Resin Composition
By adding epoxy resin, a specific curing agent, polyester polyol resin, and inorganic filler to the resin composition, the warping and flow mark problems of insulating materials are solved, and a cured product with high bonding strength and low linear thermal expansion coefficient is achieved, which is suitable for semiconductor chip packaging and circuit boards of small high-function electronic devices.
Patent Information
- Application Number
- CN202111242312.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-10-27
- Filing Date
- 2021-10-25
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2041-10-25
AI Technical Summary
In the prior art, the cured insulating material is prone to warping and flow marks in sealing applications. At the same time, its bonding strength with other layers and its coefficient of linear thermal expansion are relatively high, making it difficult to meet the needs of small, high-performance electronic devices.
By adding epoxy resin, a specific curing agent, a polyester polyol resin with an aliphatic structure, and inorganic fillers to a resin composition, the proportions and structure of each component are controlled to form a cured product that inhibits warping and flow marks.
It achieves high bonding strength with other layers, low coefficient of linear thermal expansion, and suppresses warping and flow marks in the cured product, making it suitable for semiconductor chip packaging and circuit boards for small, high-performance electronic devices.
Smart Images

Figure BDA0003319634980000271
Abstract
Description
Technical Field
[0001] This invention relates to resin compositions. More specifically, it relates to resin sheets, circuit boards, semiconductor chip packages, and semiconductor devices obtained using the resin compositions. Background Technology
[0002] In recent years, the demand for small, high-performance electronic devices such as smartphones and tablets has increased, leading to a greater demand for higher functionality in the insulating materials used in the packaging of semiconductor chips in these devices. Such insulating layers are known to be formed by curing resin compositions (see, for example, Patent Document 1).
[0003] Existing technical documents Patent documents Patent Document 1: Japanese Patent Application Publication No. 2017-008312. Summary of the Invention
[0004] The technical problem that the invention aims to solve For insulating materials used in sealing applications, it is desirable to suppress warping of the cured material and to reduce flow marks. Furthermore, for the sealing layer, high bonding strength with other layers and a low coefficient of linear thermal expansion (CTE) are also desirable.
[0005] The objective of this invention is to provide a resin composition that yields a cured product with high bonding strength to other layers, low coefficient of linear thermal expansion, and suppressed warpage and flow marks; and resin sheets, circuit boards, semiconductor chip packages, and semiconductor devices obtained using the resin composition.
[0006] Methods for solving problems The inventors have conducted intensive research on the above-mentioned problems and have found that by including epoxy resin, a specified curing agent, a specified amount of polyester polyol resin having an aliphatic structure, and an inorganic filler in the resin composition, the above-mentioned problems can be solved, thereby completing the present invention.
[0007] That is, the present invention includes the following: [1] A resin composition comprising the following components (A) to (D): (A) Epoxy resin, (B) A curing agent selected from at least one of acid anhydride curing agents, amine curing agents, and phenolic curing agents. (C) Polyester polyol resins with aliphatic structures, and (D) Inorganic filler materials, Wherein, when the non-volatile component in the resin composition is set to 100% by mass, the content of component (C) is more than 1% by mass and less than 20% by mass; [2] The resin composition according to [1], wherein component (A) comprises a fused ring backbone; [3] The resin composition according to [1] or [2], wherein the terminal of component (C) is either a hydroxyl group or a carboxyl group; [4] The resin composition according to any one of [1] to [3], wherein component (C) is a resin having a structure derived from polyester and a structure derived from polyol; [5] The resin composition according to [4], wherein the structure derived from the polyol comprises any one of an ethylene oxide structure, a propylene oxide structure and a butene oxide structure; [6] The resin composition according to any one of [1] to [5], wherein when the non-volatile component in the resin composition is set to 100% by mass, the content of component (D) is 60% by mass or more; [7] The resin composition according to any one of [1] to [6] is used for a sealing layer; [8] A resin sheet comprising: Support body, and A resin composition layer comprising any one of [1] to [7] disposed on the support; [9] A circuit board comprising a cured layer formed using a cured resin composition of any one of [1] to [7];
[10] A semiconductor chip package comprising: [9] The circuit board and Semiconductor chips mounted on the circuit board;
[11] A semiconductor chip package comprising a semiconductor chip sealed with a resin composition of any one of [1] to [7] or a resin sheet of [8];
[12] A semiconductor device comprising the semiconductor chip package described in
[10] or
[11] .
[0008] The effects of the invention According to the present invention, a resin composition is provided that yields a cured product with high bonding strength to other layers, low coefficient of linear thermal expansion, and suppressed warpage and flow marks; resin sheets, circuit boards, semiconductor chip packages, and semiconductor devices are obtained using the resin composition. Detailed Implementation
[0009] The present invention will now be described in detail with reference to its preferred embodiments. However, the present invention is not limited to the embodiments and examples described below, and can be implemented in any way without departing from the scope of the claims and their equivalents.
[0010] [Resin Composition] The resin composition comprises (A) an epoxy resin, (B) at least one curing agent selected from anhydride-based, amine-based, and phenol-based curing agents, (C) a polyester polyol resin having an aliphatic structure, and (D) an inorganic filler, wherein when the non-volatile component in the resin composition is set to 100% by mass, the content of component (C) is 1% by mass or more and 20% by mass or less. According to this resin composition, a cured product with high bonding strength to other layers, low coefficient of linear thermal expansion, and suppressed warpage and flow marks can be obtained.
[0011] The resin composition may further include any component in combination with components (A) to (D). Examples of such components include, for example, (E) a curing accelerator and (F) other additives. The components contained in the resin composition will be described in detail below.
[0012] <(A) Epoxy Resin> The resin composition contains epoxy resin (A) as component (A). Examples of epoxy resin (A) include, for example, bixylenol type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol AF type epoxy resin, dicyclopentadiene type epoxy resin, triphenol type epoxy resin, naphtholnovolac type epoxy resin, phenol novolac type epoxy resin, tert-butylcatechol type epoxy resin, naphthol type epoxy resin, anthracene type epoxy resin, glycidylamine type epoxy resin, glycidyl ester type epoxy resin, and cresol phenolic resin. Novolac type epoxy resins, biphenyl type epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, epoxy resins containing spirocyclic rings, cyclohexane type epoxy resins, cyclohexanediethanol type epoxy resins, naphthyl ether type epoxy resins, trimethylolpropionic acid type epoxy resins, tetraphenylethane type epoxy resins, glycidyl ether type epoxy resins, etc. As component (A), from the viewpoint of significantly obtaining the effects of the present invention, it is preferably selected from one or more of naphthyl type epoxy resins, alicyclic epoxy resins, and glycidyl ether type epoxy resins, more preferably any one of naphthyl type epoxy resins and alicyclic epoxy resins. As epoxy resin (A), it is preferably a fused-ring skeleton comprising naphthyl type epoxy resins, naphthol type epoxy resins, anthracene type epoxy resins, etc. Epoxy resins can be used alone or in combination of two or more.
[0013] For the resin composition, as epoxy resin (A), it is preferable to include epoxy resin having two or more epoxy groups in one molecule. From the viewpoint of significantly obtaining the desired effects of the present invention, the proportion of epoxy resin having two or more epoxy groups in one molecule is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more, relative to 100% by mass of the non-volatile component of epoxy resin (A).
[0014] Epoxy resins include epoxy resins that are liquid at a temperature of 20°C (hereinafter, sometimes referred to as "liquid epoxy resins") and epoxy resins that are solid at a temperature of 20°C (hereinafter, sometimes referred to as "solid epoxy resins"). In the resin composition, as epoxy resin (A), liquid epoxy resins or solid epoxy resins can be used, and liquid epoxy resins and solid epoxy resins can be used in combination. From the viewpoint of significantly obtaining the effects of the present invention, it is preferable to use only liquid epoxy resins.
[0015] As a liquid epoxy resin, it is preferable to be a liquid epoxy resin having two or more epoxy groups in one molecule.
[0016] As liquid epoxy resins, preferred are bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AF type epoxy resins, naphthalene type epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, phenolic varnish type epoxy resins, alicyclic epoxy resins with ester skeletons, cyclohexane type epoxy resins, cyclohexanediol type epoxy resins, glycidyl amine type epoxy resins, glycidyl ether type epoxy resins, glycidyl ether type epoxy resins, and epoxy resins with butadiene structures; more preferably are naphthalene type epoxy resins, alicyclic epoxy resins, and glycidyl ether type epoxy resins.
[0017] Specific examples of liquid epoxy resins include: DIC's "HP4032", "HP4032D", and "HP4032SS" (naphthalene-type epoxy resin); Mitsubishi Chemical's "828US", "jER828EL", "825", and "EPIKOTE828EL" (bisphenol A type epoxy resin); Mitsubishi Chemical's "jER807" and "1750" (bisphenol F type epoxy resin); Mitsubishi Chemical's "jER152" (phenolic varnish type epoxy resin); Mitsubishi Chemical's "630" and "630LSD" (glycidylamine type epoxy resin); Nippon Steel Chemical Materials Co., Ltd.'s "ZX1059" (a mixture of bisphenol A and bisphenol F type epoxy resins); Nagase ChemteX's "EX-721" (glycidyl ester type epoxy resin); and Daicel's "Celloxide"... 2021P (alicyclic epoxy resin with an ester skeleton); PB-3600 (butadiene-structured epoxy resin) manufactured by Daicel Corporation; ZX1658 and ZX1658GS (liquid 1,4-glycidylcyclohexane type epoxy resin) manufactured by Nippon Steel Chemical Materials Co., Ltd.; and EX-992LEX and EX-992L (glycidyl ester type epoxy resin) manufactured by Nagase ChemteX. These can be used individually or in combination of two or more.
[0018] As a solid epoxy resin, it is preferable to be a solid epoxy resin having three or more epoxy groups in one molecule, and more preferably an aromatic solid epoxy resin having three or more epoxy groups in one molecule.
