A kind of micro-foamed PVC and its application in wood coating
By adding specific components to micro-foamed PVC and performing sealing and hot-pressing treatments, the problems of heavy metal poisoning, environmental pollution and low impact resistance of micro-foamed PVC are solved, achieving a combination of high toughness and impact resistance. material to avoid the decay and deformation of wood in humid environments.
Patent Information
- Application Number
- CN202210154455.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-21
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-02-21
AI Technical Summary
Micro-foamed PVC has risks of heavy metal poisoning and environmental pollution during use. At the same time, its impact strength is low and it is prone to decay, moisture absorption, deformation and cracking in humid environments.
Micro-hair foam using PVC resin powder, CPVC, tin methyl mercaptide, montmorillonite, polyethylene wax, calcium stearate, azodicarboxylic acid amine, sodium bicarbonate, PP flame retardant and ammonium polyphosphate. Foam PVC, melted by heating and attached to the wood, combined with sealing treatment and hot pressing treatment, improves toughness and impact resistance, and solves the sealing problem of wood ports.
It significantly improves the environmental performance, high temperature resistance, aging resistance and impact resistance of micro-foamed PVC, enhances the overall toughness and impact strength of the composite material, and avoids the problems of wood decay, hygroscopic deformation and cracking.
Smart Images

Figure 942451DEST_PATH_IMAGE001
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials, and in particular relates to a micro-foamed PVC and an application thereof. Background Art
[0002] Wood is an excellent green engineering material and industrial raw material. The consumption of wood is growing exponentially every year, and the shortage of wood resources is becoming increasingly severe. Therefore, it is particularly urgent to vigorously develop wood substitutes. Compared with conventional PVC resin, micro-foamed PVC (polyvinyl chloride) has a lower density, a fine pore structure inside, and a surface similar to natural wood. It is produced into profiles or plates through molding, injection molding or extrusion processing technology, which is called "synthetic wood". These synthetic woods are widely used in furniture, building materials, and decoration. Micro-foamed PVC has the advantages of being resistant to insect infestation, waterproof and anti-corrosion, and good wear resistance. Various colorants can also be added during molding to avoid paint pollution of wood. Moreover, micro-foamed PVC does not have the disadvantages of wood such as diagonal texture and knots. Therefore, using it to replace wood has broad development prospects in my country.
[0003] However, compared with traditional wood, micro-foamed PVC still has many areas that need to be improved. On the one hand, micro-foamed PVC contains lead salt stabilizers, which are easily enriched in the human body during use and cause heavy metal poisoning. In addition, the waste products after use still cause great pollution to the environment after decomposition. On the other hand, PVC resin is a polar non-crystalline polymer with strong interaction between molecules. It is a hard and brittle material with low impact strength and easy aging. It still needs to be impact-modified to replace wood.
[0004] The invention patent with the publication number CN105295222 A and the invention name "A new type of coated co-extruded wood-plastic composite material and its preparation method" uses polymer resin and wood powder or bamboo powder as the main raw materials, and coats it on the core layer through the coating co-extrusion process. However, the specific gravity of the wood powder or bamboo powder used is relatively small, and the degree of improvement in the toughness of the PVC resin is limited, and the characteristics of the wood cannot be better reflected; and increasing the specific gravity of the wood powder or bamboo powder may cause problems such as poor compatibility.
[0005] There are also examples of PVC composite materials covering natural wood in the prior art, but after covering, the ports of the covered products need to be processed to meet the aesthetics and durability during use. The traditional method is to spray hydrophobic or glue waterproof plastic sheets on the ports. However, due to the water absorption of wooden products themselves, when wood is used in a humid environment, the wood itself will absorb moisture from the air. Especially when the product is used in an outdoor environment, due to direct contact with the external environment, the wood is prone to swelling after absorbing water, and the sprayed hydrophobic or glued waterproof plastic sheets are prone to falling off and aging, resulting in poor port sealing effect, which makes it easy for the wood material to decay, deform due to moisture absorption, and crack. Summary of the invention
[0006] In view of this, the present invention provides a micro-foamed PVC with high environmental protection performance and the properties of high temperature resistance, aging resistance, strong impact resistance and the like.
