A method for manufacturing a perovskite film, a solar cell and a stacked cell

By forming a metal halide skeleton layer in perovskite-silicon-based stacked solar cells, the problems of incomplete deposition of perovskite layer and poor film formation quality are solved, and the complete coverage and uniform reaction of perovskite layer are achieved, thereby improving the battery efficiency and quality.

CN114335359BActive Publication Date: 2024-11-15LONGI SOLAR TECH (XIAN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111461110.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-30
Publication Date
2024-11-15
Estimated Expiration
2041-11-30

AI Technical Summary

Technical Problem

In perovskite-silicon-based stacked solar cells, perovskite layers are easily deposited at the bottom of the suede structure when preparing the solution method, resulting in a battery short circuit. It is difficult for organic components to react with dense inorganic components in vacuum evaporation. This leads to poor film formation quality.

Method used

The metal halide skeleton layer is formed on the base of the suede structure, covering the suede structure in a conformal manner, and forming a perovskite light absorbing layer on it. The metal halide skeleton layer plays an anchoring role to ensure the perovskite layer Completely cover and react completely with the organic components to improve the film formation quality.

Benefits of technology

The short circuit phenomenon is avoided, the trapping effect and anti-reaction effect of the suede structure are ensured, the uniformity of the perovskite light absorption layer and the film formation quality are improved, and the power generation efficiency of the stacked battery is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114335359B_ABST
    Figure CN114335359B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for manufacturing a perovskite film, a solar cell and a stacked cell, and relates to the field of photovoltaic technology, in order to solve the problem that when a perovskite layer is prepared by a solution method in the prior art, the perovskite solution will be deposited at the bottom of a velvet structure, resulting in a short circuit in the battery, and the problem that organic components are difficult to react with dense inorganic components in a vacuum evaporation method. The method for manufacturing the perovskite film comprises: providing a substrate, the surface of the substrate having a velvet structure; forming a metal halide skeleton layer on the substrate having the velvet structure, the metal halide skeleton layer conformally covering the velvet structure; and conformally forming a perovskite light absorption layer on the metal halide skeleton layer having the velvet structure. The method for manufacturing the perovskite film provided by the present invention is used for manufacturing solar cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of photovoltaic technology, and in particular to a method for manufacturing a perovskite film, a solar cell and a stacked cell. Background Art

[0002] Tandem solar cells are solar cells formed by connecting a top cell with a wide bandgap and a bottom cell with a narrow bandgap in series. Compared with single-junction solar cells, tandem solar cells make more comprehensive use of the energy of photons and are therefore more efficient.

[0003] At present, in perovskite-silicon-based stacked solar cells, the commonly used methods for making perovskite layers are solution method and vacuum evaporation method. The perovskite layer prepared by solution method on the velvet structure is easy to deposit to the bottom of the velvet structure, resulting in the failure to completely cover the top of the velvet structure, making it difficult to form a complete perovskite film, and then short circuit phenomenon occurs. The vacuum evaporation method is generally carried out in two steps. First, a layer of lead iodide of about 400nm is evaporated on the velvet structure of the silicon substrate, and then the organic component is coated on the lead iodide layer. The formed lead iodide layer is too dense, and it is difficult for the organic component to react with the internal lead iodide, resulting in a large amount of residual lead iodide and poor film quality of the perovskite layer. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a perovskite film, a solar cell and a stacked cell, which solves the problem in the prior art that when a perovskite layer is prepared by a solution method, the perovskite solution is deposited at the bottom of a velvet structure, causing a short circuit in the battery, and the problem that organic components are difficult to react with dense inorganic components in a vacuum evaporation method.

[0005] In a first aspect, the present invention provides a method for preparing a perovskite film, comprising:

[0006] Providing a substrate, wherein the surface of the substrate has a suede structure;

[0007] forming a metal halide skeleton layer on the substrate having a suede structure, wherein the metal halide skeleton layer conformally covers the suede structure;

[0008] A perovskite light absorption layer is conformally formed on the metal halide skeleton layer with a velvet structure.

[0009] In the case of adopting the above technical scheme, a metal halide skeleton layer that can conformally cover the velvet structure is formed on the substrate with a velvet structure, and then a perovskite light absorption layer is conformally formed on the metal halide skeleton layer with the velvet structure. The formed metal halide skeleton layer plays an anchoring role, so that the subsequently formed perovskite light absorption layer can form a layer of perovskite film along with the ups and downs of the velvet structure. Compared with the prior art, the perovskite light absorption layer prepared by the method for making a perovskite film provided by the present invention not only completely covers the entire velvet structure, avoiding the occurrence of short circuit phenomenon, but also conformally fits on the velvet structure, ensuring the good light trapping effect and anti-reflection effect of the velvet structure. In addition, in the method for making a perovskite film provided by the present invention, the metal halide skeleton layer formed first can completely react with the organic component when the perovskite component is formed later, so that the components of the formed perovskite light absorption layer are uniform, thereby improving the film formation quality.

[0010] In a possible implementation, the thickness of the metal halide ore skeleton layer is in the range of 5 nm to 15 nm.

[0011] When the above technical solution is adopted, compared with the prior art, the thickness of the metal halide skeleton layer in the present invention is only 5nm-15nm. When reacting with the organic component later, the extremely thin metal halide skeleton layer can be directly penetrated by the organic component solution and react completely with it, thereby avoiding the problem that the existing lead iodide layer with a thickness of several hundred nanometers is too dense when reacting with the organic amine component, so that the lead iodide inside is difficult to participate in the reaction and remains, thereby making the final perovskite light absorption layer have better film quality.

[0012] In a possible implementation, forming a metal halide skeleton layer on the substrate having a velvet structure includes: evaporating metal halide on the substrate having a velvet structure to form the metal halide skeleton layer.

[0013] In the case of adopting the above technical solution, a thin layer of metal halide can be evaporated on the substrate with a velvet structure to form a metal halide skeleton layer. The metal halide skeleton layer formed by pre-evaporation is equivalent to a seed layer, which completely covers the pyramid, making it easy for the subsequent perovskite light absorption layer to form a film on the velvet structure, avoiding the phenomenon of incomplete coverage of the velvet structure and battery short circuit caused by directly using a one-step solution method in the prior art. In addition, the metal halide skeleton layer prepared by vacuum evaporation technology can be evenly attached to the velvet structure.

[0014] In a possible implementation, the metal halide is at least one of lead halide, cesium halide and rubidium halide.

[0015] In the case of adopting the above technical solution, the formed metal halide skeleton layer can be composed of one of lead halide, cesium halide and rubidium halide, or a combination of lead halide, cesium halide and rubidium halide. Metal halide can provide inorganic components for the perovskite light absorption layer as one of the raw materials for formation, and cesium halide and / or rubidium halide are co-evaporated with lead halide to form a metal halide skeleton layer, and the formed perovskite light absorption layer can be bandgap adjusted to facilitate the bandgap matching of the bottom battery when the formed perovskite film is used in a stacked battery. The halogen element in the metal halide can be at least one of iodine, chlorine and bromine, so the metal halide can include at least one of lead iodide, lead chloride, lead bromide, cesium iodide, cesium bromide, cesium chloride and rubidium iodide.

[0016] In a possible implementation, the metal halide is a mixture of lead halide and cesium halide, and the molar ratio of lead halide to cesium halide is 2:0.1-2:1.

