A nanomaterial film modified ITO sensor and preparation method thereof

By modifying the three-layer film of SnO2, graphene and gold nanoparticles on the ITO sensor, the problem of insufficient sensor detection performance and membrane stability is solved, and the detection effect with high sensitivity and low cost is achieved, simplifying the preparation process.

CN114414639BActive Publication Date: 2024-11-12BEIJING RESEARCH CENTER FOR AGRICULTURAL STANDARDS AND TESTING +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202111610115.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-27
Publication Date
2024-11-12
Estimated Expiration
2041-12-27

AI Technical Summary

Technical Problem

Existing ITO sensors have shortcomings in detection performance and membrane stability, and it is difficult to meet the needs of high sensitivity and reliability.

Method used

The preparation method of ITO sensor modified by three-layer films of SnO2, graphene and gold nanoparticles is adopted. The stable nanomaterial film is formed by acetone, isopropanol cleaning, SnO2 sol calcination, electrochemical reduction method and gold nanoparticle drop coating. .

Benefits of technology

It improves the stability, anti-interference and reproducibility of the sensor, achieves low-cost and high-sensitivity detection performance, simplifies the preparation process and reduces sample usage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114414639B_ABST
    Figure CN114414639B_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing a nanomaterial film-modified ITO sensor. The ITO sensor comprises an ITO conductive glass, and a first SnO2 modified film, a graphene film, and a gold nanoparticle modified film sequentially coated on the surface thereof. The nanomaterial film-modified ITO sensor can improve interface stability and anti-interference, has the advantage of good reproducibility, and has good research value for improving the existing ITO sensor film preparation method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of analytical chemistry and electrochemical sensing technology, and relates to a method for preparing a nanomaterial film-modified ITO sensor. The method can prepare an ITO sensor modified with three layers of SnO2 film, graphene film and gold nanoparticle film, thereby improving the detection performance of the ITO sensor. Background Art

[0002] Biosensors are a rapid detection technology developed in recent years. They have the advantages of being fast, simple, and portable, and can especially meet the needs of field detection methods. Compared with traditional solid carbon electrode and glassy carbon electrode sensors, ITO sensors are inexpensive, easy to prepare in batches, and flexible in design. They can meet different detection needs, have good parallelism between electrode batches, and have a simple activation process. They are increasingly favored by analysts and can also avoid the memory effect of conventional solid electrodes and the complicated and lengthy pretreatment process.

[0003] The key to sensor detection performance is the preparation of the sensing membrane. Nanomaterial sensing membrane can improve the detection sensitivity of the sensor, but the stability of the membrane is the key to ensuring the reliability of the detection results. Therefore, preparing a sensing membrane with high stability is the core of sensor preparation.

[0004] Therefore, the development of a new nanomaterial sensing film modified ITO sensor has important research significance and good application value for improving the existing membrane preparation method, and has broad application prospects in the field of analytical chemistry detection. Summary of the invention

[0005] In view of this, the present invention provides a nanomaterial film modified ITO sensor and a preparation method thereof, which has important research significance and good application value for improving the existing film preparation method.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A nanomaterial film modified ITO sensor, comprising:

[0008] ITO conductive glass;

[0009] A first SnO2 modified film is coated on the surface of the ITO conductive glass;

[0010] A second graphene film, modified on the surface of the first SnO2 modified film;

[0011] The third gold nanoparticle modified film is modified on the surface of the second graphene film.

[0012] Another object of the present invention is to provide a method for preparing a nanomaterial film-modified ITO sensor, comprising:

[0013] a) providing interface activated ITO conductive glass;

[0014] b) coating a first SnO2 modified film on the surface of the ITO conductive glass;

[0015] c) modifying the surface of the first SnO2 modified film with a second graphene film;

[0016] d) modifying the surface of the second graphene modified film with a third gold nanoparticle film.

