Electrolyte sheet for solid oxide fuel cell, method for producing electrolyte sheet for solid oxide fuel cell, and single cell for solid oxide fuel cell

Hydrostatic pressing technology is used to pressurize the unsintered plate body and resin layer of the solid oxide fuel cell, which solves the warping problem of the ceramic plate body caused by uneven thickness of the resin layer and achieves the stability of the battery shape. and improvement of power generation efficiency.

CN114270583BActive Publication Date: 2024-10-08MURATA MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080058633.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-08-22
Filing Date
2020-08-18
Publication Date
2024-10-08
Estimated Expiration
2040-08-18

AI Technical Summary

Technical Problem

In the prior art, when manufacturing electrolyte sheets for solid oxide fuel cells, the uneven thickness of the resin layer causes the ceramic plate body to warp, thereby affecting the shape stability and power generation efficiency of the battery.

Method used

The hydrostatic pressing method is used to pressurize the unsintered plate-shaped body and the resin layer to ensure that the resin layer is burned out and the ceramic plate-shaped body is sintered, thereby suppressing warpage and thermal shrinkage deviations, and controlling the ceramics through preheating and uniform pressure The shape and density of plates.

Benefits of technology

It effectively suppresses the warpage and thermal shrinkage deviation of the ceramic plate body, improves the shape stability of the electrolyte sheet and the power generation efficiency of the battery, and avoids damage and gas leakage problems during battery assembly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114270583B_ABST
    Figure CN114270583B_ABST
Patent Text Reader

Abstract

The warpage height of the electrolyte sheet 10 for a solid oxide fuel cell of the present invention is 300 μm or less. When viewed from the thickness direction, if the maximum value of the difference between the X coordinates of the second side D2 and the second virtual straight line V2 is set to Q, the maximum value of the difference between the Y coordinates of the third side D3 and the third virtual straight line V3 is set to R, the maximum value of the difference between the X coordinates of the fourth side D4 and the fourth virtual straight line V4 is set to S, and the length of the virtual rectangle surrounded by the first virtual straight line V1, the second virtual straight line V2, the third virtual straight line V3 and the fourth virtual straight line V4 in the X-axis direction is set to L X , set the length of the virtual rectangle in the Y-axis direction to L Y , then 100×Q / L X , 100×R / L Y and 100×S / L X The maximum value in is less than 1.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electrolyte sheet for a solid oxide fuel cell, a method for producing an electrolyte sheet for a solid oxide fuel cell, and a single cell for a solid oxide fuel cell. Background Art

[0002] Solid oxide fuel cell (SOFC) is a fuel cell that uses H2+O 2- →H2O+2e - 、Air electrode: (1 / 2)O2+2e - →O 2- A device that extracts electrical energy through a reaction. A solid oxide fuel cell can be used by stacking a plurality of single cells to form a stacked structure. The single cell is formed by providing a fuel electrode and an air electrode on an electrolyte sheet for a solid oxide fuel cell composed of a ceramic plate.

[0003] On the other hand, in order to improve the power generation efficiency of solid oxide fuel cells, the electrolyte sheet for solid oxide fuel cells is required to be thinner. However, if a thin unsintered plate-like body is sintered in order to achieve the thinning of the electrolyte sheet for solid oxide fuel cells, the obtained ceramic plate-like body is prone to warping. Therefore, when seeking to thin the electrolyte sheet for solid oxide fuel cells, it is required to suppress the warping of the ceramic plate-like body.

[0004] For example, Patent Document 1 discloses a production method in which a resin sheet or a resin layer is laminated on the surface of an unsintered plate-like body using a resin slurry containing spherical resin powder and then pressure-bonded to obtain a ceramic plate-like body having high smoothness.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2018-199598 Summary of the invention

[0008] However, when such a resin sheet or resin layer is used in the production method described in Patent Document 1, the thickness may be non-uniform, thereby causing warping.

[0009] If such a resin sheet or resin layer is stacked with an unsintered plate-like body, the load caused by the resin sheet or resin layer applied to the unsintered plate-like body will deviate. If the unsintered plate-like body is calcined in such a state, the obtained ceramic plate-like body will have a large warp. In addition, during calcination, the unsintered plate-like body is difficult to heat shrink in areas with a large load, and is easy to heat shrink in areas with a small load, resulting in a deviation in the degree of heat shrinkage in the unsintered plate-like body. If the degree of heat shrinkage in the unsintered plate-like body deviates, the obtained ceramic plate-like body will be greatly deformed from the unsintered plate-like body and deviate from the target shape (size).

[0010] If a solid oxide fuel cell stack is manufactured by combining a solid oxide fuel cell electrolyte sheet composed of a ceramic plate-like body deformed from a target shape with a metal separator manufactured as a target shape, at least a portion of the solid oxide fuel cell electrolyte sheet protrudes or is recessed from the metal separator. In the portion where the solid oxide fuel cell electrolyte sheet protrudes from the metal separator, if a collision occurs when the solid oxide fuel cell stack is installed in a thermal module, the protruding solid oxide fuel cell electrolyte sheet is damaged. In addition, in the portion where the solid oxide fuel cell electrolyte sheet is recessed from the metal separator, the width of the gas sealing portion formed between the solid oxide fuel cell electrolyte sheet and the metal separator is insufficient, resulting in gas leakage. In this way, if the solid oxide fuel cell electrolyte sheet is damaged or gas leaks, the solid oxide fuel cell stack is degraded, or the power generation efficiency of the solid oxide fuel cell is reduced.

[0011] The present invention is made to solve the above-mentioned problems, and its object is to provide a solid oxide fuel cell electrolyte sheet with suppressed deformation and warping. In addition, the present invention aims to provide a method for manufacturing the above-mentioned solid oxide fuel cell electrolyte sheet. Furthermore, the present invention aims to provide a solid oxide fuel cell cell having the above-mentioned solid oxide fuel cell electrolyte sheet.

[0012] The electrolyte sheet for a solid oxide fuel cell of the present invention is characterized in that the warpage height is 300 μm or less, and when viewed from above in the thickness direction, it has a shape surrounded by a first side arranged in clockwise order, a second side adjacent to the first side via a first corner, a third side adjacent to the second side via a second corner, and a fourth side adjacent to the third side via a third corner and adjacent to the first side via a fourth corner, and when viewed from above in the thickness direction, a first virtual straight line approximated by 10 points on the first side is set as the X-axis, a second virtual straight line passing through a point having an average value of the X-coordinates of the 10 points on the second side as the X-coordinate and being orthogonal to the first virtual straight line is set as the Y-axis, and an intersection point of the first virtual straight line and the second virtual straight line is set as a virtual In the XY coordinate system of the pseudo-origin, when defining a third virtual straight line that passes through a point having an average value of Y coordinates of 10 points on the third side as a Y coordinate and is parallel to the first virtual straight line, and a fourth virtual straight line that passes through a point having an average value of X coordinates of 10 points on the fourth side as an X coordinate and is orthogonal to the first virtual straight line, if the maximum value of the difference between the X coordinates of the second side and the second virtual straight line is set to Q, the maximum value of the difference between the Y coordinates of the third side and the third virtual straight line is set to R, the maximum value of the difference between the X coordinates of the fourth side and the fourth virtual straight line is set to S, and the length of the virtual rectangle enclosed by the first virtual straight line, the second virtual straight line, the third virtual straight line, and the fourth virtual straight line in the X-axis direction is set to L X , the length of the Y axis of the virtual rectangle is set to L Y , then 100×Q / L X , 100×R / L Y and 100×S / L X The maximum value in is less than 1.