[0017] In the case of adopting the above technical solution, when the metal halide is a combination mixture of lead halide and cesium halide, the molar ratio between the lead halide and the cesium halide can be 2:0.1-2:1. Lead halide and cesium halide within this molar ratio range can play a better role in band gap adjustment to obtain a battery with a wider adjustable band gap range. Among them, the halogen elements in the cesium halide and the lead halide can be at least one of iodine, bromine and chlorine.

[0018] In a possible implementation, conformally forming a perovskite light absorption layer on a metal halide skeleton layer includes:

[0019] A perovskite precursor solution is coated on the metal halide skeleton layer with a velvet structure by a solution method to form a perovskite light absorption layer.

[0020] In the case of adopting the above technical solution, a perovskite precursor solution is coated on a metal halide skeleton layer with a velvet structure by a one-step solution method to form a perovskite light absorption layer. The coated perovskite precursor solution will contact and react with the pre-evaporated metal halide skeleton layer, nucleate and crystallize at the position of the metal halide skeleton layer to form a perovskite component. Based on this, the perovskite light absorption layer prepared by the one-step solution method will be distributed at the pre-evaporated metal halide skeleton layer, replacing the position of the metal halide skeleton layer, completely covering the entire substrate, and conforming to the velvet structure, solving the problem of short circuit of the battery device caused by the perovskite precursor solution directly depositing to the bottom of the valley, exposing the top of the velvet structure when the perovskite light absorption layer is prepared by the solution method in the prior art.

[0021] In a possible implementation, the solute of the perovskite precursor solution is an ABX3 type structure, wherein A is a ternary mixed cation comprising Cs, FA and MA, B is a metal cation comprising Pb, and X is an anion comprising I and Br. The solvent of the perovskite precursor solution comprises one or more of N,N-dimethylformamide, dimethyl sulfoxide, N-methylpyrrolidone and acetonitrile.

[0022] In the case of adopting the above technical solution, the formed perovskite light absorption layer is an ABX3 structure, wherein A is a ternary mixed cation including Cs, FA and MA, B is a metal cation including Pb, and can also be a metal cation including Sn, and X is a mixed anion including I and Br. When the perovskite precursor solution is coated on the metal halide skeleton, the organic component reacts with the metal halide to generate a perovskite component. In order to prevent incomplete reaction, an excess of metal halide as an inorganic component can be added. In the method for making the perovskite film provided by the present invention, the band gap width of the perovskite light absorption layer can be adjusted by adjusting the ratio of Cs and Br in the perovskite component, so that when the present invention is applied in a stacked battery, a band gap matching the bottom battery can be obtained, thereby obtaining a stacked battery with higher efficiency, solving the problem of difficult band gap adjustment in the two-step evaporation method in the prior art. When adjusting the band gap, the larger the radius of the A-site ion, the smaller the band gap; the larger the radius of the X-site ion, the smaller the band gap. Especially in the mixed halide system, the band gap gradually widens with the increase of bromide ion content.

[0023] In one possible implementation, the band gap of the perovskite precursor solution is in the range of 1.5 eV-1.8 eV.

[0024] When the above technical solution is adopted, the band gap of the formed perovskite light absorption layer can also be adjusted, and the adjustment range is between 1.5eV-1.8eV. When the perovskite film method provided by the present invention is applied to a tandem battery, the band gap of the perovskite light absorption layer can be adjusted within this range according to the band gap of the bottom battery, so as to better utilize solar energy and make the manufactured tandem battery more efficient in generating electricity.

[0025] In a possible implementation, the thickness of the perovskite light absorption layer is 350nm-500nm. The perovskite light absorption layer is prepared by using a perovskite precursor solution with an ABX3-type structure as a solute on a thin metal halide ore skeleton layer. The thickness of the perovskite light absorption layer is between 350nm-500nm, which is equivalent to the perovskite light absorption layer prepared by a one-step method, with controllable components and high quality of the perovskite light absorption layer.

[0026] In a second aspect, the present invention further provides a solar cell, which is prepared by the above-mentioned method for preparing a perovskite thin film, and the solar cell comprises: a substrate, the substrate having a velvet structure; a metal halide skeleton layer, conformally covered on the substrate having the velvet structure; and a perovskite light absorption layer, conformally formed on the metal halide skeleton layer having the velvet structure.

[0027] The beneficial effects of the solar cell provided in the second aspect are the same as the beneficial effects of the method for manufacturing a perovskite film described in the first aspect or any possible implementation of the first aspect, and are not described in detail here.

[0028] In a third aspect, the present invention also provides a stacked battery, which is prepared by the above-mentioned method for making a perovskite film, and the stacked battery includes: a substrate, a silicon substrate battery with a velvet structure, a first transparent conductive layer, and a first carrier transport layer stacked in sequence on the substrate. A metal halide skeleton layer, conformally covered on the first carrier transport layer with a velvet structure. A perovskite light absorption layer, conformally formed on the metal halide skeleton layer with a velvet structure. A second carrier transport layer, a second transparent conductive layer, and an electrode are sequentially formed on the perovskite light absorption layer.

[0029] The beneficial effects of the stacked battery provided in the third aspect are the same as the beneficial effects of the method for manufacturing the perovskite film described in the first aspect or any possible implementation of the first aspect, and are not described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0031] Figure 1 It is a schematic diagram of a perovskite light absorption layer prepared by a solution method in the prior art;

[0032] Figure 2 This is a surface SEM image of a perovskite light absorption layer prepared by a solution method in the prior art;

[0033] Figure 3 This is a cross-sectional SEM image of a perovskite light absorption layer prepared by a solution method in the prior art;

[0034] Figure 4 is a schematic diagram of a perovskite light absorption layer prepared in an embodiment of the present invention;

[0035] Figure 5 This is a surface SEM image of the perovskite light absorption layer prepared in an embodiment of the present invention;

[0036] Figure 6 This is a cross-sectional SEM image of a perovskite light absorbing layer prepared in an embodiment of the present invention;

[0037] Figure 7 A schematic diagram of a stacked battery in an embodiment of the present invention;

[0038] Figure 8 A schematic diagram of a stacked battery with a formal structure in an embodiment of the present invention;

[0039] Fig. 9 Schematic diagram of a stacked battery with a trans-structure in an embodiment of the present invention.

[0040] Reference numerals:

[0041] 100-perovskite top cell, 200-intermediate carrier exchange layer, 300-silicon base cell, 400-first photoelectric transmission layer, 401-second photoelectric transmission layer, 500-electron transmission layer, 501-hole transmission layer, 101-perovskite light absorption layer. DETAILED DESCRIPTION

[0042] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0043] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it can be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element.

[0044] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. The meaning of "several" is one or more, unless otherwise clearly and specifically defined.

[0045] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by the terms "up", "down", "front", "back", "left", "right", etc. are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the present invention.