[0007] Furthermore, the present invention also provides the use of the above-mentioned micro-foamed PVC in coating wood, so that the obtained composite material has good toughness and strong impact resistance. At the same time, by sealing the ports of the wood to be coated, the problems of easy decay, moisture absorption deformation and cracking of the wood are eliminated.
[0008] In order to solve the above problems, the present invention provides the following technical solutions:
[0009] The invention provides a micro-foamed PVC, which comprises the following components in parts by weight: 80-100 parts of PVC resin powder, 20-40 parts of CPVC, 3-8 parts of methyl tin mercaptide, 10-25 parts of montmorillonite, 3-6 parts of polyethylene wax, 2-5 parts of calcium stearate, 4.4-7.3 parts of azodicarbonamide, 1.6-2.7 parts of sodium bicarbonate, 1-3 parts of PP flame retardant and 1-3 parts of ammonium polyphosphate.
[0010] Preferably, 2 to 6 parts of colorant are also included.
[0011] The present invention provides the use of the micro-foamed PVC described in the above scheme in coating wood.
[0012] Preferably, the method for coating wood comprises the following steps:
[0013] 1) Sealing the wood ends to obtain the wood to be coated;
[0014] 2) The micro-foamed PVC is heated to a molten state, and the molten micro-foamed PVC is attached to the wood to be coated in step 1) to obtain a composite material of PVC coated wood.
[0015] Preferably, the sealing liquid for sealing treatment in step 1) comprises the following components in parts by weight: 40.5 parts of styrene, 38.9 parts of methyl methacrylate, 20.6 parts of acrylonitrile, 0.5-1.1 parts of benzoyl peroxide, 5-7 parts of paraffin emulsion, 1.6-3.7 parts of melamine phosphate, 1.4-3.3 parts of pentaerythritol and 2-5 parts of polyoxyethylene octylphenol ether-10.
[0016] Preferably, the sealing liquid further comprises 2 to 7 parts of pigment by weight.
[0017] Preferably, the sealing treatment method in step 1) comprises the following steps:
[0018] (1) impregnating the wood end with a sealing liquid to obtain an impregnated wood;
[0019] (2) The impregnated wood of step (1) is heated at 85-100° C. for 2-3.5 h and dried to obtain the wood to be coated.
[0020] Preferably, the impregnation is carried out under vacuum pressure conditions; the vacuum degree of the vacuum pressure conditions is 0.05-0.2 MPa and the pressure is 0.8-1 MPa.
[0021] Preferably, in the step 1), before the sealing treatment, the process further comprises performing a groove treatment on the wood along the longitudinal direction of the wood.
[0022] Preferably, after obtaining the PVC-coated wood composite material, the method further comprises subjecting the composite material to hot pressing treatment; the hot pressing time is 5 to 10 min, the hot pressing pressure is 1 to 3 MPa, and the hot pressing temperature is 80 to 90°C.
[0023] The present invention provides a micro-foamed PVC. Adding CPVC to the micro-foamed PVC component provided by the present invention can make the pores evenly distributed and of appropriate size, and improve the high temperature resistance and aging resistance of the product. Methyl tin mercaptan is used to replace the lead salt stabilizer to improve the environmental protection performance of PVC. At the same time, polyethylene (PE) wax and calcium stearate are added as lubricants to overcome the shortcomings of poor lubricity and easy adhesion of methyl tin mercaptan during processing. Methyl tin mercaptan is well compatible with PVC resin powder and other additives, and improves the transparency and long-term thermal stability of the product. PP flame retardant and APP (ammonium polyphosphate) are prepared in proportion as a composite flame retardant, so that the oxygen index of the composite material is significantly improved, and the combustion characteristic values such as heat release rate, average mass loss rate and effective combustion calorific value in the whole combustion process are significantly reduced.