[0013] The method for manufacturing an electrolyte sheet for a solid oxide fuel cell of the present invention is characterized in that it comprises: a step of preparing an unsintered body obtained by pressurizing an unsintered plate-like body containing ceramic material powder and a resin layer containing resin powder, a step of preparing a ceramic plate-like body by calcining the unsintered body, burning out the resin layer and sintering the unsintered plate-like body; in the step of preparing the unsintered body, pressurizing the unsintered plate-like body and the resin layer by hydrostatic pressing.

[0014] The solid oxide fuel cell unit cell of the present invention is characterized by comprising: a fuel electrode, an air electrode, and the solid oxide fuel cell electrolyte sheet of the present invention disposed between the fuel electrode and the air electrode.

[0015] According to the present invention, a solid oxide fuel cell electrolyte sheet with suppressed deformation and warping can be provided. In addition, according to the present invention, a method for manufacturing the above-mentioned solid oxide fuel cell electrolyte sheet can be provided. Furthermore, according to the present invention, a solid oxide fuel cell single cell having the above-mentioned solid oxide fuel cell electrolyte sheet can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a schematic plan view showing an example of the electrolyte sheet for a solid oxide fuel cell of the present invention.

[0017] Figure 2 To express Figure 1 Schematic cross-sectional view of the portion corresponding to the line segment A1 - A2 in FIG.

[0018] Figure 3 This is a schematic plan view for explaining a method for evaluating the degree of deformation of an electrolyte sheet.

[0019] Figure 4 This is a schematic plan view showing an example of a process for producing a ceramic green sheet.

[0020] Figure 5 This is a schematic plan view showing an example of the process of producing a ceramic green sheet.

[0021] Figure 6 This is a schematic plan view showing an example of the process of producing a ceramic green sheet.

[0022] Figure 7 It is a schematic cross-sectional view showing an example of the process of producing an unsintered plate-shaped body.

[0023] Figure 8 It is a schematic plan view showing an example of the process of producing the resin layer.

[0024] Fig. 9 It is a schematic plan view showing an example of the process of producing the resin layer.

[0025] Fig.10 It is a schematic plan view showing an example of the process of producing the resin layer.

[0026] Fig.11 This is a schematic cross-sectional view showing a state in which an unsintered plate-like body and a resin layer are stacked in one example of a process for producing an unsintered body.

[0027] Fig.12 This is a schematic cross-sectional view showing a state in which an assembly in which a laminated body block is accommodated in a hydrostatic pressing die is vacuum-sealed in an example of a process for producing an unsintered body.

[0028] Fig.13 This is a schematic cross-sectional view showing a state of hydrostatic pressing in an example of a process for producing an unsintered body.

[0029] Fig.14 This is a schematic cross-sectional view showing a state where an unsintered plate-like body and a resin layer are pressurized in one example of a process for producing an unsintered body.

[0030] Fig.15 A schematic cross-sectional view showing an example of a process for producing a ceramic plate-like body.

[0031] Fig.16 It is a schematic cross-sectional view showing an example of a single cell for a solid oxide fuel cell according to the present invention. DETAILED DESCRIPTION

[0032] Hereinafter, the electrolyte sheet for solid oxide fuel cells of the present invention (hereinafter also referred to as electrolyte sheet), the method for manufacturing the electrolyte sheet for solid oxide fuel cells of the present invention (hereinafter also referred to as the method for manufacturing the electrolyte sheet), and the single cell for solid oxide fuel cells of the present invention (hereinafter also referred to as single cell) are described. It should be noted that the present invention is not limited to the following configurations, and can be appropriately changed within the scope of the present invention. In addition, the scheme obtained by combining each of the preferred configurations described below also belongs to the present invention.

[0033] The drawings shown below are schematic diagrams, and their dimensions, aspect ratios, and other aspects may differ from those of actual products.

[0034] [Electrolyte sheet for solid oxide fuel cells]

[0035] Figure 1 This is a schematic plan view showing an example of the electrolyte sheet for a solid oxide fuel cell of the present invention. Figure 2 To express Figure 1 Schematic cross-sectional view of the portion corresponding to the line segment A1 - A2 in FIG.

[0036] like Figure 1 and Figure 2 The solid oxide fuel cell electrolyte sheet 10 shown is composed of a ceramic plate-like body.

[0037] The ceramic plate-like body is, for example, a sintered body of a solid electrolyte such as scandia-stabilized zirconia or yttria-stabilized zirconia. Among them, the electrolyte sheet 10 is preferably composed of a ceramic plate-like body of a sintered body of scandia-stabilized zirconia. Since the electrolyte sheet 10 is composed of a ceramic plate-like body of a sintered body of scandia-stabilized zirconia, the conductivity of the electrolyte sheet 10 is improved. Therefore, when the electrolyte sheet 10 is assembled in a solid oxide fuel cell, the power generation efficiency of the solid oxide fuel cell is improved.

[0038] In the thickness direction ( Figure 2 When viewed from above (in the vertical direction), the electrolyte sheet 10 is as shown Figure 1 The shape shown is surrounded by the first side D1, the second side D2, the third side D3 and the fourth side D4 arranged in a clockwise order. The second side D2 is adjacent to the first side D1 via the first corner C1. The third side D3 is adjacent to the second side D2 via the second corner C2. The fourth side D4 is adjacent to the third side D3 via the third corner C3, and is adjacent to the first side D1 via the fourth corner C4.

[0039] When viewed from above in the thickness direction, although not shown in the figure, the electrolyte sheet 10 preferably has roundness at the first corner C1, the second corner C2, the third corner C3, and the fourth corner C4. In the electrolyte sheet 10, the first corner C1, the second corner C2, the third corner C3, and the fourth corner C4 may all be given roundness, or may be given roundness to only a portion.

[0040] Although not shown in the figure, it is preferred that through holes penetrating in the thickness direction are provided in the electrolyte sheet 10. The through holes function as gas flow paths in the solid oxide fuel cell.

[0041] The number of the through-holes may be only one, or may be two or more.

[0042] When viewed in plan from the thickness direction, the through hole may be circular or may have other shapes.

[0043] The position of the through hole is not particularly limited.

[0044] The size of the electrolyte sheet 10 in a plan view is, for example, 109 mm×109 mm.

[0045] The thickness of the electrolyte sheet 10 is preferably 200 μm or less, and more preferably 130 μm or less. The thickness of the electrolyte sheet 10 is preferably 30 μm or more, and more preferably 50 μm or more.