[0046] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0047] The development of solar cells for clean and renewable energy is driven by the reduction of the levelized cost of energy (LCOE). Improving the power conversion efficiency (PCE) of solar panels can not only generate more electricity, but also reduce related costs such as transportation, installation, land use, etc., which helps to reduce LCOE. Silicon-based solar cells dominate the terrestrial solar panel market with an average PCE of about 20%. The record cell efficiency is close to the SQ limit (Shockley-Quiesser limit) of single-junction solar cells. Thin-film solar cells based on copper indium gallium selenide (CIGS) and cadmium telluride (CdTe) have also developed rapidly in the past 20 years. However, due to the sub-bandgap absorption loss and thermal relaxation loss of hot carriers, the PCE of single-junction solar cells cannot exceed the SQ limit. Integrating a low-cost, high-efficiency wide-bandgap top solar cell with a low-bandgap (e.g., Si, CIGS, CdTe, etc.) bottom solar cell to form a tandem solar cell is more efficient than a single-junction solar cell because it can better utilize the energy of short-wave photons in the sunlight spectrum. The top cell composed of a high-bandgap semiconductor generates photocurrent from the short-wave portion of the solar spectrum at a high voltage. Longer wavelength light, exceeding the bandgap of the top cell, is transmitted to the bottom cell composed of a low-bandgap semiconductor with a wide absorption coefficient. The efficiency potential of tandem cells makes them the most likely candidate for continued significant price reductions of photovoltaic modules in the coming decades.

[0048] like Figure 1-Figure 3 As shown, at present, when the solution method is used to prepare stacked batteries, the perovskite is spin-coated on the velvet surface and easily deposited to the bottom of the pyramid valley and accumulated at the bottom of the valley, resulting in failure to completely cover the pyramid tip, making it difficult to form a complete perovskite film. The exposed pyramid causes the prepared battery to short-circuit, and the prepared battery has low efficiency.

[0049] When preparing stacked cells by a two-step evaporation method, a 400nm thick lead iodide layer is usually first evaporated on the substrate to introduce inorganic components, and then organic components are introduced by spin coating, such as formamidine hydroiodide (FAI), methylamine hydrobromide (MABr), methylammonium chloride (MACl), etc. In the second step, when the organic component solution is spin-coated, the evaporated lead iodide layer is too dense, and it is difficult for the organic component solution to penetrate into the lead iodide layer. The organic cations do not fully participate in the reaction, resulting in a large amount of residual lead iodide and poor film quality of the perovskite layer.

[0050] like Figure 4-Figure 6 As shown, in order to solve the above technical problems, an embodiment of the present invention provides a method for manufacturing a perovskite film, comprising the following steps:

[0051] Step S100, providing a substrate, wherein the surface of the substrate has a suede structure;

[0052] Step S200, forming a metal halide skeleton layer on the substrate having a suede structure, wherein the metal halide skeleton layer conformally covers the suede structure;

[0053] Step S300 , conformally forming a perovskite light absorbing layer 101 on the metal halide skeleton layer having a suede structure.

[0054] Based on this, Figure 4-Figure 6 As shown, a metal halide skeleton layer that can conformally cover the velvet structure is formed on a substrate having a velvet structure, and then a perovskite light absorption layer 101 is conformally formed on the metal halide skeleton layer having the velvet structure. The formed metal halide skeleton layer plays an anchoring role, so that the subsequently formed perovskite light absorption layer 101 can form a layer of perovskite film along with the undulations of the velvet structure. Compared with the prior art, the perovskite light absorption layer 101 prepared by the method for making a perovskite film provided in an embodiment of the present invention not only completely covers the entire velvet structure, avoiding the occurrence of short circuits, but also conforms to the velvet structure, ensuring the good light trapping effect and anti-reflection effect of the velvet structure. In addition, in the method for making a perovskite film provided in an embodiment of the present invention, the metal halide skeleton layer formed first can completely react with the organic component when the perovskite component is formed later, so that the components of the formed perovskite light absorption layer 101 are uniform, thereby improving the film formation quality.

[0055] As a possible implementation, Figure 4-Figure 6 As shown, the thickness of the metal halide mineral skeleton layer ranges from 5nm to 15nm.

[0056] Compared with the lead iodide layer with a thickness of several hundred nanometers required for the two-step evaporation method in the prior art, the thickness of the metal halide skeleton layer in the embodiment of the present invention is only 5nm-15nm. When reacting with the organic component later, the extremely thin metal halide skeleton layer can be directly penetrated by the organic component solution and react completely with it, thereby avoiding the problem that the existing lead iodide layer with a thickness of several hundred nanometers is too dense when reacting with the organic amine component, so that the lead iodide inside is difficult to participate in the reaction and remains, so that the finally formed perovskite light absorption layer 101 has better film quality, and can form a dense and smooth perovskite film to completely cover the suede structure.

[0057] As a possible implementation manner, forming a metal halide skeleton layer on the substrate having a velvet structure includes: evaporating metal halide on the substrate having a velvet structure to form the metal halide skeleton layer.

[0058] Based on this, a thin layer of metal halide can be evaporated on the substrate with a velvet structure to form a metal halide skeleton layer. The metal halide skeleton layer formed by pre-evaporation is equivalent to a seed layer, which completely covers the pyramid, making it easier for the subsequent perovskite light absorption layer 101 to form a film on the velvet structure, thereby avoiding the incomplete coverage of the velvet structure and the occurrence of battery short circuits caused by the direct use of a one-step solution method in the prior art. In addition, the metal halide skeleton layer prepared by vacuum evaporation technology can be evenly attached to the velvet structure.

[0059] As a possible implementation manner, the metal halide is at least one of lead halide, cesium halide and rubidium halide.

[0060] Based on this, the formed metal halide skeleton layer can be composed of one of lead halide, cesium halide and rubidium halide, or a combination of lead halide, cesium halide and rubidium halide. Metal halide can provide inorganic components for the perovskite light absorbing layer 101 as one of the raw materials for formation, and cesium halide and / or rubidium halide are co-evaporated with lead halide to form a metal halide skeleton layer, and the formed perovskite light absorbing layer 101 can be bandgap adjusted to facilitate the bandgap matching of the bottom battery when the formed perovskite film is used in a stacked battery. The halogen element in the metal halide can be at least one of iodine, chlorine and bromine, so the metal halide can include at least one of lead iodide, lead chloride, lead bromide, cesium iodide, cesium bromide, cesium chloride and rubidium iodide.

[0061] In some examples, preferably, the metal halide is lead iodide, and a layer of lead iodide is directly evaporated as the metal halide skeleton layer during evaporation. Of course, other metal halides, such as lead bromide, cesium iodide, cesium bromide, etc., can also be used as raw materials for the metal halide skeleton layer.

[0062] In some examples, in addition to the above-mentioned halides, metal halides can also be selected to react with the perovskite precursor solution and other similar materials to be pre-evaporated on the substrate, which can also obtain the same efficiency gain. The material must have lateral conductivity, surface roughness, and compatibility with the perovskite preparation process, and cannot affect the transport of carriers in the device. For example, potassium salts such as potassium iodide (KI), after reacting with the perovskite precursor solution, can inhibit the hysteresis effect unique to perovskite cells.

[0063] As a possible implementation, the metal halide is a mixture of lead halide and cesium halide, and the molar ratio of lead halide to cesium halide is 2:0.1-2:1.

[0064] Based on this, when the metal halide is a combination mixture of lead halide and cesium halide, the molar ratio between the lead halide and the cesium halide can be 2:0.1-2:1. Lead halide and cesium halide within this molar ratio range can play a better role in band gap adjustment to obtain a battery with a wider adjustable band gap range. Among them, the halogen elements in the cesium halide and the lead halide can be at least one of iodine, bromine and chlorine.