[0017] Specifically, the preparation method comprises:

[0018] 1) Activation treatment of ITO conductive glass:

[0019] The ITO glass was cleaned with acetone, isopropanol and ultrapure water in sequence, and then dried in an oven for later use;

[0020] 2) Preparation of SnO2 modified film:

[0021] Apply 1.5-15% SnO2 sol to the surface of ITO glass and calcine in a muffle furnace at 300-650℃ for 1-6h;

[0022] 3) Preparation of graphene modified film:

[0023] The graphene oxide solution is applied to the SnO2 modified film, and after being dried naturally, the film is treated by electrochemical reduction for 1-60 min, washed with ultrapure water, dried with nitrogen, and set aside;

[0024] 4) Preparation of gold nanoparticle film:

[0025] The 4-mercaptobenzenediazonium tetrafluoroborate solution was drop-coated on the graphene modified film, left to stand for 1-24 hours, washed with ultrapure water, dried with nitrogen, and then a proper amount of gold nanoparticle solution was drop-coated on the above interface, then rinsed with phosphate buffer, and dried with nitrogen;

[0026] According to the above operation steps, the nanomaterial film modified ITO sensor was finally prepared.

[0027] Preferably, in the above step 1), the ITO glass is cleaned with acetone and isopropanol for 5 minutes each.

[0028] Preferably, the concentration of the SnO2 sol spin coating in the above step 2) is 10-15%.

[0029] Preferably, in the above step 2), the ratio of the SnO2 sol spin coating volume to the ITO spin coating area is greater than 5.

[0030] Preferably, the SnO2 modified film in the above step 2) is calcined at a temperature of 450°C.

[0031] Preferably, the concentration of the graphene oxide solution in the above step 3) is 0.5-1 mg / ml.

[0032] Preferably, the reduction potential of the electrochemical reduction method in the above step 3) is less than -0.2V.

[0033] The present invention also includes a nano material film ITO sensor prepared by the above method.

[0034] The nano material film ITO sensor prepared by the method of the present invention has high stability, strong anti-interference and good reproducibility. The preparation method also has the advantages of being simple and practical.

[0035] The present invention proposes a method for preparing a nanomaterial film ITO sensor, establishes, improves and develops a method for preparing a three-layer nanomaterial film ITO sensor of SnO2 film, graphene film and gold nanoparticle film, which is helpful to develop a new high-sensitivity, low-cost ITO sensor, and has important significance and good application value for improving existing detection technical means.

[0036] The present invention establishes a method for preparing a nanomaterial film ITO sensor, which has the advantages of short cycle, simple and rapid preparation, low cost, small sample amount, high sensitivity, etc., and provides a new method for preparing ITO sensing film, which is of great significance in improving existing sensor detection technology.

[0037] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:

[0038] 1) The SnO2 film forming method on the ITO surface of the present invention is simple and easy, and the film has good stability;

[0039] 2) The nanomaterial film ITO sensor prepared by the present invention has the advantages of low cost and high sensitivity;

[0040] 3) The nanomaterial film ITO sensor prepared by the present invention has the characteristics of high stability and easy batch preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0042] Figure 1 A diagram showing the effect of the SnO2 modified film ITO electrode prepared in Example 2 of the present invention.

[0043] Figure 2 Graphene oxide dispersion effect before and after ultrasonic treatment. DETAILED DESCRIPTION

[0044] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] If not specifically indicated, the technical means used in the embodiments are conventional means well known to those skilled in the art. The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0046] Example 1

[0047] Preparation of SnO2 sol coating solution

[0048] Prepare an aqueous solution containing TritonX-100 with a mass concentration of 0.03% with ultrapure water, vortex and shake evenly, take out 25 ml and add it to a glass beaker, then take 50 ml of SnO2 sol with a mass concentration of 15% and add it to the above glass beaker, stir evenly, and obtain a SnO2 sol spin coating liquid with a mass concentration of TritonX-100 of 0.01% and a mass concentration of SnO2 sol of 10%, which is recorded as liquid A;

