed to prepare an n-type bismuth telluride-based thermo-electromagnetic composite ingot. The obtained ingot had a diameter of 25 mm and a thickness of 13 mm;

[0076] 2-3; The obtained p-type and n-type bismuth telluride-based thermo-electromagnetic composite ingots are first cut into sheets with a thickness of 5 mm along the axial direction by an inner circle slicer, and then the obtained sheets are cut into arc-shaped seeds by a precision dicing machine. The cut arc-shaped seeds (20°) have the following dimensions: the outer diameter and inner diameter of the arc are Φ100 mm and Φ80 mm respectively, the thickness is 5 mm, and the outer diameter of the seeds is the side with the highest Gd ball content;

[0077] 3) Surface treatment of seeds:

[0078] The obtained p-type and n-type seeds were first polished with 2000-grit sandpaper, then immersed in acetone for 20 seconds for degreasing, and finally a layer of metal Ni layer was sprayed on the upper and lower surfaces of the thermoelectromagnetic material seeds by arc spraying. The voltage was 50V, the current was 70A, the speed was 15mm / s, and the Ni layer thickness was 10μm.

[0079] 4) Device assembly and integration

[0080] Place the arc-shaped p-type seeds and n-type seeds that have been surface treated in step 3) in the mold, wherein the p-type seeds and n-type seeds are aligned with each other along the radial direction, and dip the solder paste and evenly apply it on the upper surface of the seeds along the circumferential direction of the outer diameter;

[0081] The arc-shaped copper electrode block is aligned along the outer peripheral cross-section of the p-type seed and the n-type seed and placed on the surface of the p-type seed and the n-type seed, and the copper electrode is welded to the thermo-electromagnetic material using a hot pressing welding machine, wherein the hot end pressure head temperature during welding is 350°C, the welding pressure is 0.1MPa, and the time is 20s;

[0082] After power-off, cooling and demolding, wires are welded to the lower surface of the thermo-electromagnetic material seeds, and power is turned on to test whether the circuit is open, thereby assembling a Π-shaped thermo-electromagnetic all-solid-state refrigeration device.

[0083] Example 3

[0084] A thermal electromagnetic energy conversion all-solid-state refrigeration device, the preparation method of which comprises the following steps:

[0085] 1) Preparation of thermoelectromagnetic materials:

[0086] Bi powder, Te powder and Sb powder were used as raw materials respectively, and p-type bismuth telluride (Bi 0.5 T3S 1.5 ) and n-type bismuth telluride (Bi2Te 0.3 Se 2.7 )

[0087] The weighed raw material powders were mixed evenly, sealed in a vacuum tube, and placed in a rocking furnace for heat preservation at 650° C. for 2 h to obtain an n-type bismuth telluride solid solution alloy and a p-type bismuth telluride solid solution alloy, respectively;

[0088] The obtained n-type bismuth telluride solid solution alloy and p-type bismuth telluride solid solution alloy are placed in a pulling furnace for purification, wherein the temperature is set to 630° C. and the pulling speed is 15 mm / h, to obtain n-type and p-type bismuth telluride based crystal rods, respectively;

[0089] 2) Seed processing and cutting:

[0090] 2-1; The p-type bismuth telluride-based crystal rods obtained in step 1) are crushed and ground and sieved through 120 mesh, 36.06g of the obtained p-type bismuth telluride-based powder is taken, and it is divided into 4 parts by mass, 9.02g of Gd balls are weighed according to a mass fraction of 20% (accounting for the total amount of bismuth telluride-based powder and Gd balls), and then the weighed Gd balls are divided into 4 parts according to a mass ratio of 0:1:2:3, and then respectively placed in a ball mill with the above 4 parts of bismuth telluride powder, and ball milled for 30 minutes under the conditions of a ball-to-material ratio of 10:1 and a rotation speed of 150rpm; the mixed 4 parts of thermal electromagnetic composite powder are mixed according to the Gd ball The content gradient is sequentially added into the mold and compacted, and SPS sintering is performed. The specific sintering process is: first, pre-pressurize to 20MPa at room temperature, heat to 330℃ after 5min, heat to 348℃ after 1min, keep warm to 350℃ for 5min, then heat to 420℃ at 50MPa for 7min, heat to 428℃ after 1min, and keep warm to 430℃ for 5min, and cool to room temperature with the furnace to obtain a p-type bismuth telluride-based thermo-electromagnetic composite ingot with an alloy doping amount of 20wt% and a gradient distribution of Gd elements. The obtained ingot has a diameter of 25mm and a thickness of 13mm;

[0091] 2-2; Referring to the step described in 2-1, 39.83 g of the obtained n-type bismuth telluride-based powder and 9.96 g of Gd balls with a doping amount of 20 wt% were weighed to prepare an n-type bismuth telluride-based thermo-electromagnetic composite ingot. The obtained ingot had a diameter of 25 mm and a thickness of 13 mm;

[0092] 2-3; The obtained p-type and n-type bismuth telluride-based thermo-electromagnetic composite ingots are first cut into sheets with a thickness of 5 mm along the axial direction using an inner circle slicer, and then the obtained sheets are cut into arc-shaped seeds using a precision dicing machine. The dimensions of the cut arc-shaped seeds (20°) are: the outer diameter and inner diameter of the arc are Φ100 mm and Φ80 mm respectively, the thickness is 5 mm, and the outer diameter of the seeds is the side with the highest Gd ball content.