[0065] As a possible implementation manner, forming the perovskite light absorbing layer 101 on the metal halide skeleton layer includes: coating a perovskite precursor solution on the metal halide skeleton layer having a suede structure by a solution method to form the perovskite light absorbing layer 101 .

[0066] Based on this, a perovskite precursor solution is coated on a metal halide skeleton layer with a velvet structure by a one-step solution method to form a perovskite light absorbing layer 101. The coated perovskite precursor solution will contact and react with the pre-evaporated metal halide skeleton layer, nucleate and crystallize at the position of the metal halide skeleton layer to form a perovskite component. Based on this, the perovskite light absorbing layer 101 prepared by the one-step solution method will be distributed at the pre-evaporated metal halide skeleton layer, replacing the position of the metal halide skeleton layer, completely covering the entire substrate, and conforming to the velvet structure, solving the problem of short circuit of the battery device caused by the perovskite precursor solution directly depositing to the bottom of the valley, exposing the top of the velvet structure, when the perovskite light absorbing layer 101 is prepared by the solution method in the prior art.

[0067] In the current two-step vacuum evaporation method, there is still the problem of difficulty in band gap adjustment, which makes it difficult to match the band gap of the bottom cell when used in a stacked cell, and it is impossible to obtain a high-efficiency stacked cell.

[0068] As a possible implementation, the solute of the perovskite precursor solution is an ABX3 type structure, wherein A is a ternary mixed cation comprising Cs, FA and MA, B is a metal cation comprising Pb, and X is an anion comprising I and Br. The solvent of the perovskite precursor solution comprises one or more of N,N-dimethylformamide, dimethyl sulfoxide, N-methylpyrrolidone and acetonitrile.

[0069] Based on this, the formed perovskite light absorbing layer 101 is an ABX3 structure, wherein A is a ternary mixed cation including Cs, FA and MA, B is a metal cation including Pb, and can also be a metal cation including Sn, and X is a mixed anion including I and Br. When the perovskite precursor solution is coated on the metal halide skeleton, the organic component reacts with the metal halide to form a perovskite component. In order to prevent incomplete reaction, an excess of metal halide as an inorganic component can be added. In the method for making a perovskite film provided in an embodiment of the present invention, the band gap width of the perovskite light absorbing layer 101 can be adjusted by adjusting the ratio of Cs and Br in the perovskite component, so that when the embodiment of the present invention is applied in a stacked battery, a band gap matching the bottom battery can be obtained, thereby obtaining a stacked battery with higher efficiency, solving the problem of difficult band gap adjustment in the two-step evaporation method in the prior art. When adjusting the band gap, the larger the radius of the A-site ion, the smaller the band gap; the larger the radius of the X-site ion, the smaller the band gap. Especially in the mixed halide system, the band gap gradually widens with the increase of bromide ion content.

[0070] As a possible implementation, the band gap of the perovskite precursor solution is in the range of 1.5eV-1.8eV.

[0071] Based on this, the band gap of the formed perovskite light absorbing layer 101 can also be adjusted, and the adjustment range is between 1.5eV-1.8eV. When the method of the perovskite film provided by the embodiment of the present invention is applied to a tandem battery, the band gap of the perovskite light absorbing layer 101 can be adjusted within this range according to the band gap of the bottom battery, so as to better utilize solar energy and make the manufactured tandem battery more efficient in generating electricity.

[0072] As a possible implementation, the thickness of the perovskite light absorbing layer 101 is 350nm-500nm. The perovskite light absorbing layer 101 is prepared by using a perovskite precursor solution with an ABX3 type structure as a solute on a thin metal halide ore skeleton layer. The thickness of the perovskite light absorbing layer 101 is between 350nm-500nm, which is equivalent to the perovskite light absorbing layer 101 prepared by a one-step method, the components are controllable, and the quality of the perovskite light absorbing layer 101 is high.

[0073] The embodiment of the present invention further provides a solar cell, which is prepared by the above-mentioned method for preparing a perovskite thin film, and the solar cell comprises: a substrate having a velvet structure; a metal halide skeleton layer conformally covering the substrate having the velvet structure; and a perovskite light absorption layer 101 conformally formed on the metal halide skeleton layer having the velvet structure.

[0074] Compared with the prior art, the beneficial effects of the solar cell provided by the embodiment of the present invention are the same as the beneficial effects of the above-mentioned method for manufacturing the perovskite thin film, which will not be described in detail here.

[0075] like Figure 7 As shown, an embodiment of the present invention further provides a stacked battery, wherein the top battery is a perovskite battery prepared by the above-mentioned method for making a perovskite film, and the bottom battery is a silicon-based battery. The stacked battery includes: a substrate, a silicon substrate battery 300 with a velvet structure, a first transparent conductive layer, and a first carrier transport layer stacked in sequence on the substrate. A metal halide skeleton layer, conformally covering the first carrier transport layer with a velvet structure. A perovskite light absorption layer 101, conformally formed on the metal halide skeleton layer with a velvet structure. A second carrier transport layer, a second transparent conductive layer, and an electrode are sequentially formed on the perovskite light absorption layer 101.

[0076] Compared with the prior art, the beneficial effects of the stacked battery provided by the embodiment of the present invention are the same as the beneficial effects of the above-mentioned method for manufacturing the perovskite film, which will not be described in detail here.

[0077] As a possible implementation, Figure 7 As shown, the prepared stacked cell may be composed of a perovskite top cell 100 , an intermediate carrier exchange layer 200 , a silicon base cell 300 , a first photoelectric transmission layer 400 and a second photoelectric transmission layer 401 .

[0078] As a possible implementation, Figure 8 As shown, the prepared stacked cell can also be composed of a perovskite top cell 100, an intermediate carrier exchange layer 200, a silicon base cell 300, a first photoelectric transmission layer 400, a second photoelectric transmission layer 401, a first carrier transport layer and a second carrier transport layer. Figure 8 As shown, the first carrier can be an electron, and the second carrier can be a hole, that is, the first carrier transport layer is an electron transport layer 500, and the second carrier transport layer is a hole transport layer 501, at which time a perovskite-silicon-based stacked battery with a formal structure is formed.

[0079] In some examples, since the perovskite top cell 100 and the silicon base cell 300 are both symmetrical structures, Figure 8 The same enhancement effect can be achieved by inverting the battery structure shown. Fig. 9 As shown, the first carrier at this time may be a hole, and the second carrier may be an electron, that is, the first carrier transport layer is a hole transport layer 501, and the second carrier transport layer is an electron transport layer 500, and a perovskite-silicon-based stacked battery with an inverted structure is formed.

[0080] In some examples, the prepared stacked cell may also include a perovskite light absorption layer 101, a first transparent electrode, a second transparent electrode, a first passivation layer, a second passivation layer, a p-type amorphous silicon layer, an n-type amorphous silicon layer, a first transparent conductive layer, a second transparent conductive layer, a p-type doped microcrystalline silicon layer, and an n-type doped microcrystalline silicon layer, wherein the p-type amorphous silicon layer may serve as a back field structure of the stacked cell, and the n-type amorphous silicon layer may serve as a front emitter of the stacked cell; the p-type doped microcrystalline silicon layer and the n-type doped microcrystalline silicon layer may serve as tunneling layers to realize the transmission of carriers between the top cell and the bottom cell.

