Method for synthesizing silver nanosheets and silver nanosheets coated with precious metals, and use thereof in transparent films

By synthesizing silver nanosheets at high concentrations and applying precious metal coatings, the problems of brittleness and complex production of existing transparent conductive film materials are solved, and a transparent conductive film with high stability and multiple application requirements is achieved.

CN114255906BActive Publication Date: 2024-10-11EKC TECHNOLOGY INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111313319.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2015-12-09
Filing Date
2016-12-02
Publication Date
2024-10-11
Estimated Expiration
2036-12-02

AI Technical Summary

Technical Problem

Existing transparent conductive film materials such as indium tin oxide (ITO) have problems such as brittleness, complex production processes, and easy rupture. They also perform poorly on flexible substrates, making it difficult to meet the needs of a wide range of applications.

Method used

A high-concentration synthesis method of silver nanosheets is adopted, and stable silver nanosheets are formed by gradually adding hydrogen peroxide and reducing agents, and then a noble metal coating is applied on the silver nanosheets to form precious metal-coated silver nanosheets with high stability. sheet, used to prepare transparent conductive films.

Benefits of technology

It achieves large-scale production of stable silver nanosheets and precious metal coatings, improves the mechanical strength and optical properties of the film, reduces production costs, and performs well on flexible substrates to meet a variety of application needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114255906B_ABST
    Figure CN114255906B_ABST
Patent Text Reader

Abstract

The present invention describes a desirable method for larger scale synthesis of silver nanosheets and a method for applying a noble metal coating to the silver nanosheets to form coated silver nanosheets with a desired absorption spectrum. The silver nanosheets are suitable for use in coatings to change the hue of transparent films. Transparent conductive films may particularly desire hue adjustment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to improved stable silver nanosheets, large-scale stable synthesis of silver nanosheets, precious metal coated silver nanosheets with desired absorption properties, and synthesis of precious metal coatings on silver nanosheets. Background Art

[0002] Transparent polymer films are used in a wide range of products (e.g., electronic displays). Functional transparent films can provide desired functionality, such as transparent conductive films. For example, conductive films may be important for dissipating static electricity when static electricity generation is undesirable or dangerous. Optical films can be used to provide various functions, such as polarization, anti-reflection, phase shift, brightness enhancement, or other functions. High-quality displays may include one or more optical coatings. Based on various applications, visual appearance (e.g., color, transparency, haze, etc.) may be an important aspect of transparent polymer films.

[0003] Transparent conductors can be used in several optoelectronic applications, including, for example, touch screens, liquid crystal displays (LCDs), flat panel displays, organic light emitting diodes (OLEDs), solar cells, and smart windows. Historically, indium tin oxide (ITO) has been the material of choice due to its relatively high transparency at reasonable conductivity. However, ITO still has several disadvantages. For example, ITO is a brittle ceramic that is typically deposited using sputtering, which involves high temperatures and a vacuum and thus the fabrication process can be relatively slow. Additionally, ITO is known to be prone to cracking on flexible substrates. Summary of the invention

[0004] In a first aspect, the present invention relates to a method for synthesizing silver nanosheets, the method comprising the steps of gradually adding a second amount of hydrogen peroxide to an aqueous solution of a blend of silver ions, polycarboxylate anions, a multifunctional hydroxide compound, a first amount of hydrogen peroxide, and a reducing agent under mixing conditions. Typically, the aqueous solution may have a silver ion concentration of about 0.00025 M to about 0.1 M, and the molar ratio of total hydrogen peroxide to reducing agent may be about 10 to about 120.

[0005] In another aspect, the invention relates to a dispersion of silver nanoplatelets having an average equivalent circular diameter of no more than about 120 nm, the dispersion being free of polymeric capping agents and / or inorganic coatings and having stability for at least 21 days of dark storage at ambient conditions as measured by a shift in the peak absorption spectrum wavelength of no more than about 40 nm.

[0006] In another aspect, the present invention is directed to a dispersion of precious metal coated silver nanoflakes having at least about 5 wt. % precious metal and having a light absorption at 600 nm of at least about 0.6 normalized absorption units, and the corresponding silver nanoflakes without the precious metal coating also have a light absorption at 600 nm of at least about 0.6 normalized absorption units.

[0007] In other aspects, the present invention relates to a method for applying a noble metal coating to silver nanosheets, the method comprising the steps of gradually adding a coating solution comprising a complexed noble metal ion aqueous solution and a polymer capping agent to a reaction solution comprising an aqueous dispersion of silver nanosheets, a polycarboxylate anion, a polymer capping agent, a ligand, and a reducing agent. Typically, the total concentration of all forms of silver may be at least about 0.75 mM. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] Figure 1 is a partial side view of a film having a sparse metallic conductive layer and various additional transparent layers on both sides of the sparse metallic conductive layer.

[0009] Figure 2 is a top view of a representative schematic patterned structure having three conductive paths formed using a sparse metal conductive layer.

[0010] Figure 3 is a plot of the normalized optical absorption spectra of the solution after the first step of hydrogen peroxide addition and after the second addition of hydrogen peroxide when forming silver nanosheets.

[0011] Figure 4 is a plot of the normalized optical absorption spectra of treated silver nanosheets from silver solution based on two-step hydrogen peroxide addition compared to the corresponding reaction involving a single addition of hydrogen peroxide.

[0012] Figures 5A-5J : is a plot of the normalized optical absorption spectra of silver nanosheets synthesized at different silver concentrations (A=12×, B=16×, C=24×, D=32×, E=44×, F=68×, G=88×, H=100×, I=128× and J=156×) using the method of Example 1.

[0013] Figure 6 is a plot of the normalized optical absorption of three silver nanosheet samples synthesized using diacetone alcohol, ethyl lactate, or propylene glycol as alternative stabilizers instead of glycerol.

[0014] Figure 7 is a plot of normalized optical absorption for a representative sample of silver nanoflakes synthesized in Example 1 and gold-coated silver nanoflakes synthesized as described in Example 2.

[0015] Figure 8is a plot of the normalized light absorption of the as-synthesized silver nanosheets, the gold-coated silver nanosheets formed with the addition of citrate during the coating process, and the gold-coated silver nanosheets formed without the addition of citrate during the coating process.

[0016] Fig. 9 is a transmission electron micrograph of a typical gold-coated silver nanosheet.

[0017] Fig.10 is a plot of light absorption of uncoated silver nanosheets and three groups of gold-coated silver nanosheets with different gold coating thicknesses.

[0018] Fig.11 is a plot of light absorption of gold-coated silver nanosheets before freezing and after freeze-thaw cycles.

[0019] Fig.12 is a plot of light absorption of PVP-coated commercial silver nanosheets before freezing and after freeze-thaw cycles.

[0020] Fig.13 is a plot of light absorption of gold-coated silver nanosheets dispersed in propylene glycol monomethyl ether before and after heating at 90° C. for 100 hours.

[0021] Fig.14 is a plot of light absorption of uncoated silver nanosheets dispersed in propylene glycol monomethyl ether before and after heating at 90° C. for 100 hours.

[0022] Fig.15 is a plot of the b* value for transparent conductive ink films with a polymer hardcoat or with a polymer hardcoat loaded with silver nanoflakes as a function of storage days at 60°C and 90% relative humidity.

[0023] Fig.16 is a plot of the b* value for transparent conductive ink films with a polymer hardcoat or with a polymer hardcoat loaded with gold-coated silver nanoflakes as a function of storage days at 60° C. and 90% relative humidity.

[0024] Fig.17 is a transmission electron micrograph of typical gold-coated silver nanosheets well dispersed in a conductive fused metal nanostructured network.

[0025] Fig.18 is a set of three histogram plots for samples of conductive fused metal nanostructured networks comprising increasing amounts of silver nanoplatelets included in the conductive layer and a polymer binder, wherein the histogram plots relate to b*, a*, and haze. DETAILED DESCRIPTION

[0026] It has been found that the hue of light transmission through a transparent conductive film can be controlled using nanoscale colorants without significantly changing the overall light transmission, haze, or conductivity of the film. In particular, metal nanosheets have been modified to produce specific colors based on surface plasmon resonance. Synthetic methods for forming stable silver nanosheets optionally with a noble metal (e.g., gold) coating are described herein for forming commercial quantities of nanosheets. Synthetic procedures have been successfully developed based on increasing the concentration of the reaction solution and / or increasing the total volume, with no undesirable changes in the morphology or stability of the nanosheets. The noble metal coating can be applied on a large scale without undesirable changes in the color of the coated nanosheets. In some embodiments, silver nanosheets used as colorants can be incorporated into a conductive layer and / or coating together with a polymer binder. The silver nanosheets can at least partially compensate for the color (due to the conductive component) transmitted through the transparent conductive film and / or can introduce a desired hue to the film. In particular, transparent conductive films can be effectively formed from metal nanowires and / or from fused metal nanostructured networks, but in other or alternative embodiments, other transparent conductive materials (e.g., appropriate metal oxides) can be used. In some embodiments, nanoscale colorants can improve the whiteness of light transmission through a nanowire-based conductive layer without significantly increasing haze or reducing light transmission.

[0027] This article describes an improved synthesis method that can be used to produce nanosheets with absorption spectra that effectively produce whiter colors from silver nanowire-based conductive films. Likewise, precious metal-coated silver nanosheets are synthesized to be incorporated into films with high stability over time. The precious metal coating can be applied in a stable deposition process that forms a uniform precious metal coating on the silver nanosheets. The precious metal-coated silver nanosheets can be incorporated into a coating on a sparse metal conductive layer with the desired results, as shown in the examples below. With respect to changes in hue / color and the inclusion of metal nanosheets in the corresponding films, unless explicitly excluded, the silver nanosheets mentioned also include precious metal-coated nanosheets.

[0028] Color spaces can be defined to relate spectral wavelengths to human color perception. CIELAB is a color space defined by the International Commission on Illumination (CIE). The CIELAB color space uses a three-dimensional coordinate set L*, a*, and b*, where L* relates to color lightness, a* relates to the color position between red and green, and b* relates to the color position between yellow and blue. The "*" value represents a normalized value relative to a standard white point. As described below, these CIELAB parameters can be determined from measurements made in a spectrophotometer using commercial software.

[0029] Transparent conductive films can be formed from various nanomaterials such as carbon nanotubes, metal nanowires, and the like. Likewise, conductive metal oxides can be used to form conductive films, such as indium tin oxide (ITO), aluminum-doped zinc oxide (AZO), and the like. Conductive metal oxides can be formed as a conductive layer in a layer with a polymer binder or may be formed as particles. In the case of silver nanowires used for transparent conductive films, for a given optical transparency and clarity, the use of longer and thinner nanowires generally produces better conductivity. However, it has been observed that some films formed using thinner silver nanowires may appear slightly yellow.

[0030] It has been found that the color of transparent conductive films can be made less yellow (i.e., the absolute value of b* is smaller) by incorporating metal nanosheets, metal nanoshells, nanobelts, or other nanoscale colorants (e.g., pigments). Nanosheets can be adjusted based on surface plasmon resonance for specific color properties, and other nanoscale colorants can be selected based on color and low contribution to reducing total transmittance. Metal nanostructures can be coated with polymers, different metals, and / or non-metallic compositions (e.g., silicon dioxide). This article describes a synthetic method for effective coating using precious metals (e.g., Pt, Pd, Ir, Rh, Ru, Os, or a combination thereof). Small amounts of nanoscale colorants can be incorporated into the film to change the overall color properties, and in some embodiments, the total transmittance is not significantly reduced and / or the haze is increased. It has been found that certain size ranges and types of nanosheets and nanoshells can even reduce haze. In particular, silver nanosheets, nanoshells, or other nanoscale components can compensate for the color distortion introduced by the conductive components in the film to produce whiter transmitted light. In other embodiments, accordingly, if desired, the desired color can be introduced into the transmitted light using the selected nanoscale component. The discussion herein focuses on producing whiter light, but those skilled in the art understand that the desired hue of the transmitted light can be introduced by introducing the selected nanoscale colorant, while forming a transparent film with a total transmittance of visible light of typically at least about 85% in some embodiments. In appropriate embodiments, the nanoscale particles can be effectively incorporated into the conductive layer, the coating, or both. The general use of nanoscale colorants for controlling hue is described in the published U.S. patent application 2016 / 0108256 entitled "Transparent Films with Control of Light Hue Using Nanoscale Colorants" by Yang et al. (incorporated herein by reference).

[0031] As described herein, a color-adjusting coating can be formed with a moderate reduction in total visible light transmission. Various polymers can be introduced as binders with relatively good mechanical strength to provide a good high transparency matrix. Generally, a coating with a small thickness can be formed while providing the desired color adjustment. In some embodiments, a small thickness is desirable for use with adjacent transparent conductive layers because conductivity can be maintained throughout the thin outer coating. Therefore, a desired degree of color adjustment can be obtained with an average coating thickness of no more than about 100 microns and in some embodiments no more than one micron.

[0032] Good coating properties generally involve forming a good dispersion of silver nanoplatelets in the matrix polymer solution so that the resulting coating has reduced particle agglomeration effects. The silver nanoplatelets can generally be incorporated into a relatively smooth thin coating and so that the particles do not alter the optical properties beyond the desired range. Generally, the coating has a silver nanoplatelet loading of no more than about 30% by weight. The concentrations of the polymer binder and the silver nanoplatelets in the coating solution can be adjusted to obtain the desired coating properties for the solution, such as the viscosity and thickness of the final coating. The ratio of the solid concentration in the coating solution can be adjusted to obtain the desired coating concentration after the coating is dried. The polymer components of the coating can generally be cross-linked using UV radiation or other means suitable for the polymer binder to further strengthen the coating.