[0019] As solid epoxy resins, the preferred types are xylenol-type epoxy resins, naphthalene-type epoxy resins, naphthalene-type tetrafunctional epoxy resins, cresol-phenolic varnish-type epoxy resins, dicyclopentadiene-type epoxy resins, triphenol-type epoxy resins, naphthol-type epoxy resins, biphenyl-type epoxy resins, naphthylene ether-type epoxy resins, anthracene-type epoxy resins, bisphenol A-type epoxy resins, bisphenol AF-type epoxy resins, and tetraphenylethane-type epoxy resins.
[0020] Specific examples of solid epoxy resins include DIC's "HP4032H" (naphthalene-type epoxy resin); DIC's "HP-4700" and "HP-4710" (naphthalene-type tetrafunctional epoxy resins); DIC's "N-690" (cresol phenolic varnish type epoxy resin); DIC's "N-695" (cresol phenolic varnish type epoxy resin); and DIC's "HP-7200," "HP-7200HH," and "HP-720..." 0H (dicyclopentadiene type epoxy resin); DIC's "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", "HP6000" (naphthyl ether type epoxy resin); Nippon Kayaku Co., Ltd.'s "EPPN-502H" (triphenol type epoxy resin); Nippon Kayaku Co., Ltd.'s "NC7000L" (naphthol phenolic varnish type epoxy resin); Nippon Kayaku Co., Ltd.'s "NC3000" H, NC3000, NC3000L, NC3100 (biphenyl type epoxy resin); Nippon Steel Chemical Materials Co., Ltd.'s "ESN475V" (naphthol type epoxy resin); Nippon Steel Chemical Materials Co., Ltd.'s "ESN485" (naphthol phenolic varnish type epoxy resin); Mitsubishi Chemical Co., Ltd.'s "YX4000H", "YX4000", "YL6121" (biphenyl type epoxy resin); Mitsubishi Chemical Co., Ltd.'s "YX4000HK" (bixylenol type epoxy resin). These include: resins such as Mitsubishi Chemical's "YX8800" (anthracene-type epoxy resin); Osaka Gas Chemical's "PG-100" and "CG-500"; Mitsubishi Chemical's "YL7760" (bisphenol AF type epoxy resin); Mitsubishi Chemical's "YL7800" (fluorene type epoxy resin); Mitsubishi Chemical's "jER1010" (solid bisphenol A type epoxy resin); and Mitsubishi Chemical's "jER1031S" (tetraphenylethane type epoxy resin). These resins can be used individually or in combination of two or more.
[0021] As for epoxy resin (A), when liquid epoxy resin and solid epoxy resin are used in combination, their mass ratio (liquid epoxy resin: solid epoxy resin) is preferably 1:0.01 to 1:20, more preferably 1:0.05 to 1:10, and particularly preferably 1:0.1 to 1:1. By keeping the mass ratio of liquid epoxy resin to solid epoxy resin within the above range, the desired effects of the present invention can be significantly obtained. Furthermore, a cured product with sufficient breaking strength can generally be obtained.
[0022] (A) The epoxy equivalent of the epoxy resin is preferably 50 g / eq. to 5000 g / eq., more preferably 50 g / eq. to 3000 g / eq., further preferably 80 g / eq. to 2000 g / eq., and even more preferably 110 g / eq. to 1000 g / eq. By falling within this range, the crosslinking density of the cured resin composition becomes sufficient, resulting in an insulating layer with low surface roughness. The epoxy equivalent is the mass of the resin containing 1 equivalent of epoxy groups. This epoxy equivalent can be determined according to JIS K7236.
[0023] From the viewpoint of achieving the desired effects of the present invention, (A) the weight-average molecular weight (Mw) of the epoxy resin is preferably 100 to 5000, more preferably 250 to 3000, and even more preferably 400 to 1500. The weight-average molecular weight of the resin can be determined by gel permeation chromatography (GPC) as a value converted to polystyrene.
[0024] From the viewpoint of obtaining a cured product exhibiting good mechanical strength and insulation reliability, when the non-volatile component in the resin composition is set to 100% by mass, the content of epoxy resin (A) is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 4% by mass or more. From the viewpoint of significantly obtaining the effects of the present invention, the upper limit of the epoxy resin content is preferably 20% by mass or less, more preferably 15% by mass or less, and particularly preferably 10% by mass or less. It should be noted that, in the present invention, the content of each component in the resin composition, unless otherwise specified, refers to the value when the non-volatile component in the resin composition is set to 100% by mass.
[0025] From the viewpoint of obtaining a cured product exhibiting good mechanical strength and insulation reliability, when the resin component in the resin composition is set to 100% by mass, the content of (A) epoxy resin is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more. From the viewpoint of significantly obtaining the desired effects of the present invention, the upper limit of the epoxy resin content is preferably 75% by mass or less, more preferably 70% by mass or less, and particularly preferably 65% by mass or less. "Resin component" refers to the component remaining after removing (C) inorganic filler material from the non-volatile components of the resin composition.
[0026] <(B) At least one curing agent selected from anhydride-based curing agents, amine-based curing agents, and phenol-based curing agents> The resin composition contains (B) at least one curing agent selected from anhydride-based curing agents, amine-based curing agents, and phenol-based curing agents as component (B). The curing agent typically has the function of reacting with component (A) to cure the resin composition. In particular, by containing these curing agents in the resin composition, in addition to the function of reacting with component (A) to cure the resin composition, a cured product in which warpage and flow marks are suppressed can be obtained. Component (B) can be used alone or in combination of two or more.
[0027] Anhydride-based curing agents include those having one or more anhydride groups per molecule. Specific examples of anhydride-based curing agents include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, 4-methylhexahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenylsuccinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, and pyromellitic anhydride. Tetracarboxylic anhydride, benzophenone tetracarboxylic anhydride, biphenyl tetracarboxylic anhydride, naphthalene tetracarboxylic anhydride, oxybis(phthalic anhydride), 3,3'-4,4'-diphenylsulfone tetracarboxylic anhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(trimethoxybenzoic anhydride), and styrene-maleic acid resin obtained by copolymerizing styrene and maleic acid are polymeric anhydrides.
[0028] Anhydride-based curing agents can be commercially available, such as "MH-700" manufactured by Shin Nippon Rikka Co., Ltd.
[0029] As amine-based curing agents, examples include curing agents having one or more amino groups per molecule, such as aliphatic amines, polyether amines, alicyclic amines, and aromatic amines. From the viewpoint of achieving the desired effect of this invention, aromatic amines are preferred. The amine-based curing agent is preferably a primary or secondary amine, and more preferably a primary amine. Specific examples of amine-based curing agents include 4,4'-methylenebis(2,6-dimethylaniline), diphenyl diamino sulfone, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, m-phenylenediamine, m-phenylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenyl ether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, and 2,2-bis(3-amino-4-diphenyl ether). 2,2-bis(4-aminophenyl)propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, bis(4-(3-aminophenoxy)phenyl)sulfone, etc.
[0030] Amine-based curing agents can be commercially available, such as "KAYABOND C-200S", "KAYABOND C-100", "KAYAHARD AA", "KAYAHARD AB", and "KAYAHARD AS" manufactured by Nippon Kayaku Co., Ltd., and "EPICURE W" manufactured by Mitsubishi Chemical Co., Ltd.
[0031] Examples of phenolic curing agents include those having one or more, preferably two or more, hydroxyl groups bonded to an aromatic ring (benzene ring, naphthalene ring, etc.) per molecule. Among these, compounds having hydroxyl groups bonded to a benzene ring are preferred. Furthermore, from the viewpoint of heat resistance and water resistance, phenolic curing agents with a novolacic structure are preferred. Further, from the viewpoint of adhesion, nitrogen-containing phenolic curing agents are preferred, and phenolic curing agents containing a triazine backbone are even more preferred. In particular, from the viewpoint of highly satisfying heat resistance, water resistance, and adhesion, phenolic varnish curing agents containing a triazine backbone are preferred.
[0032] Specific examples of phenolic curing agents include: MEH-7700, MEH-7810, MEH-7851, and MEH-8000H manufactured by Meiwa Chemical Co., Ltd.; NHN, CBN, and GPH manufactured by Nippon Kayaku Co., Ltd.; TD-2090, TD-2090-60M, LA-7052, LA-7054, LA-1356, LA-3018, LA-3018-50P, EXB-9500, HPC-9500, KA-1160, KA-1163, and KA-1165 manufactured by DIC Co., Ltd.; GDP-6115L, GDP-6115H, and ELPC75 manufactured by Kunei Chemical Co., Ltd.; and 2,2-diallylbisphenol A manufactured by Sigma-Aldrich.
[0033] From the viewpoint of achieving significant effects of the present invention, when the non-volatile component in the resin composition is set to 100% by mass, the content of component (B) is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, even more preferably 0.3% by mass or more, preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less.
[0034] When the number of epoxy groups in component (A) is set to 1, the number of active groups in component (B) is preferably 0.1 or more, more preferably 0.3 or more, even more preferably 0.5 or more, preferably 2 or less, more preferably 1.8 or less, and even more preferably 1.5 or less. Here, "the number of epoxy groups in component (A)" refers to the sum of all values obtained by dividing the mass of the non-volatile component of component (A) present in the resin composition by the epoxy equivalent. Furthermore, "the number of active groups in component (B)" refers to the sum of all values obtained by dividing the mass of the non-volatile component of component (B) present in the resin composition by the active group equivalent. By setting the number of active groups in component (B) when the number of epoxy groups in component (A) is set to 1 to the aforementioned range, the desired effects of the present invention can be significantly obtained.
[0035] <(C) Polyester polyol resin with aliphatic structure> The resin composition contains (C) a polyester polyol resin with an aliphatic structure as component (C). The aliphatic structure in component (C) imparts flexibility to the cured resin composition, thereby suppressing warping. Furthermore, the functional groups of the polyester polyol in component (C) enhance compatibility with other components in the resin composition to a level that maintains the suppression of warping and flow marks, resulting in a cured product with high bond strength and suppressed warping and flow marks. In addition, component (C) imparts flexibility to the cured resin composition, thereby mitigating stress and reducing the coefficient of linear thermal expansion (CTE) of the cured product. Component (C) can be used alone or in combination of two or more.