[0081] For example, in the perovskite-silicon based stacked cell, the silicon base cell 300 can use a commercial grade M2 ​​n-type silicon wafer as the substrate, the resistivity of the silicon wafer is 1Ω·cm-10Ω·cm, the thickness is 150um-200um, and other layers are prepared on it after undergoing polishing, texturing and cleaning procedures. The first passivation layer and the second passivation layer can both be intrinsic amorphous silicon passivation layers, with a thickness of 5nm-10nm. The phosphorus doping concentration of the p-type amorphous silicon layer can be 10 19 cm -3 -10 20 cm -3 , the boron doping concentration of the n-type amorphous silicon layer can be 10 19 cm -3 -10 20 cm -3 In addition, the back field structure can also be composed of n-type SiO x The concentration range of boron doping is the same as that of n-type amorphous silicon layer; n-type SiO x The thickness of the first transparent conductive layer, the n-type amorphous silicon layer and the p-type amorphous silicon layer are all 5nm-15nm. The materials selected for the first transparent conductive layer and the second transparent conductive layer can be any one of indium tin oxide (ITO), tungsten-doped indium oxide (IWO), titanium-doped indium oxide (ITiO) and hydrogenated indium oxide (IOH), and the thickness is 1nm-20nm. The doping concentration of phosphorus doping and the doping concentration of boron doping in the p-type doped microcrystalline silicon layer and the n-type doped microcrystalline silicon layer can be 10 19 cm -3 -10 21 cm -3, with a thickness of 1nm-10nm. The material selected for the hole transport layer 501 can be an organic transport layer material, such as 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Sprio-OMeTAD), tetrakis(di-p-tolylamino)spiro-9,9'-bifluorene (Spiro-TTB), 2,2',7,7'-tetrakis(diphenylamino)-9,9'-spirobifluorene (Sprio-TAD) or mannose trifluorosulfonate (TATM), etc., or an inorganic hole transport layer 501 material, such as molybdenum oxide (MoO x ), nickel oxide (NiO x ) or cuprous oxide (Cu2O), etc. The thickness of the hole transport layer 501 is 10nm-15nm. The perovskite light absorption layer 101 is responsible for absorbing incident photons and generating photogenerated carriers (holes-electrons). The components are generally MAPbI3, FAPbI3, (Cs 0.15 FA 0.85 )Pb(I 0.7 Br 0.3 )3 and other component systems, with a thickness of 350nm-500nm; the perovskite precursor solution is an ABX3 type structure, wherein the A position uses a ternary mixed cation of Cs, FA and MA, wherein the Cs content is preferably 5%; the B position is a Pb or Sn metal ion, preferably a Pb ion; the X position can use a mixed anion type of I and Br, and the ratio of I to Br is between 7:3 and 8:2; the solvent can be a mixed solvent of DMF and DMSO; in the process of coating the perovskite precursor solution, an anti-solvent can also be added for extraction treatment, and common anti-solvents include chlorobenzene, anisole or ethyl acetate. When preparing the electron transport layer 500, a layer of organic material, such as carbon 60 (C60) and fullerene derivatives (PCBM), can be first prepared on the aluminum oxide film by evaporation, and then an inorganic electron transport layer 500 material, such as tin oxide (SnO2) or titanium oxide (TiO2), can be prepared by atomic layer deposition (ALD) technology to achieve longitudinal transport of carriers; the thickness of the electron transport layer 500 is 10nm-20nm. The materials selected for the first transparent electrode and the second transparent electrode can be any one of indium tin oxide (ITO), tungsten-doped indium oxide (IWO), titanium-doped indium oxide (ITiO) and indium zinc oxide (IZO), with a thickness of 70nm-120nm, and can be prepared by magnetron sputtering to collect photogenerated carriers and transmit them to the back gate electrode; in particular, after the process of the intermediate carrier exchange layer 200 is completed, the first transparent electrode at the bottom can be prepared first, and after the process of the electron transport layer 500 is completed, the second transparent electrode at the top can be prepared by the same process.

[0082] When preparing a perovskite-silicon-based stacked cell, an n-type microcrystalline silicon layer can be first prepared on the silicon-based cell 300, followed by a 1-20 nm TCO layer as an intermediate layer, and then an n-type doped microcrystalline silicon layer, followed by a hole transport layer 501, a perovskite light absorption layer 101, an electron transport layer 500, and a first photoelectric transport layer 400 and a second photoelectric transport layer 401. Finally, the transparent electrode, the metal electrode, and the anti-reflection film layer are prepared to obtain a complete perovskite-silicon-based stacked cell.

[0083] In order to more fully illustrate the beneficial effects of the method for making a perovskite film provided by the embodiment of the present invention, the following is an illustration of the application of the method for making a perovskite film in a stacked battery. The following is an illustration by comparing the embodiment and the comparative example.

[0084] Embodiment 1

[0085] The application of the method for manufacturing the perovskite thin film provided in the embodiment of the present invention in the stacked battery is specifically described as follows:

[0086] In the first step, a commercial grade M2 ​​n-type silicon wafer with a thickness of 180 um and a resistivity of 5 Ω·cm is provided, and an n-type silicon wafer substrate with a pyramid texture surface is formed by alkaline solution polishing, texture making, and cleaning.

[0087] In the second step, a 10 nm intrinsic amorphous silicon passivation layer is deposited on the front and back sides of the n-type silicon wafer substrate in a plasma enhanced chemical vapor deposition (PECVD) device to passivate the dangling bonds on the crystalline silicon surface.

[0088] The third step is to use hydrogen-diluted phosphine and silane mixed gas to deposit a 10nm thick n-type amorphous silicon emitter, and use hydrogen-diluted diborane and silane mixed gas to deposit a 15nm thick p-type amorphous silicon back field to form a silicon substrate battery.

[0089] In the fourth step, the silicon substrate cell is placed in a PECVD device, and on the n-type amorphous silicon, a silane with a hydrogen dilution ratio (hydrogen / silane flow ratio is 250) and phosphine mixed gas is used to prepare 5nm heavily doped n-type microcrystalline silicon, and a silane with a hydrogen dilution ratio (hydrogen / silane flow ratio is 250) and diborane mixed gas is used to prepare 10nm heavily doped p-type microcrystalline silicon to form a tunneling composite junction.

[0090] The fifth step is to prepare a hole transport layer on the tunneling composite junction by evaporation at a rate of The thickness is 10nm and the material is Sprio-TTB.

[0091] Step 6: Place the above structure in a vacuum coating device. A 10 nm lead iodide layer was deposited at an evaporation rate of 1.3 Å as a metal halide skeleton layer.

[0092] Step 7: Place the device obtained above on a spin coater and take 100 μL of 1.5 mol perovskite component (Cs 0.05 FA 0.8 MA 0.15 PbB 0.6 I 2.4 ) DMF / DMSO (4:1) solution was used as the perovskite precursor solution, and the band gap of the prepared precursor solution was about 1.65ev.

[0093] In the eighth step, the taken out perovskite precursor solution is added dropwise onto the surface of the device obtained in the sixth step, and spin-coated at a speed of 1000 rpm and then 4000 rpm for 10 s and 30 s respectively. 5 s before the end of spin coating, 200 μl of anisole anti-solvent is quickly added dropwise onto the device surface (within 1 s). After the spin coating is completed, the obtained device is annealed on a hot stage at 100°C for 10 min to obtain a perovskite light absorption layer with a thickness of 450 nm.