[0033] In general, silver nanosheets can be introduced into a passive protective coating and / or directly into a transparent conductive layer. The transparent conductive layer can be covered with or without a passive transparent protective coating. A common feature of these coatings is the compatibility of the components in the coating solution and the resulting composite material. Compatibility refers to the ability to effectively disperse in a relatively uniform material without an unacceptable degree of aggregation (e.g., agglomeration) of the components. In particular, compatibility allows the material to be well distributed in the coating solution to form a moderately uniform composite material that can form a coating. A more uniform composite material is believed to contribute to the desired optical properties of the coating, such as good transparency and low haze.

[0034] For passive coatings, the coating solution may include a solvent, a dissolved matrix polymer, a nanoscale colorant, possible combinations thereof, and optional other components. A variety of matrix polymers suitable for transparent films may be used, as described below. Wetting agents (e.g., surfactants) and other processing aids may be used. Generally, the solvent may include water, an organic solvent, or a suitable mixture thereof. For active coatings, the coating solution typically further includes components that contribute to active functionality, such as metal nanowires that contribute to conductivity.

[0035] Nanoplates have an average thickness of no more than 100 nm and two other dimensions that may be greater than or not greater than 100 nm. Metal nanoplates have been synthesized using solution-based techniques and their optical properties have been examined. See, for example, published U.S. Patent Application No. 2012 / 0101007, entitled “Silver Nanoplates”, by Ahern et al., and published U.S. Patent Application No. 2014 / 0105982, entitled “Silver Nanoplate Compositions and Methods”, by Oldenburg et al., both of which are incorporated herein by reference. Silver nanoplates that adjust absorption properties based on surface plasmon resonance can be purchased from nanoComposix, Inc., San Diego, CA, USA, Beijing Nanomeet Technology Co. Ltd., China, and Suzhou ColdStones Technology Co., Ltd., China. Similarly, nanoplatelets can be directly synthesized, for example, using known synthesis techniques, see, e.g., Kelly et al., ACTA PHYSICA POLONICA A, (2012), 122:337-345, “Triangular Silver Nanoparticles: Their Preparation, Functionalisation and Properties”; Jiang et al., Inorganic Chemistry, (2004), 43:5877-5885, “Ultrasonic-Assisted Synthesis of Monodisperse Single-Crystalline Silver Nanoplates and Gold Nanorings”; and Xiong et al., Langmuir (2006), 20:8563-8570, “Poly(vinyl pyrrolidone): a dual functional reductant and stabilizer for the facilesynthesis of noble metal nanoplates in aqueous solutions”, all three of which are incorporated herein by reference. As reported by nanoComposix, silver nanoplatelets have a thickness of about 10 nm and an (equivalent circle) diameter of 40-60 nm (550 nm nanoplatelets) or 60-80 nm (650 nm nanoplatelets), respectively, which are particularly useful for correcting the yellowness of coatings.Some commercial nanosheets are available with a polyvinyl pyrrolidone (PVP) coating or with a silicon dioxide (silicon oxide) coating.

[0036] This article describes an improved synthesis method for effectively synthesizing nanosheets using higher concentrations during synthesis and the product nanosheets have the desired visible absorption. Specifically, the nanosheet synthesis involves the use of significantly higher reactant concentrations that can be effectively used to produce commercial quantities of silver nanosheets. High-yield synthesis can be implemented based on the production of nanosheets with desired absorption properties. The formation of nanosheets is guided to a significant extent using multifunctional carboxylic acids. The use of C3 or larger alcohols (such as glycerol, lactate, propylene glycol, etc.) with additional alcohols or other selected functional groups provides stability, which provides effective amplification and stability of the nanosheets themselves in a single-step process. The reduction of silver ions is driven by sodium borohydride, etc. Similarly, peroxide compounds are added in a two-step gradual addition process to stabilize high-concentration synthesis. The use of alcohol-based compounds for stabilization provides surprising improvements because the multifunctional carboxylic acids have been complexed with silver ions and can coat the surface of the nanosheets. The synthesis of nanosheets inherently involves a balance of conditions and stabilizing compounds because the nanosheets themselves are not thermodynamically stable relative to the transformation to nanoparticles or other structures, and the nanostructure growth guided in the entire process and stabilization provide a larger amount of product nanosheets Synthesis.

[0037] In the synthesis of silver nanoplates, citrate has been found to be a valuable ion in solution to guide the formation of nanoplate structures. It has also been found that other polycarboxylate anions successfully guide the formation of successful nanoplates, and in addition to citrate, succinate and citramalate have also been found to be particularly effective, as described in Zhang et al., "A Systematic Study of the Synthesis of Silver Nanoplates: Is Citrate a "Magic" Reagent?" Journal of the American Chemical Society, (2011), 133: 18931-18939, which is incorporated herein by reference (hereinafter referred to as "Zhang JACS"). However, polyvinyl pyrrolidone is also used and non-citrate-based synthesis of nanoplates is achieved under applied heat, as described in Zhang et al., "Citrate-Free Synthesis of Silver Nanoplates and the Mechanistic Study", ACS Applied Materials and Interfaces, (2013), 5: 6333-6345, which is incorporated herein by reference. A scale-up procedure using a separate seed (Ag nanoparticle) formation step has been described, such as Liu et al., entitled "One-Step Growth of Triangular Silver Nanoplates with Predictable Sizes on a LargeScale", Nanoscale, (2014), 6: 4513-4516 (see Supplementary Materials), which is incorporated herein by reference in terms of Supplementary Materials. In contrast, the scale-up procedure described herein does not involve a seed particle step.

[0038] An effective method for forming a noble metal coating on silver nanosheets is described herein. In the coating method, a dispersion is formed using silver nanosheets, a capping agent, a ligand, and a mild reducing agent. A solution containing noble metal ions, a capping agent, and a complexing agent is gradually added to form a coating. Because the noble metal ion complex can be easily reduced, a mild reducing agent (e.g., ascorbic acid, oxalic acid, tartaric acid, hydroxylamine, formic acid, or a mixture thereof) effectively drives the coating process. It has been found that suitable multifunctional carboxylic acid anions (e.g., citrate) and polyvinyl pyrrolidone together effectively form the desired coated nanosheets, and a gold coating is exemplified below. It has been found that the presence of citrate or other suitable multifunctional carboxylates or combinations thereof changes the absorption spectrum of the coated nanosheets by reducing the spectral blue shift associated with the coating process, providing the nanosheets with desired features as a hue-changing polymer filler.

[0039] Gold coating of silver nanoplates is described in Gao et al., "Highly Stable Silver Nanoplates for Surface Plasmon Resonance Biosensing", Angewandte Chemie International Edition, (2012), 51: 5629-5633, which is incorporated herein by reference (hereinafter referred to as "Gao 2012"). In this article, silver nanoplates are synthesized starting from silver seeds that are subsequently used to synthesize nanoplates. In this application, an effective synthesis method that can be based on large-scale implementation that is different from the Gao method to deliver a smooth coating with an effective thickness is described.

[0040] Silver nanowires or fused metal nanostructured networks with low surface resistance have been used to form transparent conductive films with good optical clarity and low haze. However, in some embodiments, these films may be observed to have a slight yellow tint, which corresponds to a positive b* value in the CIELAB scale. It has been found that the inclusion of a small amount of nanoscale colorants such as silver nanoplatelets can improve the hue to a neutral gray and reduce b*. The parameter L* provides a range from black to white along the neutral gray scale. Although silver nanoplatelets can slightly reduce transparency and slightly increase the absolute value of a*, these adverse effects may generally be minor and within acceptable levels.

[0041] In terms of using silver nanoflakes to improve the whiteness of transmitted light through a transparent conductive film, the silver nanoflakes can be selected to have a small compensating absorption and / or scattering that complements the absorption / scattering of the conductive material. Based on CIELAB parameters, in principle, the film can be modified to obtain a desired degree of whiteness, usually based on the smaller absolute values ​​of b* and a* in the CIELAB scale. However, in terms of practical limitations, the film design can guide the result to produce whiter light within certain desired ranges (absolute values ​​of b* and a* below the target cutoff value), as achieved using the silver nanoflakes exemplified herein. As further explained below, reasonable whiteness values ​​can be obtained and the reduction in total transmission of visible light is acceptable.

[0042] Similarly, silver nanosheets may be selected to introduce a desired hue or color instead of white light. For appropriate embodiments, the inherent contribution of the conductive layer based on the transparent conductive film to the color may be considered when selecting and loading the silver nanosheets to achieve the desired color, which may be represented by the b* and a* values ​​in the CIELAB system. The selected hue may be patterned appropriately for a specific application, such as a display, etc.

[0043] In general, the metal nanosheets can be incorporated into a curable polymer matrix coating material and / or directly into a sparse metal conductive film, which can include a polymer binder (e.g., a curable polymer summarized below) and metal nanowires and an optional fusing agent. The metal nanosheets in the conductive layer may or may not be fused with the fused metal nanostructured network and incorporated therein. However, in either case, for example, the absorption properties of the metal nanosheets can still be effectively used in the conductive layer to change the hue of the film. The coating solution can be solution coated, dried, and in some embodiments cured using, for example, UV light, heat curing, other radiation curing, or other appropriate crosslinking methods. The coating thickness can be selected for a specific application.

[0044] Coating / binder polymers suitable for solution coating are commercially available or can be formulated for use. Polymers that are soluble in aqueous or non-aqueous solvents can be selected. Suitable types of radiation-curable polymers and / or thermally curable polymers are further described below. The polymer binder can crosslink itself when exposed to radiation, and / or it can be crosslinked with a photoinitiator or other crosslinking agent.

[0045] For processing, the silver nanosheets can be dispersed in a coating solution, for example, to form a coating or to form a transparent conductive layer. In some embodiments, a dispersion of nanosheets can be dispersed first and then added to a solution of other components (e.g., polymer binder, metal nanowires, other additives, etc.). The concentration of the silver nanosheets can be selected to obtain a desired loading in the final resulting layer formed from the coating solution. Based on the concentration of the coating solution, the wet coating thickness can be selected to obtain a desired dry coating thickness based on the empirical decrease in coating thickness after drying and further processing.

[0046] To form a transparent conductive layer, various sparse metal conductive layers can be formed from metal nanowires. Metal nanowires can be formed from a variety of metals, and metal nanowires are commercially available or can be synthesized. Although metal nanowires are inherently conductive, it is believed that the vast majority of resistance in metal nanowire-based films should be attributed to the contacts between nanowires. Depending on the processing conditions and the properties of the nanowires, the sheet resistance of a relatively transparent nanowire film as deposited can be very large, for example in the giga-ohm / sq range or even higher. Various methods have been proposed to reduce the resistance of nanowire films without destroying optical transparency.

[0047] Films formed using metal nanowires and treated to flatten the nanowires at the junctions to improve conductivity are described in U.S. Pat. No. 8,049,333 to Alden et al., entitled "Transparent Conductors Comprising Metal Nanowires," which is incorporated herein by reference. Structures including surface-embedded metal nanowires to increase metal conductivity are described in U.S. Pat. No. 8,748,749 to Srinivas et al., entitled "Patterned Transparent Conductors and Related Manufacturing Methods," which is incorporated herein by reference. However, it has been found that fused metal nanostructured networks have desirable properties with respect to high conductivity and desirable optical properties with respect to transparency and low haze. Fusion of adjacent metal nanowires can be performed based on a chemical process at low temperatures and commercially appropriate processing conditions.

[0048] In particular, a significant advance towards achieving conductive films based on metal nanowires has been the discovery of a sufficiently controllable process to form fused metal networks in which adjacent portions of the metal nanowires fuse. Fusion of metal nanowires with various fusion sources is further described in the following literature: published U.S. patent applications 2013 / 0341074, entitled “Metal Nanowire Networks and Transparent Conductive Material,” by Virkar et al. and 2013 / 0342221, entitled “Metal Nanostructured Networks and Transparent Conductive Material,” by Virkar et al. (the '221 application), 2014 / 0238833, entitled “Fused Metal Nanostructured Networks, Fusing Solutions with Reducing Agents and Methods for Forming Metal Networks,” by Virkar et al. (the '833 application), and published U.S. patent application 2015 / 0144380, entitled “Transparent Conductive Coatings Based on Metal Nanowires and Polymer Binders, Solution Processing Thereof, and Patterning Approaches,” by Yang et al. (the '380 application), and published U.S. patent application 2015 / 0144380, entitled “Transparent Conductive Coatings Based on Metal Nanowires and Polymer Binders, Solution Processing Thereof, and Patterning Approaches,” by Li et al. 9,183,968, all of which are incorporated herein by reference.

[0049] Transparent conductive films may typically include several components or layers that contribute to the processability and / or mechanical properties of the structure without adversely changing the optical properties. The sparse metal conductive layer may be designed to have desired optical properties when incorporated into the transparent conductive film. The sparse metal conductive layer may further include or exclude a polymer binder. Unless otherwise indicated, reference to thickness refers to the average thickness on the referenced layer or film, and adjacent layers may be intertwined at their boundaries depending on the specific material. In some embodiments, the total film structure may have a total transmittance of at least about 85% of visible light, a haze of no more than about 2%, and a sheet resistance of no more than about 250 ohms / sq, although significantly better performance is described herein.