[0024] Furthermore, the present invention also provides the use of the above-mentioned micro-foamed PVC in coating wood. In the present invention, wood is used as the core material and coated in the micro-foamed PVC. The wood has strong toughness. Using wood as the core material improves the overall impact strength of the composite material. At the same time, the present invention also provides a sealing liquid for sealing the wood port, which plays a role in fire prevention, waterproofing, and aging resistance. Before the micro-foamed PVC is coated on the wood, the wood port is further sealed to isolate the wood from the external environment, thereby solving the problems of wood decay, moisture absorption deformation, and cracking. DETAILED DESCRIPTION
[0025] The invention provides a micro-foamed PVC, which comprises the following components in parts by weight: 80-100 parts of PVC resin powder, 20-40 parts of CPVC, 3-8 parts of methyl tin mercaptide, 10-25 parts of montmorillonite, 3-6 parts of polyethylene wax, 2-5 parts of calcium stearate, 4.4-7.3 parts of azodicarbonamide, 1.6-2.7 parts of sodium bicarbonate, 1-3 parts of PP flame retardant and 1-3 parts of ammonium polyphosphate.
[0026] The micro-foamed PVC provided by the present invention comprises 80 to 100 parts by weight of PVC resin powder, preferably 90 parts. In the present invention, the PVC resin powder is selected from PVC resin powder with a molecular weight of 20,000 provided by Zhengzhou Binhai Chemical.
[0027] The micro-foamed PVC provided by the present invention includes CPVC, which includes 20 to 40 parts by weight, preferably 30 parts. In the present invention, the CPVC is a processing modifier, which can make the pore size suitable and evenly distributed during foaming, and improve the high temperature resistance and aging resistance of the product. The present invention has no special limitation on the source of the CPVC, and conventional commercial products in the field can be used. In the embodiment of the present invention, it is purchased from Lanxi Tangzhengge Plastic Products Factory.
[0028] The micro-foamed PVC provided by the present invention includes 3 to 8 parts by weight of tin methyl mercaptan, preferably 5 parts. In the present invention, the tin methyl mercaptan is a heat stabilizer. The present invention has no special restrictions on the source of the tin methyl mercaptan, and conventional commercial products in the field can be used. In the embodiment of the present invention, it is purchased from Songteng Polymer Materials Co., Ltd.
[0029] The micro-foamed PVC provided by the present invention includes montmorillonite, which is calculated by weight and includes 10 to 25 parts, preferably 20 parts. In the present invention, the montmorillonite can change the processing performance of PVC and improve the thermal stability of the product. The present invention has no special limitation on the source of the montmorillonite, and a conventional commercial product in the field can be used. In the embodiment of the present invention, it is purchased from Shijiazhuang Chenxi Refractory Materials Co., Ltd.
[0030] The micro-foamed PVC provided by the present invention includes polyethylene (PE) wax, which includes 3 to 6 parts by weight, preferably 4 parts. The present invention has no special limitation on the source of the PE wax, and a conventional commercial product in the art can be used. In the embodiment of the present invention, the PE wax is purchased from Jiangxi Fumei Technology Development Co., Ltd.
[0031] The micro-foamed PVC provided by the present invention includes calcium stearate, which is calculated by weight, including 2 to 5 parts, preferably 3 parts. In the present invention, the calcium stearate and PE wax are used as lubricants to overcome the shortcomings of poor lubricity and easy adhesion during processing of methyl mercaptan tin. The present invention has no special restrictions on the source of the calcium stearate, and conventional commercial products in the field can be used. In the embodiments of the present invention, it is purchased from Zhengzhou Huixi Chemical Products Co., Ltd.
[0032] The micro-foamed PVC provided by the present invention includes 4.4 to 7.3 parts of azodicarboxylic acid amide, preferably 5.9 parts. The present invention has no special limitation on the source of the azodicarboxylic acid amide, and a conventional commercial product in the art can be used. In the embodiment of the present invention, it is purchased from Zhengzhou Xingchang Chemical Products Co., Ltd.
[0033] The micro-foamed PVC provided by the present invention includes sodium bicarbonate, which is 1.6 to 2.7 parts by weight, preferably 2.2 parts. In the present invention, the sodium bicarbonate is mixed with azodicarboxylic acid amide in proportion to play the role of a foaming agent. The present invention has no special limitation on the source of the azodicarboxylic acid amide, and a conventional commercial product in the field can be used.
