Li ion conductor and method for producing the same
By using the interface connection technology of garnet-type composite metal oxide and eutectic mixture in lithium-ion conductors, the problem of insufficient conductor performance in lithium-ion secondary batteries is solved, high energy density and safety are improved, and it is suitable for solid Electrolyte materials.
Patent Information
- Application Number
- CN202080063450.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-13
- Filing Date
- 2020-09-08
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-09-08
AI Technical Summary
Existing Li ion conductors have problems with insufficient safety and long-term cycle stability in lithium-ion secondary batteries. In particular, all-solid-state batteries with solid electrolytes still have room for improvement in terms of high energy density and safety.
A garnet-type composite metal oxide phase containing Li, La, Zr and O is used, and by using a eutectic mixture with a melting point below 600°C for interface connection, combined with mechanochemical treatment and heat treatment, a lithium ion conductive material with excellent lithium ion conductivity is prepared. Li ion conductor. The specific method includes mixing a garnet-type composite metal oxide with a eutectic mixture, and performing heat treatment below 600°C, preferably using a eutectic mixture such as LiF, ZrCl4, AlCl3, NbCl5 or TaCl5, applying pressure and annealing in an inactive atmosphere to Forming pellets with good electrical conductivity.
It has achieved a Li ion conductivity of more than 1.0×10-7S/cm at room temperature, and an activation energy lower than 0.6eV, which significantly improves the performance of lithium ion conductors and is suitable for use as solid electrolyte materials for secondary batteries.
Smart Images

Figure CN114365318B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to Li ion conductors. Background Art
[0002] Research and development of Li-ion secondary batteries is being vigorously carried out for portable devices, hybrid vehicles, electric vehicles, and household power storage applications. Li-ion secondary batteries used in these fields are required to have high safety, long-term cycle stability, high energy density, etc.
[0003] Among them, all-solid-state batteries using solid electrolytes have attracted attention due to their high safety. For example, the lithium ion conductor LIC of Patent Document 1 is manufactured by first preparing an ion conductor, then mixing lithium halide and the ion conductor and heating them. 12 In the case of LLZ-MgSr powder obtained by elemental substitution of Mg and Sr, the raw materials of each element comprising LLZ-MgSr (Li2CO3, MgO, La(OH)3, SrCO3, ZrO2, SrCO3, ZrO2) are mixed for 15 hours, calcined at 1000°C for 10 hours, and then mixed with powder of lithium halide (e.g. LiI) to obtain a mixed powder, which is pressurized together with a stainless steel current collector using a press to obtain a pressed powder, and heat treated at 80°C for 17 hours.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2017-91788 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] An object of the present invention is to provide a Li ion conductor different from Patent Document 1, which contains a garnet-type composite metal oxide phase and exhibits good lithium ion conductivity, and a method for producing the same.
[0009] Solutions for solving problems
[0010] The present invention is as follows.
[0011] [1] A Li ion conductor having a garnet-type composite metal oxide phase (L) containing Li, La, Zr and O, wherein the Li ion conductor has a diffraction peak at at least one of 2θ=13.8°±1° and 2θ=15.2°±1° in an X-ray diffraction measurement using CuKα rays.
[0012] [2] The Li ion conductor according to [1], which has a metal-containing phase (K) different from the phase (L), wherein the phase (K) contains a halogen element and Li.
[0013] [3] The Li ion conductor according to [1] or [2], wherein the cubic Li 6.25 Ga 0.25 La3Zr2O 12 Among the diffraction peaks, a diffraction peak corresponding to 2θ=30.9° was observed at 2θ=30.5° or more and 30.9° or less.
[0014] [4] The Li ion conductor according to any one of [1] to [3], wherein the lattice constant exceeds And for the following.
[0015] [5] The Li ion conductor according to any one of [1] to [4], wherein the activation energy Ea obtained by impedance measurement is 0.6 eV or less.