[0050] With respect to silver nanosheets, it has been found that colorants can be added to the sparse metal conductive layer at levels effective to significantly reduce yellowness without significantly sacrificing other optical properties of the coating. For incorporation into a transparent coating for a transparent conductive film or directly into an ink for forming a sparse metal conductive layer, an appropriate amount of silver nanosheets in the overcoat and / or transparent conductive layer generally does not significantly increase the sheet resistance. In some embodiments, the sheet resistance of the film with silver nanosheets increases by no more than about 20% relative to the sheet resistance of the corresponding unloaded film, and similarly, the total transmittance of visible light in the film with silver nanosheets (expressed as a percentage) may be reduced by no more than about 5% relative to the unloaded film. The haze may not be significantly changed by the presence of silver nanosheets, and in some embodiments, the silver nanosheets may slightly reduce the haze. A reference unloaded film is produced for comparison, with the same concentration of other components in the solvent of the coating solution, and is processed in the same manner, so that the final thickness may be slightly different.

[0051] Transparent conductive films have important applications, for example, in solar cells and touch screens. Transparent conductive films formed from metal nanowire components offer the promise of lower processing costs and more suitable physical properties relative to conventional materials. In multilayer films having various structural polymer layers, the resulting film structures have been found to be robust in terms of processing while maintaining the desired conductivity, and the incorporation of the desired components as described herein can additionally provide stability without degrading the functional properties of the film, so that devices incorporating the film can have a suitable lifetime in normal use.

[0052] Nanosheet synthesis and precious metal coating

[0053] Silver nanosheets and gold-coated silver nanosheets are found to be effective colorants for transparent polymer films. In particular, gold-coated nanosheets are found to contribute to stable hue control of transparent conductive films in established accelerated wear tests. Improved methods for large-scale synthesis of silver nanosheets and coating of silver nanosheets with noble metals are described. Also, methods for depositing noble metal coatings are described that limit the blue spectral absorption shift originating from the coatings, thereby effectively providing hue adjustment to transparent films, such as nanowire-based transparent conductive films, by the noble metal-coated nanosheets. The synthesis approach is solution-based and effectively produces stable, uniform nanosheets using significantly more concentrated solutions that are more suitable for producing commercial quantities of nanosheets.

[0054] The synthesis involves an aqueous solution containing a soluble silver salt (e.g., silver nitrate). In contrast to the synthesis of silver nanowires, which typically involves medium molecular weight polymer capping agents, the use of small molecule capping agents directs nanosheet formation. In particular, it has been found that citrate salts (e.g., sodium citrate) direct the synthesis of nanosheet shapes with high specificity. The citrate anion is a cation having the formula (OOCCH2COH(COO)CH2COO)-3 tricarboxylate molecules. Based on the work of the Yin group (see Zhang JACS cited above), other polycarboxylate anions can effectively replace citrate. As found by Zhang JACS, effective compounds have 2 or 3 carboxylate groups separated by one or two carbon atoms, which can effectively guide nanosheet synthesis. Anions that effectively guide approximately 100% nanosheet yield and stabilize nanosheets include (for example) citrate, succinate and citramalate, where malonate, tartrate, isocitrate, cis-aconate and homotricarboxylate are used to obtain 80-90% nanosheet yield. These substances can be called polycarboxylate capping agents, and mixtures of polycarboxylate anions can be used.

[0055] Hydrogen peroxide is often added to further direct the formation of nanosheets. Hydrogen peroxide is a powerful oxidant that can oxidize metallic silver. After the addition of the reducing agent, there is a dynamic equilibrium established using the peroxide etchant and the reducing agent that drives the formation of silver metal. Zhang JACS hypothesizes that this equilibrium is such that the formation of silver seeds is ultimately directed as reactants are consumed for planar growth of nanosheets based at least in part on citrate or an equivalent polycarboxylate capping agent. Sodium borohydride is often used as the reducing agent, but it is speculated that other reducing agents (e.g., hydrazine, NaBH4, LiAlH4, ascorbic acid, oxalic acid, formic acid, combinations thereof, etc.) may be used instead.

[0056] To scale up the reaction by using higher concentrations, the silver nitrate concentration can be increased by 2 times or more from the small-scale synthesis, and under appropriate adjustments, silver nanosheets are obtained with high yield and high quality. Results based on an increase in reactant concentration by 100 times or more and amplification of the reactant volume are described in the examples. Several adjustments in successful synthetic scale-up include adding a multifunctional alcohol stabilizer, increasing the ratio of hydrogen peroxide to borohydride, and gradually adding hydrogen peroxide. Appropriate concentrations are presented below. Scaling up the reaction and / or increasing the reactant concentration without these changes typically results in apparent destabilization of nanoparticle synthesis and nanosheets.

[0057] It has been found that multifunctional alcohols can stabilize the resulting silver nanosheets. In addition, multifunctional alcohols can also amplify the synthesis of silver nanoparticles by increasing the concentration of silver ions. Multifunctional alcohols can be represented by the formula R1C(OH)R2R3, wherein R1 is a moiety having a hydroxyl group, an ester group, a ketone group, a heterocyclic group, an amino group, an amide group, an ether group, an aldehyde group, a carboxylic acid group, or a plurality thereof, and R2 and R3 are independently H or an alkyl moiety optionally having a hydroxyl group, an ester group, a ketone group, a heterocyclic group, an amino group, an amide group, an ether group, an aldehyde group, a carboxylic acid group, or a plurality thereof, wherein the R1, R2 and R3 moieties have carbon atoms bonded to the C(OH) group, and the designated functional groups, when present, are adjacent to the -C(OH)- moiety or separated by a methylene -CH2- moiety. Specific suitable multifunctional alcohols (having additional hydroxide or ether functionality) include, for example, glycerol (CH2(OH)CH(OH)C(OH)H2), ethyl lactate (CH3CH2OC(O)CH(OH)CH3), diacetone alcohol (CH3C(O)CH2C(OH)(CH3)2), ethylene glycol monomethyl ether (CH3OCH2CH2OH), propylene glycol monomethyl ether (CH3OCH(CH3)CH2OH), ethylene glycol, propylene glycol, diethylene glycol, polyethylene glycol, polyvinyl alcohol, and the like.

[0058] In general, the nanosheet synthesis reaction is carried out in water. The growth solution may have a silver salt concentration of about 0.00025M to about 0.1M, about 0.0005M to about 0.05M in other embodiments, and about 0.001M to about 0.025M in other embodiments. The growth solution may include a polycarboxylate anion of about 0.0003M to about 0.005M and about 0.0006M to about 0.0035M in other embodiments. For polyfunctional alcohols, the growth solution may include about 0.0002M to about 0.0025M and about 0.00035M to about 0.002M in other embodiments. For redox components, the growth solution may include about 0.05M to about 1M hydrogen peroxide, about 0.00005M to about 0.0002M reducing agent, and about 0.075M to about 0.8M hydrogen peroxide and about 0.0001M to about 0.001M reducing agent in other embodiments. For larger scale reactions, the molar ratio of hydrogen peroxide to reducing agent, particularly a borohydride reducing agent, may be from about 10 to about 120, in other embodiments from about 15 to about 100, and in other embodiments from about 20 to about 80. One skilled in the art will recognize that other ranges of reactant concentrations that fall within the explicit ranges above are contemplated and within the present invention.

[0059] To implement the synthesis reaction, the reactants are added to water under good mixing conditions, wherein the first portion of peroxide is added penultimately while retaining the reducing agent. Once the other reactants are mixed, the reducing agent is quickly injected into the mixed growth solution. Then the reaction continues for an appropriate period of time to form nanosheets. In a more concentrated amplified synthesis, the second portion of hydrogen peroxide is gradually added after the addition of the reducing agent. The ratio of the second amount of hydrogen peroxide to the first amount of hydrogen peroxide is at least about 0.5, at least about 0.75 in other embodiments, and about 1 to about 10 in other embodiments. The second amount of peroxide is added over the following time period: about 1 minute to about 2 hours, about 2 minutes to about 1.5hr in other embodiments, and about 3 minutes to about 1hr in other embodiments. After completing the addition of the second amount of peroxide, the reaction continues for at least two minutes, at least about 5 minutes in other embodiments, and about 8 minutes to about 3 hours in other embodiments. Those skilled in the art will recognize that the present invention encompasses other ranges of reaction times and reactant addition times within the above-mentioned clear ranges and is within the present invention. Nanosheets can be harvested from the solution and can be resuspended. However, for noble metal electroplating processes, the nanosheets can continue to be used in the growing (ie, synthesizing) coating solution, which saves the separation step and also avoids the loss of nanosheets during harvesting (eg, due to nanosheet instability).

[0060] Synthetic silver nanosheets are formed without polymer coatings or other inorganic coatings. The nanosheets may have an equivalent circular diameter (obtained by averaging a line segment extending from the edge through the mathematical center of the nanosheet) of about 20 nm to about 150 nm, in other embodiments about 25 nm to about 120 nm, and in other embodiments about 25 nm to about 90 nm. Likewise, the synthetic silver nanosheets may have a peak absorption wavelength of about 450 nm to about 850 nm, and in other embodiments about 500 nm to about 750 nm. For some applications, it may be desirable that the normalized absorption at 600 nm be at least about 0.6, in other embodiments at least about 0.65, and in other embodiments at least about 0.7. Those skilled in the art will recognize that the present invention encompasses other property ranges that fall within the above explicit ranges and are within the present invention.

[0061] In some embodiments, a noble metal coating may be applied to the silver nanosheets. The silver nanosheets may be synthesized using the above process, or other techniques may be used to synthesize silver nanosheets for coating and may be obtained from commercial sources if desired. In any case, a relatively mild organic reducing agent may be used to uniformly apply a gold coating. The coating process is usually carried out using a polymer capping agent to promote coating deposition. A ligand may be included in the reaction solution to adjust the coating process. It has been found that the inclusion of a polycarboxylate further promotes the formation of coated nanosheets having desired optical properties. Although the experiments herein are carried out using citrate, it is expected that polycarboxylate anions suitable for promoting nanosheet synthesis are also effective in providing the desired effect on the coating process, and suitable polycarboxylate anions include, for example, citrate, succinate, citramalate, malonate, tartrate, isocitrate, cis-aconate, tricarballylate, mixtures thereof, and other dicarboxylic acids and tricarboxylic acids having 1 or 2 carbon atoms spaced apart from the carboxylic acid functional group.

[0062] For coating reactions, the coating solution is typically added gradually to the reaction solution. The reaction solution comprises about 0.00025 wt% to about 0.1 wt% silver nanosheets, about 0.0005 wt% to about 0.05 wt% silver nanosheets in other embodiments, and about 0.001 wt% to about 0.025 wt% silver nanosheets in other embodiments. For end-capping polymers, the reaction solution may comprise about 0.005 wt% to about 5 wt%, about 0.0075 wt% to about 3 wt% in other embodiments, and about 0.01 wt% to about 2 wt% in other embodiments. Suitable end-capping polymers include, for example, PVP, polyvinyl alcohol, polyacrylic acid, combinations thereof, and the like. The reaction solution may include about 0.005 M to about 2 M multidentate ligands, about 0.004 M to about 1.5 M multidentate ligands in other embodiments, and about 0.005 M to about 1 M multidentate ligands in other embodiments. In general, suitable ligands include, for example, nitrite, diethylamine, ethylenediamine, nitrilotriacetic acid, iminobis(methylenephosphonic acid), aminotris(methylenephosphonic acid), ethylenediaminetetraacetic acid (EDTA), 1,3-propylenediaminetetraacetic acid (1,3-PDTA), triethylenetetramine, tris(2-aminoethyl)amine, diethylenetriaminepentaacetic acid, 1,2-cyclohexanediaminotetraacetic acid, iminodiacetic acid, methyliminodiacetic acid, N-(2-acetamido)iminoacetic acid, N-(2-carboxyethyl)iminodiacetic acid, N-(2-carboxymethyl)iminodipropionic acid, picolinic acid, picolinic acid, histidine, and combinations thereof. With respect to the reducing agent, the reaction solution may include from about 0.001 M to about 0.1 M reducing agent, in other embodiments from about 0.002 M to about 0.08 M reducing agent, and in other embodiments from about 0.0025 M to about 0.05 M reducing agent. Likewise, the reaction solution may include from about 0.0005M to about 0.2M polycarboxylate, in other embodiments from about 0.00075M to about 0.05M polycarboxylate anion, and in other embodiments from about 0.001M to about 0.025M polycarboxylate anion. One skilled in the art will recognize that other ranges of reaction solution compositions that fall within the explicit ranges above are contemplated and are within the present invention.

[0063] Silver nanosheets in the solution used to synthesize the nanosheets can be used and coated directly without purification and in some embodiments without dilution. The exact composition of the solution containing the product nanosheets may be unknown, but can be reasonably inferred based on the composition added for synthesis. In either case, the silver nanosheet solution used for coating can be characterized based on the total silver concentration in any form, which can be determined based on the silver added to the reaction solution to form the silver nanosheets. In some embodiments, the solution may include at least about 0.00075M, at least about 0.00085M in other embodiments, at least about 0.001M in other embodiments, and at least about 0.0011M in other embodiments. Those skilled in the art will recognize that the present invention encompasses other ranges of total silver concentrations within the above-defined ranges and they are within the present invention.

[0064] The coating solution may include complexed gold ions at a concentration of about 0.0002M to about 0.02M, in other embodiments about 0.0003M to about 0.01M, and in other embodiments about 0.0004M to about 0.0075M. For the capped polymer, the coating solution may include about 0.05wt% to about 5wt%, in other embodiments about 0.075wt% to about 3wt%, and in other embodiments about 0.1wt% to about 2wt%. The coating solution includes a ligand to complex with the gold ions, thereby reducing the effective reduction potential of the Au salt. This is illustrated by the Gao 2012 article cited above. Gao 2012 and the examples below use iodide ions (I-) as the selected ligand to reduce the reduction potential. However, other ligands may also be effectively used in this role, including (for example) Br - , sulfite, CN - 、SCN - , thiosulfate (S2O3 -2 ), mixtures thereof, and the like. The molar ratio of ligand to gold ion or other precious metal ion may be greater than 1 and in other embodiments greater than 1.5. Those skilled in the art will recognize that the present invention encompasses other ranges of coating solution compositions that fall within the above-defined ranges and are within the present invention. Those skilled in the art will recognize that the present invention encompasses other composition ranges of coating solutions that fall within the above-defined ranges and are within the present invention.