[0049] Prepare an aqueous solution containing TritonX-100 with a mass concentration of 0.3% with ultrapure water, vortex and shake evenly, take out 25 ml and add it to a glass beaker, then take 50 ml of SnO2 sol with a mass concentration of 15% and add it to the above glass beaker, stir evenly, and obtain a SnO2 sol spin coating liquid with a mass concentration of 0.1% TritonX-100 and a mass concentration of 10% SnO2 sol, which is recorded as liquid B;

[0050] Prepare an aqueous solution containing 3% TritonX-100 by mass concentration with ultrapure water, vortex and shake evenly, take out 25 ml and add it to a glass beaker, then take 50 ml of SnO2 sol with a mass concentration of 15% and add it to the above glass beaker, stir evenly, and obtain a SnO2 sol spin coating liquid with a mass concentration of 1% TritonX-100 and a mass concentration of 10% SnO2 sol, which is recorded as liquid C;

[0051] Use ultrapure water to prepare an aqueous solution containing TritonX-100 with a mass concentration of 30%, vortex and shake evenly, take out 25 ml and add it to a glass beaker, then take 50 ml of SnO2 sol with a mass concentration of 15% and add it to the above glass beaker, stir evenly, and obtain a SnO2 sol spin coating liquid with a mass concentration of TritonX-100 of 10% and a mass concentration of SnO2 sol of 10%, recorded as liquid D.

[0052] Example 2

[0053] Preparation of SnO2 Modified ITO Electrode

[0054] 60 μL of the above coating solutions A, B, C, and D were applied to the ITO conductive glass interface, and then calcined at 450°C for 4 h to obtain SnO2 modified film ITO electrodes, which were marked as (a), (b), (c), and (d), respectively.

[0055] from Figure 1 It can be seen that when the concentration of TritonX-100 is less than 0.1%, a uniform SnO2 modified ITO film can be prepared. When the concentration of TritonX-100 is greater than 1%, a white opaque film appears on the ITO interface. The results show that SnO2 sol coating solution containing low concentration TritonX-100 can prepare a better SnO2 modified ITO film.

[0056] Example 3 Study on the influence of calcination temperature

[0057] The ITO modified film was prepared by using the coating liquid prepared in Example 2, and calcined at 25°C, 320°C, and 450°C, respectively, and then heated in a mixture containing 100nM Ru(bpy)2 2+ The photoelectrochemical signal was measured in sodium oxalate buffer solution. The results are shown in Table 1.

[0058] Table 1 Effect of calcination temperature on ITO film properties

[0059]

[0060] Example 4 Preparation of graphene oxide solution

[0061] Weigh a certain amount of nano-graphene oxide particles into a glass bottle, dilute with 0.01M phosphate buffer solution to 1mg / ml, vortex mix, and then treat in an ultrasonic instrument for 6 hours, take out, and place away from light for later use. Figure 2 shown.

[0062] As can be seen from Figure (a), the graphene oxide solution system did not disperse before ultrasonic treatment and agglomerated at the bottom of the test tube; as can be seen from Figure (b), after 6 hours of ultrasonic treatment, the graphene oxide was evenly dispersed in the system and the agglomeration phenomenon disappeared, indicating that this method can obtain a better graphene oxide dispersion solution that can be used for coating.