[0046] The thickness of the electrolyte sheet 10 can be determined as follows. First, the thickness of any nine locations in the region 5 mm inward from the peripheral edge of the electrolyte sheet 10 is measured using a U-shaped steel plate micrometer "PMU-MX" manufactured by Mitutoyo Corporation. Then, the average value calculated from the measured thickness values ​​of the nine locations is determined as the thickness of the electrolyte sheet 10.

[0047] Although not shown, it is preferred that recessed portions are dispersed on one main surface and the other main surface of the electrolyte sheet 10. By dispersing recessed portions on one main surface and the other main surface of the electrolyte sheet 10, when the electrolyte sheet 10 is assembled in a solid oxide fuel cell, the contact area between the electrode and the gas becomes larger, resulting in an improvement in the power generation efficiency of the solid oxide fuel cell. The recessed portions may be dispersed only on one main surface of the electrolyte sheet 10.

[0048] In the electrolyte sheet 10, the warping height is 300 μm or less. By making the warping height of the electrolyte sheet 10 300 μm or less, the electrolyte sheet 10 with suppressed warping can be realized. Therefore, when the electrolyte sheet 10 is assembled in a solid oxide fuel cell, the power generation efficiency of the solid oxide fuel cell is improved. The warping height of the electrolyte sheet 10 is preferably 200 μm or less.

[0049] The warping height of the electrolyte sheet 10 can be determined as follows. First, the height of 16 points of the electrolyte sheet 10 is measured using an image measuring system "NEXIV VMZ-R6555" manufactured by Nikon Instec, for example, to perform virtual plane leveling. Thereafter, the height of the outer edge of the electrolyte sheet 10 from the virtual plane is calculated as the warping height.

[0050] In the electrolyte sheet 10, when viewed from above in the thickness direction, a first virtual straight line approximated by 10 points on the first side D1 is set as the X-axis, a second virtual straight line passing through a point having an average value of the X-coordinates of the 10 points on the second side D2 as the X-coordinate and being orthogonal to the first virtual straight line is set as the Y-axis, and an intersection point of the first virtual straight line and the second virtual straight line is set as a virtual origin in an XY coordinate system, a third virtual straight line passing through a point having an average value of the Y-coordinates of the 10 points on the third side D3 as the Y-coordinate and being parallel to the first virtual straight line is defined, and When passing through the fourth virtual straight line which has the average value of the X coordinates of the 10 points on the fourth side D4 as the point of the X coordinate and is orthogonal to the first virtual straight line, if the maximum value of the difference between the X coordinates of the second side D2 and the second virtual straight line is set to Q, the maximum value of the difference between the Y coordinates of the third side D3 and the third virtual straight line is set to R, the maximum value of the difference between the X coordinates of the fourth side D4 and the fourth virtual straight line is set to S, and the length of the virtual rectangle enclosed by the first virtual straight line, the second virtual straight line, the third virtual straight line, and the fourth virtual straight line in the X-axis direction is set to L X , set the length of the virtual rectangle in the Y-axis direction to LY , then 100×Q / L X , 100×R / L Y and 100×S / L X The maximum value of is less than 1. That is, in the electrolyte sheet 10, 100×Q / L is satisfied. X ≤1, 100×R / L Y ≤1 and 100×S / L X ≤1.

[0051] The above “100×Q / L X ”, “100×R / L Y ” and “100×S / L X " represents the degree of deformation (deviation ratio) of the electrolyte sheet 10 relative to the virtual rectangle regarded as the target shape. By making the maximum value of these deformation degrees less than 1%, it is possible to realize an electrolyte sheet 10 in which deformation from the target shape is suppressed, that is, the straightness of the first side D1, the second side D2, the third side D3 and the fourth side D4 is high and the right angles of two adjacent sides of these four sides are high. According to such an electrolyte sheet 10, even if it is combined with a metal separator made in the target shape to make a stack for solid oxide fuel cells, the electrolyte sheet 10 will not protrude or sink from the metal separator. Therefore, deterioration of the solid oxide fuel cell stack caused by damage to the electrolyte sheet 10, leakage of gas, etc., reduction in the power generation efficiency of the solid oxide fuel cell, etc. will not occur. In the electrolyte sheet 10, 100×Q / L X , 100×R / L Y and 100×S / L X The maximum value of is preferably 0.5 or less.

[0052] Figure 3 This is a schematic plan view for explaining a method for evaluating the degree of deformation of an electrolyte sheet. It should be noted that each coordinate shown below can be measured using, for example, an image measuring system "NEXIV VMZ-R6555" manufactured by Nikon Instec.

[0053] like Figure 3 As shown, first, the first virtual straight line V1 approximated by 10 points on the first side D1 is determined. At this time, the XY coordinates of the 10 points on the first side D1 are measured for arbitrary X-axis and Y-axis, and the first virtual straight line V1 can be determined from the XY coordinates of these 10 points using an approximation method such as the least squares method.

[0054] Thereafter, the first virtual straight line V1 is set as the X-axis, and the second virtual straight line V2 is determined, which passes through a point having an average value of the X coordinates of the 10 points on the second side D2 as the X coordinate and is orthogonal to the first virtual straight line V1. At this time, an arbitrary straight line orthogonal to the first virtual straight line V1 can be set as the Y-axis and the X coordinates of the 10 points on the second side D2 can be measured, thereby determining the second virtual straight line V2 which passes through a point having an average value of the X coordinates of the 10 points as the X coordinate and is orthogonal to the first virtual straight line V1.

[0055] Then, an XY coordinate system is determined in which the first virtual straight line V1 is set as the X axis, the second virtual straight line V2 is set as the Y axis, and the intersection point P1 of the first virtual straight line V1 and the second virtual straight line V2 is set as the virtual origin.

[0056] In this XY coordinate system, by measuring the Y coordinates of 10 points on the third side D3, a third virtual straight line V3 passing through a point having an average Y coordinate of the 10 points and parallel to the first virtual straight line V1 is determined.

[0057] In the same XY coordinate system, by measuring the X coordinates of 10 points on the fourth side D4, a fourth virtual straight line V4 passing through a point having an average X coordinate of the 10 points and being orthogonal to the first virtual straight line V1 is determined.

[0058] When measuring the coordinates of 10 points on each of the first side D1 , the second side D2 , the third side D3 , and the fourth side D4 , it is preferable to select 10 points located at positions that divide the length of each side into equal parts.

[0059] Next, in the above XY coordinate system, a virtual rectangle P1P2P3P4 is determined, which is surrounded by the first virtual straight line V1, the second virtual straight line V2, the third virtual straight line V3, and the fourth virtual straight line V4. Then, the length L of the virtual rectangle P1P2P3P4 in the X-axis direction, i.e., the extending direction of the first virtual straight line V1, is calculated. X and the length L of the virtual rectangle P1P2P3P4 in the Y-axis direction, that is, the extending direction of the second virtual straight line V2 Y In the virtual rectangle P1P2P3P4, L X ≠L Y The rectangle of L X =L Y In addition, in the same XY coordinate system, the maximum value Q of the difference between the X coordinates of the second side D2 and the second virtual straight line V2, the maximum value R of the difference between the Y coordinates of the third side D3 and the third virtual straight line V3, and the maximum value S of the difference between the X coordinates of the fourth side D4 and the fourth virtual straight line V4 are respectively obtained.