[0065] For the coating process, first, the components of the reaction solution are fully mixed. The coating solution is gradually added to the reaction solution. Typically, the coating solution is added over a period of about 2 minutes to about 5 hours, about 5 minutes to about 4 hours in other embodiments, and about 7 minutes to about 3 hours in other embodiments. The amount of time for adding the coating solution can be adjusted to a certain extent based on the amount of the coating solution added, and the amount of the coating solution added generally determines the amount of the deposited coating. The coating solution is generally added at a rate suitable for achieving the above-mentioned target time, and can be added in reasonable increments to obtain good dilution diffusion in a certain period of time. The amount of the deposited gold coating affects the chemical stability of the resulting coated nanosheets and the corresponding devices formed from the coated nanosheets. The amount and concentration of the added coating solution determine the amount of the deposited coating. In some embodiments, the gold-coated silver nanosheets include about 2 atomic % to about 45 atomic % gold, and about 5 atomic % to about 40 atomic % gold in other embodiments, and about 7.5 atomic % to about 35 atomic % gold in other embodiments. Those skilled in the art should recognize that the present invention encompasses other ranges of process time and coating amount within the above-mentioned clear range and it is within the present invention.

[0066] The absorption of silver nanosheets to visible light and adjacent parts of the electromagnetic spectrum is characterized by plasmon resonance. A deposited gold coating may not change the basic characteristics of the absorption spectrum, but a quantitative change is generally produced. The plasmon resonance of the nanosheet shifts the absorption spectrum toward the red portion of the spectrum. It has been observed that a gold coating shifts the spectrum back to the blue end of the spectrum. However, it has been found that the use of polycarboxylate anions during the coating process reduces the blue shift of the absorption after coating, so that thicker coatings can be applied without blue shifting the absorption spectrum more than desired.

[0067] Nanosheets can be characterized by size and absorption spectrum. The diameter can be measured in the plane of the structure as the average line length through the center of the nanosheet. In general, the nanosheet may have an average diameter of no more than 200nm, no more than about 170nm in other embodiments, about 20nm to about 150nm in other embodiments, and about 25nm to about 120nm in other embodiments. The absorption spectrum can be characterized in several ways. The silver nanosheets of particular interest typically have an electromagnetic absorption peak in the visible portion of the spectrum at a wavelength of about 500nm to about 725nm and about 520nm to about 700nm in other embodiments. When referring to the value of the normalized absorption spectrum with the visible absorption peak set to 1, the relative absorption at 600nm can be considered. In some embodiments, the normalized absorption at 600nm may be at least about 0.6, at least about 0.65 in other embodiments, and at least about 0.7 in other embodiments. Those skilled in the art will recognize that the present invention encompasses other ranges of nanosheet sizes and absorption properties within the above-mentioned clear ranges and they are within the present invention.

[0068] As described above, silver nanosheets can be unstable in terms of reconstitution to other silver materials (e.g., nanoparticles). Using the synthetic methods described herein, relatively stable nanosheets can be formed. In the absence of a noble metal coating, the product nanosheets can be stable in a dispersion without a polymer coating or a ceramic coating at room temperature and ambient atmosphere in dark storage for at least about 2 weeks, in other embodiments at least about 3 weeks, and in other embodiments at least about 4 weeks or longer. The application of a noble metal coating greatly stabilizes the silver nanosheets relative to various conditions (including temperature changes), as shown in the examples.

[0069] Clear coatings and films

[0070] A transparent coating having a silver nanosheet loaded polymer as described herein can generally be applied to a transparent substrate for incorporation into a desired structure. The general structure is described, and specific applications for transparent conductive films can be found in the following section. In general, a precursor solution for a transparent filler coating can be deposited on a transparent substrate using an appropriate coating method to form a transparent structure. In some embodiments, the transparent substrate can be a film for incorporation into a final device or alternatively or additionally an integral optical component (e.g., a light emitting device or a light receiving device). The discussion in this section focuses on simple passive transparent substrates, and other structures are discussed in subsequent sections.

[0071] In general, any reasonable transparent substrate may be suitable. Therefore, suitable substrates may be formed, for example, from inorganic glass (e.g., silicate glass), transparent polymer films, inorganic crystals, etc. In some embodiments, the substrate is a polymer film. Suitable polymers for substrates include, for example, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyacrylates, poly(methyl methacrylate), polyolefins, polyvinyl chloride, fluoropolymers, polyamides, polyimides, polysulfones, polysiloxanes, polyetheretherketones, polybornene, polyesters, polystyrene, polyurethanes, polyvinyl alcohol, polyvinyl acetate, acrylonitrile-butadiene-styrene copolymers, cyclic olefin polymers, cyclic olefin copolymers, polycarbonates, copolymers thereof, or blends thereof, etc. In some embodiments, the polymer film may have a thickness of about 5 microns to about 5 mm, about 10 microns to about 2 mm in other embodiments, and about 15 microns to about 1 mm in other embodiments. Those skilled in the art will recognize that the present invention encompasses other thickness ranges within the above-mentioned clear ranges and is within the present invention. The substrate may include a plurality of layers differing in composition and / or other properties. Some commercial transparent sheets may include coatings, such as hard abrasion resistant coatings.

[0072] The transparent coating (e.g., with silver nanosheet filler) may typically have a thickness of no more than about 100 microns, in other embodiments from about 15 nanometers (nm) to about 50 microns, and in other embodiments from about 50 nm to about 20 microns. The coating properties on the transparent conductive layer are described below. The transparent hue adjustment coating may include from about 0.001 weight percent (wt%) to about 10 wt% silver nanosheets, in other embodiments from about 0.005 wt% to about 6 wt% silver nanosheets, in other embodiments from about 0.01 wt% to about 5 wt% silver nanosheets, and in other embodiments from about 0.02 wt% to about 2.5 wt% silver nanosheets. The transparent coating may further include a polymer binder, optional property modifiers, such as crosslinkers, wetting agents, viscosity modifiers, and / or stabilizers for transparent conductive films, and an optional sparse metal conductive layer. Those skilled in the art will recognize that the present invention encompasses other ranges of thickness and nanosheet concentration in the loaded polymer that fall within the above explicit ranges and are within the present invention.

[0073] The nanoscale nature of the silver nanosheets can provide good distribution throughout the polymer matrix, thereby maintaining the desired degree of transparency for a given color contribution. Generally, as used herein, nanoscale refers to the average value (size cutoff) of at least one dimension of the particles not exceeding about 100 nm, in other embodiments not exceeding about 75 nm and in other embodiments not exceeding about 50 nm. Therefore, suitable nanosheets have an average thickness not exceeding the size cutoff, and the other two average dimensions are at least 10 times greater than the average thickness, and the other dimensions are roughly along the major axis of the particles. Metal nanosheets can provide adjusted color contributions based on size via assumed surface plasmon resonance, although the applicant does not wish to be limited by theory. Silver nanosheets with polyvinyl pyrrolidone coatings or silicon oxide (silicon dioxide) coatings can be commercially available. According to the examples below, data on gold-coated silver nanoparticles synthesized using the techniques described herein are presented. Due to the inertness of gold and other precious metals, precious metal-coated silver nanosheets can be stable with respect to corrosion and other environmental impacts.

[0074] A transparent loading coating can be formed by coating the precursor solution using an appropriate coating method. Silver nanosheets can be incorporated into a selected suitable solvent to deposit a coating with appropriate compatibility. Suitable solvents generally include, for example, water, alcohols, ketones, esters, ethers (e.g., glycol ethers), aromatic compounds, alkanes, etc. and mixtures thereof. Specific solvents include, for example, water, ethanol, isopropanol, isobutanol, tert-butanol, methyl ethyl ketone, glycol ether, methyl isobutyl ketone, toluene, hexane, ethyl acetate, butyl acetate, ethyl lactate, PGMEA (2-methoxy-1-methylethyl acetate), N,N-dimethylformamide, N,N-dimethylacetamide, acetonitrile, formic acid, dimethyl carbonate, or mixtures thereof.

[0075] In general, polymers (usually crosslinkable polymers) used for coatings can be supplied in the form of commercial coating compositions or formulated using selected polymer compositions with the addition of nanoscale colorants and / or other additives. Following common practice, in the context of adhesives, the term polymer refers to oligomers, which can be derivatized to introduce other functionalities. Crosslinking agents and other adhesive precursor components can be multifunctional (e.g., three or more functional groups) and are used to form highly crosslinked polymer products under appropriate crosslinking conditions, which can be considered as functionalized monomers or functionalized oligomers depending on the specific structure. Suitable polymers for coatings may include, for example, radiation-curable polymers and / or thermally curable polymers. Suitable classes of radiation-curable polymers and / or heat-curable polymers include, for example, polysiloxanes, polysilsesquioxanes, polyurethanes, acrylic resins, acrylic copolymers, cellulose ethers and esters, nitrocellulose, other structured polysaccharides, polyethers, polyesters, polystyrenes, polyimides, fluoropolymers, styrene-acrylate copolymers, styrene-butadiene copolymers, acrylonitrile butadiene styrene copolymers, polysulfides, epoxy-containing polymers, copolymers thereof, and mixtures thereof. Suitable commercial coating compositions include, for example, those from Hybrid Plastics, Inc. (Mississippi, USA). Coatings' coating solutions, from California Hardcoating Company (CA, USA), silica-filled siloxane coatings from Dexerials Corporation (Japan), CrystalCoat UV curable coatings from SDC Technologies, Inc. (CA, USA). Hard coatings with some desirable properties are described in co-pending U.S. patent application Ser. No. 14 / 741,119 to Gu et al., entitled "Transparent Polymer Hardcoats and Corresponding Transparent Films" (incorporated herein by reference). In some embodiments, the crosslinkable adhesive precursor composition may include non-volatile relatively high molecular weight monomers (with or without oligomers) in the formulation or include lower molecular weight polymers in addition to the monomers. In general, non-volatile polymerizable compounds (which may be monomers, oligomers, or lower molecular weight polymers) may be referred to as non-volatile polymer adhesive precursor compounds.

[0076] The polymer concentration and correspondingly the concentration of other non-volatile agents can be selected to achieve the desired rheology of the coating solution, such as the appropriate viscosity for the selected coating process. Solvents can be added or removed to adjust the total non-volatile concentration, which is different from volatile solvents. The relative amount of non-volatiles can be selected to adjust the composition of the final coating composition, and the total solids can be adjusted to achieve the desired thickness of the dried coating. Typically, the coating solution may have a non-volatile component concentration of about 0.1 wt% to about 80 wt%, about 0.5 wt% to about 60 wt% in other embodiments, and about 0.75 wt% to about 55 wt% in other embodiments. Those skilled in the art will recognize that the present invention encompasses other ranges of polymer concentrations within the above-mentioned specific ranges and they are within the present invention.

[0077] Silver nanosheets may be incorporated into a coating solution for forming a coating. The coating precursor solution may include about 0.0001 wt % to about 2 wt % silver nanosheets, in other embodiments about 0.00025 wt % to about 0.2 wt % silver nanosheets, and in other embodiments about 0.0005 wt % to about 0.02 wt % silver nanosheets. One skilled in the art will recognize that the present invention encompasses other ranges of silver nanosheets in the coating solution that fall within the above explicit ranges and are within the present invention. Other additives (e.g., crosslinking agents, wetting agents, viscosity modifiers, dispersing aids, stabilizers, etc.) may be added as desired, and suitable compositions are described below.

[0078] In some embodiments, a transparent coating with polymer nanosheets may reduce the total transmittance of visible light by no more than about 5 percentage points, in other embodiments no more than about 3 percentage points, and in other embodiments no more than about 1.5 percentage points relative to a corresponding coating without silver nanosheets. Similarly, in some embodiments, a transparent coating with silver nanosheets may increase the haze by no more than about 1.5 percentage points, in other embodiments no more than about 1 percentage point, and in other embodiments no more than about 0.6 percentage points relative to a corresponding unloaded coating. Those skilled in the art will recognize that other ranges of changes in optical properties resulting from loaded polymer coatings that fall within the above explicit ranges are encompassed by the present invention and are within the present invention. The corresponding unloaded coating has the same concentration of components other than the lack of silver nanosheets in the solvent and is processed in the same manner so that the final thickness of the coating may be slightly different from that of the corresponding coating.

[0079] To deposit the coating precursor solution, any reasonable deposition means may be used, such as dip coating, spray coating, knife edge coating, rod coating, Meyer-rod coating, slot die coating, gravure printing, inkjet printing, screen printing, spin coating, etc. The deposition means determines the amount of liquid deposited, and the concentration of the solution may be adjusted to provide the desired thickness of the product coating on the surface. After the dispersion is used to form a coating, the coating may be dried to remove the liquid and appropriately crosslinked.

[0080] Transparent conductive film

[0081] Transparent conductive structures or films typically include a sparse metal conductive layer that provides conductivity without significantly adversely changing optical properties and various other layers that provide mechanical support and protection of conductive elements. A polymer overcoat may be placed on the sparse metal conductive layer. Nanoscale colorants as described herein may be placed in an overcoat, an undercoat, and / or directly in the sparse metal conductive layer. In other embodiments, the conductive layer may include a conductive metal oxide in the form of a film or particulate. Nanoscale colorants may be selected to reduce the b* value of the transparent film, which typically improves the observed whiteness or provides a desired hue to the film.