[0016] [6] The Li ion conductor according to any one of [1] to [5], wherein the Li ion conductivity σ at room temperature obtained by impedance measurement is total 1.0×10 -7 S / cm or more.
[0017] [7] A method for producing a Li ion conductor, wherein the Li ion conductor has a garnet-type composite metal oxide phase (L) containing Li, La, Zr and O, wherein the interface of the garnet-type composite metal oxide phase (L) is connected using a eutectic mixture having a melting point of 600° C. or less.
[0018] [8] A manufacturing method according to [7], wherein a eutectic mixture having a melting point below 600°C and a mixture of a garnet-type composite metal oxide containing Li, La, Zr and O are formed, and the resulting formed product is heat treated at below 600°C, thereby connecting the interface of the aforementioned phase (L).
[0019] [9] The production method according to [7] or [8], wherein the eutectic mixture is a eutectic mixture of two metal halides.
[0020]
[10] A production method according to any one of [7] to [9], wherein the eutectic mixture is a eutectic mixture of LiF, ZrCl4, AlCl3, NbCl5 or TaCl5 and LiCl, or a eutectic mixture of LiF and TaF5.
[0021] Effects of the Invention
[0022] According to the Li ion conductor of the present invention, a good lithium ion conductor can be provided and can be used as a member of an excellent solid electrolyte for secondary batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is the XRD diffraction pattern of Example 1.
[0024] Figure 2 The following are photographs in place of drawings showing SEM observation images of Examples and Comparative Examples.
[0025] Figure 3 This is an enlarged view of the XRD diffraction pattern of Example 1. DETAILED DESCRIPTION
[0026] The present inventors have conducted research to obtain a Li ion conductor that exhibits good lithium ion conductivity, and have found that the object of the present invention can be achieved by connecting the interface of a garnet-type composite metal oxide phase (L) using a eutectic mixture having a melting point of 600° C. or less. More specifically, (1) the garnet-type composite metal oxide and the eutectic mixture having a melting point of 600° C. or less can be mixed and heat treated, and (2) the raw material of the garnet-type composite metal oxide and the eutectic mixture having a melting point of 600° C. or less can be mechanochemically treated.
[0027] The aforementioned eutectic mixture is preferably a eutectic mixture of two metal halides, for example, it is preferably a eutectic mixture of LiF, ZrCl4, AlCl3, NbCl5, or TaCl5 and LiCl, or it is a eutectic mixture of LiF and TaF5, more preferably it is a eutectic mixture of LiF, ZrCl4, AlCl3, NbCl5, or TaCl5 and LiCl, further preferably it is a eutectic mixture of LiF, AlCl3, NbCl5, or TaCl5 and LiCl, particularly preferably it is a eutectic mixture of AlCl3, NbCl5, or TaCl5 and LiCl, and most preferably it is a eutectic mixture of TaCl5 and LiCl.
[0028] In the method of mixing a garnet-type composite metal oxide and a eutectic mixture having a melting point of 600°C or less and heat-treating the mixture, it is preferred to mix a garnet-type composite metal oxide and a eutectic mixture having a melting point of 600°C or less, and heat-treat a shaped body such as pellets produced by applying pressure to the obtained mixture. As the heat treatment, annealing the shaped body at 600°C or less, preferably 500°C or less, and more preferably 300°C or less for 5 minutes to 600 minutes, preferably 10 minutes to 480 minutes, can be cited. The lower limit of the annealing temperature is not particularly limited, and for example, it can be 150°C or 200°C. In addition, the annealing temperature is preferably 150°C or more (preferably 200°C or more), and is above (melting point - 10°C) of the eutectic mixture (more preferably above the melting point). Annealing is preferably performed in an inert gas atmosphere such as nitrogen or Ar. The pressure during the production of the shaped body is preferably set to about 300MPa to 450MPa, for example. The mixing of the garnet-type composite metal oxide and the eutectic mixture having a melting point of 600° C. or less, the molding of the obtained mixture, and the annealing are preferably performed in a glove box or a drying room, etc., in an environment with sufficiently reduced humidity, for example, the dew point temperature is preferably set to -40° C. to -90° C. In the method (1) above, the ratio of the eutectic mixture to 100 parts by mass of the garnet-type composite metal oxide can be appropriately set according to the type of the eutectic mixture used, the pressure during the production of the molded body, the annealing conditions, etc., and can be set to, for example, 15 to 60 parts by mass, preferably 20 to 50 parts by mass.