[0036] Regarding the content of component (C), from the viewpoint of obtaining a cured product with high bonding strength while simultaneously suppressing warping and flow marks, when the non-volatile component in the resin composition is set to 100% by mass, the content of component (C) is 1% by mass or more, preferably 1.2% by mass or more, more preferably 1.5% by mass or more, and even more preferably 2% by mass or more. From the viewpoint of obtaining a cured product with excellent bonding strength and linear thermal expansion coefficient, the upper limit is 20% by mass or less, preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 8% by mass or less.
[0037] From the viewpoint of suppressing warping and flow marks in the cured product, while simultaneously improving bond strength and hydrolytic stability, component (C) is preferably a resin having a structure derived from polyester and a structure derived from polyol. This resin can be obtained, for example, by reacting a polyol with a polyacid. Furthermore, the polyester-derived structure and the polyol-derived structure of component (C) are aliphatic.
[0038] Regarding component (C), from the viewpoint of improving compatibility and bonding strength with epoxy resin (A), it is preferable that the molecular chain of component (C) ends with either a hydroxyl group or a carboxyl group, more preferably a hydroxyl group. The number of hydroxyl and carboxyl groups contained in component (C) is preferably two or more per molecule, preferably six or fewer, more preferably four or fewer, further preferably three or fewer, and particularly preferably two.
[0039] From the viewpoint of achieving significant effects of the present invention, the structure derived from the polyol is preferably an olefinic structure with 2 or more carbon atoms, such as an ethylene oxide structure (-CH2CH2O-), a propylene oxide structure (-CH2CH2CH2O-), or a butene oxide structure (-CH2CH2CH2CH2O-), and more preferably an propylene oxide structure.
[0040] Examples of polyols include linear aliphatic polyols such as polyethylene glycol, polypropylene glycol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, neopentyl glycol, 1,3-butanediol, and polytetramethylene ether glycol; and polyols with alicyclic structures such as cyclohexanediol. Among these, linear aliphatic polyols are preferred. A single polyol can be used, or two or more can be used in combination.
[0041] The number average molecular weight of the polyol is preferably above 50, preferably below 1500, more preferably below 1000, and even more preferably below 700.
[0042] Commercially available polyols can be used. Examples of commercially available products include "polypropylene glycol, glycol type, 3000" and "polyethylene glycol 1540" manufactured by Fujifilm and Koujun Pharmaceutical Co., Ltd.; and "polytetramethylene ether glycol PTMG1000" manufactured by Mitsubishi Chemical Co., Ltd.
[0043] Examples of polybasic acids include aliphatic polybasic acids such as succinic acid, adipic acid, sebacic acid, and dodecanoic acid; lactones such as ε-caprolactone; and their anhydrides or esters.
[0044] Polybasic acids can be used alone or in combination of two or more. Aliphatic polybasic acids and lactones are preferred, with lactones being even more desirable. Commercially available polybasic acids are acceptable. Examples of commercially available products include "PLACCEL M" manufactured by Daicel Corporation.
[0045] From the viewpoint of obtaining a cured product with high bonding strength while simultaneously suppressing warping and flow marks, component (C) preferably has functional groups. Examples of functional groups include hydroxyl, carboxyl, amino, anhydride, vinyl, allyl, and maleimide groups. Among these, hydroxyl is preferred.
[0046] (C) Component (a) can be manufactured, for example, by reacting a polyol with a polyacid. The reaction temperature is preferably 80°C or higher, more preferably 100°C or higher, more preferably 200°C or lower, and even more preferably 150°C or lower. Furthermore, the reaction time is preferably 1 hour or higher, and more preferably 100 hours or lower.
[0047] During the reaction, a catalyst may be used as needed. Examples of catalysts include tin-based catalysts such as stannous(II) 2-ethylhexanoate and dibutyltin oxide; titanium-based catalysts such as tetraisopropyl titanate and tetrabutyl titanate; and organic sulfonic acid catalysts such as p-toluenesulfonic acid. A single catalyst may be used, or two or more catalysts may be used in combination.
[0048] From the viewpoint of enabling the reaction to proceed effectively, the content of the catalyst is preferably 0.0001 parts by mass or more, more preferably 0.0005 parts by mass or more, more preferably 0.01 parts by mass or less, and more preferably 0.005 parts by mass or less, relative to a total of 100 parts by mass of polyol and polyacid.
[0049] Regarding the hydroxyl value of component (C), from the viewpoint of significantly obtaining the effects of the present invention, it is preferably 2 mg KOH / g or more, more preferably 4 mg KOH / g or more, further preferably 6 mg KOH / g or more, 10 mg KOH / g or more, 25 mg KOH / g or more, 30 mg KOH / g or more, or 35 mg KOH / g or more, preferably 450 mg KOH / g or less, more preferably 100 mg KOH / g or less, further preferably 50 mg KOH / g or less, 45 mg KOH / g or less, or 40 mg KOH / g or less. The hydroxyl value can be determined according to the method of JIS K0070.
[0050] Furthermore, regarding the acid value of component (C), from the viewpoint of significantly obtaining the effects of the present invention, it is preferable to have an acid value of 2 mg KOH / g or higher, more preferably 4 mg KOH / g or higher, even more preferably 6 mg KOH / g or higher, 10 mg KOH / g or higher, 25 mg KOH / g or higher, 30 mg KOH / g or higher, or 35 mg KOH / g or higher, preferably 450 mg KOH / g or lower, more preferably 100 mg KOH / g or lower, even more preferably 50 mg KOH / g or lower, 45 mg KOH / g or lower, or 40 mg KOH / g or lower. The acid value can be determined using the method according to JIS K0070.
[0051] From the viewpoint of obtaining a cured product that can simultaneously suppress warping and flow marks, the number-average molecular weight of component (C) is preferably 500 or more, more preferably 1000 or more, more preferably 2000 or more, even more preferably 3000 or more, preferably 15000 or less, more preferably 12000 or less, and even more preferably 10000 or less. The number-average molecular weight can be determined using GPC (gel permeation chromatography).
[0052] From the viewpoint of improving compatibility, the solubility parameter (SP value) of component (C) is preferably 6.5 or higher, more preferably 7.0 or higher, even more preferably 7.5 or higher, preferably 22 or lower, even more preferably 21 or lower, and even more preferably 20 or lower. The solubility parameter can be calculated using Fedors' theory.
[0053] From the viewpoint of improving the fluidity of compression molding, the melting point of component (C) is preferably above -20°C, more preferably above -15°C, even more preferably above 0°C, preferably below 100°C, more preferably below 90°C, and even more preferably below 80°C.
[0054] When the content of component (A) in the resin composition is 100% by mass and is defined as a1, and the content of component (C) in the resin composition is 100% by mass and is defined as c1, the ratio of a1 / c1 is preferably 0.1 or more, more preferably 0.3 or more, even more preferably 0.5 or more, preferably 20 or less, more preferably 15 or less, and even more preferably 10 or less. By setting a1 / c1 within the aforementioned range, the effects of the present invention can be significantly obtained.
[0055] When the content of component (B) in the resin composition, which is 100% by mass of non-volatile components, is set as b1, the b1 / c1 is preferably 0.01 or more, more preferably 0.05 or more, even more preferably 0.1 or more, preferably 10 or less, more preferably 5 or less, and even more preferably 3 or less. By setting b1 / c1 within the aforementioned range, the effects of the present invention can be significantly obtained.
[0056] <(D) Inorganic filler materials> The resin composition contains (D) inorganic filler as component (D). By including (D) inorganic filler in the resin composition, a cured product with a low coefficient of linear thermal expansion can be obtained.
[0057] Inorganic compounds are used as inorganic filler materials. Examples of inorganic filler materials include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica is particularly preferred. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. Furthermore, spherical silica is preferred as silica. (D) One inorganic filler material may be used alone or in combination of two or more.
[0058] Commercially available products as (D) inorganic filler materials include, for example, "UFP-30" manufactured by Denka Kagaku Kogyo Co., Ltd.; "SP60-05" and "SP507-05" manufactured by Nippon Steel & Sumitomo Metal Materials Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", and "YA010C" manufactured by Yatuma Co., Ltd.; "UFP-30" manufactured by Denka Kagaku Kogyo (DENKA) Co., Ltd.; "SILFIL NSS-3N", "SILFIL NSS-4N", and "SILFIL NSS-5N" manufactured by Tokuyama Co., Ltd.; and "SC2500SQ", "SO-C4", "SO-C2", "SO-C1", and "SC2050-SXF" manufactured by Yatuma Co., Ltd.
[0059] From the viewpoint of significantly achieving the desired effect of the present invention, (D) the average particle size of the inorganic filler material is preferably 0.01 μm or more, more preferably 0.05 μm or more, particularly preferably 0.1 μm or more, preferably 10 μm or less, more preferably 7 μm or less, and even more preferably 5 μm or less.
[0060] (D) The average particle size of inorganic filler materials can be determined by laser diffraction-scattering based on the Mie scattering theory. Specifically, a laser diffraction-scattering particle size distribution measuring device can be used to prepare the particle size distribution of the inorganic filler material on a volume basis, and the median particle size can be used as the average particle size for measurement. The sample for testing can be obtained by weighing 100 mg of inorganic filler material and 10 g of methyl ethyl ketone into a tube and dispersing it ultrasonically for 10 minutes. For the sample for testing, a laser diffraction-scattering particle size distribution measuring device is used, with the light source wavelength set to blue and red, and the volume-based particle size distribution of the inorganic filler material is measured in a flow cell manner. The average particle size is calculated based on the obtained particle size distribution as the median particle size. Examples of laser diffraction-scattering particle size distribution measuring devices include the "LA-960" manufactured by Horiba Manufacturing Co., Ltd. and the "SALD-2200" manufactured by Shimadzu Corporation.