[0082] In some embodiments, a transparent conductive element (e.g., a film) may include a sparse metal conductive layer. The conductive layer is typically sparse to provide a desired amount of optical transparency, so the coverage of the metal has very significant voids within the layer of the conductive element. For example, a transparent conductive film may include metal nanowires deposited along a layer that may provide sufficient contact for electron percolation to provide a suitable conductive path. In other embodiments, the transparent conductive film may include a fused metal nanostructured network, which has been found to exhibit desired electrical and optical properties. In general, nanowires may be formed from a variety of metals, such as silver, gold, indium, tin, iron, cobalt, platinum, palladium, nickel, cobalt, titanium, copper, and alloys thereof, which may be desirable due to high conductivity. Commercial metal nanowires can be purchased from Sigma-Aldrich (Missouri, USA), Cangzhou Nano-Channel Material Co., Ltd. (China), Blue Nano (North Carolina, USA), EMFUTUR (Spain), Seashell Technologies (California, USA), C3Nano-Aiden (Korea), nanoComposix (USA), Nanopyxis (Korea), K&B (Korea), ACS Materials (China), KeChuang Advanced Materials (China), and Nanotrons (USA). Alternatively, silver nanowires can also be synthesized using a variety of known synthetic pathways or variations thereof.

[0083] For suitable embodiments, a sparse metal conductive layer may be formed on a substrate having one or more layers in the structure of the substrate. The substrate may generally be identified as a self-supporting film or sheet structure. A thin solution-treated layer (referred to as a primer) may optionally be placed along the top surface of the substrate film and directly below the sparse metal conductive layer. Likewise, the sparse metal conductive layer may be coated with one or more other layers that provide some protection on the side opposite the sparse metal conductive layer to the substrate. In general, the conductive structure may be placed in any orientation in the final product, that is, with the substrate facing outward or the substrate against the surface of the product supporting the conductive structure. In some embodiments, multiple coatings (e.g., primers and / or topcoats) may be applied, and each layer may or may not have a selected nanoscale colorant.

[0084] Reference Figure 1, a representative transparent conductive film 100 includes a substrate 102, a primer layer 104, a sparse metal conductive layer 106, an outer coating layer 108, an optically transparent adhesive layer 110, and a protective surface layer 112, but not all embodiments include all layers. The transparent conductive film generally includes a sparse metal conductive layer and at least one layer on each side of the sparse metal conductive layer. The total thickness of the transparent conductive film may generally have a thickness of 10 microns to about 3 millimeters (mm), about 15 microns to about 2.5 mm in other embodiments, and about 25 microns to about 1.5 mm in other embodiments. Those skilled in the art will recognize that the present invention encompasses other thickness ranges within the above-mentioned clear ranges and they are within the present invention. In some embodiments, the length and width of the film produced as is may be selected to be suitable for a specific application, so that the film may be directly introduced for further processing into a product. In other or alternative embodiments, the width of the film may be selected for a specific application, and the length of the film may be longer, and it is expected that the film may be cut to a desired length for use. For example, the film may be in the form of a long sheet or roll. Similarly, in some embodiments, the film may be on a roll or in another large standard format and elements of the film may be cut according to the desired length and width for use.

[0085] The substrate 102 typically includes a durable support layer formed from one or more suitable polymers. In some embodiments, the substrate may have a thickness of about 10 microns to about 1.5 mm, about 15 microns to about 1.25 mm in other embodiments, and about 25 microns to about 1 mm in other embodiments. Those skilled in the art will recognize that the present invention encompasses other substrate thickness ranges within the above-mentioned clear range and that they are in the present invention. Suitable optically transparent polymers with very good transparency, low haze, and good protection can be used for the substrate. Suitable polymers include, for example, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyacrylates, poly(methyl methacrylate), polyolefins, polyvinyl chloride, fluoropolymers, polyamides, polyimides, polysulfones, polysiloxanes, polyetheretherketones, polynorbornenes, polyesters, polystyrene, polyurethanes, polyvinyl alcohol, polyvinyl acetate, acrylonitrile-butadiene-styrene copolymers, cyclic olefin polymers, cyclic olefin copolymers, polycarbonates, copolymers thereof, or blends thereof, etc. Suitable commercial polycarbonate substrates include, for example, MAKROFOL SR243 1-1 CG, available from Bayer Material Science; Plastics, available from TAP Plastics; and LEXAN TM 8010CDE, available from SABIC Innovative Plastics. The protective surface layer 112 can independently have a thickness and composition covering the same thickness ranges and composition ranges as the substrate as described above in this paragraph.

[0086] The optional primer layer 104 and / or the optional overcoat layer 108 independently selected for inclusion may be placed below or above the sparse metal conductive layer 106, respectively. The optional coatings 104, 108 may include a curable polymer, such as a heat curable or radiation curable polymer. Suitable polymers for coatings 104, 108 are described below as binders for inclusion in metal nanowire inks, and the list of polymers, corresponding crosslinkers, and additives are equally applicable to optional coatings 104, 108, and are not explicitly repeated here. Coatings 104, 108 may have a thickness of about 25nm to about 2 microns, about 40nm to about 1.5 microns in other embodiments, and about 50nm to about 1 micron in other embodiments. Those skilled in the art will recognize that the present invention encompasses other overcoat thickness ranges within the above explicit ranges and they are in the present invention. Generally, the thinness of the overcoat 108 allows for conductivity in the overcoat 108 so that electrical connection can be made with the sparse metallic conductive layer 106, but in some embodiments the overcoat may include sub-layers where conductivity is provided in some but not necessarily all sub-layers.

[0087] Optional optically clear adhesive layer 110 can have a thickness of about 10 microns to about 300 microns, about 15 microns to about 250 microns in other embodiments, and about 20 microns to about 200 microns in other embodiments. Those skilled in the art will recognize that the present invention encompasses other optically clear adhesive layer thickness ranges within the above-mentioned clear scope and it is in the present invention. Suitable optically clear adhesive can be a contact adhesive. Optically clear adhesives include, for example, coating compositions and adhesive tapes. UV curable liquid optically clear adhesives are obtained based on acrylic acid or polysiloxane chemicals. Suitable adhesive tapes are commercially available, for example, from Lintec Corporation (MO series); Saint Gobain Performance Plastics (DF713 series); Nitto Americas (Nitto Denko) (LUCIACS CS9621T and LUCIAS CS9622T); DIC Corporation (DAITAC LT series OCA, DAITAC WS series OCA, and DAITAC ZB series); PANAC Plastic Film Company (PANACLEAN series); Minnesota Mining and Manufacturing (3M, Minnesota USA - product numbers 8146, 8171, 8172, 8173 and similar products) and Adhesive Research (e.g., product 8932).

[0088] The amount of nanowires delivered to the substrate for the sparse metal conductive layer 106 may involve a balance of factors to obtain the desired amount of transparency and conductivity. Although in principle a scanning electron microscope can be used to assess the thickness of the nanowire network, the network may be relatively sparse to provide optical transparency, which can complicate the measurement. In general, a sparse metal conductive structure (e.g., a fused metal nanowire network) may have an average thickness of no more than about 5 microns, no more than about 2 microns in other embodiments, and about 10 nm to about 500 nm in other embodiments. However, a sparse metal conductive structure is typically a relatively open structure with a significant surface texture at the submicron level. The loading of nanowires can provide useful network parameters that can be easily evaluated, and the loading value provides an alternative parameter related to thickness. Therefore, as used herein, the nanowire loading on a substrate is generally expressed as milligrams of nanowires for one square meter of substrate. In general, whether fused or not, a metal conductive network may have an average thickness of about 0.1 milligrams (mg) / m 2 About 300 mg / m 2 In other embodiments, about 0.5 mg / m 2 About 200 mg / m 2 and in other embodiments about 1 mg / m 2 About 150 mg / m 2 The transparent conductive layer may include about 0.05 wt % to about 70 wt % metal in the conductive network, about 0.075 wt % to about 60 wt % metal in other embodiments, and about 0.1 wt % to about 50 wt % metal in other embodiments. Those skilled in the art will recognize that the present invention encompasses other ranges of thickness, metal loading and concentration that fall within the above-specified ranges and are within the present invention. If the sparse metal conductive layer is patterned, the discussion of thickness and loading applies only to areas where the patterning process does not exclude or significantly reduce the metal. In addition to the polymer binder, the sparse metal conductive layer may include silver nanosheets and other processing aids. The concentration ranges of silver nanosheets loaded in the transparent polymer layer described above are generally also applicable to the sparse metal conductive layer. In other words, the weight ratio of metal nanowires to silver nanosheets used to form sparse metal conductive elements may be about 250:1 to about 5:1 and about 100:1 to about 10:1 in other embodiments. It is possible that in related embodiments, the silver nanosheets incorporated into the sparse metal conductive layer may or may not be fused or partially fused into a fused metal nanostructured network, but unless explicitly stated, references to silver nanosheets in a layer having a fused metal nanostructured network generally refer to structures regardless of whether the silver nanosheets are fused into a network. No significant changes in conductivity or color are expected to be observed after the introduction of metal nanosheets into the sparse metal conductive layer. Accordingly, references to silver nanosheets as nanoscale colorants do not refer to metal nanowires incorporated into a fused metal nanostructured network.

[0089] Typically, within the above-mentioned total thickness of a particular component of the transparent conductive film 100, the layers 102, 104, 106, 108, 110, 112 can be subdivided into, for example, sublayers having different compositions from other sublayers. For example, the outer coating may include sublayers having different property enhancement components. Thus, a more complex stack can be formed. The treatment of the sublayers may be similar or different from other sublayers within a particular layer, for example, one sublayer may be laminated while another sublayer may be coated and cured. For example, a nanoscale colorant may be supplied to the coating and property enhancement nanoparticles (e.g., nanodiamonds) may be supplied to another layer on this layer to provide protective hardness. Polymer coatings with property enhancement nanoparticles (e.g., nanodiamonds) are described in the co-pending published U.S. patent application 2016 / 0096967 (incorporated herein by reference) entitled "Property Enhancing Fillers for Transparent Coatings and Transparent Conductive Films" by Virkar et al.

[0090] For some applications, it is desirable to pattern the conductive portions of the film to introduce desired functionality, such as different areas of a touch sensor. Patterning can be performed by printing metal nanowires at selected locations to vary the metal loading on the substrate surface and effectively lacking metal at other locations, or etching or otherwise ablating the metal at selected locations before and / or after fusing the nanowires (if the nanowires are fused in a particular embodiment). For appropriate embodiments, it has been found that a high contrast in conductivity can be achieved between fused and unfused portions of a layer having substantially equal metal loadings, such that patterning can be performed by selectively fusing the metal nanowires. This ability to pattern based on fusion provides significant additional patterning options based on selective fusion of nanowires, for example, via selective delivery of a fusion solution or vapor. Patterning based on selective fusion of metal nanowires is described in the '833 application and the '380 application above.

[0091] As an illustrative example, the fused metal nanostructured network may form a conductive pattern along the substrate surface 120 having a plurality of conductive paths 122, 124, and 126 surrounded by resistive regions 128, 130, 132, and 134, as shown in FIG. Figure 2 As shown in Figure 2 As shown in FIG. 1 , the fused region corresponds to three different conductive regions, which correspond to conductive paths 122, 124, and 126. Figure 2In the diagram, three independently connected conductive regions are illustrated, but it should be understood that patterns with 2, 4, or more than 4 conductive independent conductive paths or regions can be formed as desired. For many commercial applications, a large number of elements can be used to form quite complex patterns. In particular, using available patterning techniques suitable for patterning of the films described herein, very fine patterns with highly resolved (resovled) features can be formed. Similarly, the shape of a particular conductive region can be selected as desired.

[0092] Transparent conductive films are typically built around sparse metal conductive elements that are deposited to form the functional features of the film. Individual layers are coated, laminated, or otherwise added to the structure using appropriate film processing methods. Deposition of sparse metal conductive layers is further described below in the context of fused metal nanostructured layers, but unfused metal nanowire coatings can be deposited similarly, except that the fused component is absent.

[0093] Typically, the sparse metallic conductive layer is solution coated on the substrate, which may or may not have a coating on top of the substrate that then forms an undercoat adjacent to the sparse metallic conductive layer. In some embodiments, the overcoat may be solution coated onto the sparse metallic conductive layer. Crosslinking may be performed under application of UV light, heat, or other radiation to crosslink the polymer binder in the coating and / or sparse metallic conductive layer, which may be performed in one step or in multiple steps.

[0094] Sparse metal conductive layer

[0095] Sparse metal conductive layers are typically formed from metal nanowires. Using sufficient loading and selected nanowire properties, reasonable conductivity can be obtained using nanowires with corresponding appropriate optical properties. It is expected that the stabilized film structures described herein can produce the desired performance for films with various sparse metal conductive structures. However, particularly desirable properties have been obtained using fused metal nanostructured networks.

[0096] As summarized above, several practical methods have been developed to accomplish metal nanowire fusing. Metal loading can be balanced to obtain a desired degree of conductivity and good optical properties. In general, metal nanowire processing can be accomplished by depositing two inks, wherein the first ink comprises metal nanowires and the second ink comprises a fusing composition, or by depositing an ink that combines the fusing composition into a metal nanowire dispersion. The ink may or may not further comprise other processing aids, binders, etc. An appropriate patterning method can be selected to suit a particular ink system.