[0060] Using the values ​​obtained above, calculate "100×Q / L X ”, “100×R / L Y ” and “100×S / L X ". As long as the calculation of "100×Q / L X ”, “100×R / L Y ” and “100×S / L X The maximum value in " can be less than 1.

[0061] It should be explained that Figure 3 In order to easily explain the method of evaluating the degree of deformation of the electrolyte sheet 10, the electrolyte sheet 10 is shown as deforming from a virtual rectangle P1P2P3P4. However, in the electrolyte sheet 10, due to the above-mentioned "100×Q / L X ”, “100×R / L Y ” and “100×S / L X " is less than 1, so strictly speaking, the electrolyte sheet 10 has a shape that is the same as or close to the virtual rectangle P1P2P3P4.

[0062] [Method for producing electrolyte sheet for solid oxide fuel cell]

[0063] The electrolyte sheet for a solid oxide fuel cell of the present invention can be produced, for example, by the following method.

[0064] <Process of manufacturing ceramic green sheets>

[0065] Figure 4 , Figure 5 and Figure 6 This is a schematic plan view showing an example of the process of producing a ceramic green sheet.

[0066] First, ceramic material powder, binder, dispersant, organic solvent, etc. are mixed to prepare ceramic slurry. Then, the obtained ceramic slurry is applied to one main surface of the carrier film to produce a Figure 4 The ceramic green tape (Green tape) 1t is shown.

[0067] As a method for producing the ceramic green tape 1t, a tape forming method is preferably used, and a doctor blade method or a calendaring method is particularly preferably used. Figure 4 In FIG. 1 , the casting direction when the strip forming method is used is represented by X, and the direction perpendicular to the casting direction is represented by Y.

[0068] As the ceramic material powder, for example, solid electrolyte powders such as scandia-stabilized zirconia powder and yttria-stabilized zirconia powder can be used. Among them, the ceramic material powder preferably contains scandia-stabilized zirconia powder.

[0069] Next, if Figure 5 As shown, the ceramic green tape 1t is punched into a predetermined size by a known method, and the carrier film is peeled off to produce a ceramic green tape 1t. Figure 6 The ceramic green sheet 1g is shown. There is no limitation on the order of punching out the ceramic green tape 1t and peeling off the carrier film.

[0070] <Process for producing unsintered plate-shaped body>

[0071] Figure 7 It is a schematic cross-sectional view showing an example of the process of producing an unsintered plate-shaped body.

[0072] like Figure 7 As shown in FIG. 1 , the unsintered plate-shaped body 1s is produced by stacking and pressing three ceramic green sheets 1g.

[0073] The number of ceramic green sheets 1g used to prepare the unsintered plate-like body 1s can be as follows: Figure 7 The figure shows three sheets, but it can also be two sheets, or it can be four or more sheets. Such a plurality of ceramic green sheets 1g can be pressed together, or they can be simply stacked without being pressed together. When the unsintered plate-like body 1s is produced from a plurality of ceramic green sheets 1g, the thickness of the ceramic plate-like body obtained later can be appropriately and easily controlled.

[0074] It should be noted that the unsintered plate-like body 1s may be produced from one ceramic green sheet 1g. Figure 7 The process shown.

[0075] <Process of preparing resin layer>

[0076] Figure 8 , Fig. 9 and Fig.10 It is a schematic plan view showing an example of the process of producing the resin layer.

[0077] First, a resin slurry is prepared by mixing resin powder, a binder, a dispersant, an organic solvent, etc. Then, the obtained resin slurry is applied to one main surface of a carrier film to produce a Figure 8 The resin belt 2t is shown.

[0078] As a method for producing the resin tape 2t, a tape forming method is preferably used, and a doctor blade method or a calendaring method is particularly preferably used. Figure 8 In FIG. 1 , the casting direction when the strip forming method is used is represented by X, and the direction perpendicular to the casting direction is represented by Y.

[0079] As the resin powder, it is preferred to use a resin material that is poorly soluble in the organic solvent used to prepare the resin slurry. The resin powder being poorly soluble in the organic solvent means that when 0.1 g of the resin powder is mixed with 100 g of the organic solvent at room temperature (25°C) for 24 hours, there is visually dissolved residue. The organic solvent used to prepare the resin slurry is, for example, at least one (monomer or mixture) selected from toluene, ethanol, isopropanol, butyl acetate, ethyl acetate, pinene alcohol and water. At this time, as the material of the resin powder, for example, a cross-linked acrylic resin can be used.

[0080] The resin powder is preferably spherical. In the case where the resin powder is spherical, the median particle size D 50 For example, it is 0.3 μm to 10 μm.

[0081] When the resin powder is spherical, the median particle size D 50 For example, the particle size distribution of the resin powder can be measured using a laser diffraction particle size distribution measuring device, and the particle size at which the cumulative value is 50% can be determined in the distribution expressed as cumulative % relative to the particle size scale. It should be noted that the shape of the resin powder includes the strain generated in the manufacturing process, etc., and the median particle size D 50 Indicates the equivalent circular diameter.

[0082] When the resin powder is spherical, its surface area per unit weight becomes smaller, so the amount of binder required to prepare a resin slurry with high fluidity becomes smaller. As a result, a resin layer with a high content of resin powder can be produced, so that a large number of recesses can be formed on one main surface and the other main surface of the ceramic plate body obtained later.

[0083] Next, if Fig. 9 As shown, the resin tape 2t is punched into a predetermined size by a known method, and the carrier film is peeled off to produce a Fig.10 The resin sheet shown is the resin layer 2e. There is no limitation on the order of punching out the resin tape 2t and peeling off the carrier film.

[0084] When the resin layer 2e is produced, the resin paste may be applied to at least one main surface of the green plate-like body 1s instead of producing the resin sheet.

[0085] The thickness of the resin layer 2e after drying is, for example, 10 μm to 18 μm.

[0086] <Process for producing unsintered body>

[0087] Fig.11 This is a schematic cross-sectional view showing a state in which an unsintered plate-like body and a resin layer are stacked in one example of a process for producing an unsintered body. Fig.12This is a schematic cross-sectional view showing a state in which an assembly in which a laminated body block is accommodated in a hydrostatic pressing mold is vacuum-sealed in an example of a process for producing an unsintered body. Fig.13 This is a schematic cross-sectional view showing a state of hydrostatic pressing in one example of a process for producing an unsintered body. Fig.14 This is a schematic cross-sectional view showing a state in which an unsintered plate-like body and a resin layer are pressurized in one example of a process for producing an unsintered body.

[0088] First, if Fig.11 As shown in FIG. 1 , a laminated body block 10b is produced by laminating an unsintered plate-like body 1s containing ceramic material powder and a resin layer 2e containing resin powder 2b. More specifically, the resin layer 2e is laminated on one main surface ( Fig.11 The upper surface in the middle) and the other main surface ( Fig.11 In this step, the resin layer 2e may be laminated on only one main surface of the unsintered plate-like body 1s.