[0061] From the viewpoint of achieving the desired effect of the present invention, the specific surface area of (D) the inorganic filler material is preferably 1 m². 2 / g or higher, preferably 2m 2 / g or higher, especially 3m 2 / g or more. There is no particular upper limit, but 60m is preferred. 2 / g or less, 50m 2 / g or less or 40m 2 / g or less. The specific surface area can be obtained as follows: using a BET fully automated specific surface area measuring device (Macsorb HM-1210 manufactured by Mountech), nitrogen gas is adsorbed onto the sample surface, and the specific surface area is calculated using the BET multi-point method, thereby determining the specific surface area of the inorganic filler material.
[0062] From the perspective of improving moisture resistance and dispersibility, (D) inorganic filler materials are preferably treated with surface treatment agents. Examples of surface treatment agents include fluorinated silane coupling agents such as 3,3,3-trifluoropropyltrimethoxysilane; aminosilane coupling agents such as 3-aminopropyltriethoxysilane, N-phenyl-8-aminooctyl-trimethoxysilane, and N-phenyl-3-aminopropyltrimethoxysilane; epoxysilane coupling agents such as 3-epoxypropoxypropyltrimethoxysilane; mercaptosilane coupling agents such as 3-mercaptopropyltrimethoxysilane; silane coupling agents; alkoxysilanes such as phenyltrimethoxysilane; organosilazane compounds such as hexamethyldisilazane; and titanate coupling agents. Furthermore, a single surface treatment agent can be used, or two or more can be used in combination.
[0063] Commercially available surface treatment agents include, for example: KBM403 (3-epoxypropoxypropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Industry Co., Ltd., KBM803 (3-mercaptopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Industry Co., Ltd., KBE903 (3-aminopropyltriethoxysilane) manufactured by Shin-Etsu Chemical Industry Co., Ltd., KBM573 (N-phenyl-3-aminopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Industry Co., Ltd., SZ-31 (hexamethyldisilazane) manufactured by Shin-Etsu Chemical Industry Co., Ltd., KBM103 (phenyltrimethoxysilane) manufactured by Shin-Etsu Chemical Industry Co., Ltd., KBM-4803 (long-chain epoxy silane coupling agent) manufactured by Shin-Etsu Chemical Industry Co., Ltd., and KBM-7103 (3,3,3-trifluoropropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Industry Co., Ltd.
[0064] From the perspective of improving the dispersibility of inorganic fillers, the degree of surface treatment with a surface treatment agent is preferably within a specified range. Specifically, it is preferable that 100 parts by mass of inorganic filler are surface treated with 0.2 to 5 parts by mass of a surface treatment agent, more preferably with 0.2 to 3 parts by mass of a surface treatment agent, and even more preferably with 0.3 to 2 parts by mass of a surface treatment agent.
[0065] The degree of surface treatment with surface treatment agents can be evaluated by the carbon content per unit surface area of the inorganic filler. From the perspective of improving the dispersibility of inorganic fillers, the carbon content per unit surface area of the inorganic filler is preferably 0.02 mg / m².2 The above is preferred, ideally 0.1 mg / m². 2 The above, and even better, is 0.2 mg / m². 2 That's all. On the other hand, from the viewpoint of suppressing the increase in melt viscosity of the resin varnish and melt viscosity in sheet form, 1 mg / m³ is preferable. 2 The following is preferable: 0.8 mg / m² 2 The following is even better: 0.5 mg / m² 2 the following.
[0066] (D) The carbon content per unit surface area of the inorganic filler material can be determined after cleaning the surface-treated inorganic filler material with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, sufficient MEK as a solvent is added to the surface-treated inorganic filler material, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid components, the carbon content per unit surface area of the inorganic filler material can be determined using a carbon analyzer. A carbon analyzer such as the "EMIA-320V" manufactured by Horiba Corporation can be used.
[0067] From the viewpoint of significantly obtaining the effects of the present invention, when the content of the non-volatile component in the resin composition is set to 100% by mass, it is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 75% by mass or more, preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less.
[0068] <(E) Curing Accelerator> In addition to the above-mentioned components, the resin composition may, as an optional component, further contain a curing accelerator as component (E).
[0069] Examples of component (E) include epoxy resin curing accelerators such as phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, guanidine-based curing accelerators, and metal-based curing accelerators; and thermal polymerization curing accelerators such as peroxide-based curing accelerators. Component (E) can be used alone or in combination of two or more.
[0070] Examples of phosphorus-based curing accelerators include triphenylphosphine, phosphonium borate compounds, tetraphenylphosphonium tetraphenylborate, n-butylphosphonium tetraphenylborate, tetrabutylphosphonium decanoate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, and butyltriphenylphosphonium thiocyanate, with triphenylphosphine and tetrabutylphosphonium decanoate being preferred.
[0071] Examples of amine-based curing accelerators include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene, with 4-dimethylaminopyridine and 1,8-diazabicyclo(5,4,0)-undecene being preferred.
[0072] Examples of imidazole-based curing accelerators include: 2-methylimidazolium, 2-undecylimidazolium, 2-heptadecylimidazolium, 1,2-dimethylimidazolium, 2-ethyl-4-methylimidazolium, 1,2-dimethylimidazolium, 2-ethyl-4-methylimidazolium, 2-phenylimidazolium, 2-phenyl-4-methylimidazolium, 1-benzyl-2-methylimidazolium, 1-benzyl-2-phenylimidazolium, 1-cyanoethyl-2-methylimidazolium, 1-cyanoethyl-2-undecylimidazolium, 1-cyanoethyl-2-ethyl-4-methylimidazolium, 1-cyanoethyl-2-phenylimidazolium, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-triazine, 2,4- Diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-triazine isocyanuric acid adduct, 2-phenylimidazolyl isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazolium, 2-phenyl-4-methyl-5-hydroxymethylimidazolium, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, 2-phenylimidazoline and other imidazole compounds, and adducts of imidazole compounds with epoxy resins, preferably 2-ethyl-4-methylimidazolium and 1-benzyl-2-phenylimidazolium.
[0073] As an imidazole-based curing accelerator, commercially available products can be used, such as "P200-H50" manufactured by Mitsubishi Chemical Corporation.
[0074] Examples of guanidine-based curing accelerators include: dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanidine, 1-ethylbiguanidine, 1-n-butylbiguanidine, 1-n-octadecylbiguanidine, 1,1-dimethylbiguanidine, 1,1-diethylbiguanidine, 1-cyclohexylbiguanidine, 1-allylbiguanidine, 1-phenylbiguanidine, 1-(o-tolyl)biguanidine, etc., with dicyandiamide and 1,5,7-triazabicyclo[4.4.0]dec-5-ene being preferred.
[0075] Examples of organometallic curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include: cobalt(II) acetylacetonate, cobalt(III) acetylacetonate, cobalt(II) acetylacetonate, copper(II) acetylacetonate, zinc(II) acetylacetonate, iron(III) acetylacetonate, nickel(II) acetylacetonate, and manganese(II) acetylacetonate. Examples of organometallic salts include zinc octoate, tin octoate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.
[0076] Examples of peroxide-based curing accelerators include di-tert-butyl peroxide, tert-butyl cumene peroxide, tert-butyl peroxyacetate, α,α'-di(tert-butylperoxy)diisopropylbenzene, tert-butyl peroxylaurate, tert-butyl peroxy2-ethylhexanoate, tert-butyl peroxyneodecanate, and tert-butyl peroxybenzoate.
[0077] Commercially available peroxide-based curing accelerators include, for example, those manufactured by Nippon Oil Company such as "PERHEXYL D", "PERBUTYL C", "PERBUTYL A", "PERBUTYL P", "PERBUTYL L", "PERBUTYL O", "PERBUTYL ND", "PERBUTYL Z", "PERCUMYL P", and "PERCUMYL D".
[0078] From the viewpoint of significantly achieving the desired effect of the present invention, when the non-volatile component in the resin composition is set to 100% by mass, the content of component (E) is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, even more preferably 0.3% by mass or more, preferably 1% by mass or less, more preferably 0.8% by mass or less, and even more preferably 0.5% by mass or less.
[0079] From the viewpoint of achieving the desired effect of the present invention, when the resin component in the resin composition is set to 100% by mass, the content of component (E) is preferably 0.1% by mass or more, more preferably 1% by mass or more, even more preferably 2% by mass or more, preferably 10% by mass or less, more preferably 8% by mass or less, and even more preferably 3% by mass or less.
[0080] <(F) Other Additives> In addition to the components described above, the resin composition may, as an optional component, further include other additives. Examples of such additives include resin additives such as colorants, pigments, thermoplastic resins, thickeners, defoamers, leveling agents, and adhesion promoters. These additives may be used individually or in combination of two or more. Those skilled in the art can appropriately determine their respective contents.
[0081] The resin composition may further contain any solvent as a volatile component. Examples of solvents include organic solvents. Furthermore, a single solvent may be used, or two or more may be used in combination in any ratio. The less solvent, the better. The amount of solvent relative to 100% by mass of the non-volatile components in the resin composition is preferably 3% by mass or less, more preferably 1% by mass or less, further preferably 0.5% by mass or less, further preferably 0.1% by mass or less, further preferably 0.01% by mass or less, and particularly preferably not contained (0% by mass). Furthermore, with such a small amount of solvent, the resin composition can be in paste form. The viscosity of the paste-like resin composition at 25°C is preferably in the range of 20 Pa·s to 1000 Pa·s.
[0082] The preparation method of the resin composition of the present invention is not particularly limited, and examples include adding compounding components, adding solvents as needed, and mixing and dispersing using a rotary mixer or the like.
[0083] <Properties and Uses of Resin Compositions> The cured product using the above-described resin composition exhibits the characteristic that the formation of flow marks is suppressed. Therefore, the cured product provides an insulating or sealing layer that suppresses the formation of flow marks. Specifically, the resin composition is compressed onto a silicon wafer to form a resin composition layer, and the resin composition layer is heated to obtain a cured product layer. In this case, the formation of flow marks on the surface of the cured product can be suppressed. Details regarding the determination of flow mark formation can be performed according to the methods described in the examples below.