[0097] In general, one or more solutions or inks for forming metal nanostructured networks may collectively include well-dispersed metal nanowires, a fusing agent, and optional other components, such as a polymer binder, a crosslinking agent, a wetting agent (e.g., a surfactant), a thickener, a dispersant, other optional additives, or a combination thereof. The solvent used for the metal nanowire ink and / or the fusing solution (if different from the nanowire ink) may include an aqueous solvent, an organic solvent, or a mixture thereof. In particular, suitable solvents include, for example, water, alcohols, ketones, esters, ethers (e.g., glycol ethers), aromatic compounds, alkanes, and the like, and mixtures thereof. Specific solvents include, for example, water, ethanol, isopropanol, isobutanol, tert-butanol, methyl ethyl ketone, glycol ethers, methyl isobutyl ketone, toluene, hexane, ethyl acetate, butyl acetate, ethyl lactate, PGMEA (acetic acid 2-methoxy-1-methylethyl ester), dimethyl carbonate, or a mixture thereof. Although the solvent should be selected based on the ability to form a good dispersion of metal nanowires, the solvent should also be compatible with other selected additives so that the additives are soluble in the solvent. For embodiments where a fusing agent is included in a single solution with metal nanowires, the solvent or a component thereof may or may not be a significant component of the fusing solution (eg, an alcohol) and may be selected accordingly as desired.

[0098] The metal nanowire ink in one ink or two ink configurations may include about 0.01 wt % to about 1 wt % metal nanowires, in other embodiments about 0.02 wt % to about 0.75 wt % metal nanowires, and in other embodiments about 0.04 wt % to about 0.5 wt % metal nanowires. One skilled in the art will recognize that other concentration ranges of metal nanowires that fall within the explicit ranges above are contemplated and are within the present invention. The concentration of the metal nanowires affects the loading of the metal on the substrate surface as well as the physical properties of the ink.

[0099] In general, nanowires can be formed from a variety of metals, such as silver, gold, indium, tin, iron, cobalt, platinum, palladium, nickel, cobalt, titanium, copper and alloys thereof, which may be desirable due to high electrical conductivity. Commercial metal nanowires are available from Sigma-Aldrich (Missouri, USA), Cangzhou Nano-Channel Material Co., Ltd. (China), Blue Nano (North Carolina, USA), EMFUTUR (Spain), Seashell Technologies (California, USA), Aiden (Korea), nanoComposix (USA), Nanopyxis (Korea), K&B (Korea), ACS Materials (China), KeChuang Advanced Materials (China) and Nanotrons (USA). Silver in particular provides excellent electrical conductivity, and commercial silver nanowires are available. Alternatively, silver nanowires may also be synthesized using a variety of known synthetic pathways or variations thereof. In order to have good transparency and low haze, it is desirable that the nanowires have a range of small diameters. In particular, it is desirable that the average diameter of the metal nanowires is no more than about 250 nm, in other embodiments no more than about 150 nm, and in other embodiments about 10 nm to about 120 nm. In terms of average length, it is expected that nanowires with greater lengths provide better conductivity within the network. In general, the average length of the metal nanowires may be at least 1 micron, in other embodiments at least 2.5 microns, and in other embodiments about 5 microns to about 100 microns, but improved synthesis techniques developed in the future may make longer nanowires possible. The aspect ratio may be specified as the ratio of the average length divided by the average diameter, and in some embodiments, the aspect ratio of the nanowires may be at least about 25, in other embodiments about 50 to about 10,000, and in other embodiments about 100 to about 2000. Those skilled in the art will recognize that the present invention encompasses other size ranges of nanowires that fall within the above explicit ranges and are within the present invention.

[0100] The polymer binder and the solvent are typically selected in unison so that the polymer binder is soluble or dispersible in the solvent. In suitable embodiments, the metal nanowire ink typically includes about 0.02 wt % to about 5 wt % binder, in other embodiments about 0.05 wt % to about 4 wt % binder and in other embodiments about 0.1 wt % to about 2.5 wt % polymer binder. In some embodiments, the polymer binder includes a crosslinkable organic polymer, such as a radiation crosslinkable organic polymer and / or a thermally curable organic binder. To promote crosslinking of the binder, the metal nanowire ink may include about 0.0005 wt % to about 1 wt % crosslinker in some embodiments, about 0.002 wt % to about 0.5 wt % crosslinker in other embodiments, and about 0.005 wt % to about 0.25 wt % crosslinker in other embodiments. The nanowire ink may optionally include a rheology modifier or a combination thereof. In some embodiments, the ink may include a wetting agent or surfactant to reduce surface tension, and the wetting agent may be used to improve coating properties. The wetting agent is typically soluble in the solvent. In some embodiments, the nanowire ink may include about 0.01 wt % to about 1 wt % wetting agent, in other embodiments about 0.02 wt % to about 0.75 wt % wetting agent, and in other embodiments about 0.03 wt % to about 0.6 wt % wetting agent. A thickener may optionally be used as a rheology modifier to stabilize the dispersion and reduce or eliminate sedimentation. In some embodiments, the nanowire ink may optionally include about 0.05 wt % to about 5 wt % thickener, in other embodiments about 0.075 wt % to about 4 wt % thickener, and in other embodiments about 0.1 wt % to about 3 wt % thickener. One skilled in the art will recognize that other concentration ranges of binders, wetting agents, and thickeners that fall within the above explicit ranges are contemplated by the present invention and are intended for use herein.

[0101] A variety of polymer binders may be suitable for dissolving / dispersing in solvents for use with metal nanowires, and suitable binders include polymers developed for coating applications. Hard coating polymers (e.g., radiation curable coatings) are commercially available, for example as hard coating materials for a variety of applications, which may be selected to be soluble in aqueous or non-aqueous solvents. Suitable types of radiation curable polymers and / or thermally curable polymers include, for example, polyurethanes, acrylic resins, acrylic copolymers, cellulose ethers and esters, other water-insoluble structural polysaccharides, polyethers, polyesters, epoxy-containing polymers, and mixtures thereof. Examples of commercial polymer binders include, for example, Branded acrylic resins (DMS NeoResins), Acrylic acid copolymers of the trademark (BASF Resins), Trademark acrylic resin (Lucite International), Trademark urethane (Lubrizol Advanced Materials), cellulose acetate butyrate polymer (CAB trademark, from Eastman TM Chemical), BAYHYDROL TM Polyurethane dispersions of the trademark (Bayer Material Science), Polyurethane dispersions of the trademark Cytec Industries, Inc. Polyvinyl butyral (Kuraray America, Inc.), cellulose ethers (e.g., ethyl cellulose or hydroxypropyl methyl cellulose), other polysaccharide-based polymers (e.g., chitosan and pectin), synthetic polymers (e.g., polyvinyl acetate), etc. The polymer binder can crosslink itself when exposed to radiation, and / or it can be crosslinked with a photoinitiator or other crosslinking agent. In some embodiments, the photocrosslinker can form free radicals when exposed to radiation, and these free radicals then initiate the crosslinking reaction based on a free radical polymerization mechanism. Suitable photoinitiators include, for example, commercially available products such as Trademark (BASF), GENOCURE TM Trademark (Rahn USA Corp.) and Trademark (Double Bond Chemical Ind., Co., Ltd.), combinations thereof, and the like.

[0102] Wetting agents can be used to improve the coatability of metal nanowire inks and the quality of metal nanowire dispersions. In particular, wetting agents can reduce the surface energy of the ink so that the ink is fully spread on the surface after coating. The wetting agent can be a surfactant and / or a dispersant. Surfactants are a class of materials used to reduce surface energy, and surfactants can improve the solubility of materials. Surfactants generally have a hydrophilic portion of the molecule and a hydrophobic portion of the molecule, which contribute to its properties. A variety of surfactants (e.g., nonionic surfactants, cationic surfactants, anionic surfactants, zwitterionic surfactants) are commercially available. In some embodiments, if the properties associated with the surfactant are not a problem, non-surfactant wetting agents (e.g., dispersants) are also known in the art and can effectively improve the wetting ability of the ink. Suitable commercial wetting agents include, for example, COATOSIL TM Epoxy-functional silane oligomers of the trademark Momentum Performance Materials, SILWET TM Trademark organic silicone surfactants (Momentum Performance Materials), THETAWET TMTrademark short-chain nonionic fluorinated surfactants (ICT Industries, Inc.), Polymer dispersants of the trademark Air Products Inc. Trademark polymer dispersant (Lubrizol), XOANONS WE-D545 surfactant (Anhui Xoanons Chemical Co., Ltd), EFKA TM PU 4009 polymer dispersant (BASF), MASURF FP-815CP, MASURF FS-910 (Mason Chemicals), NOVEC TM FC-4430 fluorinated surfactant (3M), mixtures thereof, etc.

[0103] Thickeners can be used to improve the stability of the dispersion by reducing or eliminating the settling of solids from the metal nanowire ink. Thickeners may or may not significantly change the viscosity or other fluid properties of the ink. Suitable thickeners are commercially available and include, for example, CRAYVALLAC TM Modified urea of ​​the trademark (e.g. LA-100 (Cray Valley Acrylics, USA)), polyacrylamide, THIXOL TM 53L trademark acrylic thickener, COAPUR TM 2025, COAPUR TM 830W, COAPUR TM 6050、COAPUR TM XS71(Coatex, Inc.), Modified urea of ​​the trademark (BYK Additives), Acrysol DR73, Acrysol RM-995, Acrysol RM-8W (Dow Coating Materials), Aquaflow NHS-300, Aquaflow XLS-530 hydrophobic modified polyether thickener (Ashland Inc.), Borchi Gel L 75N, Borchi Gel PW25 (OMG Borchers), etc.

[0104] As described above, the ink used to deposit the sparse metal conductive layer may further include silver nanoplatelets. The solution forming the sparse metal conductive layer may include about 0.0001 wt% to about 2.5 wt% silver nanoplatelets, in other embodiments about 0.0002 wt% to about 2 wt% silver nanoplatelets, and in other embodiments about 0.0005 wt% to about 1.5 wt% silver nanoplatelets. It should be recognized by those skilled in the art that the present invention encompasses other ranges of silver nanoplatelet concentrations that fall within the above explicit ranges and are within the present invention.

[0105] Other additives may be added to the metal nanowire ink, each typically in an amount of no more than about 5 wt %, in other embodiments no more than about 2 wt %, and in other embodiments no more than about 1 wt %. Other additives may include, for example, antioxidants, UV stabilizers, defoamers or anti-foaming agents, anti-settling agents, viscosity modifiers, and the like.

[0106] As described above, the fusion of metal nanowires can be accomplished via a variety of agents. Without wishing to be bound by theory, the fusion agent is thought to mobilize metal ions, and the free energy appears to be reduced in the fusion process. In some embodiments, excessive metal migration or growth can lead to degradation of optical properties, and therefore, the desired results can be obtained in a reasonably controlled manner (usually for a short period of time) via equilibrium shift, thereby producing sufficient fusion to obtain the desired conductivity while maintaining the desired optical properties. In some embodiments, the initiation of the fusion process can be controlled by partially drying the solution to increase the concentration of the components, and the quenching of the fusion process can be accomplished by, for example, rinsing or more completely drying the metal layer. The fusion agent can be incorporated into a single ink with the metal nanowires. This one ink solution can provide appropriate control of the fusion process.

[0107] In some embodiments, a process is used in which a sparse nanowire film is first deposited and then treated with or without deposition of another ink to fuse the metal nanowires into a conductive metal nanostructured network. The fusion process can be implemented using controlled exposure to a fusing vapor and / or via deposition of a fusing agent in solution. A sparse metallic conductive layer is typically formed on a selected substrate surface. The as-deposited nanowire film is typically dried to remove the solvent. The treatment can be adapted to patterning of the film.

[0108] To deposit the metal nanowire ink, any reasonable deposition means may be used, such as dip coating, spray coating, knife edge coating, rod coating, Meyer rod coating, slot die coating, gravure printing, spin coating, etc. The ink may have properties (e.g., viscosity) appropriately adjusted using additives for the desired deposition method. Similarly, the deposition method determines the amount of liquid deposited, and the concentration of the ink may be adjusted to provide the desired loading of metal nanowires on the surface. After forming a coating using the dispersion, the sparse metal conductive layer may be dried to remove the liquid.

[0109] The film can be dried using, for example, a heat gun, a furnace, a heat lamp, etc., but in some embodiments, an air-dryable film is desired. In some embodiments, during drying, the film can be heated to a temperature of about 50° C. to about 150° C. After drying, the film can be washed one or more times using, for example, an alcohol or other solvent or solvent blend (such as ethanol or isopropanol) to remove excess solids to reduce haze. Patterning can be achieved in several convenient ways. For example, printing of metal nanowires can directly cause patterning. Additionally or alternatively, litographic techniques and / or ablation methods can be used to remove portions of the metal nanowires to form patterns before or after fusion. One or more outer coatings can be applied to the sparse metal conductive layer, as described above.

[0110] The optically transparent adhesive layer and the thicker protective film covering the sparse metal conductive layer can form holes, etc. in appropriate locations to provide electrical connections to the conductive layer. In general, various polymer film processing techniques and equipment can be used for the processing of these polymer sheets, and these equipment and techniques are fully developed in the art, and future developed processing techniques and equipment can be correspondingly applied to the materials herein.

[0111] Properties of Hue Adjustment Film

[0112] Silver nanoplatelets are generally selected to provide the desired color adjustment of the transparent film without reducing the overall transparency by an amount exceeding an acceptable level. The acceptable amount of transparency reduction may be application specific. In some embodiments, it is also desirable that the film with silver nanoplatelets has a continuously low haze. In particular, it has been found that silver nanoplatelets can provide good color adjustment and have a low contribution to haze. Generally, the transparent film further includes a transparent conductive layer, such as a sparse metal conductive layer.