[0034] The micro-foamed PVC provided by the present invention includes PP flame retardant, which includes 1 to 3 parts by weight, preferably 2 parts. The present invention has no special limitation on the source of the PP flame retardant, and a conventional commercial product in the field can be used. In the embodiment of the present invention, it is purchased from Foshan Kangfu New Materials Co., Ltd.
[0035] The micro-foamed PVC provided by the present invention includes ammonium polyphosphate, which includes 1 to 3 parts by weight, preferably 2 parts. In the present invention, the PP flame retardant and APP (ammonium polyphosphate) are prepared in proportion as a composite flame retardant, which can significantly improve the oxygen index of the composite material, and significantly reduce the combustion characteristic values such as the heat release rate, average mass loss rate and effective combustion calorific value during the entire combustion process. The present invention does not specifically limit the source of the ammonium polyphosphate, and conventional commercial products in the field can be used. In the embodiment of the present invention, it is purchased from Zhengzhou Haorong Chemical Products Co., Ltd.
[0036] The micro-foamed PVC provided by the present invention preferably further comprises a colorant, preferably 2 to 6 parts by weight, more preferably 5 parts. The present invention has no particular limitation on the source of the colorant, and conventional commercial products in the art can be used.
[0037] The present invention also provides the use of the micro-foamed PVC described in the above scheme in coating wood.
[0038] In the present invention, the method for coating wood preferably comprises the following steps:
[0039] 1) Sealing the wood ends to obtain the wood to be coated;
[0040] 2) The micro-foamed PVC is heated to a molten state, and the molten micro-foamed PVC is attached to the wood to be coated in step 1) to obtain a composite material of PVC coated wood.
[0041] In the present invention, the wood end is preferably sealed to obtain the wood to be coated. In the present invention, before the sealing treatment, it is preferred to further include a groove treatment along the longitudinal direction (long axis direction) of the wood, more preferably a ring-shaped or semi-ring-shaped groove treatment. In the present invention, the uniform groove treatment on the wood surface can allow PVC to be further filled into the groove during the further coating process, thereby promoting the close combination of PVC and wood. In the present invention, the wood is preferably natural wood, more preferably poplar or fir.
[0042] In the present invention, the sealing liquid for sealing treatment preferably includes the following components in parts by weight: 40.5 parts of styrene, 38.9 parts of methyl methacrylate, 20.6 parts of acrylonitrile, 0.5-1.1 parts of benzoyl peroxide, 5-7 parts of paraffin emulsion, 1.6-3.7 parts of melamine phosphate, 1.4-3.3 parts of pentaerythritol and 2-5 parts of polyoxyethylene octylphenol ether-10, more preferably 40.5 parts of styrene, 38.9 parts of methyl methacrylate, 20.6 parts of acrylonitrile, 0.7 parts of benzoyl peroxide, 6 parts of paraffin emulsion, 3.2 parts of melamine phosphate, 2.8 parts of pentaerythritol and 4 parts of polyoxyethylene octylphenol ether-10. In the present invention, the sealing liquid preferably also includes 2-7 parts of pigment, more preferably 5 parts.
[0043] In the present invention, the styrene, methyl methacrylate and acrylonitrile are mixed into a mixed resin liquid in proportion and then polymerized to play a sealing role. The benzoyl oxide and paraffin emulsion are polymerization initiators, which initiate the polymerization reaction under heating conditions. Melamine phosphate and pentaerythritol are mixed into a composite flame retardant in proportion to play a flame retardant function. Polyoxyethylene octylphenol ether (PP)-10 plays the role of an emulsifier.