[0089] Next, the laminated body block 10b is placed in the mold 20 and sandwiched between the first mold member 21 and the second mold member 22, thereby manufacturing the assembly 30. Fig.12 As shown, the assembly 30 is placed in a bag 40 and vacuum-sealed. Examples of the material of the bag 40 include resins and the like.

[0090] Next, if Fig.13 As shown, the assembly 30 vacuum-sealed by the bag 40 is sunk into the water 60 in the pressure vessel 50, and then the water 60 is pressurized by the pump 70. Thus, a predetermined hydrostatic pressure is applied to the laminated body block 10b via the mold 20, and the unsintered plate-like body 1s and the resin layer 2e are pressurized by hydrostatic pressing.

[0091] As above make Fig.14 The unsintered body 10g is obtained by pressing the unsintered plate-like body 1s and the resin layer 2e. It should be noted that the unsintered body 10g can be cut as needed to have a shape calculated using the heat shrinkage of the unsintered plate-like body 1s assumed during the calcination of the unsintered body 10g described later and the target shape of the ceramic plate-like body to be obtained later.

[0092] When the unsintered plate-like body 1s and the resin layer 2e are pressurized by hydrostatic pressing, the resin layer 2e is pressed against one main surface and the other main surface of the unsintered plate-like body 1s. As a result, recessed portions having a shape derived from the resin powder 2b are scattered on one main surface and the other main surface of the unsintered plate-like body 1s.

[0093] By using hydrostatic pressing as a pressurizing method, a uniform pressure is applied to the stacked body block 10b, and therefore, the deviation of the load applied to the unsintered plate-like body 1s can be suppressed. Therefore, if the unsintered plate-like body 1s is sintered in the process of making a ceramic plate-like body described later, the warping of the ceramic plate-like body obtained later can be suppressed even without using a special heavy stone such as a conventional porous gasket. In addition, if the deviation of the load applied to the unsintered plate-like body 1s is suppressed, the deviation of the degree of thermal shrinkage in the unsintered plate-like body 1s is suppressed when the unsintered plate-like body 1s is sintered. Therefore, the deformation of the ceramic plate-like body obtained later is suppressed.

[0094] When hydrostatic pressing is used as a pressurization method, the temperature of the laminate block 10b is approximately the same as the temperature of the water 60, and the higher the temperature of the water 60, the higher the fluidity of the binder present in the laminate block 10b. At this time, in the unsintered plate-like body 1s, the fluidity of the binder is improved, so the density and thickness become uniform, and the warping is suppressed. Similarly, in the resin layer 2e, the fluidity of the binder is improved, so the density and thickness become uniform, and the warping is suppressed. When such an unsintered plate-like body 1s and the resin layer 2e are pressurized to produce an unsintered body 10g, the deviation of the load applied to the unsintered plate-like body 1s is significantly suppressed in combination with the uniform pressure applied to the laminate block 10b by hydrostatic pressing. Therefore, if the unsintered plate-like body 1s is sintered in the process of producing a ceramic plate-like body described later, the warping of the ceramic plate-like body obtained thereafter is significantly suppressed. In addition, when the deviation of the load applied to the unsintered plate-like body 1s is significantly suppressed, the density and thickness of the unsintered plate-like body 1s are uniformly combined with each other, and when the unsintered plate-like body 1s is sintered, the deviation of the degree of thermal shrinkage in the unsintered plate-like body 1s is significantly suppressed. Therefore, the deformation of the ceramic plate-like body obtained thereafter is significantly suppressed.

[0095] When the unsintered plate-like body 1s and the resin layer 2e are pressurized together by hydrostatic pressing as in the production of the unsintered body 10g, it is required to improve the fluidity of the binder present in the laminated body block 10b as a whole so as to achieve a state in which the density and thickness are uniform and the warping is suppressed in the unsintered plate-like body 1s and the resin layer 2e. From such a viewpoint, it is preferred to preheat the unsintered plate-like body 1s and the resin layer 2e at 60°C or higher and less than 100°C for more than 5 minutes before pressurizing the unsintered plate-like body 1s and the resin layer 2e by hydrostatic pressing. Specifically, from the time when the assembly 30 vacuum-sealed with the bag 40 begins to sink into the water 60 to the time when the water 60 begins to be pressurized by the pump 70, it is preferred to set a preheating period in which the laminated body block 10b is preheated at 60°C or higher and less than 100°C for more than 5 minutes. As a method of setting such a preheating period, for example, the assembly 30 vacuum-sealed with the bag 40 may be immersed in water 60 at a temperature of 60°C or higher and lower than 100°C, the temperature of the laminated body block 10b may be maintained at 60°C or higher and lower than 100°C for 5 minutes, and then the water 60 may be pressurized by the pump 70. Alternatively, the assembly 30 vacuum-sealed with the bag 40 may be immersed in water 60, and then the temperature of the water 60 may be increased to 60°C or higher and lower than 100°C, thereby the temperature of the laminated body block 10b may be 60°C or higher and lower than 100°C, and this state may be maintained for 5 minutes, and then the water 60 may be pressurized by the pump 70. It should be noted that when the temperature of the water 60 is 100°C or higher, the water 60 boils, and therefore, hydrostatic pressing cannot be performed. The preheating time (length of the preheating period) is preferably 5 to 15 minutes. The preheating temperature (temperature during the preheating period) may be the same as the pressurizing temperature during hydrostatic pressing.

[0096] On the other hand, when uniaxial pressing is used as a pressurizing method, it is difficult to apply uniform pressure to the laminated body block 10b due to the strain of the pressing shaft, the warping of the pressure plate, and the like. If uniform pressure is not applied to the laminated body block 10b, it is impossible to suppress the deviation of the load applied to the unsintered plate-like body 1s. Therefore, if the unsintered plate-like body 1s is sintered in such a state, it is impossible to suppress the warping of the ceramic plate-like body obtained later. In addition, when the unsintered plate-like body 1s is sintered, it is impossible to suppress the deviation of the degree of thermal shrinkage in the unsintered plate-like body 1s, and it is impossible to suppress the deformation of the ceramic plate-like body obtained later.

[0097] <Step of forming through holes in unsintered body>

[0098] Although not shown in the drawings, a through hole penetrating the green body 10g in the stacking direction may be formed.

[0099] The through hole is preferably formed by a drill. At this time, the drill is advanced from one main surface of the unsintered body 10g to the other main surface, thereby forming a through hole that penetrates the unsintered body 10g in the stacking direction. The processing conditions using the drill are not particularly limited.

[0100] The number of the through-holes may be only one, or may be two or more.

[0101] It should be noted that the through hole may not be formed. In this case, this step is omitted.

[0102] <Process of manufacturing ceramic plate body>

[0103] Fig.15 A schematic cross-sectional view showing an example of a process for producing a ceramic plate-like body.

[0104] By calcining 10 g of the unsintered body, Fig.15 As shown, the resin layer 2e is burned out and the green plate-like body 1s is sintered to produce a ceramic plate-like body 10p. When the through hole is formed in the green plate-like body 10g, the through hole penetrating in the thickness direction is provided in the ceramic plate-like body 10p.