Claims

1. A nanomaterial film modified ITO sensor, comprising: ITO conductive glass; A first SnO2 modified film is coated on the surface of the ITO conductive glass; A second graphene film, modified on the surface of the first SnO2 modified film; A third gold nanoparticle modified film, modified on the surface of the second graphene film; The preparation method of a nanomaterial film-modified ITO sensor comprises: a) providing interface activated ITO conductive glass; b) coating a first SnO2 modified film on the surface of the ITO conductive glass; c) modifying the surface of the first SnO2 modified film with a second graphene film; d) modifying the surface of the second graphene modified film with a third gold nanoparticle film; Specifically include: 1) Activation treatment of ITO conductive glass: The ITO glass was cleaned with acetone, isopropanol and ultrapure water in sequence, and then dried in an oven for later use; 2) Preparation of SnO2 modified film: Apply 1.5-15% SnO2 sol to the ITO glass surface and calcine in a muffle furnace at 300-650℃ for 1-6h; 3) Preparation of graphene modified film: The graphene oxide solution is applied to the SnO2 modified film, and after being dried naturally, the film is treated by electrochemical reduction for 1-60 min, washed with ultrapure water, dried with nitrogen, and set aside; 4) Preparation of gold nanoparticle film: The 4-mercaptobenzenediazonium tetrafluoroborate solution was drop-coated on the graphene modified film, left to stand for 1-24 hours, washed with ultrapure water, dried with nitrogen, and then a proper amount of gold nanoparticle solution was drop-coated on the above interface, then rinsed with phosphate buffer, and dried with nitrogen; According to the above operation steps, the nanomaterial film modified ITO sensor was finally prepared.

2. A method for preparing a nanomaterial film-modified ITO sensor, comprising: a) providing interface activated ITO conductive glass; b) coating a first SnO2 modified film on the surface of the ITO conductive glass; c) modifying the surface of the first SnO2 modified film with a second graphene film; d) modifying the surface of the second graphene modified film with a third gold nanoparticle film; Specifically include: 1) Activation treatment of ITO conductive glass: The ITO glass was cleaned with acetone, isopropanol and ultrapure water in sequence, and then dried in an oven for later use; 2) Preparation of SnO2 modified film: Apply 1.5-15% SnO2 sol to the ITO glass surface and calcine in a muffle furnace at 300-650℃ for 1-6h; 3) Preparation of graphene modified film: The graphene oxide solution is applied to the SnO2 modified film, and after being dried naturally, the film is treated by electrochemical reduction for 1-60 min, washed with ultrapure water, dried with nitrogen, and set aside; 4) Preparation of gold nanoparticle film: The 4-mercaptobenzenediazonium tetrafluoroborate solution was drop-coated on the graphene modified film, left to stand for 1-24 hours, washed with ultrapure water, dried with nitrogen, and then a proper amount of gold nanoparticle solution was drop-coated on the above interface, then rinsed with phosphate buffer, and dried with nitrogen; According to the above operation steps, the nanomaterial film modified ITO sensor was finally prepared.

3. The preparation method according to claim 2, characterized in that: Preparation step 1) The ITO conductive glass is cleaned with acetone and isopropanol for 5 minutes each.

4. The preparation method according to claim 2, characterized in that: Preparation step 2) The SnO2 sol spin coating concentration is 10-15%.

5. The preparation method according to claim 2, characterized in that: Preparation step 2) The ratio of the SnO2 sol spin coating volume to the ITO spin coating area is greater than 5.

6. The preparation method according to claim 2, characterized in that: Preparation step 2) The SnO2 modified film is preferably calcined at a temperature of 450°C.

7. The preparation method according to claim 2, characterized in that: Preparation step 3) The concentration of the graphene oxide solution is 0.5~1 mg / ml.

8. The preparation method according to claim 2, characterized in that: Preparation step 3) The electrochemical reduction potential is less than -0.2V.

9. The nanomaterial film ITO sensor prepared by the method according to any one of claims 2 to 8.

Citation Information

Patent Citations

  • Biomolecular functionalized graphene / gold nano-particle composite film and preparation method thereof

    CN102504533A

  • Preparation method of glyphosate molecularly-imprinted electrochemical sensor

    CN106226370A

  • Construction and application of aptamer sensor taking nanogold / zinc oxide-graphene composite material as photoelectric sensitive element

    CN111562296A

  • Photoelectrochemical aptamer sensor and preparation method and application thereof

    CN112240898A

  • Room temperature hydrogen gas sensor

    US20190339227A1