[0084] Cured products obtained by thermosetting resin compositions at 180°C for 90 minutes exhibit excellent bond strength. Bond strength can be expressed, for example, by shear strength. Therefore, the cured products typically result in insulating or sealing layers with excellent shear strength. This shear strength indicates the difficulty of peeling when a force is applied in an in-plane direction perpendicular to the thickness direction. Specifically, consider the case where a cured layer of a resin composition is formed on a surface made of a material (e.g., polyimide). In this case, the shear strength indicates the magnitude of the force applied in the in-plane direction to the cured layer at which it can be peeled from the surface. A preferred shear strength is 1.7 kgf / mm². 2 The above is better, preferably 2.0 kgf / mm 2 The above, and even better, is 2.5 kgf / mm. 2 That's all. There's no specific upper limit; it can be set to 10 kgf / mm. 2 The shear strength can be evaluated according to the methods described in the examples below.
[0085] The cured product obtained by heat curing the resin composition at 180°C for 90 minutes exhibits the characteristic of suppressed warpage. Therefore, the cured product provides an insulating or sealing layer with suppressed warpage. Specifically, the resin composition is compressed and molded on a silicon wafer to form a resin composition layer. A sample substrate is obtained by heat curing the resin composition layer. The warpage of the sample substrate at 25°C is determined using a shadow moire measuring device according to JEITA EDX-7311-24 standard. The warpage is preferably less than 2 mm. Details of the warpage measurement can be obtained by the method described in the examples below.
[0086] The cured product obtained by heat curing the resin composition at 150°C for 60 minutes exhibits a low coefficient of linear thermal expansion (CTE). Therefore, the cured product provides an insulating or sealing layer with a low CTE. Preferably, the CTE is less than 15 ppm / °C, more preferably less than 13 ppm / °C, and even more preferably less than 13 ppm / °C. The lower limit is not particularly limited and can be set to 0.01 ppm / °C or higher. The CTE can be evaluated according to the method described in the examples below.
[0087] Due to the aforementioned properties, the resin composition is suitable for use as a resin composition for sealing electronic devices such as organic EL devices and semiconductors (resin composition for sealing). In particular, it is suitable for use as a resin composition for sealing semiconductors (resin composition for semiconductor sealing), and more preferably as a resin composition for sealing semiconductor chips (resin composition for semiconductor chip sealing). Furthermore, in addition to sealing applications, the resin composition can also be used as a resin composition for insulating applications, such as an insulating layer. For example, the aforementioned resin composition is suitable for use as a resin composition for forming an insulating layer for semiconductor chip packages (resin composition for insulating layers of semiconductor chip packages) and as a resin composition for forming an insulating layer for circuit boards (including printed wiring boards) (resin composition for insulating layers of circuit boards).
[0088] Examples of semiconductor chip packaging include: FC-CSP, MIS-BGA packaging, ETS-BGA packaging, fan-out type WLP (Wafer Level Package), fan-in type WLP, fan-out type PLP (Panel Level Package), and fan-in type PLP.
[0089] In addition, the above-mentioned resin composition can be used as an underfill material, for example, as a material for MUF (Molding Under Filling) used after connecting a semiconductor chip to a substrate.
[0090] Furthermore, the above-mentioned resin composition can be used in a wide range of applications, including resin sheets, sheet laminates such as prepregs, solder resists, chip bonding materials, via-filling resins, and component embedding resins.
[0091] [Resin Sheets] The resin sheet of the present invention has a support and a resin composition layer disposed on the support. The resin composition layer is a layer containing the resin composition of the present invention and is generally formed from the resin composition.
[0092] From the viewpoint of thinning, the thickness of the resin composition layer is preferably 600 μm or less, more preferably 550 μm or less, and even more preferably 500 μm or less, 400 μm or less, 350 μm or less, 300 μm or less, or 200 μm or less. There is no particular limitation on the lower limit of the resin composition layer thickness; for example, it can be 1 μm or more, 5 μm or more, 10 μm or more, etc.
[0093] Examples of supports include films made of plastic materials, metal foils, and release paper, with films and metal foils made of plastic materials being preferred.
[0094] When using a film formed of a plastic material as a support, examples of plastic materials include: polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"); acrylic polymers such as polycarbonate (hereinafter sometimes abbreviated as "PC"); polymethyl methacrylate (hereinafter sometimes abbreviated as "PMMA"); cyclic polyolefins; triacetyl cellulose (hereinafter sometimes abbreviated as "TAC"); polyether sulfides (hereinafter sometimes abbreviated as "PES"); polyether ketones; and polyimides. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.
[0095] When using metal foil as a support, examples of metal foils include copper foil and aluminum foil. Copper foil is preferred. Copper foil can be made from copper alone or from an alloy of copper with other metals such as tin, chromium, silver, magnesium, nickel, zirconium, silicon, and titanium.
[0096] For the support, the surface that bonds with the resin composition layer can be treated with matte finish, corona treatment, antistatic treatment, etc.
[0097] Furthermore, as a support, a support with a release layer can be used on the surface that bonds to the resin composition layer. Examples of release agents used in the release layer of the support with a release layer include, for example, one or more release agents selected from alkyd resins, polyolefin resins, polyurethane resins, and silicone resins. Commercially available release agents include, for example, "SK-1," "AL-5," and "AL-7" manufactured by Lintec Corporation, which are alkyd resin-based release agents. Furthermore, examples of supports with a release layer include, for example, "LUMIRROR T60" manufactured by Toray Industries, Ltd., "Purex" manufactured by Teijin Corporation, and "Unipeel" manufactured by Unitika Corporation.
[0098] The thickness of the support is preferably in the range of 5μm to 75μm, and more preferably in the range of 10μm to 60μm. It should be noted that when using a support with a release layer, it is preferable that the overall thickness of the support with the release layer is within the above range.
[0099] Regarding resin sheets, they can be manufactured by coating the resin composition onto a support using a coating apparatus such as a die coater. Alternatively, if necessary, the resin composition can be dissolved in an organic solvent to prepare a resin varnish, which is then applied to manufacture the resin sheet. By using a solvent, the viscosity can be adjusted, improving coatability. When using a resin varnish, it is typically dried after coating to form a resin composition layer.
[0100] Examples of organic solvents include: ketone solvents such as acetone, methyl ethyl ketone, and cyclohexanone; acetate solvents such as ethyl acetate, butyl acetate, acetic acid solvents, propylene glycol monomethyl ether acetate, and carbitol acetate; carbitol solvents such as solvents and butyl carbitol; aromatic solvents such as toluene and xylene; and amide solvents such as dimethylformamide, dimethylacetamide (DMAc), and N-methylpyrrolidone. Organic solvents can be used alone or in combination of two or more in any ratio.
[0101] Drying can be carried out by known methods such as heating or hot air blowing. Regarding drying conditions, drying is typically performed when the content of organic solvent in the resin composition layer is typically 10% by mass or less, preferably 5% by mass or less. Depending on the boiling point of the organic solvent in the resin varnish, for example, when using a resin varnish containing 30% to 60% by mass of organic solvent, the resin composition layer can be formed by drying at 50°C to 150°C for 3 to 10 minutes.
[0102] Resin sheets may include any layer other than the support and the resin composition layer, as needed. For example, in a resin sheet, a protective film selected according to the support may be provided on the side of the resin composition layer that is not bonded to the support (i.e., the side opposite to the support). The thickness of the protective film is, for example, 1 μm to 40 μm. The protective film prevents dust and other contaminants from adhering to the surface of the resin composition layer or causing damage to it. When a resin sheet has a protective film, it can be used by peeling off the protective film. Furthermore, the resin sheet can be stored by rolling it into a roll.
[0103] Resin sheets are suitable for forming insulating layers in the manufacture of semiconductor chip packages (insulating resin sheets for semiconductor chip packages). For example, resin sheets can be used to form insulating layers on circuit boards (insulating resin sheets for circuit boards). Examples of packages using such substrates include FC-CSP, MIS-BGA packages, and ETS-BGA packages.
[0104] In addition, resin sheets can be suitable for sealing semiconductor chips (resin sheets for sealing semiconductor chips). Examples of suitable semiconductor chip packages include: fan-out WLP, fan-in WLP, fan-out PLP, and fan-in PLP.
[0105] In addition, resin sheets can be used as materials for MUFs (Mechanical Units) after semiconductor chips are connected to substrates.
[0106] Furthermore, resin sheets can be used in a wide range of other applications requiring high insulation reliability. For example, resin sheets can be suitably used to form the insulating layer of circuit boards such as printed wiring boards.
[0107] [Circuit board] The circuit board of the present invention comprises a cured layer formed from a cured resin composition of the present invention. The cured layer may serve as an insulating layer or a sealing layer. This circuit board can be manufactured, for example, by a manufacturing method including steps (1) and (2) described below. (1) A process of forming a resin composition layer on a substrate; (2) The process of heat curing the resin composition layer to form an insulating layer.
[0108] In step (1), a substrate is prepared. Examples of substrates include glass epoxy boards, metal substrates (stainless steel, cold-rolled steel sheet (SPCC), etc.), polyester substrates, polyimide substrates, BT resin substrates, and thermosetting polyphenylene ether substrates. Furthermore, as part of the substrate, a metal layer such as copper foil may be formed on its surface. For example, a substrate with a peelable first metal layer and a second metal layer on both surfaces may also be used. When using such a substrate, typically, a conductor layer that functions as a wiring layer for circuit wiring is formed on the side of the second metal layer opposite to the first metal layer. Examples of materials for the metal layer include copper foil, copper foil with a carrier, and materials for the conductor layer described later; copper foil is preferred. Furthermore, commercially available products can be used as substrates having such a metal layer; examples include Mitsui Metals & Minerals Co., Ltd.'s ultra-thin copper foil with a carrier, "MicroThin."