[0029] The garnet-type composite metal oxide used in the method of (1) above can be obtained by mixing raw materials of the composite metal oxide and calcining them at 1000-1100° C. for about 6-12 hours, or by subjecting the raw materials of the composite metal oxide to a mechanochemical treatment. The mechanochemical treatment can be performed by compressing and shearing a mixture of raw material powders of the composite metal oxide under dry conditions.
[0030] In addition, the method of mechanochemically treating the raw material of the garnet-type composite metal oxide and the eutectic mixture having a melting point of 600° C. or less in (2) can be performed by, for example, compressing and shearing the mixture of the raw material powder of the composite metal oxide and the eutectic mixture having a melting point of 600° C. or less under dry conditions. After the mechanochemical treatment in (2), the heat treatment described in (1) can be further performed.
[0031] In any of the above (1) and (2), the raw material of the garnet-type composite metal oxide is at least one of a Li source powder, a La source powder, and a Zr source powder, and further, as required, an Al source powder and a Ga source powder. As the Li source powder, the La source powder, the Zr source powder, the Al source powder and the Ga source powder, for example, oxides, carbonates, hydroxides, chlorides, alkoxides, etc. of each metal (Li, La, Zr, Al, or Ga) can be used.
[0032] The preferred Li ion conductor obtained by the above method is preferably a Li ion conductor having a garnet-type composite metal oxide phase (L) containing Li, La, Zr and O, and having a diffraction peak at at least one of 2θ=13.8° and 15.2° in an X-ray diffraction measurement using CuKα rays. In the crystal structure derived from the diffraction peak at 2θ=13.8° or 2θ=15.2°, sometimes the atoms constituting the crystal are replaced by other atoms. In this case, the angle at which the diffraction peak appears may be shifted within the range of ±1°. The Li ion conductor of the present invention also includes the case where it is a Li ion conductor having a garnet-type composite metal oxide phase (L) containing Li, La, Zr and O, and having a diffraction peak at at least one of 2θ=13.8°±1° and 2θ=15.2°±1° in an X-ray diffraction measurement using CuKα rays. The range of 2θ=13.8°±1° is preferably 2θ=13.8°±0.5°, more preferably 13.8°±0.3°, and further preferably 13.8°. The range of 2θ=15.2°±1° is preferably 2θ=15.2°±0.5°, more preferably 15.2°±0.3°, and further preferably 15.2°.
[0033] The garnet-type composite metal oxide phase (L) containing Li, La, Zr and O is A3B2C3O 12 The position of A in the crystal represented by the composition formula is La 3+ Occupies B, the position is occupied by Zr 4+ The positions occupied by C and the inter-lattice positions are occupied by Li + The phase occupied can usually be Li7La3Zr2O 12 The aforementioned phase (L) is preferably a cubic crystal. In addition, the aforementioned garnet-type composite metal oxide phase (L) also preferably contains Al and / or Ga. In this case, Li7La3Zr2O is more preferred. 12 Li + A portion of the site is covered by Al 3+ and / or Ga 3+ Substitution. Hereinafter, including the case of substitution with other elements, the garnet-type composite metal oxide containing Li, La, Zr, and O may be referred to as “LLZ”.
[0034] As described above, in the phase (L) of the present invention, Li7La3Zr2O 12 Li + A portion of the sites can be 3+ and / or Ga 3+ It is preferred that the Al and Ga elements are not substituted.