[0105] When the unsintered body 10g is fired, as described above, the load applied to the unsintered plate body 1s is suppressed from varying, so the warping of the ceramic plate body 10p is suppressed. In addition, the degree of thermal shrinkage in the unsintered plate body 1s is suppressed, so the deformation of the ceramic plate body 10p is suppressed.

[0106] When calcining 10 g of the unsintered body, it is preferable to perform a degreasing treatment and a sintering treatment.

[0107] Through the above operation, a ceramic plate-like body 10p with recesses scattered on one main surface and the other main surface is manufactured. In the above-mentioned method for manufacturing the electrolyte sheet, in the process of manufacturing the unsintered body 10g, the unsintered plate-like body 1s and the resin layer 2e are pressurized by hydrostatic pressing. Therefore, in the ceramic plate-like body 10p, the warpage height is less than 300 μm, referring to Figure 3 The "100 × Q / L" which indicates the degree of deformation (deviation ratio) relative to the virtual rectangle regarded as the target shape is explained. X ”, “100×R / L Y ” and “100×S / L X " is less than 1. That is, according to the above-mentioned method for manufacturing an electrolyte sheet, an electrolyte sheet for a solid oxide fuel cell of the present invention (for example Figure 1 and Figure 2 The electrolyte sheet 10).

[0108] [Single cell for solid oxide fuel cell]

[0109] An example of a single cell for a solid oxide fuel cell according to the present invention will be described below. Fig.16 It is a schematic cross-sectional view showing an example of a single cell for a solid oxide fuel cell according to the present invention.

[0110] like Fig.16 As shown, the solid oxide fuel cell unit cell 100 includes a fuel electrode 110 , an air electrode 120 , and an electrolyte sheet 130 . The electrolyte sheet 130 is disposed between the fuel electrode 110 and the air electrode 120 .

[0111] As the fuel electrode 110 , a known fuel electrode for solid oxide fuel cells can be used.

[0112] As the air electrode 120 , a known air electrode for solid oxide fuel cells can be used.

[0113] As the electrolyte sheet 130, the solid oxide fuel cell electrolyte sheet of the present invention (for example, Figure 1 and Figure 2 Therefore, according to the single cell 100, the power generation efficiency of the solid oxide fuel cell can be improved.

[0114] [Method for manufacturing a single cell for solid oxide fuel cell]

[0115] The solid oxide fuel cell unit cell of the present invention can be produced, for example, by the following method.

[0116] First, prepare the slurry for the fuel electrode and the slurry for the air electrode. The slurry for the fuel electrode can be prepared by appropriately adding a binder, a dispersant, a solvent, etc. to the powder of the material of the fuel electrode. The slurry for the air electrode can be prepared by appropriately adding a binder, a dispersant, a solvent, etc. to the powder of the material of the air electrode.

[0117] As the material of the fuel electrode, a known material for a fuel electrode for a solid oxide fuel cell can be used.

[0118] As the material of the air electrode, a known material for an air electrode for a solid oxide fuel cell can be used.

[0119] As the binder, dispersant, solvent and the like contained in the fuel electrode slurry and the air electrode slurry, those known in the method of forming a fuel electrode and an air electrode for a solid oxide fuel cell can be used.

[0120] Next, the fuel electrode slurry is applied to one main surface of the electrolyte sheet and the air electrode slurry is applied to the other main surface of the electrolyte sheet to a predetermined thickness, and these coatings are dried to form a fuel electrode green layer and an air electrode green layer.

[0121] Then, the fuel electrode and the air electrode are formed by firing the short fuel electrode green layer and the air electrode green layer. The firing conditions such as the firing temperature may be appropriately determined according to the types of materials of the fuel electrode and the air electrode.

[0122] Example

[0123] Examples of the electrolyte sheet for solid oxide fuel cells of the present invention are shown below in more detail, but the present invention is not limited to these examples.

[0124] [Example 1]

[0125] The electrolyte sheet of Example 1 was produced by the following method.

[0126] <Process of manufacturing ceramic green sheets>

[0127] First, scandium oxide stabilized zirconia powder, a binder, a dispersant, and an organic solvent are mixed in a predetermined ratio. As the organic solvent, a mixture of toluene and ethanol (weight ratio 7:3) is used. Then, the obtained mixture is stirred at 1000 rpm for 3 hours with a medium composed of partially stabilized zirconia to prepare a ceramic slurry.

[0128] Next, the obtained ceramic slurry is tape-formed on one main surface of a carrier film made of polyethylene terephthalate by a known method to produce a ceramic green tape.

[0129] Thereafter, the ceramic green tape was punched into square pieces of 125 mm by a known method, and the carrier film was peeled off to produce ceramic green sheets.

[0130] <Process for producing an unsintered plate-shaped body>

[0131] An unsintered plate-shaped body is produced by stacking and pressing three ceramic green sheets.

[0132] <Process of preparing resin layer>

[0133] First, a resin powder, a binder, a dispersant, and an organic solvent are mixed in a predetermined ratio. As the resin powder, a cross-linked acrylic resin having a median particle size D 50The resin powder was spherical and had a particle size of 5 μm. A mixture of toluene and ethanol (weight ratio 7:3) was used as an organic solvent. The resulting mixture was stirred at 1000 rpm for 3 hours with a medium composed of partially stabilized zirconium oxide to prepare a resin slurry.

[0134] Next, the obtained resin slurry is tape-formed on one main surface of a carrier film made of polyethylene terephthalate by a known method to produce a resin tape.

[0135] Then, the resin tape is punched out into the same shape as the ceramic green sheet by a known method, and the carrier film is peeled off to prepare a resin sheet as a resin layer. The thickness of the resin layer after drying is 10 μm to 18 μm.

[0136] <Process for producing unsintered body>

[0137] First, a laminated body block is produced by laminating an unsintered plate-like body and a resin layer. More specifically, a laminated body block is produced by laminating a resin layer on two main surfaces, one main surface and the other main surface of the unsintered plate-like body.

[0138] Next, the laminated body block is placed in a mold and sandwiched between a first mold member and a second mold member to produce an assembly. The assembly is then placed in a resin bag and vacuum-sealed.

[0139] Next, the assembly was immersed in 50°C water in a pressure vessel, and the temperature of the laminated body block was maintained at 50°C for 2 minutes. Thus, the unsintered plate-like body and the resin layer were preheated at 50°C for 2 minutes. Then, a pressure of 1200 kgf / cm was applied to the mold through the laminated body block by applying pressure to the water with a pump. 2 The unsintered plate-like body and the resin layer were pressurized by hydrostatic pressing at a hydrostatic pressure of 120 MPa. The pressing temperature was the same as the preheating temperature, 50°C.

[0140] The unsintered body is then cut into a shape calculated by back-calculating the heat shrinkage of the unsintered plate body assumed during the calcination of the unsintered body described later and the target shape of the ceramic plate body to be obtained later.

[0141] <Process of manufacturing ceramic plate body>

[0142] The unsintered body was calcined in a calcining furnace as follows. First, the unsintered body was subjected to a degreasing treatment at 400°C for a predetermined time. Then, the degreasing unsintered body was subjected to a sintering treatment at 1400°C for 5 hours. By calcining the unsintered body as above, the resin layer was burned out, and the unsintered plate-like body was sintered to produce a ceramic plate-like body. The thickness of the obtained ceramic plate-like body was 90 μm.