[0094] The ninth step is to place the structure prepared above in a vacuum coating device, first using 10 nm of C60 was evaporated at an evaporation rate of 1.06 Å, and 10 nm of SnO2 was further prepared by an atomic layer deposition device as a laminated electron transport material to obtain an electron transport layer.

[0095] In the tenth step, the device obtained above is deposited on both sides in a magnetron sputtering device to prepare a 110 nm ITO film to form a transparent conductive anti-reflection film.

[0096] The eleventh step is to use a mask method to evaporate a 200nm silver grid line electrode on the transparent conductive anti-reflection film to form a perovskite cell.

[0097] In the twelfth step, a 70nm MgF2 anti-reflection film is prepared on the front side (perovskite cell side) by electron beam evaporation to reduce light reflection on the cell surface and obtain a perovskite-silicon-based tandem solar cell.

[0098] Embodiment 2

[0099] The application of the method for manufacturing the perovskite thin film provided in the embodiment of the present invention in the stacked battery is specifically described as follows:

[0100] In the first step, a commercial grade M2 ​​n-type silicon wafer with a thickness of 180 um and a resistivity of 5 Ω·cm is provided, and an n-type silicon wafer substrate with a pyramid texture surface is formed by alkaline solution polishing, texture making, and cleaning.

[0101] In the second step, a 10 nm intrinsic amorphous silicon passivation layer is deposited on the front and back sides of the n-type silicon wafer substrate in a plasma enhanced chemical vapor deposition (PECVD) device to passivate the dangling bonds on the crystalline silicon surface.

[0102] The third step is to use hydrogen-diluted phosphine and silane mixed gas to deposit a 10nm thick n-type amorphous silicon emitter, and use hydrogen-diluted diborane and silane mixed gas to deposit a 15nm thick p-type amorphous silicon back field to form a silicon substrate battery.

[0103] In the fourth step, the above silicon substrate battery is placed in a PECVD device. On the n-type amorphous silicon emitter, a silane with a hydrogen dilution ratio (hydrogen / silane flow ratio is 250) and phosphine mixed gas is used to prepare 5nm heavily doped n-type microcrystalline silicon, and a silane with a hydrogen dilution ratio (hydrogen / silane flow ratio is 250) and diborane mixed gas is used to prepare 10nm heavily doped p-type microcrystalline silicon to form a tunneling composite junction.

[0104] The fifth step is to prepare an electron transport layer on the tunneling composite junction using a solution method, with a rotation speed of 3000 rpm for 30 s, and the material is SnO2 aqueous solution.

[0105] Step 6: Place the above structure in a vacuum coating device. A 10 nm lead iodide layer is deposited at an evaporation rate of 1.5 Å as a metal halide skeleton layer.

[0106] In the seventh step, the device obtained above was placed on a spin coater, and 60 μL of 1.5 mol perovskite component (Cs 0.05 FA 0.8 MA 0.15 PbB 0.6 I 2.4 ) in DMF / DMSO (4:1) solution was used as the perovskite precursor solution and was spin-coated at 1000 rpm and then 4000 rpm for 10 s and 30 s respectively. 5 s before the end of spin coating, 200 μl of anisole anti-solvent was dripped on the device surface, and then annealed on a hot stage at 100°C for 10 min to obtain a perovskite light absorption layer with a thickness of 450 nm.

[0107] In the eighth step, the hole transport layer was prepared by solution method on the structure prepared above, with the rotation speed of 3000 revolutions and the time of 30 seconds, and the material was Spiro-TAD.

[0108] In the ninth step, the structure prepared above is deposited on both sides in a magnetron sputtering device to prepare a 110 nm ITO film to form a transparent conductive anti-reflection film.

[0109] The tenth step is to use a mask method to evaporate a 200nm silver grid line electrode on the transparent conductive anti-reflection film to form a perovskite cell.

[0110] In the eleventh step, a 70nm MgF2 anti-reflection film is prepared on the front side (perovskite cell side) by electron beam evaporation to reduce light reflection on the cell surface and obtain a perovskite-silicon substrate stacked solar cell.

[0111] Embodiment 3

[0112] The application of the method for manufacturing the perovskite thin film provided in the embodiment of the present invention in the stacked battery is specifically described as follows:

[0113] In the first step, a commercial grade M2 ​​n-type silicon wafer with a thickness of 180 um and a resistivity of 5 Ω·cm is provided, and an n-type silicon wafer substrate with a pyramid texture surface is formed by alkaline solution polishing, texture making, and cleaning.

[0114] In the second step, a 10 nm intrinsic amorphous silicon passivation layer is deposited on the front and back sides of the n-type silicon wafer substrate in a plasma enhanced chemical vapor deposition (PECVD) device to passivate the dangling bonds on the crystalline silicon surface.

[0115] The third step is to use hydrogen-diluted phosphine and silane mixed gas to deposit a 10nm thick n-type amorphous silicon emitter, and use hydrogen-diluted diborane and silane mixed gas to deposit a 15nm thick p-type amorphous silicon back field to form a silicon substrate battery.

[0116] In the fourth step, the silicon substrate cell is placed in a PECVD device, and on the n-type amorphous silicon, a silane with a hydrogen dilution ratio (hydrogen / silane flow ratio is 250) and phosphine mixed gas is used to prepare 5nm heavily doped n-type microcrystalline silicon, and a silane with a hydrogen dilution ratio (hydrogen / silane flow ratio is 250) and diborane mixed gas is used to prepare 10nm heavily doped p-type microcrystalline silicon to form a tunneling composite junction.

[0117] The fifth step is to prepare a hole transport layer on the tunneling composite junction by evaporation at a rate of The thickness is 10nm and the material is Sprio-TTB.

[0118] In the sixth step, the structure obtained above is placed in a vacuum coating device, and lead iodide and cesium bromide are co-evaporated in a molar ratio of 2:1 to obtain a 5nm metal halide skeleton layer, wherein the evaporation rate of lead iodide is The evaporation rate of cesium bromide is

[0119] In the seventh step, the device obtained above is placed on a spin coater, and 100 microliters of a DMF / DMSO (4:1) solution with a concentration of 1.5 mol of the perovskite component (CsPbI3) is taken as the perovskite precursor solution. The prepared precursor solution has a band gap of about 1.7 ev.

[0120] In the eighth step, the taken out perovskite precursor solution is dripped on the surface of the device obtained in step 4, and spin-coated at a speed of 1000 rpm and then 4000 rpm for 10 s and 30 s respectively. 5 s before the end of spin coating, 200 microliters of anisole anti-solvent is quickly dripped on the device surface (within 1 s). After the spin coating is completed, the obtained device is annealed on a hot stage at 100°C for 10 min to obtain a perovskite light absorption layer with a thickness of 350 nm.

[0121] The ninth step is to place the structure prepared above in a vacuum coating device, first using 10 nm of C60 was evaporated at an evaporation rate of 1.06 Å, and 10 nm of SnO2 was further prepared by an atomic layer deposition device as a laminated electron transport material to obtain an electron transport layer.