[0109] Furthermore, a conductor layer may be formed on one or both surfaces of the substrate. In the following description, the component comprising the substrate and the conductor layer formed on the surface of the substrate is sometimes appropriately referred to as a "substrate with wiring layer". Examples of conductor materials included in the conductor layer include materials containing one or more metals selected from gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin, and indium. Single metals or alloys can be used as conductor materials. Examples of alloys include alloys of two or more metals selected from the above-mentioned metals (e.g., nickel-chromium alloys, copper-nickel alloys, and copper-titanium alloys). From the viewpoint of versatility, cost, and ease of pattern formation in conductor layer formation, alloys of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper as single metals; and alloys of nickel-chromium alloys, copper-nickel alloys, and copper-titanium alloys as alloys are preferred. Among these, single metals of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper; and nickel-chromium alloys are more preferred; and single metals of copper are particularly preferred.
[0110] For conductor layers, for example, to function as wiring layers, patterning can be performed. In this case, the linewidth (circuit width) / line spacing (width between circuits) ratio of the conductor layer is not particularly limited, but it is preferably 20 / 20 μm or less (i.e., a spacing of 40 μm or less), more preferably 10 / 10 μm or less, further preferably 5 / 5 μm or less, even more preferably 1 / 1 μm or less, and particularly preferably 0.5 / 0.5 μm or more. The spacing does not need to be uniform throughout the conductor layer. The minimum spacing of the conductor layer can be, for example, 40 μm or less, 36 μm or less, or 30 μm or less.
[0111] The thickness of the conductor layer varies depending on the design of the circuit board, preferably 3μm to 35μm, more preferably 5μm to 30μm, even more preferably 10μm to 20μm, and particularly preferably 15μm to 20μm.
[0112] The conductor layer can be formed, for example, by a method comprising the following steps: laminating a dry film (photosensitive resist) onto a substrate; exposing and developing the dry film under specified conditions using a photomask to form a pattern, thereby obtaining a patterned dry film; using the developed patterned dry film as a plating mask, forming the conductor layer using a plating method such as electroplating; and peeling off the patterned dry film. As the dry film, a photosensitive dry film formed from a photoresist composition can be used, for example, a dry film formed from resins such as phenolic varnish resin or acrylic resin. The lamination conditions of the substrate and the dry film can be the same as the lamination conditions of the substrate and resin sheet described later. The peeling off of the dry film can be carried out, for example, using an alkaline peeling solution such as sodium hydroxide solution.
[0113] After preparing the substrate, a resin composition layer is formed on the substrate. If a conductor layer is formed on the surface of the substrate, the resin composition layer is preferably formed by embedding the conductor layer within the resin composition layer.
[0114] The resin composition layer is formed, for example, by laminating a resin sheet to a substrate. This lamination can be performed, for example, by heating and pressing the resin sheet to the substrate from the support side, thereby bonding the resin composition layer to the substrate. Examples of components for heating and pressing the resin sheet to the substrate (hereinafter sometimes simply referred to as "heat-pressing components") include, for example, heated metal plates (SUS end plates, etc.) or metal rollers (SUS rollers, etc.). It should be noted that, preferably, the heat-pressing components are not directly pressed onto the resin sheet, but rather the resin sheet is pressed through an elastic material such as heat-resistant rubber to allow it to fully conform to the surface irregularities of the substrate.
[0115] The lamination of the substrate and the resin sheet can be carried out, for example, by vacuum lamination. In vacuum lamination, the heat-pressing temperature is preferably in the range of 60°C to 160°C, more preferably 80°C to 140°C. The heat-pressing pressure is preferably in the range of 0.098 MPa to 1.77 MPa, more preferably 0.29 MPa to 1.47 MPa. The heat-pressing time is preferably in the range of 20 seconds to 400 seconds, more preferably 30 seconds to 300 seconds. Lamination is preferably carried out under reduced pressure conditions below 13 hPa.
[0116] After lamination, the laminated resin sheets can be smoothed under normal pressure (atmospheric pressure), for example, by pressing the heated pressing components from the support side. The pressing conditions for smoothing can be the same as the heating and pressing conditions for lamination described above. It should be noted that lamination and smoothing can be performed continuously using a vacuum laminator.
[0117] Furthermore, the resin composition layer can be formed, for example, by compression molding. The specific operation of compression molding involves, for example, preparing an upper mold and a lower mold as a die. The resin composition is coated onto a substrate. The substrate coated with the resin composition is mounted onto the lower mold. Then, the upper and lower molds are closed, and heat and pressure are applied to the resin composition to perform compression molding.
[0118] Furthermore, the specific operation of compression molding can also be performed as follows: An upper mold and a lower mold are prepared as the molds for compression molding. The resin composition is carried on the lower mold. A substrate is then mounted on the upper mold. Then, the upper and lower molds are closed such that the resin composition carried on the lower mold is in contact with the substrate mounted on the upper mold, and heat and pressure are applied to perform compression molding.
[0119] The molding conditions in compression molding vary depending on the composition of the resin composition. The mold temperature during molding is preferably a temperature at which the resin composition exhibits excellent compressibility, for example, preferably 80°C or higher, more preferably 100°C or higher, even more preferably 120°C or higher, preferably 200°C or lower, more preferably 170°C or lower, even more preferably 150°C or lower. Furthermore, the pressure applied during molding is preferably 1 MPa or higher, more preferably 3 MPa or higher, even more preferably 5 MPa or higher, preferably 50 MPa or lower, more preferably 30 MPa or lower, even more preferably 20 MPa or lower. The curing time is preferably 1 minute or higher, more preferably 2 minutes or higher, particularly preferably 5 minutes or higher, preferably 60 minutes or lower, more preferably 30 minutes or lower, and especially preferably 20 minutes or lower. Typically, the mold is removed after the resin composition layer has been formed. Mold removal can be performed before or after heat curing of the resin composition layer.
[0120] After a resin composition layer is formed on a substrate, the resin composition layer is thermocured to form an insulating layer. Although the thermocuring conditions of the resin composition layer vary depending on the type of resin composition, the curing temperature is generally in the range of 120°C to 240°C (preferably 150°C to 220°C, more preferably 170°C to 200°C), and the curing time is in the range of 5 minutes to 120 minutes (preferably 10 minutes to 100 minutes, more preferably 15 minutes to 90 minutes).
[0121] The resin composition layer can be preheated at a temperature below the curing temperature before thermal curing. For example, the resin composition layer can be preheated for at least 5 minutes (preferably 5 to 150 minutes, more preferably 15 to 120 minutes) at a temperature of 50°C or higher and below 120°C (preferably 60°C or higher and below 110°C, more preferably 70°C or higher and below 100°C) before thermal curing.
[0122] By operating as described above, a circuit board with an insulating layer can be manufactured. Furthermore, the method for manufacturing the circuit board may include any steps. For example, when using a resin sheet to manufacture the circuit board, the method may include a step of peeling off a support from the resin sheet. The support may be peeled off before the resin composition layer is thermocured, or it may be peeled off after the resin composition layer has been thermocured.
[0123] The manufacturing method of a circuit board may include, for example, a step of grinding the surface of the insulating layer after its formation. There are no particular limitations on the grinding method. For example, a surface grinder can be used to grind the surface of the insulating layer.
[0124] The manufacturing method of a circuit board may include, for example, a process (3) of interlayer bonding of conductor layers, namely, the process of creating holes in the insulating layer. This allows the formation of vias, through-holes, and other holes in the insulating layer. Examples of methods for forming vias include laser irradiation, etching, and mechanical drilling. The size and shape of the vias can be appropriately determined according to the design of the circuit board. It should be noted that, for process (3), interlayer bonding can be achieved by grinding or polishing the insulating layer.
[0125] After forming the through-hole, it is preferable to perform a process to remove contaminants from the through-hole. This process is sometimes referred to as a decontamination process. For example, when a conductor layer is formed on an insulating layer by a plating process, a wet decontamination treatment can be performed on the through-hole. Furthermore, when a conductor layer is formed on an insulating layer by a sputtering process, a dry decontamination process, such as a plasma treatment process, can be performed. Moreover, the insulating layer can also be roughened by the decontamination process.
[0126] Furthermore, the insulating layer can be roughened before forming the conductor layer on the insulating layer. This roughening process typically roughens the surface of the insulating layer, including the interior of vias. Both dry and wet roughening processes can be performed. Examples of dry roughening processes include plasma treatment. Examples of wet roughening processes include methods that sequentially perform swelling treatment using a swelling solution, roughening treatment using an oxidizing agent, and neutralization treatment using a neutralizing solution.
[0127] After forming the via, a conductor layer is formed on the insulating layer. By forming a conductor layer at the location where the via has been formed, the newly formed conductor layer becomes conductive with the conductor layer on the substrate surface, thus achieving interlayer bonding. Methods for forming the conductor layer include, for example, plating, sputtering, and vapor deposition, with plating being preferred. In a preferred embodiment, a suitable method such as a semi-additive or fully additive method is used to plating the surface of the insulating layer to form a conductor layer with the desired wiring pattern. Furthermore, when the support in the resin sheet is a metal foil, a subtractive method can be used to form a conductor layer with the desired wiring pattern. The material of the formed conductor layer can be a single metal or an alloy. Moreover, the conductor layer can have a single-layer structure or a multilayer structure containing two or more layers of different types of materials.
[0128] Here, an example of an embodiment for forming a conductor layer on an insulating layer is described in detail. A plating seed layer is formed on the surface of the insulating layer by electroless plating. Next, corresponding to the desired wiring pattern, a mask pattern is formed on the formed plating seed layer, exposing a portion of the plating seed layer. An electroplated layer is formed on the exposed plating seed layer by electroplating, and then the mask pattern is removed. Then, the unwanted plating seed layer is removed by etching or other processes, and a conductor layer having the desired wiring pattern can be formed. It should be noted that the dry film used in forming the mask pattern when forming the conductor layer is the same as the dry film described above.