[0143] Through the above operations, the electrolyte sheet (ceramic plate-like body) of Example 1 was manufactured.

[0144] [Example 2]

[0145] The electrolyte sheet of Example 2 was produced in the same manner as the electrolyte sheet of Example 1, except that the preheating temperature and the pressing temperature in the step of producing the green body were changed to 60°C.

[0146] [Example 3]

[0147] The electrolyte sheet of Example 3 was produced in the same manner as the electrolyte sheet of Example 1, except that the preheating temperature and the pressing temperature in the step of producing the green body were changed to 70°C.

[0148] [Example 4]

[0149] The electrolyte sheet of Example 4 was produced in the same manner as the electrolyte sheet of Example 1, except that the preheating temperature and the pressing temperature in the step of producing the green body were changed to 90°C.

[0150] [Example 5]

[0151] The electrolyte sheet of Example 5 was produced in the same manner as the electrolyte sheet of Example 1, except that the preheating time in the step of producing the green body was changed to 5 minutes.

[0152] [Example 6]

[0153] The electrolyte sheet of Example 6 was produced in the same manner as the electrolyte sheet of Example 5, except that the preheating temperature and the pressing temperature in the step of producing the green body were changed to 60°C.

[0154] [Example 7]

[0155] The electrolyte sheet of Example 7 was produced in the same manner as the electrolyte sheet of Example 5, except that the preheating temperature and the pressing temperature in the step of producing the green body were changed to 70°C.

[0156] [Example 8]

[0157] The electrolyte sheet of Example 8 was produced in the same manner as the electrolyte sheet of Example 5, except that the preheating temperature and the pressing temperature in the step of producing the green body were changed to 90°C.

[0158] [Example 9]

[0159] The electrolyte sheet of Example 9 was produced in the same manner as the electrolyte sheet of Example 1, except that the preheating time in the step of producing the green body was changed to 10 minutes.

[0160] [Example 10]

[0161] The electrolyte sheet of Example 10 was produced in the same manner as the electrolyte sheet of Example 9, except that the preheating temperature and the pressing temperature in the step of producing the green body were changed to 60°C.

[0162] [Example 11]

[0163] The electrolyte sheet of Example 11 was produced in the same manner as the electrolyte sheet of Example 9 except that the preheating temperature and the pressing temperature in the step of producing the green body were changed to 70°C.

[0164] [Example 12]

[0165] The electrolyte sheet of Example 12 was produced in the same manner as the electrolyte sheet of Example 9, except that the preheating temperature and the pressing temperature in the step of producing the green body were changed to 90°C.

[0166] [Comparative Example 1]

[0167] The electrolyte sheet of Comparative Example 1 was produced in the same manner as the electrolyte sheet of Example 1 except that the following conditions were changed.

[0168] The step of forming the resin layer is omitted.

[0169] In the step of producing the green body, the green plate-like body and a 100 g porous ceramic separator provided on one main surface of the green plate-like body are pressurized to produce the green body.

[0170] [Comparative Example 2]

[0171] The electrolyte sheet of Comparative Example 2 was produced in the same manner as the electrolyte sheet of Comparative Example 1, except that the preheating temperature and the pressing temperature in the step of producing the green body were changed to 60°C.

[0172] [Comparative Example 3]

[0173] The electrolyte sheet of Comparative Example 3 was produced in the same manner as the electrolyte sheet of Comparative Example 1, except that the preheating temperature and the pressing temperature in the step of producing the green body were changed to 70°C.

[0174] [Comparative Example 4]

[0175] The electrolyte sheet of Comparative Example 4 was produced in the same manner as the electrolyte sheet of Comparative Example 1, except that the preheating temperature and the pressing temperature in the step of producing the green body were changed to 90°C.

[0176] [Comparative Example 5]

[0177] The electrolyte sheet of Comparative Example 5 was produced in the same manner as the electrolyte sheet of Comparative Example 1, except that the preheating time in the step of producing the green body was changed to 5 minutes.

[0178] [Comparative Example 6]

[0179] The electrolyte sheet of Comparative Example 6 was produced in the same manner as the electrolyte sheet of Comparative Example 5, except that the preheating temperature and the pressing temperature in the step of producing the green body were changed to 60°C.

[0180] [Comparative Example 7]

[0181] The electrolyte sheet of Comparative Example 7 was produced in the same manner as the electrolyte sheet of Comparative Example 5, except that the preheating temperature and the pressing temperature in the step of producing the green body were changed to 70°C.

[0182] [Comparative Example 8]

[0183] The electrolyte sheet of Comparative Example 8 was produced in the same manner as the electrolyte sheet of Comparative Example 5, except that the preheating temperature and the pressing temperature in the step of producing the green body were changed to 90°C.

[0184] [Comparative Example 9]

[0185] The electrolyte sheet of Comparative Example 9 was produced in the same manner as the electrolyte sheet of Comparative Example 1, except that the preheating time in the step of producing the green body was changed to 10 minutes.

[0186] [Comparative Example 10]

[0187] The electrolyte sheet of Comparative Example 10 was produced in the same manner as the electrolyte sheet of Comparative Example 9, except that the preheating temperature and the pressing temperature in the step of producing the green body were changed to 60°C.

[0188] [Comparative Example 11]

[0189] The electrolyte sheet of Comparative Example 11 was produced in the same manner as the electrolyte sheet of Comparative Example 9, except that the preheating temperature and the pressing temperature in the step of producing the green body were changed to 70°C.

[0190] [Comparative Example 12]

[0191] The electrolyte sheet of Comparative Example 12 was produced in the same manner as the electrolyte sheet of Comparative Example 9, except that the preheating temperature and the pressing temperature in the step of producing the green body were changed to 90°C.

[0192] [Comparative Example 13]

[0193] The electrolyte sheet of Comparative Example 13 was produced in the same manner as the electrolyte sheet of Example 1, except that the pressurizing method in the step of producing the green body was changed to uniaxial pressing (without preheating).

[0194] [Comparative Example 14]

[0195] The electrolyte sheet of Comparative Example 14 was produced in the same manner as the electrolyte sheet of Comparative Example 13 except that the following conditions were changed.

[0196] The step of forming the resin layer is omitted.

[0197] In the step of producing the green body, the green plate-like body and a 100 g porous ceramic separator provided on one main surface of the green plate-like body are pressurized to produce the green body.

[0198] [evaluate]

[0199] The electrolyte sheets of Examples 1 to 12 and Comparative Examples 1 to 14 were evaluated as follows.

[0200] <Deformation degree>

[0201] For the electrolyte sheets of Examples 1 to 12 and Comparative Examples 1 to 14, the above method was used to calculate "100 × Q / L X ”, “100×R / L Y ” and “100×S / L X ", and the degree of deformation was evaluated. The results are shown in Tables 1 and 2. It should be noted that the judgment criteria are as follows.

[0202] ○: "100×Q / L X ”, “100×R / L Y ” and “100×S / L X " is less than 0.5.