[0113] In the context of a sparse metallic conductive layer, silver nanoplatelets may be selected to reduce the overall value of b* in the CIE color scale. It may be found that a highly conductive sparse metallic conductive layer has a yellowish hue, and reducing b* may produce a whiter film appearance. As shown in the examples, it has been found that several specific silver nanoplatelets successfully reduce the b* value of the film. Additionally or alternatively, a selected color or color pattern may be introduced through the inclusion of selected silver nanoplatelets. For example, a pattern of a colored panel may be introduced.

[0114] In some embodiments, the silver nanoplatelets may reduce b* by at least about 0.2, at least about 0.25, and at least about 0.3 relative to the corresponding film without silver nanoplatelets. Likewise, it may be desirable that the absolute value of b* for a transparent film does not exceed 1.2, at least 1.1, and at least 1.0 in other embodiments. For embodiments with desired whiter transmission, the absolute value of a* for a film with silver nanoplatelets may not exceed about 1, at least about 0.65, at least about 0.6, and at least about 0.5 in other embodiments. Those skilled in the art will recognize that the present invention encompasses other optical parameter ranges that fall within the above-specified ranges and are in the present invention. The values ​​of b* and a* may be evaluated using equations in the standard CIE DE2000, Center International Commission on Illumination (Commission Internationale de L'Eclairage), see Colorimetry, 3rd Edition, CIE, 2004, which is incorporated herein by reference. Commercial spectrophotometers and software (e.g., Konica Minolta spectrophotometer CM-3700A and SpectraMagic TM NX software) to perform these calculations.

[0115] General electrical and optical properties of transparent conductive films are presented in the following sections, and various effects of silver nanoflakes on these properties are discussed below. For incorporation into a transparent coating for a transparent conductive film or directly into an ink for forming a sparse metal conductive layer, the loaded overcoat generally does not significantly increase the sheet resistance of the sparse metal conductive layer with a thin overcoat relative to an equivalent film without silver nanoflakes, and the sheet resistance is increased by no more than about 20% in some embodiments, no more than about 15% in other embodiments, and no more than about 10% in other embodiments relative to the sheet resistance of the corresponding film without silver nanoflakes. While achieving the desired reduction in b*, the silver nanoflakes can reduce the total light transmittance (in units of transmission percentage) relative to incident visible light by less than about 3 in some embodiments and less than about 2 in other embodiments, and no more than about 1.5 in some embodiments relative to the corresponding film without silver nanoflakes. Likewise, it can be expected that the use of silver nanoflakes in the film will not significantly increase the haze. In some embodiments, haze may be increased (haze measurement in percent) by no more than about 0.5, in other embodiments no more than about 0.4, in other embodiments no more than about 0.3, in other embodiments no more than about 0.25, in some embodiments no more than about 0.2, and in other embodiments no more than about 0.15 relative to a corresponding film without silver nanoplatelets. In some embodiments using silver nanoplatelets, haze is actually observed to be reduced, such that in addition to improving the whiteness of transmitted light, haze can be reduced using appropriate concentrations of silver nanoplatelets, but nanoscale pigments tested to date significantly increase haze. Those skilled in the art will recognize that other ranges of sheet resistance increase, total light transmittance change, and haze change that fall within the explicit ranges above are contemplated and within the present invention.

[0116] Transparent Conductive Films-Electrical and Optical Properties

[0117] Sparse metal conductive layers (e.g., fused metal nanostructured networks) can provide low resistance while providing good optical properties. Therefore, the film can be used as a transparent conductive electrode, etc. The transparent conductive electrode can be suitable for a variety of applications, such as electrodes along the light receiving surface of a solar cell. For displays and in particular for touch screens, the film can be patterned to provide a conductive pattern formed by the film. The substrate with the patterned film generally has good optical properties at each portion of the pattern.

[0118] The resistance of a film may be expressed as a sheet resistance, which is reported in units of ohms per square (Ω / □ or ohms / sq) to distinguish this value from the overall resistance value according to parameters associated with the measurement process. The sheet resistance of a film is typically measured using a four-point probe measurement or another suitable process. In some embodiments, the sheet resistance of the fused metal nanowire network may be no more than about 300 ohms / sq, in other embodiments no more than about 200 ohms / sq, in other embodiments no more than about 100 ohms / sq, and in other embodiments no more than about 60 ohms / sq. One skilled in the art will recognize that other ranges of sheet resistance that fall within the explicit ranges above are contemplated by the present invention and are within the present invention. Depending on the particular application, commercial specifications for sheet resistance in a device may not necessarily point to lower values ​​of sheet resistance (e.g., when other costs may be involved), and current commercially relevant values ​​may be, for example, 270 ohms / sq, versus 150 ohms / sq, 100 ohms / sq, 50 ohms / sq, 40 ohms / sq, 30 ohms / sq, or less, as target values ​​for touch screens of varying quality and / or size, and each of these values ​​defines a range between specific values ​​as endpoints of the range (e.g., 270 ohms / sq to 150 ohms / sq, 270 ohms / sq to 100 ohms / sq, 150 ohms / sq to 100 ohms / sq, etc.), with 15 specific ranges defined. Thus, lower cost films may be suitable in certain applications in exchange for moderately higher sheet resistance values. Generally, sheet resistance can be reduced by increasing the nanowire loading, but increased loading may be undesirable from other perspectives, and metal loading is only one factor among many used to achieve low values ​​of sheet resistance.

[0119] For applications as transparent conductive films, it is desirable that the fused metal nanowire network or other sparse metal conductive layer maintain good optical transparency. In principle, optical transparency is inversely related to loading, where higher loading leads to reduced transparency, but processing of the network can also significantly affect transparency. Similarly, polymer binders and other additives can be selected to maintain good optical transparency. Optical transparency can be evaluated relative to the transmitted light through the substrate. For example, the transparency of the conductive film described herein can be measured by using a UV-visible spectrophotometer and measuring the total transmittance through the conductive film and the supporting substrate. Transmittance is the ratio of the transmitted optical density (I) to the incident optical density (I o ) ratio. The transmittance of light through the film (T film ) can be obtained by dividing the measured total light transmittance (T) by the light transmittance through the supporting substrate (T sub ) to estimate. (T=I / Io and T / T sub =(I / I o ) / (I sub / I o )=I / Isub =T film ) Therefore, the reported total transmittance can be corrected to remove the transmission through the substrate to obtain the transmittance of the conductive layer, overcoat or other component alone. Although it is generally desirable to have good optical transparency in the visible spectrum, for convenience, the optical transmittance can be reported at a wavelength of 550nm of light. Alternatively or additionally, the transmittance can be reported as the total transmittance of wavelengths of light from 400nm to 700nm, and such results are reported in the examples below. In general, for fused metal nanowire films, the measurements of 550nm transmittance and total transmittance from 400nm to 700nm (or just "total transmittance" for convenience) are not qualitatively different. In some embodiments, the total transmittance (TT%) of the film formed by the fused network is at least 80%, in other embodiments at least about 85%, in other embodiments at least about 90%, in other embodiments at least about 94%, and in some embodiments from about 95% to about 99%. The transparency of films on transparent polymer substrates can be evaluated using the standard ASTM D1003 ("Standard Test Method for Haze and Luminous Transmittance of Transparent Plastics"), which is incorporated herein by reference. One skilled in the art will recognize that other light transmittance ranges that fall within the explicit ranges above are contemplated and are within the present invention. When adjusting the measured optical properties of the films for the substrates in the examples below, the films had very good light transmittance and haze values, which were obtained along with the low sheet resistance observed.

[0120] The fused metal network may also have low haze and high visible light transmittance while having a desired low sheet resistance. The haze may be measured using a haze meter based on the ASTM D1003 mentioned above, and the haze contribution of the substrate may be removed to provide a haze value for the transparent conductive film. In some embodiments, the haze value of the sintered network film may not exceed about 1.2%, in other embodiments not more than about 1.1%, in other embodiments not more than about 1.0%, and in other embodiments from about 0.9% to about 0.2%. As described in the examples, using appropriately selected silver nanowires, very low values ​​of haze and sheet resistance are obtained simultaneously. The loading may be adjusted to balance the sheet resistance and haze values, wherein very low haze values ​​may be obtained with still good sheet resistance values. Specifically, a haze value of no more than 0.8% and from about 0.4% to about 0.7% in other embodiments may be obtained at a sheet resistance value of at least about 45 ohms / sq. Likewise, haze values ​​of 0.7% to about 1.2%, and in some embodiments, about 0.75% to about 1.05%, can be obtained at sheet resistance values ​​of about 30 ohms / sq to about 45 ohms / sq. All of these films maintain good optical clarity. One skilled in the art will recognize that other haze ranges within the explicit ranges above are contemplated and are within the present invention.

[0121] As with the corresponding properties of multilayer films, the other components are generally selected to have little effect on the optical properties, and a variety of coatings and substrates are commercially available for use in transparent elements. Suitable optical coatings, substrates, and related materials are summarized above. Some structural materials can be electrically insulating, and if thicker insulating layers are used, the film can be patterned to provide locations where gaps or voids through the insulating layer can be accessed and electrically contacted to other embedded conductive elements.

[0122] Examples

[0123] Example 1. High concentration synthesis (0.12 mg / mL) of silver nanosheets with 2-step H2O2 addition.

[0124] This example demonstrates efficient high concentration synthesis of nanosheets and presents results for the basic synthesis process and variations of the basic process.

[0125] First, the use of citrate surfactant and glycerol stabilizer was used to show efficient scale-up of the reaction with approximately 60 times the reaction volume and approximately 12 times (12×) the silver concentration relative to the values ​​in a similar published procedure (Zhang JACS, Supplementary Materials page S29). This high concentration synthesis of silver nanosheets was achieved using a novel two-step addition of hydrogen peroxide. In this scale-up procedure, 1443 mL of DI (deionized) water was first added to a 4 L Erlenmeyer flask. Then, 18 mL of silver nitrate aqueous solution (0.1 M), 30 mL of trisodium citrate aqueous solution (75 mM), 10 mL of glycerol aqueous solution (35 mM), and the first portion of hydrogen peroxide solution (30 wt%) were added, and the mixture solution was vigorously stirred in air at room temperature. 37.5 mL of sodium borohydride (0.1 M) aqueous solution was quickly injected into this mixture. The colloidal solution turned dark yellow. In the following minutes, the color of the colloidal solution gradually turned to dark brownish. Then, another 12 mL of hydrogen peroxide solution (30 wt%) was added dropwise over about 5 minutes until the color of the colloidal solution turned blue. After the addition of hydrogen peroxide was complete, stirring was continued for 20 minutes.

[0126] Use this volume of the second portion of hydrogen peroxide solution to help form the AgNPL with the target absorption peak. Figure 3 , shows the UV-visible absorption spectra of the solution before and after the dropwise addition of the second amount of H2O2. The formation of silver nanosheets provides a characteristic shift of the absorption peak toward the red. If all the hydrogen peroxide is added to the initial reaction flask, only silver nanoparticles are observed instead of nanosheets. This product difference can be seen in Figure 4 , where absorption spectra are shown with all hydrogen peroxide added at once or with a two-step addition and the second amount added gradually. It is believed that the yield of nanosheets is close to 100%, but a few nanoparticles can be observed dispersed in the solution.

[0127] Example 2. High-concentration synthesis of silver nanostructures with H2O2 addition in step 1 (0.12 mg / mL)

[0128] As a comparison to the 2-step H2O2 addition method in Example 1, a one-step addition method of H2O2 was implemented to demonstrate the difference. The same procedure as Example 1 was followed, except that a combined amount of hydrogen peroxide solution (30 wt%) from the first and second additions in Example 1 was used before a rapid injection of boron borohydride (0.1 M) aqueous solution. The colloidal solution turned dark yellow after 30 minutes, indicating the formation of silver nanoparticles. Figure 4 The UV-vis spectra shown in confirm that only silver nanoparticles were formed.

[0129] Example 3. Synthesis of silver nanosheets at a higher concentration (>0.12 mg / mL)

[0130] Nanosheets have been successfully produced at even greater silver concentrations, and it has been found that a larger portion of the hydrogen peroxide needs to be added dropwise as the concentration increases, and the relative amounts of the stabilizing compounds should be adjusted to achieve the desired nanosheet properties, as characterized by the absorption spectrum. It is believed that the absorption spectrum of the nanosheet is affected by the size and aspect ratio of the nanosheet. For example, to synthesize silver nanosheets at a concentration of 0.68 mg / mL, 1443 mL of DI (deionized) water was first added to a 4 L Erlenmeyer flask. Then, 10.2 mL of an aqueous silver nitrate solution (1 M), 6 mL of an aqueous sodium citrate solution (0.75 mM), 14 mL of an aqueous glycerol solution (35 mM), and a first portion of a hydrogen peroxide solution (30 wt %) were added, and the mixture solution was vigorously stirred in air at room temperature. 13.2 mL of an aqueous sodium borohydride solution (1 M) was quickly injected into this mixture. The colloidal solution turned dark yellow. Over the next few minutes, the color of the colloidal solution gradually turned to a dark brownish color. Then, another 110 mL of hydrogen peroxide solution (30 wt %) was added dropwise until the color of the colloidal solution turned blue, indicating the formation of silver nanosheets.