[0122] In the tenth step, the device obtained above is deposited on both sides in a magnetron sputtering device to prepare a 110 nm ITO film to form a transparent conductive anti-reflection film.

[0123] The eleventh step is to use a mask method to evaporate a 200nm silver grid line electrode on the transparent conductive anti-reflection film to form a perovskite cell.

[0124] In the twelfth step, a 70nm MgF2 anti-reflection film is prepared on the front side (perovskite cell side) by electron beam evaporation to reduce light reflection on the cell surface and obtain a perovskite-silicon-based tandem solar cell.

[0125] Embodiment 4

[0126] The application of the method for manufacturing the perovskite thin film provided in the embodiment of the present invention in the stacked battery is specifically described as follows:

[0127] In the first step, a commercial grade M2 ​​n-type silicon wafer with a thickness of 180 um and a resistivity of 5 Ω·cm is provided, and an n-type silicon wafer substrate with a pyramid texture surface is formed by alkaline solution polishing, texture making, and cleaning.

[0128] In the second step, a 10 nm intrinsic amorphous silicon passivation layer is deposited on the front and back sides of the n-type silicon wafer substrate in a plasma enhanced chemical vapor deposition (PECVD) device to passivate the dangling bonds on the crystalline silicon surface.

[0129] The third step is to use hydrogen-diluted phosphine and silane mixed gas to deposit a 10nm thick n-type amorphous silicon emitter, and use hydrogen-diluted diborane and silane mixed gas to deposit a 15nm thick p-type amorphous silicon back field to form a silicon substrate battery.

[0130] In the fourth step, the silicon substrate cell is placed in a PECVD device, and on the n-type amorphous silicon, a silane with a hydrogen dilution ratio (hydrogen / silane flow ratio is 250) and phosphine mixed gas is used to prepare 5nm heavily doped n-type microcrystalline silicon, and a silane with a hydrogen dilution ratio (hydrogen / silane flow ratio is 250) and diborane mixed gas is used to prepare 10nm heavily doped p-type microcrystalline silicon to form a tunneling composite junction.

[0131] The fifth step is to prepare a hole transport layer on the tunneling composite junction by evaporation at a rate of The thickness is 10nm and the material is Sprio-TTB.

[0132] In the sixth step, the structure obtained above is placed in a vacuum coating device, and lead iodide and cesium bromide are co-evaporated in a molar ratio of 2:0.1 to obtain a 15nm metal halide skeleton layer, wherein the evaporation rate of lead iodide is The evaporation rate of cesium bromide is

[0133] Step 7: Place the device obtained above on a spin coater and take 100 μL of 1.5 mol perovskite component (Cs 0.05 FA 0.7 MA 0.25 PbB 0.5 I 2.5 ) DMF / DMSO (4:1) solution was used as the perovskite precursor solution, and the band gap of the prepared precursor solution was about 1.65ev.

[0134] In the eighth step, the taken out perovskite precursor solution is dripped on the surface of the device obtained in step 4, and spin-coated at a speed of 1000 rpm and then 4000 rpm for 10 s and 30 s respectively. 5 s before the end of spin coating, 200 microliters of anisole anti-solvent is quickly dripped on the device surface (within 1 s). After the spin coating is completed, the obtained device is annealed on a hot stage at 100°C for 10 min to obtain a perovskite light absorption layer with a thickness of 500 nm.

[0135] The ninth step is to place the structure prepared above in a vacuum coating device, first using 10 nm of C60 was evaporated at an evaporation rate of 1.06 Å, and 10 nm of SnO2 was further prepared by an atomic layer deposition device as a laminated electron transport material to obtain an electron transport layer.

[0136] In the tenth step, the device obtained above is deposited on both sides in a magnetron sputtering device to prepare a 110 nm ITO film to form a transparent conductive anti-reflection film.

[0137] The eleventh step is to use a mask method to evaporate a 200nm silver grid line electrode on the transparent conductive anti-reflection film to form a perovskite cell.

[0138] In the twelfth step, a 70nm MgF2 anti-reflection film is prepared on the front side (perovskite cell side) by electron beam evaporation to reduce light reflection on the cell surface and obtain a perovskite-silicon-based tandem solar cell.

[0139] Embodiment 5

[0140] The application of the method for manufacturing the perovskite thin film provided in the embodiment of the present invention in the stacked battery is specifically described as follows:

[0141] In the first step, a commercial grade M2 ​​n-type silicon wafer with a thickness of 180 um and a resistivity of 5 Ω·cm is provided, and an n-type silicon wafer substrate with a pyramid texture surface is formed by alkaline solution polishing, texture making, and cleaning.

[0142] In the second step, a 10 nm intrinsic amorphous silicon passivation layer is deposited on the front and back sides of the n-type silicon wafer substrate in a plasma enhanced chemical vapor deposition (PECVD) device to passivate the dangling bonds on the crystalline silicon surface.

[0143] The third step is to use hydrogen-diluted phosphine and silane mixed gas to deposit a 10nm thick n-type amorphous silicon emitter, and use hydrogen-diluted diborane and silane mixed gas to deposit a 15nm thick p-type amorphous silicon back field to form a silicon substrate battery.

[0144] In the fourth step, the silicon substrate cell is placed in a PECVD device, and on the n-type amorphous silicon, a silane with a hydrogen dilution ratio (hydrogen / silane flow ratio is 250) and phosphine mixed gas is used to prepare 5nm heavily doped n-type microcrystalline silicon, and a silane with a hydrogen dilution ratio (hydrogen / silane flow ratio is 250) and diborane mixed gas is used to prepare 10nm heavily doped p-type microcrystalline silicon to form a tunneling composite junction.

[0145] The fifth step is to prepare a hole transport layer on the tunneling composite junction by evaporation at a rate of The thickness is 10nm and the material is Sprio-TTB.

[0146] In the sixth step, the structure obtained above is placed in a vacuum coating device, and lead iodide and cesium bromide are co-evaporated in a molar ratio of 2:0.5 to obtain a 10nm metal halide skeleton layer, wherein the evaporation rate of lead iodide is The evaporation rate of cesium bromide is

[0147] In the seventh step, the device obtained above is placed on a spin coater, and 100 microliters of a 1.5 mol DMF / DMSO (4:1) solution of the perovskite component (CH3NH3PbI3) is taken as a perovskite precursor solution. The prepared precursor solution has a band gap of about 1.55 ev.

[0148] In the eighth step, the taken out perovskite precursor solution is dripped on the surface of the device obtained in step 4, and spin-coated at a speed of 1000 rpm and then 4000 rpm for 10 s and 30 s respectively. 5 s before the end of spin coating, 200 microliters of anisole anti-solvent is quickly dripped on the device surface (within 1 s). After the spin coating is completed, the obtained device is annealed on a hot stage at 100°C for 10 min to obtain a perovskite light absorption layer with a thickness of 450 nm.

[0149] The ninth step is to place the structure prepared above in a vacuum coating device, first using 10 nm of C60 was evaporated at an evaporation rate of 1.06 Å, and 10 nm of SnO2 was further prepared by an atomic layer deposition device as a laminated electron transport material to obtain an electron transport layer.

[0150] In the tenth step, the device obtained above is deposited on both sides in a magnetron sputtering device to prepare a 110 nm ITO film to form a transparent conductive anti-reflection film.