[0035] Furthermore, the Li ion conductor of the present invention has the following characteristics: in X-ray diffraction measurement using CuKα rays, a peak is observed at at least one of 2θ=13.8°±1° and 15.2°±1°, preferably at both of 2θ=13.8°±1° and 15.2°±1°.
[0036] The Li ion conductor of the present invention is preferably a cubic Li ion conductor as measured by X-ray diffraction using CuKα rays. 6.25 Ga 0.25 La3Zr2O 12 In the diffraction peaks, a diffraction peak corresponding to 2θ=30.9° is observed at 2θ=30.5° or more and 30.9° or less. There is a tendency that if LLZ is replaced by an element having an ionic radius smaller than that of Li, La, Zr and O, the diffraction peak corresponding to 2θ=30.9° is shifted and appears on the angle side higher than 30.9°, and on the contrary, if it is replaced by an element having a larger ionic radius, the diffraction peak corresponding to 2θ=30.9° is shifted and appears on the angle side lower than 30.9°. The diffraction peak corresponding to 2θ=30.9° preferably appears at 2θ=30.5° or more and less than 30.9°. For example, when it is believed that a part of the garnet-type composite metal oxide phase (L) containing Li, La, Zr and O is replaced by the Cl element, a diffraction peak corresponding to 2θ=30.9° is observed at 2θ=30.5° or more and less than 30.9°.
[0037] The Li ion conductor of the present invention preferably has a lattice constant exceeding And for Hereinafter, for example, it is considered that the garnet-type composite metal oxide phase (L) containing Li, La, Zr, and O has such a lattice constant when a part of the phase is substituted with the Cl element.
[0038] As described above, the Li ion conductor of the present invention can be produced using a eutectic mixture of two metal halides in a preferred embodiment. In an example in which Li is included as a metal, which is an example of a preferred embodiment, the obtained Li ion conductor has a metal-containing phase (K) different from the aforementioned phase (L), and the phase (K) contains a halogen element and Li. In a more preferred embodiment, the aforementioned phase (K) contains Li, Ta and a halogen element.
[0039] The Li ion conductor of the present invention is particularly preferably an aggregate structure of particles having the garnet-type composite metal oxide phase (L), and having the phase (K) at the particle interface. The presence of the phase (K) at the particle interface of the phase (L) allows Li ions to be smoothly conducted from the phase (L) to the phase (L) via the phase (K).
[0040] In the Li ion conductor of the present invention, the activation energy Ea at room temperature obtained by impedance measurement can be set to 0.6 eV or less, and the Li ion conductivity σ at room temperature can be set to total Set to 1.0×10 -7 The activation energy Ea is preferably 0.57 eV or less, more preferably 0.55 eV or less, and further preferably 0.50 eV or less. The lower limit is not particularly limited, and is, for example, 0.25 eV. In addition, the Li ion conductivity σ total Preferably 2.0×10 -7 S / cm or more, more preferably 4.0×10 -7 S / cm or more, more preferably 1.0×10 -6 S / cm or more, more preferably 5.0×10 -6 S / cm or more, particularly preferably 1.0×10 -5 S / cm or more, and the upper limit is not particularly limited, for example, 7.0×10 -5 S / cm.
[0041] This application claims priority based on Japanese Patent Application No. 2019-167381 filed on September 13, 2019. The entire contents of the specification of Japanese Patent Application No. 2019-167381 filed on September 13, 2019 are incorporated herein by reference.
[0042] Example
[0043] The present invention is not limited to the following examples, and can be implemented by appropriately modifying the above and below-mentioned embodiments within the scope of the above and below-mentioned purposes, and all of them are included in the technical scope of the present invention.