[0093] 3) Surface treatment of seeds:

[0094] The obtained p-type and n-type seeds were first polished with 2000-grit sandpaper, then immersed in acetone for 20 seconds for degreasing, and finally a layer of cobalt-nickel alloy (containing about 25wt%) was sprayed on the upper and lower surfaces of the thermo-electromagnetic material seeds by arc spraying. The voltage was 45V, the current was 65A, the speed was 15mm / s, and the thickness of the alloy layer was 10μm.

[0095] 4) Device assembly and integration

[0096] Place the arc-shaped p-type seeds and n-type seeds that have been surface treated in step 3) in the mold, wherein the p-type seeds and n-type seeds are aligned with each other along the radial direction, and dip the solder paste and evenly apply it on the upper surface of the seeds along the circumferential direction of the outer diameter;

[0097] The arc-shaped copper electrode block is aligned along the outer peripheral cross-section of the p-type seed and the n-type seed and placed on the surface of the p-type seed and the n-type seed, and the copper electrode is welded to the thermo-electromagnetic material using a hot pressing welding machine, wherein the hot end pressure head temperature during welding is 350°C, the welding pressure is 0.1MPa, and the time is 20s;

[0098] After power-off, cooling and demolding, wires are welded to the lower surface of the thermo-electromagnetic material seeds, and power is turned on to test whether the circuit is open, thereby assembling a Π-shaped thermo-electromagnetic all-solid-state refrigeration device.

[0099] Figure 5 The diagram is a schematic diagram of the distribution of magnetocaloric materials in the n-type thermoelectromagnetic cooling arm and the p-type thermoelectromagnetic cooling arm obtained by the present invention, wherein the white part does not contain magnetocaloric materials, and the gray part has a magnetocaloric material content gradient increasing in the direction corresponding to the color increasing direction; the use of the gradient increasing design method starting from the content of 0 effectively ensures the heat dissipation speed of the magnetocaloric effect at the heat dissipation end of the obtained device, and reduces the thermal resistance of the magnetocaloric effect; under the same dosage conditions, the use of the arithmetic proportional gradient design method that does not start from the content of 0 has a relatively large thermal resistance and low heat exchange efficiency.

[0100] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a thermoelectromagnetic refrigeration component, characterized in that: The invention comprises the steps of preparing thermoelectromagnetic block material, processing and cutting of seeds, surface treatment of seeds and assembly and integration of devices, wherein the thermoelectromagnetic cooling components include an electrode block and an n-type thermoelectromagnetic cooling arm and a p-type thermoelectromagnetic cooling arm connected to one side of the electrode block at intervals. The specific preparation steps include: 1) Preparation of thermoelectromagnetic bulk materials The n-type and p-type thermoelectric material powders are divided into several parts respectively, and then mixed with magnetocaloric materials with increasing or decreasing contents, and laid layer by layer in a mold in sequence, and pressed and sintered to obtain n-type thermoelectromagnetic bulk materials and p-type thermoelectromagnetic bulk materials respectively; 2) Cutting the obtained n-type thermoelectromagnetic bulk material and p-type thermoelectromagnetic bulk material respectively to obtain thermoelectromagnetic material seeds; 3) providing an interface barrier layer on the upper and lower surfaces of the obtained n-type and p-type thermoelectromagnetic material seeds to obtain an n-type thermoelectromagnetic cooling arm and a p-type thermoelectromagnetic cooling arm; 4) Device assembly and integration: using electrode blocks to connect the upper surfaces of the n-type thermo-electromagnetic cooling arm and the p-type thermo-electromagnetic cooling arm that are spaced apart, thus obtaining the thermo-electromagnetic cooling component.

2. The preparation method according to claim 1, characterized in that: The n-type thermoelectric material is a Bi2(Te,Se)3-based alloy; the p-type thermoelectric material is a (Bi,Sb)2Te3-based alloy thermoelectric material; the magnetocaloric material is Gd, YbAl3 or La(Fe,Si) 13 .

3. The preparation method according to claim 1, characterized in that: In the n-type thermoelectromagnetic bulk material and the p-type thermoelectromagnetic bulk material, the content of the magnetocaloric material is 10-30 wt%.

4. The preparation method according to claim 1, characterized in that: In the preparation steps of the n-type thermoelectromagnetic bulk material and the p-type thermoelectromagnetic bulk material: the obtained n-type or p-type thermoelectric material powder is evenly divided into N parts; and the magnetocaloric material is divided into N parts starting from 0 according to an arithmetic progression.

5. The preparation method according to claim 1, characterized in that: Step 1) The sintering step adopts the SPS sintering process, and the specific process parameters include: first pre-pressurizing to 15-25MPa at room temperature, first heating to 320-340°C after 3-5min, continuing to heat to 340-350°C after 1-2min, and keeping warm to 350-360°C for 2-10min; then heating to 400-420°C at 45-60MPa for 5-10min, continuing to heat to 420-430°C after 1-3min, and finally keeping warm to 430-450°C after 3-5min, and cooling to room temperature with the furnace.

6. The preparation method according to claim 1, characterized in that: The magnetocaloric material is distributed layer by layer in an equidistant proportion along the SPS sintering pressure direction.

7. The preparation method according to claim 1, characterized in that: The n-type thermoelectromagnetic block material and the p-type thermoelectromagnetic block material are right-angled trapezoidal blocks or arc-shaped blocks.

8. The preparation method according to claim 1, characterized in that: The interface barrier layer includes a nickel layer or a nickel alloy layer.

9. The preparation method according to claim 1, characterized in that: The electrode block is a copper electrode, an aluminum electrode or a nickel electrode; its cross section is an arc or a bow; wherein the lower end surface of the electrode block matches the upper end surface of the n-type or p-type thermoelectromagnetic material grain.

10. Thermo-electromagnetic refrigeration component prepared by the preparation method according to any one of claims 1 to 9.