[0044] The present invention has no special limitation on the sources of the components in the sealing liquid. Conventional commercial products in the art can be used. In the embodiments of the present invention, styrene (Zhangjiagang Free Trade Zone Zerunxin Chemical Trading Co., Ltd.), methyl methacrylate (Weihai Xinyuan Chemical Co., Ltd.), acrylonitrile (Tianjin Shengtongtai Chemical Co., Ltd.), benzoyl peroxide (Guangxi Nanning Liandan Chemical Co., Ltd.), paraffin emulsion (Nanjing Tianshi New Materials Technology Co., Ltd.), melamine phosphate (Shanghai Suisi Chemical Technology Co., Ltd.), pentaerythritol (Jinan Haobang Chemical Co., Ltd.) and polyoxyethylene octylphenol ether-10 (Jinan Xinyuda Trading Co., Ltd.) were purchased.
[0045] In the present invention, the sealing method preferably comprises the following steps:
[0046] (1) impregnating the wood end with a sealing liquid to obtain an impregnated wood;
[0047] (2) The impregnated wood of step (1) is heated at 85-100° C. for 2-3.5 h and dried to obtain the wood to be coated.
[0048] The present invention preferably impregnates the wood end with a sealing liquid to obtain impregnated wood. In the present invention, the impregnation time is preferably 15-25 minutes. The impregnation is preferably carried out under vacuum pressure conditions; the vacuum degree of the vacuum pressure conditions is preferably 0.05-0.2 MPa, and the pressure is 0.8-1 MPa.
[0049] After obtaining the impregnated wood, the present invention preferably heats the impregnated wood at 85-100°C for 2-3.5 hours and dries to obtain the wood to be coated. In the present invention, the heating temperature is preferably 90-95°C; the heating time is preferably 3 hours. In the present invention, a polymerization reaction is initiated under heating conditions, and the sealing liquid is polymerized, so that the sealing liquid is sealed on the wood. In the present invention, the drying method is preferably natural drying.
[0050] After obtaining the wood to be coated, the present invention preferably heats the micro-foamed PVC to a molten state, and attaches the molten micro-foamed PVC to the wood to be coated to obtain a composite material of PVC coated wood. In the present invention, preferably, each component of the micro-foamed PVC is put into an extruder, and the micro-foamed PVC is heated in the barrel by an electric heating device, and decomposes when it reaches or exceeds its critical temperature, releasing N2, CO and CO2 to play a foaming role, extruding through a mold and attaching to the surface of the coated core material passing through the mold, to obtain a composite material of PVC coated wood.
[0051] In the present invention, after obtaining the composite material of PVC coated wood, it is preferred that the composite material is subjected to hot pressing. In the present invention, the time of the hot pressing is preferably 5 to 10 min, the pressure of the hot pressing is preferably 1 to 3 MPa, and the temperature of the hot pressing is preferably 80 to 90° C. In the present invention, the hot pressing is preferably performed using a calender. In the present invention, hot pressing can promote full fusion of PVC and wood.
[0052] The present invention is described in detail below by way of examples, it should be understood that these examples are only for illustrative purposes and in no way limit the scope of protection of the present invention. It should be understood by those skilled in the art that the details and forms of the technical solution of the present invention can be modified or replaced without departing from the spirit and periphery of the present invention, but these modifications or replacements all fall within the scope of protection of the present invention.
[0053] Example 1
[0054] Poplar wood is used as the core, and annular grooves are evenly distributed along the longitudinal direction (long axis direction) of the wood. The end of the wood is immersed in the sealing liquid of the impregnation tank (by weight, the sealing liquid includes the following components by weight: 40.5 parts of styrene, 38.9 parts of methyl methacrylate, 20.6 parts of acrylonitrile, 0.7 parts of benzoyl peroxide, 6 parts of paraffin emulsion, 5 parts of white titanium dioxide, 3.2 parts of melamine phosphate, 2.8 parts of pentaerythritol and 4 parts of OP-10), and the impregnation is carried out for 15-25 minutes under the conditions of vacuum degree of 0.05-0.2MPa and pressure of 0.8-1MPa to obtain impregnated wood. The obtained impregnated wood is heated at 95°C for 3 hours to initiate polymerization and sealing, and then dried naturally after sealing to obtain the wood to be coated.