[0044] Example 1
[0045] Compared with Li made by Toyoshima Manufacturing Co., Ltd. 6.25 Ga 0.25 La3Zr2O 12100 parts by mass, 50 parts by mass of a eutectic mixture of LiCl and TaCl5 (the molar ratio of LiCl to TaCl5 is 50:50, melting point: 220°C) are mixed in a mortar for 30 minutes, the obtained mixed powder is placed in a mold, and a pressure of 375 MPa is applied to form pellets with a diameter of 10 mm and a thickness of about 1 mm. The mixing in the mortar and the forming of the pellets are carried out in a drying room. The dew point temperature in the drying room is -60°C. The formed pellets are annealed at 220°C for 15 minutes in a small electric furnace (under argon atmosphere) in a glove box (dew point temperature -90°C), and Au is sputtered on both sides of the pellets to form electrodes with a diameter of 8 mm. The obtained pellet sample is installed in an all-solid-state battery evaluation unit manufactured by Hohsen Co., Ltd., connected to a potentiostat / galvanostat, and impedance measurement is performed in a temperature range of room temperature to 100°C to evaluate the Li ion conductivity. As a result, the ionic conductivity σ at room temperature total 2.2×10 -5 S / cm. In addition, activation energy was calculated from the Arrhenius plot using the values of ion conductivity at each temperature. The activation energy Ea was 0.39 eV.
[0046] In addition, the crystal structure of the powder sample obtained by crushing the annealed pellets was analyzed using an XRD (X-ray Diffraction analysis) apparatus manufactured by Bruker. The results are shown in FIG. Figure 1 XRD measurement was performed using CuKα radiation, with λ = 1.5418 nm and θ = 10 to 50°. Figure 1 , observed with cubic Li7La3Zr2O 12 At the same time, the peaks corresponding to the addition of LiCl were observed. In addition, the peaks corresponding to Li7La3Zr2O 12 , LiCl, TaCl5 different crystalline phases.
[0047] Embodiments 2 to 10
[0048] Will be with Li 6.25 Ga 0.25 La3Zr2O 12 The pellets were formed and annealed in the same manner as in Example 1 except that the type, amount, and annealing conditions of the eutectic mixture were as shown in Table 1, and the ionic conductivity and activation energy at room temperature were measured. The results are shown in Table 1. It should be noted that only Example 4 shows the measurement results at 50°C.
[0049] Comparative Example 1
[0050] Instead of using a eutectic mixture of LiCl and TaCl5, only Li 6.25 Ga 0.25 La3Zr2O 12 The ion conductivity at room temperature was measured in the same manner as in Example 1 except that the molding and annealing were performed. The results are shown in Table 1.
[0051] Reference Example 1
[0052] The same Li produced by Toyoshima Seisakusho Co., Ltd. as used in Example 1 was used. 6.25 Ga 0.25 La3Zr2O 12 The pellets were placed in a mold and subjected to a pressure of 375 MPa to form pellets with a diameter of 10 mm and a thickness of about 1 mm. The formed pellets were annealed in the atmosphere at 1230°C for 1200 minutes, and Au was sputtered on both sides of the pellets to form electrodes with a diameter of 8 mm. Then, the Li ion conductivity at room temperature was measured in the same manner as in Example 1. The results are shown in Table 1.
[0053] [Table 1]
[0054]
[0055] The ion conductor of Example 1 obtained by molding a mixture of a eutectic mixture having a eutectic point of 600°C or less and LLZ and heat treating the obtained molded product at 600°C or less showed good ion conductivity as shown in Table 1. Examples 2 to 10, in which ion conductors were prepared by the same method as Example 1, also showed good ion conductivity as shown in Table 1. On the other hand, in Comparative Example 1, in which a molded product of only LLZ was annealed under the same conditions as Example 1, no ion conduction was performed at all at room temperature.