[0151] The eleventh step is to use a mask method to evaporate a 200nm silver grid line electrode on the transparent conductive anti-reflection film to form a perovskite cell.

[0152] In the twelfth step, a 70nm MgF2 anti-reflection film is prepared on the front side (perovskite cell side) by electron beam evaporation to reduce light reflection on the cell surface and obtain a perovskite-silicon-based tandem solar cell.

[0153] Comparative Example 1

[0154] In the first step, a commercial grade M2 ​​n-type silicon wafer with a thickness of 180 um and a resistivity of 5 Ω·cm is provided, and an n-type silicon wafer substrate with a pyramid texture surface is formed by alkaline solution polishing, texture making, and cleaning.

[0155] In the second step, a 10 nm intrinsic amorphous silicon passivation layer is deposited on the front and back sides of the n-type silicon wafer substrate in a plasma enhanced chemical vapor deposition (PECVD) device to passivate the dangling bonds on the crystalline silicon surface.

[0156] The third step is to use hydrogen-diluted phosphine and silane mixed gas to deposit a 10nm thick n-type amorphous silicon emitter, and use hydrogen-diluted diborane and silane mixed gas to deposit a 15nm thick p-type amorphous silicon back field to form a silicon substrate battery.

[0157] In the fourth step, the silicon substrate cell is placed in a PECVD device, and on the n-type amorphous silicon, a silane with a hydrogen dilution ratio (hydrogen / silane flow ratio is 250) and phosphine mixed gas is used to prepare 5nm heavily doped n-type microcrystalline silicon, and a silane with a hydrogen dilution ratio (hydrogen / silane flow ratio is 250) and diborane mixed gas is used to prepare 10nm heavily doped p-type microcrystalline silicon to form a tunneling composite junction.

[0158] The fifth step is to prepare a hole transport layer on the tunneling composite junction by evaporation at a rate of The thickness is 10nm and the material is Sprio-TTB.

[0159] In the sixth step, the device with the hole transport layer was placed on a spin coater and 60 μL of 1.5 mol perovskite component (Cs 0.05 FA 0.8 MA 0.15 PbB 0.6 I 2.4 ) in DMF / DMSO (4:1) solution was used as the perovskite precursor solution and was spin-coated at 1000 rpm and then 3000 rpm for 10 s and 30 s respectively. 5 s before the end of spin coating, 200 μl of anisole anti-solvent was dripped on the device surface, and then annealed on a hot stage at 100°C for 10 min to complete the preparation of the perovskite light absorption layer, and a perovskite light absorption layer with a thickness of 450 nm was obtained.

[0160] Step 7: Place the structure prepared above in a vacuum coating device. 10 nm of C60 was evaporated at an evaporation rate of 1.06 Å, and 10 nm of SnO2 was further prepared by an atomic layer deposition device as a laminated electron transport material to obtain an electron transport layer.

[0161] In the eighth step, a 110 nm ITO film is deposited on both sides of the device prepared above by magnetron sputtering to form a transparent conductive anti-reflection film.

[0162] The ninth step is to use a mask method to evaporate a 200nm silver grid line electrode on the transparent conductive anti-reflection film to form a perovskite cell.

[0163] The tenth step is to prepare a 70nm MgF2 anti-reflection film on the front side (perovskite cell side) by electron beam evaporation to reduce light reflection on the cell surface and obtain a perovskite-silicon substrate stacked solar cell.

[0164] In order to verify the performance of the perovskite-silicon substrate stacked solar cell, the photoelectric conversion efficiency, fill factor, open circuit voltage, short circuit current and other performance parameters of the devices prepared in Example 1, Example 2, Example 3, Example 4 and Example 5 and Comparative Example 1 were tested. The performance parameter comparison is shown in Table 1.

[0165] Table 1 Performance comparison of perovskite-silicon based tandem solar cells

[0166]

[0167] As can be seen from Table 1, by comparing Example 1, Example 2, Example 3, Example 4 and Example 5 with Comparative Example 1, it can be concluded that, compared with the stacked battery prepared by the conventional one-step solution method, the stacked battery using the method for preparing the perovskite film provided by the embodiment of the present invention has significantly improved short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency in the performance test. The open-circuit voltage of the prepared stacked battery can reach above 1.7V, and the fill factor has also achieved an absolute improvement of more than 3%, which proves that the method for preparing the perovskite film provided by the embodiment of the present invention can improve the exchange and recombination ability of photogenerated carriers, enhance the photogenerated carrier collection ability of the stacked battery, and improve the photoelectric conversion efficiency of the stacked battery.

[0168] In the description of the above embodiments, specific features, structures, materials or characteristics may be combined in a suitable manner in any one or more embodiments or examples.

[0169] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing a perovskite thin film, characterized in that: include: Providing a substrate, wherein the surface of the substrate has a suede structure; Forming a metal halide skeleton layer on the substrate having a suede structure, wherein the metal halide skeleton layer conformally covers the suede structure, and the thickness of the metal halide skeleton layer is in the range of 5 nm to 15 nm; A perovskite precursor solution is coated on the metal halide skeleton layer with a velvet structure by a one-step solution method to form a perovskite light absorption layer, wherein the solute of the perovskite precursor solution is an ABX3 type structure, wherein A is a ternary mixed cation comprising Cs, FA and MA; B is a metal cation comprising Pb; and X is an anion comprising I and Br.

2. The method for preparing a perovskite thin film according to claim 1, characterized in that: The forming of the metal halide skeleton layer on the substrate having the velvet structure comprises: evaporating metal halide on the substrate having the velvet structure to form the metal halide skeleton layer.

3. The method for preparing a perovskite thin film according to claim 2, characterized in that: The metal halide is at least one of lead halide, cesium halide and rubidium halide.

4. The method for preparing a perovskite thin film according to claim 3, characterized in that: The metal halide is a mixture of lead halide and cesium halide, and the molar ratio between the lead halide and the cesium halide is 2:0.1-2:

1.

5. The method for preparing a perovskite thin film according to claim 1, characterized in that: The solvent of the perovskite precursor solution includes one or more of N,N-dimethylformamide, dimethyl sulfoxide, N-methylpyrrolidone, and acetonitrile.

6. The method for preparing a perovskite thin film according to claim 1, characterized in that: The band gap of the perovskite precursor solution is in the range of 1.5 eV-1.8 eV, and / or the thickness of the perovskite light absorbing layer is in the range of 350 nm-500 nm.

7. A solar cell, characterized in that: The solar cell is prepared by the method for preparing a perovskite film according to any one of claims 1 to 6, and comprises: A substrate having a suede structure; A metal halide skeleton layer conformally covers the substrate having a suede structure; The perovskite light absorbing layer is conformally formed on the metal halide skeleton layer having a suede structure.

8. A laminated battery, characterized in that: The laminated battery is prepared by the method for preparing a perovskite film according to any one of claims 1 to 6, and comprises: A substrate, wherein the substrate sequentially stacks a silicon substrate battery with a suede structure, a first transparent conductive layer, and a first carrier transport layer; a metal halide skeleton layer conformally covers the first carrier transport layer with a suede structure; A perovskite light absorption layer is conformally formed on the metal halide skeleton layer having a velvet structure; A second carrier transport layer, a second transparent conductive layer and an electrode are sequentially formed on the perovskite light absorbing layer.