[0055] The micro-foamed PVC raw material (the micro-foamed PVC includes the following components in parts by weight: 100 parts of PVC resin powder, 30 parts of CPVC, 5 parts of methyl tin mercaptide, 20 parts of montmorillonite, 4 parts of PE wax, 3 parts of calcium stearate, 7.3 parts of azodicarbonamide, 2.7 parts of sodium bicarbonate, 1 part of PP flame retardant, 1 part of ammonium polyphosphate, and 2 parts of titanium dioxide colorant) is uniformly stirred and then fed into an extrusion die, is molten by an electric heating device, is extruded through the die and adheres to the surface of the coated wood passing through the die, so as to obtain a composite material of PVC-coated wood.
[0056] Example 2
[0057] The fir wood is used as the core, and semi-circular grooves are evenly distributed along the longitudinal direction (long axis direction) of the wood. The end of the wood is immersed in the sealing liquid of the impregnation tank (the sealing liquid includes the following components by weight: 40.5 parts of styrene, 38.9 parts of methyl methacrylate, 20.6 parts of acrylonitrile, 1.1 parts of benzoyl peroxide, 5 parts of paraffin emulsion, 2 parts of white titanium dioxide, 1.6 parts of melamine phosphate, 1.4 parts of pentaerythritol and 5 parts of OP-10), and the impregnation is carried out for 15-25 minutes under the conditions of vacuum degree of 0.05-0.2 MPa and pressure of 0.8-1 MPa to obtain impregnated wood. The obtained impregnated wood is heated at 85°C for 3.5 hours to initiate polymerization and sealing, and is naturally dried after sealing to obtain the wood to be coated.
[0058] The micro-foamed PVC raw material (the micro-foamed PVC includes the following components in parts by weight: 80 parts of PVC resin powder, 40 parts of CPVC, 8 parts of methyl tin mercaptan, 25 parts of montmorillonite, 6 parts of PE wax, 2 parts of calcium stearate, 4.4 parts of azodicarbonamide, 1.6 parts of sodium bicarbonate, 3 parts of PP flame retardant, 2 parts of ammonium polyphosphate, and 5 parts of titanium dioxide colorant)
[0059] After being stirred evenly, it is sent to an extrusion die, becomes a molten state through an electric heating device, is extruded through the die and adheres to the surface of the wood with coating passing through the die, and a composite material of PVC coated wood is obtained. The composite material of PVC coated wood is heated by a calender, the hot pressing time is 5 min, the pressure is 2 MPa, and the temperature is 90°C, and then naturally cooled to obtain the final product of the PVC coated wood composite material.
[0060] Example 3
[0061] The fir wood is used as the core, and semi-circular grooves are evenly distributed along the longitudinal direction (long axis direction) of the wood. The end of the wood is immersed in the sealing liquid of the impregnation tank (the sealing liquid includes the following components by weight: 40.5 parts of styrene, 38.9 parts of methyl methacrylate, 20.6 parts of acrylonitrile, 0.5 parts of benzoyl peroxide, 7 parts of paraffin emulsion, 7 parts of white titanium dioxide, 3.7 parts of melamine phosphate, 3.3 parts of pentaerythritol and 2 parts of OP-10), and the impregnation is carried out for 15-25 minutes under the conditions of vacuum degree of 0.05-0.2 MPa and pressure of 0.8-1 MPa to obtain impregnated wood. The obtained impregnated wood is heated at 85°C for 3.5 hours to initiate polymerization and sealing, and is naturally dried after sealing to obtain the wood to be coated.
[0062] The micro-foamed PVC raw material (the micro-foamed PVC includes the following components in parts by weight: 90 parts of PVC resin powder, 20 parts of CPVC, 3 parts of methyl tin mercaptan, 10 parts of montmorillonite, 3 parts of PE wax, 5 parts of calcium stearate, 5.9 parts of azodicarbonamide, 2.2 parts of sodium bicarbonate, 2 parts of PP flame retardant, 3 parts of ammonium polyphosphate, and 6 parts of titanium dioxide colorant) is stirred.