[0129] The method for manufacturing a circuit board may include a step (4) of removing a substrate. By removing the substrate, a circuit board having an insulating layer and a conductor layer embedded in the insulating layer can be obtained. This step (4) may be performed, for example, when a substrate having a peelable metal layer is used.
[0130] [Semiconductor chip packaging] The first embodiment of the present invention relates to a semiconductor chip package comprising the circuit substrate described above and a semiconductor chip mounted on the circuit substrate. This semiconductor chip package can be manufactured by bonding the semiconductor chip to the circuit substrate.
[0131] Regarding the bonding conditions between the circuit board and the semiconductor chip, any condition that allows for conductive connection between the terminal electrodes of the semiconductor chip and the circuit wiring of the circuit board can be used. For example, the conditions used in flip-chip mounting of semiconductor chips can be employed. Furthermore, for example, bonding between the semiconductor chip and the circuit board can be achieved via an insulating adhesive.
[0132] As an example of a bonding method, one can cite the method of pressing a semiconductor chip onto a circuit board. As for the pressing conditions, the pressing temperature is usually in the range of 120°C to 240°C (preferably in the range of 130°C to 200°C, more preferably in the range of 140°C to 180°C), and the pressing time is usually in the range of 1 second to 60 seconds (preferably 5 seconds to 30 seconds).
[0133] In addition, as another example of bonding methods, a method of bonding semiconductor chips to a circuit board by reflow soldering can be cited. The reflow soldering conditions can be in the range of 120°C to 300°C.
[0134] After the semiconductor chip is bonded to the circuit board, a molding underfill material can be used to fill the semiconductor chip. The above-described resin composition can be used as the molding underfill material, or a resin composition layer of the above-described resin sheet can be used.
[0135] The second embodiment of the present invention relates to a semiconductor chip package comprising a semiconductor chip and a cured form of the aforementioned resin composition sealing the semiconductor chip. In this type of semiconductor chip package, the cured form of the resin composition typically functions as a sealing layer. Examples of semiconductor chip packages according to the second embodiment include, for example, fan-out type WLP and fan-out type PLP.
[0136] The manufacturing method of this type of fan-out WLP semiconductor chip package includes the following steps: (A) The process of laminating a temporary fixing film on a substrate. (B) The process of temporarily fixing the semiconductor chip onto the temporary fixing film. (C) The process of laminating the resin composition of the resin sheet of the present invention onto a semiconductor chip, or coating the resin composition of the present invention onto a semiconductor chip, and then performing thermosetting to form a sealing layer. (D) The process of peeling the substrate and temporary fixing film from the semiconductor chip. (E) The process of forming a rewiring layer (insulating layer) on the surface of a semiconductor chip where the substrate and temporary fixing film have been stripped. (F) The process of forming a conductor layer (rewiring layer) on the redistribution forming layer (insulating layer), and (G) The process of forming a solder resist layer on the conductor layer. Furthermore, the manufacturing method of a semiconductor chip package may include the following steps: (H) The process of cutting multiple semiconductor chip packages into individual semiconductor chip packages for monolithic assembly.
[0137] For details of the manufacturing method of this semiconductor chip package, please refer to paragraphs 0066 to 0081 of International Publication No. 2016 / 035577, the contents of which are incorporated herein by reference.
[0138] The semiconductor chip package according to the third embodiment of the present invention is, for example, the semiconductor chip package of the second embodiment in which a redistribution layer or a solder resist layer is formed by curing the resin composition of the present invention.
[0139] Semiconductor Devices Semiconductor devices are packaged with semiconductor chips. Examples of semiconductor devices include various semiconductor devices used in electrical products (such as computers, mobile phones, smartphones, tablets, wearable devices, digital cameras, medical devices, and televisions) and vehicles (such as motorcycles, automobiles, trams, ships, and airplanes). Example
[0140] The present invention will now be described in more detail with reference to the embodiments. However, the present invention is not limited to these embodiments. It should be noted that, unless otherwise expressly stated, "parts" and "%" in the following description refer to "parts by mass" and "% by mass," respectively.
[0141] <Synthesis Example 1: Synthesis of Aliphatic Polyester Polyol Resin A> In a reaction vessel, 22.6 g of ε-caprolactone monomer (PLACCELM, manufactured by Daicel), 10 g of polypropylene glycol (diol type, 3000) (manufactured by Fujifilm and Kohden Chemical Co., Ltd.), and 1.62 g of stannous 2-ethylhexanoate (II) (manufactured by Fujifilm and Kohden Chemical Co., Ltd.) were added. The mixture was heated to 130°C under a nitrogen atmosphere and stirred for approximately 16 hours to allow the reaction to proceed. The resulting product was dissolved in chloroform, precipitated again with methanol, and then dried to obtain polyester polyol resin A containing hydroxyl-terminated aliphatic backbone. According to GPC analysis, Mn = 9000.
[0142] <Synthesis Example 2: Synthesis of Aliphatic Polyester Polyol Resin B> In a reaction vessel, 22.6 g of ε-caprolactone monomer (PLACCELM, manufactured by Daicel), 10 g of polyethylene glycol 1540 (manufactured by Fujifilm and Kohden Chemical Co., Ltd.), and 1.3 g of stannous 2-ethylhexanoate (II) (manufactured by Fujifilm and Kohden Chemical Co., Ltd.) were added. The mixture was heated to 130°C under a nitrogen atmosphere and stirred for approximately 16 hours to allow the reaction to proceed. The resulting product was dissolved in chloroform, reprecipitated with methanol, and dried to obtain polyester polyol resin B containing hydroxyl-terminated aliphatic backbone. According to GPC analysis, Mn = 4500.
[0143] <Synthesis Example 3: Synthesis of Aliphatic Polyester Polyol Resin C> In a reaction vessel, 22.6 g of ε-caprolactone monomer (PLACCELM, manufactured by Daicel), 10 g of polytetramethylene ether glycol PTMG1000 (manufactured by Mitsubishi Chemical Corporation), and 1.3 g of stannous 2-ethylhexanoate (II) (manufactured by Fujifilm and Kazuko Pure Chemicals) were added. The mixture was heated to 130°C under a nitrogen atmosphere and stirred for approximately 16 hours to allow the reaction to proceed. The resulting product was dissolved in chloroform, precipitated again with methanol, and dried to obtain polyester polyol resin C containing hydroxyl-terminated aliphatic backbone. According to GPC analysis, Mn = 3100.
[0144] <Inorganic filler material used> Silica A: Average particle size 9μm, specific surface area 5.0m² 2 / g, a substance that has been surface-treated with KBM573 (manufactured by Shin-Etsu Chemical Co., Ltd.); Silica B: Average particle size 1.6 μm, specific surface area 3.4 m²2 / g, a substance that has been surface-treated with KBM573 (manufactured by Shin-Etsu Chemical Co., Ltd.); Alumina A: Average particle size 8.4 μm, specific surface area 0.9 m². 2 / g, a substance that has undergone surface treatment with KBM573 (Shin-Etsu Chemical Industry).
[0145] <Example 1> Using a mixer, 8 parts of naphthalene-type epoxy resin (HP4032D manufactured by DIC, epoxy equivalent 144 g / eq.), 6.6 parts of alicyclic epoxy resin (Celloxide 2021P manufactured by Daicel, epoxy equivalent 136 g / eq.), 2.5 parts of polyester polyol A obtained in Synthesis Example 1, 0.5 parts of amine curing agent (KAYAHARD AA manufactured by Nippon Kayaku Co., Ltd.), 80 parts of silica A, and 0.4 parts of curing accelerator (2MA-OK-PW manufactured by Shikoku Kasei Co., Ltd.) were uniformly dispersed to obtain resin composition 1.
[0146] <Example 2> Using a mixer, 3 parts of naphthalene-type epoxy resin (HP4032D manufactured by DIC, epoxy equivalent 144 g / eq.), 3 parts of alicyclic epoxy resin (Celloxide 2021P manufactured by Daicel, epoxy equivalent 136 g / eq.), 4 parts of polyester polyol A obtained in Synthesis Example 1, 10 parts of anhydride-based curing agent (MH-700 manufactured by Shin Nippon Rikka), 90 parts of silica B, and 0.5 parts of curing accelerator (2MA-OK-PW manufactured by Shikoku Kasei) were uniformly dispersed to obtain resin composition 2.
[0147] <Example 3> Using a mixer, 8 parts of naphthalene-type epoxy resin (HP4032D manufactured by DIC Corporation, epoxy equivalent 144 g / eq.), 7 parts of alicyclic epoxy resin (Celloxide 2021P manufactured by Daicel Corporation, epoxy equivalent 136 g / eq.), 1 part of 2,2'-diallylbisphenol A (DABPA manufactured by Daiwa Chemical Industry Co., Ltd.), 2 parts of polyester polyol A obtained in Synthesis Example 1, 80 parts of silica A, and 0.4 parts of curing accelerator (2MA-OK-PW manufactured by Shikoku Chemical Co., Ltd.) were uniformly dispersed to obtain resin composition 3.
[0148] <Example 4> In Example 2, 90 parts of silica B were replaced with 120 parts of alumina A. Except as described above, the process was the same as in Example 2 to obtain resin composition 4.
[0149] <Example 5> Using a mixer, 3 parts of naphthalene-type epoxy resin (HP4032D manufactured by DIC, epoxy equivalent 144 g / eq.), 2 parts of alicyclic epoxy resin (Celloxide 2021P manufactured by Daicel, epoxy equivalent 136 g / eq.), 1 part of glycidyl ether-type epoxy resin (polyether glycol diglycidyl ether, EX-992L manufactured by Nagase ChemteX, epoxy equivalent 680 g / eq.), 9 parts of polyester polyol A obtained in Synthesis Example 1, 10 parts of anhydride-based curing agent (MH-700 manufactured by Shin Nippon Rikka), 100 parts of silica A, and 0.5 parts of curing accelerator (2MA-OK-PW manufactured by Shikoku Kasei) were uniformly dispersed to obtain resin composition 5.