[0056] in addition, Figure 2 (a) shows a SEM observation image of the ion conductor of Example 1. Figure 2 (b) shows a SEM observation image of the ion conductor of Comparative Example 1. Figure 2 As shown, Comparative Example 1 ( Figure 2 In (b), the LLZ particle aggregate structure was observed, and the interfaces between the particles were not connected. Figure 2 (a) and Figure 2 (b) is compared with Figure 2 In (a), the LLZ granular structure was observed, but a phase connecting the LLZ granular interfaces was observed. Figure 1The peak of LiCl was observed in the XRD of , and considering the annealing temperature in Example 1 and the melting point of the eutectic mixture used in Example 1, it is believed that the phase connecting the grain structure of LLZ is a phase formed by the melting of the eutectic mixture of LiCl and TaCl5.
[0057] Furthermore, Figure 1 The XRD analysis results of Example 1 shown in the enlarged view of the vicinity of 2θ=30-40° and Li 6.25 Ga 0.25 La3Zr2O 12 XRD diffraction Figure 1 Started in Figure 3 .like Figure 3 As shown, in the ion conductor of Example 1, the diffraction peak corresponding to 2θ=30.9° is shifted to the low-angle side and is observed at a position of 2θ=30.5° or more and less than 30.9°.
[0058] In addition, for Examples 1 and 2, the diffraction peak of the (400) plane obtained in the above-mentioned XRD measurement was used to obtain the plane spacing d value by the following formulas (1) and (2), and the lattice constant was calculated. The result of Example 1 was Embodiment 2 is
[0059] 2dsinθ=nλ (1)
[0060] 1 / d 2 =(h 2 +k 2 +l 2 ) / a 2 (2)
[0061] d: interplanar spacing; a: lattice constant; h, k and l: Miller index
[0062] Industrial Applicability
[0063] The Li ion conductor of the present invention can be suitably used as a solid electrolyte material for a secondary battery.
Claims
1. A Li ion conductor, characterized in that The invention relates to a garnet-type composite metal oxide phase (L) containing Li, La, Zr and O, wherein the Li ion conductor has diffraction peaks at 2θ=13.8°±1° and 2θ=15.2°±1° in an X-ray diffraction measurement using CuKα rays, The interface of the garnet-type composite metal oxide phase (L) is connected by a eutectic mixture having a melting point of 600° C. or less, The eutectic mixture is a eutectic mixture of ZrCl4, AlCl3, NbCl5 or TaCl5 and LiCl, or a eutectic mixture of LiF and TaF5. 2 . The Li ion conductor according to claim 1 , comprising a metal-containing phase (K) different from the phase (L), wherein the phase (K) contains a halogen element and Li.
3. The Li ion conductor according to claim 1 or 2, wherein Cubic Li in X-ray diffraction measurement using CuKα radiation 6.25 Ga 0.25 La3Zr2O 12 Among the diffraction peaks, a diffraction peak corresponding to 2θ=30.9° was observed at 2θ=30.5° or more and 30.9° or less.
4. The Li ion conductor according to claim 1 or 2, wherein the lattice constant exceeds And for the following.
5. The Li ion conductor according to claim 1 or 2, wherein The activation energy Ea obtained by impedance measurement was 0.6 eV or less.
6. The Li ion conductor according to claim 1 or 2, wherein Li ion conductivity σ at room temperature obtained by impedance measurement total 1.0×10 -7 S / cm or more.
7. A method for manufacturing a Li ion conductor, characterized in that: The Li ion conductor has a garnet-type composite metal oxide phase (L) containing Li, La, Zr and O, and the Li ion conductor has diffraction peaks at 2θ=13.8°±1° and 2θ=15.2°±1° in an X-ray diffraction measurement using CuKα rays, In the production method, a mixture of a eutectic mixture having a melting point of 600° C. or less and a garnet-type composite metal oxide containing Li, La, Zr and O are molded, and the obtained molded product is heat-treated at 600° C. or less, thereby connecting the interface of the garnet-type composite metal oxide phase (L) using the eutectic mixture having a melting point of 600° C. or less, The eutectic mixture is a eutectic mixture of ZrCl4, AlCl3, NbCl5 or TaCl5 and LiCl, or a eutectic mixture of LiF and TaF5.