[0063] After being mixed evenly, it is sent to an extrusion die, becomes a molten state through an electric heating device, is extruded through the die and adheres to the surface of the wood with coating passing through the die, and a composite material of PVC coated wood is obtained. The composite material of PVC coated wood is heated by a calender, the hot pressing time is 10 min, the pressure is 3 MPa, and the temperature is 80°C, and then naturally cooled to obtain the final product of the composite material of PVC coated wood.
[0064] Example 4
[0065] The performance of the PVC-coated wood composite materials prepared in Examples 1 to 3 was tested.
[0066] (1) Test item: Light aging test - xenon radiation exposure
[0067] Sample description: White plastic parts
[0068] Test method: GB / T 16422.2-2014 cycle 1
[0069] Test conditions: Test cycle:
[0070] Radiation: (0.51±0.02)W / (㎡.nm)@340nm
[0071] Lighting: 102min, black mark temperature: (65±3)℃, relative humidity: (50±10)%
[0072] Lighting and spraying: 18min
[0073] Filter: Boro / Boro
[0074] Exposure time: 300 hours
[0075] Test results:
[0076]
[0077] Remark:
[0078] 1. Size change = size after test - size before test (the distance between the two points with the highest measurement).
[0079] 2. Intermediate sampling and post-test results are obtained within 1 hour after the above specified exposure period.
[0080] (2) Test item: vertical combustion
[0081] Sample description: White plastic parts
[0082] Test method: UL 94-2013 Rev.9-2018 Section 8
[0083] Test conditions:
[0084] Sample: 125mm×12.77mm×9.62mm
[0085] Test results:
[0086] The afterflame time of a single sample is 10s. Under any state adjustment, the total afterflame time is 10s. After the second application of flame, the afterflame time of a single sample plus the afterglow time is 2.0s. The afterflame or afterglow of any sample does not spread to the fixture, and the burning particles or drippings do not ignite the absorbent cotton, which meets the V-0 grade.
[0087] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for coating wood with micro-foamed PVC, characterized in that: The micro-foamed PVC comprises the following components in parts by weight: 80-100 parts of PVC resin powder, 20-40 parts of CPVC resin, 3-8 parts of methyl tin mercaptan, 10-25 parts of montmorillonite, 3-6 parts of polyethylene wax, 2-5 parts of calcium stearate, 4.4-7.3 parts of azodicarbonamide, 1.6-2.7 parts of sodium bicarbonate, 1-3 parts of PP flame retardant and 1-3 parts of ammonium polyphosphate; The method of cladding wood comprises the following steps: 1) Sealing the wood ends to obtain the wood to be coated; 2) heating the micro-foamed PVC to a molten state, and attaching the molten micro-foamed PVC to the wood to be coated in step 1) to obtain a composite material of PVC coated wood; The sealing liquid for sealing treatment in step 1) comprises the following components in parts by weight: 37-43 parts of styrene, 35-42 parts of methyl methacrylate, 17-23 parts of acrylonitrile, 0.5-1.1 parts of benzoyl peroxide, 5-7 parts of paraffin emulsion, 1.6-3.7 parts of melamine phosphate, 1.4-3.3 parts of pentaerythritol and 2-5 parts of polyoxyethylene octylphenol ether-10; in step 1), before the sealing treatment, the wood is grooved along the longitudinal direction of the wood; The sealing method comprises the following steps: (1) impregnating the wood end with a sealing liquid to obtain an impregnated wood; (2) heating the impregnated wood in step (1) at 85-100° C. for 2-3.5 h and drying to obtain the wood to be coated; the impregnation is carried out under vacuum pressure conditions; the vacuum degree of the vacuum pressure conditions is 0.05 MPa and the pressure is 0.8-1 MPa; After obtaining the PVC-coated wood composite material, the method further comprises subjecting the composite material to hot pressing treatment; the hot pressing time is 5 to 10 minutes, the hot pressing pressure is 1 to 3 MPa, and the hot pressing temperature is 80 to 90°C.
2. The method according to claim 1, characterized in that The micro-foamed PVC also includes 2 to 6 parts of colorant.
3. The method according to claim 1, characterized in that The sealing liquid also includes 2 to 7 parts of pigment by weight.