[0131] Higher concentration synthesis reactions tend to form silver nanosheets with a wider range of nanosheet sizes. Different synthesis parameters for various silver concentrations according to a procedure similar to Example 1 are given in Table 1 below. The UV-visible absorption spectra of various concentrations (covering 10 values) are shown in Figures 5A-5J The results show that further optimization of the process can help narrow the size distribution while still achieving the desired scale of synthesis. It is believed that the volume can also be scaled up.

[0132] Table 1

[0133]

[0134] A set of experiments was performed to test alternatives to the glycerol stabilizing compound. Specifically, propylene glycol, ethyl lactate, and diacetone alcohol were used instead in the 12× protocol above and on an equimolar basis. For the propylene glycol and ethyl lactate stabilizing compounds, good production of silver nanosheets was found. For the diacetone alcohol compound, reasonable nanosheet synthesis was observed, but a larger portion of silver nanoparticles was produced. The UV-visible absorption spectra of the three samples are shown in Figure 6 middle.

[0135] Example 4. Coating of silver nanosheets with a gold thin shell

[0136] This example shows noble metal coating of silver nanosheets and the optical properties of the resulting gold-coated nanosheets.

[0137] The prepared solution of silver nanosheets from Example 1 was used for coating without purification. 6 g polyvinyl pyrrolidone (PVP, MW 40,000), 1.32 g trisodium citrate, 12 mL diethylamine and 24 mL ascorbic acid aqueous solution (0.5 M) were added to the silver nanosheet solution (12×) from Example 1. Trisodium citrate is important to prevent a large blue shift in the absorption peak of the silver nanosheets during the gold coating process. A separate coating solution for the gold coating was prepared by mixing 6 mL PVP (5 wt %), 1.2 mL KI aqueous solution (0.2 M) and 300 μL HAuCl4 aqueous solution (0.25 M) with 45 mL DI water. The gold coating solution was slowly added to the silver nanosheet colloidal solution at a rate of 0.2 mL / min by a syringe pump. A gold layer was deposited on the surface of the silver nanosheets. The thickness of the gold layer can be controlled by the amount of gold growth solution. The gold-coated silver nanosheets were collected and washed twice with DI water and stored at room temperature for future use.

[0138] The absorption spectra of silver nanosheets and gold-coated silver nanosheets are shown in Figure 7 The gold coating shifts the absorption peak to smaller wavelengths and increases the red absorption tail. The effect of citrate added during the coating process is shown in Figure 8 , which shows the absorption spectra of uncoated nanosheets, gold-coated nanosheets formed with added citrate, and gold-coated nanosheets without additional citrate. Silver nanosheets coated without added citrate have a significantly larger shift to lower wavelengths and have a large blue absorption. A typical transmission electron micrograph of a gold-coated nanosheet is shown in Fig. 9 After gold coating, most of the nanosheets remain intact and only a small portion of the silver nanosheets are etched to have holes in the plane. Based on the micrographs, the surface of the gold-coated nanosheets is not smooth at the atomic level.

[0139] Experiments were performed to verify the reproducibility of the synthesis of gold-coated silver nanosheets. These experiments confirmed the reproducibility of the synthesis of silver nanosheets and the gold coating process. Referring to Table 2, the synthesis steps were repeated 7 times using the same reaction parameters presented above. The peak absorption wavelengths of the silver nanosheets and the gold-coated silver nanosheets are shown in Table 2. The window of the absorption peak of the gold-coated silver nanosheets is about 539 nm to about 580 nm.

[0140] Table 2

[0141]

[0142] The thickness of the gold coating can be controlled by the amount of gold coating precursor. The synthesis was performed according to a procedure similar to that of Example 4, except that the total amount of the coating solution of the gold complex and the reducing agent was varied. The absorption spectra of typical gold-coated silver nanosheets with different thicknesses are shown in FIG. Fig.10 Given in.

[0143] Example 5. Stability of (gold-coated) silver nanosheets in solution

[0144] The stability of the nanosheets with respect to various temperature conditions was examined.

[0145] In the first test, the gold-coated silver nanosheets were frozen and thawed. The UV-visible absorption spectra before freezing and after thawing are shown in Fig.11 The thawed Au-coated Ag nanosheets have similar absorption spectra, with only a shift of approximately 10 nm to lower wavelengths. For comparison, commercial silver nanosheets coated with PVP were treated in a similar manner. The absorption spectra of the PVP-coated silver nanosheets before freezing and the corresponding absorption spectra after thawing are shown in Fig.12 The absorption spectrum of the thawed polymer-coated Ag nanosheets exhibits a significant shift and changes in shape and position, indicating conversion into silver nanoparticles. Thus, the gold coating substantially improves the stability of the nanosheets with respect to freezing.

[0146] In another set of experiments, concentrated colloidal solutions of gold-coated silver nanosheets and colloidal solutions of mercury-containing silver nanosheets were diluted in propylene glycol monomethyl ether (PGME) at a 1:9 v / v ratio and then heated at up to 90°C. The color and absorption peak positions were monitored by UV-vis spectrometer after 100 hours. The gold-coated silver nanosheets were very stable in PGME at elevated temperatures. Only a slight blue shift was observed during the first 2 hours of the test, and no further shift was seen in the next 100 hours ( Fig.13 ). In contrast, the color of the uncoated silver nanosheets quickly turned to yellow under the same conditions, indicating the formation of silver nanoparticles from the original silver nanosheets, as verified by the UV-vis spectra before and after the heating test ( Fig.14 ).

[0147] Example 6. Stability of (gold-coated) silver nanosheets in film coatings

[0148] This example shows the effect on the hue of a polymer coating with silver nanoplatelets and also demonstrates the stability of the hue adjustment.

[0149] Some examples involve silver nanosheets associated with a fused metal conductive network, which results in the formation of a transparent conductive film. Examples are presented as silver nanosheets in a conductive layer with a fused metal nanostructured network or in a coating disposed on a layer with a fused metal nanostructured network. The fused metal nanostructured network is formed using silver nanowires, which are synthesized using a polyol process and using a PVP polymer. In general, the inclusion of an appropriate amount of silver nanosheets can significantly reduce b* without unacceptably reducing other properties.

[0150] The tests described herein involved forming a fused metal nanostructured network on a PET polyester substrate (125 micron thick sheet). The fused metal nanostructured network was formed using a single ink containing silver nanowires and a fused composition. A polymer hardcoat was applied to the fused metal nanostructured network.

[0151] Silver nanowires were used in the following examples with an average diameter between 25 nm and 50 nm and an average length of 10-30 microns. Silver nanowire inks were substantially as described in Example 5 of U.S. Patent 9,183,968 to Li et al., entitled "Metal Nanowire Inks for the Formation of Transparent Conductive Films with Fused Networks," which is incorporated herein by reference. The metal nanowire ink includes silver nanowires (at a content between 0.1 wt% and 1.0 wt%), silver ions between 0.05 mg / mL and 2.5 mg / mL, and a cellulose-based binder (at a concentration of about 0.01 wt% to 1 wt%). The silver nanowire ink is an aqueous solution containing a small amount of alcohol. The ink was slot coated on a PET film. After coating the nanowire ink, the film was then heated in an oven at 100-120°C for 5-10 min to dry the film.

[0152] For some films, a haze meter was used to measure the total transmittance (TT) and haze of the film samples. To adjust the haze measurements of the samples below, the substrate haze value can be subtracted from the measured value to obtain an approximate haze measurement of the transparent conductive film alone. The instrument is designed to evaluate optical properties based on the ASTM D 1003 standard ("Standard Test Method for Haze and Luminous Transmittance of Transparent Plastics"), which is incorporated herein by reference. The total transmittance and haze of these films included a base total transmittance and haze of 92.1-92.9% and 0.1%-0.4% for the PET substrate, respectively. In the following example, two different formulations of fused metal nanowire inks are presented, as well as optical and sheet resistance measurements. Commercial software was used to obtain optical properties from a Konica Minolta spectrophotometer CM-3700A with SpectraMagic TM The CIELAB values ​​of b* and a* were determined using the NX software. Sheet resistance was measured using a 4-point probe method or a non-contact resistance meter.

[0153] In the first set of stability measurements, gold-coated nanosheets (300 μL Au coating) and corresponding non-coated silver nanosheets as prepared in Examples 1 and 4 were used. The nanosheets were dispersed in a hardcoat precursor solution and slit coated on the fused metal nanostructured network with an estimated wet thickness of 25 microns. The coated acrylic polymer was dried and UV crosslinked. The samples were then tested in a controlled environment chamber maintained at 60°C and 90% relative humidity (60 / 90 test). The b* values ​​of these films were measured over 10 days. A third sample (prepared without using nanosheets in the outer coating) was tested as a reference. The absolute increase in b*, Δb* of the sample containing silver nanosheets compared to the reference sample was considered a measure of the contribution from the changes in the nanosheets. The results of b* are plotted on Fig.15 (uncoated) and 16 (Au coated). Smaller differences in Δb* indicate higher stability of the nanosheets, while larger differences in Δb* indicate greater contribution from degradation of the silver nanosheets and thus low stability. According to the plot, in this durability test, the stability of the gold-coated silver nanosheets is greater than that of the uncoated silver nanosheets in the overcoat layer.

[0154] In another set of experiments, gold-coated silver nanosheets were added to the ink to form a conductive layer. The nanosheets were well dispersed in the ink layer, as shown by Fig.17 For the test, three samples were prepared: a control and two samples with different amounts of gold-coated silver nanosheets (550nm peak absorption). Color measurements and haze were compared between these films. The results are presented in Fig.18The haze values ​​(expressed as a percentage) in the plot are average values ​​for the entire film. Fig.18 Inclusion of gold-coated silver nanosheets reduces b* without unacceptably reducing other properties as shown in . Inclusion of gold-coated silver nanosheets (with a 550 nm absorption peak) does not significantly increase the absolute value of a*.

[0155] Three other samples were prepared using conductive inks containing gold-coated silver nanosheets with different absorption peaks. A control film without nanosheets was formed. The film was treated as described above. The sheet resistance measurements and optical properties of the resulting film are presented in Table 3. The transparency of the film with nanosheets was slightly reduced, but the absolute value of b* and a* was reduced by the desired amount.

[0156] Table 3. Effects of gold-coated silver nanosheets with different absorption peaks in the conductive layer

[0157]

[0158] The above embodiments are intended to be illustrative and not limiting. Other embodiments are within the scope of the claims. In addition, although the present invention has been described herein with reference to specific embodiments, it will be appreciated by those skilled in the art that changes may be made in form and detail without departing from the spirit and scope of the present invention. Any incorporation of the above-mentioned documents is limited so as not to incorporate subject matter contrary to the express disclosure herein.

Claims

1. A dispersion of noble metal coated silver nanoplatelets, wherein the noble metal coated silver nanoplatelets have 2 atomic % to 45 atomic % of noble metal, wherein the dispersion has a light absorption of at least 0.6 normalized absorption units at 600 nm, and a dispersion of corresponding silver nanoplatelets without the noble metal coating also has a light absorption of at least 0.6 normalized absorption units at 600 nm.

2. The dispersion of claim 1, wherein the noble metal coated silver nanoplatelets have 5 atomic % to 40 atomic % of the noble metal.

3. The dispersion of claim 1, having an optical absorption at 600 nm of at least 0.7 normalized absorption units.

4. The dispersion according to claim 1, wherein the silver nanoplatelets coated with a noble metal have an average equivalent circular diameter of no more than 120 nm, and the corresponding silver nanoplatelets without a noble metal coating have an average equivalent circular diameter of no more than 120 nm.

5. A method for applying a noble metal coating to silver nanosheets, the method comprising: A coating solution including 0.0002M to 0.02M aqueous solution of complexed noble metal ions and 0.05 wt% to 5 wt% polymer capping agent is gradually added to a reaction solution comprising an aqueous dispersion of silver nanosheets, 0.00075M to 0.05M polycarboxylate anions, 0.005wt% to 5 wt% polymer capping agent, 0.005M to 2M ligand and 0.001M to 0.1M reducing agent, wherein the reaction solution contains 0.00025wt% to 0.1wt% silver nanosheets. The method according to claim 5 , wherein the noble metal ions include gold ions and / or platinum ions.

7. The method according to claim 5, wherein the complexed noble metal ions include iodide ions, bromide ions, sulfite ions, CN - 、SCN - , thiosulfate or a mixture thereof as a complexing agent.

8. The method of claim 5, wherein the polycarboxylate anion is citrate, succinate, citramalate, malonate, tartrate, isocitrate, cis-aconate, homotricarbate, or a combination thereof.

9. The method of claim 5, wherein the polymer end-capping agent comprises polyvinyl pyrrolidone.

10. The method of claim 5, wherein the ligand comprises nitrite, diethylamine, ethylenediamine, nitrilotriacetic acid, iminobis(methylenephosphonic acid), aminotris(methylenephosphonic acid), ethylenediaminetetraacetic acid, 1,3-propylenediaminetetraacetic acid, triethylenetetramine, tris(2-aminoethyl)amine, diethylenetriaminepentaacetic acid, 1,2-cyclohexanediaminotetraacetic acid, iminodiacetic acid, methyliminodiacetic acid, N-(2-acetamido)iminoacetic acid, N-(2-carboxyethyl)iminodiacetic acid, N-(2-carboxymethyl)iminodipropionic acid, picolinic acid, pyridinedicarboxylic acid, histidine, or a combination thereof.

11. The method of claim 5, wherein the reducing agent comprises ascorbic acid, oxalic acid, tartaric acid, hydroxylamine, formic acid, or a mixture thereof.

12. The method of claim 5, wherein the silver nanoflakes are provided as an unpurified solution from the synthesis of silver nanoflakes.

13. The method of claim 12, wherein the total concentration of all forms of silver in the unpurified solution is at least 0.75 mM.