[0203] △: "100×Q / L X ”, “100×R / L Y ” and “100×S / L X " is greater than 0.5 and less than 1.

[0204] ×: "100×Q / L X ”, “100×R / L Y ” and “100×S / L X The maximum value in " is greater than 1.

[0205] <Degree of warping>

[0206] The warping heights of the electrolyte sheets of Examples 1 to 12 and Comparative Examples 1 to 14 were measured by the above-mentioned method to evaluate the warping degrees. The results are shown in Tables 1 and 2. The evaluation criteria are as follows.

[0207] ○: The warping height is 200 μm or less.

[0208] △: The warpage height is greater than 200 μm and less than 300 μm.

[0209] ×: The warpage height is larger than 300 μm.

[0210] Then, based on the evaluation results of the degree of deformation and the degree of warping of the electrolyte sheet, a comprehensive evaluation was performed according to the following criteria.

[0211] ○: The degree of deformation and the degree of warping were both ○.

[0212] △: One of the degree of deformation and the degree of warping is ○ or △, and the other is △.

[0213] ×: At least one of the degree of deformation and the degree of warping is ×.

[0214] [Table 1]

[0215]

[0216] [Table 2]

[0217]

[0218] As shown in Table 1, the electrolyte sheets of Examples 1 to 12 were both suppressed in deformation and warping, and had high comprehensive evaluations. In particular, the electrolyte sheets of Examples 6 to 8 and 10 to 12 were manufactured at a preheating temperature of 60° C. or higher and less than 100° C. and a preheating time of 5 minutes or longer in the process of manufacturing the unsintered body, and therefore had high comprehensive evaluations compared to the electrolyte sheets of Examples 1 to 5 and 9.

[0219] As shown in Table 2, in the electrolyte sheets of Comparative Examples 1 to 14, deformation and warping were not suppressed, and the comprehensive evaluation was low.

[0220] Explanation of symbols

[0221] 1g Ceramic Green Sheet

[0222] 1s Unsintered plate

[0223] 1t Ceramic Green Tape

[0224] 2b Resin powder

[0225] 2e Resin layer

[0226] 2t resin belt

[0227] 10.130 Electrolyte sheet for solid oxide fuel cell (electrolyte sheet)

[0228] 10b Laminated Block

[0229] 10g unsintered body

[0230] 10p Ceramic plate

[0231] 20 Mould

[0232] 21. The first mold component

[0233] 22. Second mold component

[0234] 30 Assembly

[0235] 40 bags

[0236] 50 Pressure Vessel

[0237] 60 Water

[0238] 70 Pumps

[0239] 100 Single cell for solid oxide fuel cell (single cell)

[0240] 110 Fuel electrode

[0241] 120 Air Electrode

[0242] C1 1st corner

[0243] C2 2nd corner

[0244] C3 3rd corner

[0245] C4 4th corner

[0246] D1 Side 1

[0247] D2 Side 2

[0248] D3 3rd side

[0249] D4 4th side

[0250] L X The length of the virtual rectangle in the X-axis direction

[0251] L Y The length of the virtual rectangle in the Y-axis direction

[0252] P1 The intersection of the first virtual straight line and the second virtual straight line

[0253] P2 The intersection of the second virtual straight line and the third virtual straight line

[0254] P3 The intersection of the 3rd virtual straight line and the 4th virtual straight line

[0255] P4 The intersection of the 4th virtual straight line and the 1st virtual straight line

[0256] Q The maximum value of the difference between the X coordinates of the second side and the second virtual line

[0257] R The maximum value of the difference between the Y coordinates of the third side and the third virtual line

[0258] S The maximum value of the difference between the X coordinates of the 4th side and the 4th virtual line

[0259] V1 1st virtual straight line

[0260] V2 2nd virtual straight line

[0261] V3 3rd virtual straight line

[0262] V4 4th virtual straight line

[0263] X Casting Direction

[0264] Y Direction perpendicular to the casting direction.

Claims

1. An electrolyte sheet for a solid oxide fuel cell, characterized in that: The warpage height is less than 300μm. When viewed from above in the thickness direction, the shape is surrounded by a first side, a second side adjacent to the first side via a first corner, a third side adjacent to the second side via a second corner, and a fourth side adjacent to the third side via a third corner and adjacent to the first side via a fourth corner, arranged in clockwise order. When viewed from above in the thickness direction, a first virtual straight line approximated by 10 points on the first side is set as the X-axis, a second virtual straight line passing through a point having an average value of the X coordinates of the 10 points on the second side as the X coordinate and being orthogonal to the first virtual straight line is set as the Y-axis, and an intersection point of the first virtual straight line and the second virtual straight line is set as the virtual origin in an XY coordinate system, a third virtual straight line passing through a point having an average value of the Y coordinates of the 10 points on the third side as the Y coordinate and being parallel to the first virtual straight line and a second virtual straight line passing through a point having an average value of the Y coordinates of the 10 points on the fourth side as the Y coordinate are defined. When a fourth virtual straight line orthogonal to the first virtual straight line is selected as a point with an average value of the X coordinates of the ten points on the first virtual straight line, if the maximum value of the difference between the X coordinates of the second side and the second virtual straight line is set to Q, the maximum value of the difference between the Y coordinates of the third side and the third virtual straight line is set to R, the maximum value of the difference between the X coordinates of the fourth side and the fourth virtual straight line is set to S, and the length of the virtual rectangle enclosed by the first virtual straight line, the second virtual straight line, the third virtual straight line and the fourth virtual straight line in the X-axis direction is set to L X , the length of the virtual rectangle in the Y-axis direction is set to L Y , then 100×Q / L X , 100×R / L Y and 100×S / L X The maximum value in is less than 1.

2. The electrolyte sheet for a solid oxide fuel cell according to claim 1, which is composed of a ceramic plate-like body including a sintered body of scandia-stabilized zirconia.

3. The electrolyte sheet for a solid oxide fuel cell according to claim 1 or 2, wherein: Concave portions are scattered on at least one of the one main surface and the other main surface.

4. A method for producing an electrolyte sheet for a solid oxide fuel cell, characterized in that: have: a step of producing an unsintered body by pressing an unsintered plate-like body containing ceramic material powder and a resin layer containing resin powder, A step of manufacturing a ceramic plate-like body by calcining the unsintered body to burn out the resin layer and sinter the unsintered plate-like body; In the step of manufacturing the green body, the green plate-shaped body and the resin layer are pressurized by hydrostatic pressing.

5. The method for producing an electrolyte sheet for a solid oxide fuel cell according to claim 4, wherein: In the step of producing the green body, the green plate-shaped body and the resin layer are preheated at 60° C. or higher and lower than 100° C. for 5 minutes or more before being pressurized by hydrostatic pressing.

6. The method for producing an electrolyte sheet for a solid oxide fuel cell according to claim 4 or 5, wherein: The ceramic material powder contains scandia-stabilized zirconia powder.

7. A single cell for a solid oxide fuel cell, characterized in that: Equipped with: fuel electrode, Air pole, and An electrolyte sheet for a solid oxide fuel cell according to any one of claims 1 to 3, disposed between the fuel electrode and the air electrode.