[0150] <Example 6> In Example 2, 4 parts of polyester polyol resin A were replaced with 4 parts of polyester polyol resin B. Except as described above, the process was the same as in Example 2 to obtain resin composition 6.
[0151] <Example 7> In Example 3, 2 parts of polyester polyol resin A were replaced with 2 parts of polyester polyol resin C. Except as described above, the process was the same as in Example 3 to obtain resin composition 7.
[0152] <Example 8> In Example 5, 1 part of glycidyl ether type epoxy resin (polyether glycol diglycidyl ether, Nagase ChemteX "EX-992L", epoxy equivalent 680 g / eq.) was replaced with 1 part of fluorene type epoxy resin (Osaka Gas Chemical Co., Ltd. "EG-280", epoxy equivalent 460 g / eq.). Except for the above, the procedure was the same as in Example 5 to obtain resin composition 8.
[0153] <Comparative Example 1> In Example 1, 2.5 parts of the polyester polyol A obtained in Synthesis Example 1 were not used. Except as described above, the same procedure as in Example 1 was followed to obtain resin composition 9.
[0154] <Comparative Example 2> In Example 2, the amount of polyester polyol A obtained in Synthesis Example 1 was changed from 4 parts to 0.5 parts, and the amount of silica B was changed from 90 parts to 100 parts. Except for the above, the same procedure as in Example 2 was followed to obtain resin composition 10.
[0155] <Comparative Example 3> In Example 2, the amount of polyester polyol A obtained in Synthesis Example 1 was changed from 4 parts to 35 parts, and the amount of silica B was changed from 90 parts to 100 parts. Except for the above, the same procedure as in Example 2 was followed to obtain resin composition 11.
[0156] <Evaluation of flow marks> On a 12-inch silicon wafer, the resin compositions prepared in the examples and comparative examples were compressed and molded using a compression molding apparatus (mold temperature: 130°C, pressure: 6 MPa, curing time: 10 minutes) to form a resin composition layer with a thickness of 300 μm. Then, after heating at 150°C for 60 minutes, flow marks were confirmed by visually inspecting the surface of the resin composition layer, and the evaluation was performed according to the following criteria: 〇: No flow marks ×: Flow marks are present.
[0157] <Evaluation of Shear Strength> On a polyimide-coated silicon wafer, a silicone rubber frame with a 4mm diameter notch was used to fill the resin composition prepared in the examples and comparative examples into a cylindrical shape with a height of 5mm. After heating at 180°C for 90 minutes, the silicone rubber frame was removed, thereby producing a specimen formed from the cured resin composition. The shear strength of the interface between the polyimide and the cured resin composition was measured using a bond tester (Dage, Series 4000) at a head position 1mm away from the silicon wafer and a head speed of 700μm / s. Five tests were performed, and the average value was used for evaluation according to the following criteria: ◎: Shear strength is 2.5 kgf / mm 2 above 〇: Shear strength is 2.0 kgf / mm 2 Above and less than 2.5 kgf / mm 2 △: Shear strength is 1.7 kgf / mm 2 Above and less than 2.0 kgf / mm 2 ×: Shear strength less than 1.7 kgf / mm 2 .
[0158] <Determination of Warpage> On a 12-inch silicon wafer, the resin composition prepared in the examples and comparative examples was compressed and molded using a compression molding apparatus (mold temperature: 130°C, pressure: 6 MPa, curing time: 10 minutes) to form a resin composition layer with a thickness of 300 μm. Then, the resin composition layer was thermo-cured by heating at 180°C for 90 minutes. This yielded a sample substrate containing a cured layer of silicon wafer and resin composition. The warpage at 25°C was measured on the sample substrate using a shadow moire measuring device (Akorometrix Thermoire AXP). The measurement was performed according to JEITA EDX-7311-24, a standard of the Japan Electronics and Information Technology Industries Association. Specifically, the least squares method was used to calculate the fitted plane for all data on the substrate surface of the measurement area as a reference plane, and the difference between the minimum and maximum values in the vertical direction from this reference plane was calculated as the warpage. The evaluation was performed according to the following criteria: ◎: Warpage less than 1.8mm 〇: Warpage is greater than 1.8mm and less than 2mm ×: Warping amount is 2mm or more.
[0159] <Determination of the coefficient of linear thermal expansion (CTE)> On a 12-inch silicon wafer that had undergone demolding, the resin composition prepared in the examples and comparative examples was compressed and molded using a compression molding apparatus (mold temperature: 130°C, pressure: 6 MPa, curing time: 10 minutes) to form a resin composition layer with a thickness of 300 μm. Then, the resin composition layer was peeled off from the demolded 12-inch silicon wafer and thermo-cured at 150°C for 60 minutes to prepare a cured sample. The cured sample was cut into pieces 5 mm wide and 15 mm long to obtain test pieces. For these test pieces, thermomechanical analysis was performed using a thermomechanical analysis apparatus (Rigaku Thermo Plus TMA8310) using the tensile load method. Specifically, after mounting the test piece onto the aforementioned thermomechanical analysis apparatus, two consecutive measurements were taken under the conditions of a load of 1 g and a heating rate of 5°C / min. Then, the linear thermal expansion coefficient (ppm / °C) in the planar direction within the range of 25°C to 150°C in the second measurement was calculated and evaluated according to the following criteria: ◎: Less than 13 ppm / ℃ 〇: 13 ppm / ℃ or higher and less than 15 ppm / ℃ ×: 15ppm / ℃ or more.
[0160] [Table 1] *In the table, the contents of components (C) and (D) represent the contents when the non-volatile components in the resin composition are set to 100% by mass.
[0161] It was confirmed that in Examples 1-8, even without the (E) component, although there were differences in degree, the results were the same as those in the examples described above.
Claims
1. A resin composition comprising the following components (A) to (D): (A) Epoxy resin, (B) A curing agent selected from at least one of acid anhydride curing agents, amine curing agents, and phenolic curing agents. (C) Polyester polyol resins with aliphatic structures formed from lactones and polyols, and (D) Inorganic filler materials, (C) is a resin having a structure derived from a polyol, wherein the polyol-derived structure includes any one of an ethylene oxide structure, a propylene oxide structure, and a butene oxide structure. in, (C) The number average molecular weight of component (C) is above 2000. When the non-volatile component in the resin composition is set at 100% by mass, the content of component (C) is 1.5% by mass or more and 10% by mass or less. When the non-volatile component in the resin composition is set to 100% by mass, the content of component (D) is 60% by mass or more.
2. The resin composition according to claim 1, wherein, (A) The component contains one or more epoxy resins selected from naphthalene-type epoxy resins, alicyclic epoxy resins, and glycidyl ether-type epoxy resins.
3. The resin composition according to claim 1, wherein, (A) The components include any one of the following epoxy resins selected from naphthalene-type epoxy resins and alicyclic epoxy resins.
4. The resin composition according to claim 1, wherein, (A) The component contains a fused ring backbone.
5. The resin composition according to claim 1, wherein, (A) The components include one or more epoxy resins selected from naphthalene-type epoxy resins, naphthol-type epoxy resins, and anthracene-type epoxy resins.
6. The resin composition according to claim 1, wherein, (B) The component is at least one curing agent selected from amine curing agents and phenol curing agents having a primary amino group.
7. The resin composition according to claim 1, wherein, When the non-volatile component in the resin composition is set to 100% by mass, the content of component (B) is 0.1% by mass or more.
8. The resin composition according to claim 1, wherein, When the non-volatile component in the resin composition is set to 100% by mass, the content of component (B) is less than 10% by mass.
9. The resin composition according to claim 1, wherein, (C) The terminal of the component is either a hydroxyl group or a carboxyl group.
10. The resin composition according to claim 1, wherein, (C) The component has one or more functional groups selected from hydroxyl, carboxyl, amino, acid anhydride, vinyl, allyl, and maleimide.
11. The resin composition according to claim 1, wherein, When the content of component (A) in the resin composition is 100% by mass and the content of component (C) in the resin composition is 100% by mass and the ratio of a1 / c1 is 0.1 or higher, the ratio of a1 to c1 is greater than or equal to 0.
1.
12. The resin composition according to claim 1, wherein, When the content of component (A) in the resin composition is 100% by mass and the content of component (C) in the resin composition is 100% by mass, the ratio of a1 / c1 is 0.3 or higher.
13. The resin composition according to claim 1, wherein, When the content of component (A) in the resin composition is 100% by mass and the content of component (C) in the resin composition is 100% by mass, the ratio of a1 / c1 is 0.5 or higher.
14. The resin composition according to claim 1, wherein, When the content of component (A) in the resin composition is 100% by mass and the content of component (C) in the resin composition is 100% by mass, the ratio of a1 / c1 is 20 or less.
15. The resin composition according to claim 1, wherein, When the content of component (A) in the resin composition is 100% by mass and the content of component (C) in the resin composition is 100% by mass, the ratio of a1 / c1 is 15 or less.
16. The resin composition according to claim 1, wherein, When the content of component (A) in the resin composition is 100% by mass and the content of component (C) in the resin composition is 100% by mass, the ratio of a1 / c1 is 10 or less.
17. The resin composition according to claim 1, wherein, When the content of component (B) in the resin composition is 100% by mass, and b1 is defined as b1, the ratio of b1 / c1 is 0.01 or higher.
18. The resin composition according to claim 1, wherein, When the content of component (B) in the resin composition is 100% by mass, and b1 is defined as b1, the ratio of b1 / c1 is 0.05 or higher.
19. The resin composition according to claim 1, wherein, When the content of component (B) in the resin composition is 100% by mass, and b1 is defined as b1, the ratio of b1 / c1 is 0.1 or higher.
20. The resin composition according to claim 1, wherein, When the content of component (B) in the resin composition is 100% by mass, and b1 is defined as b1, the ratio of b1 / c1 is less than 10.
21. The resin composition according to claim 1, wherein, When the content of component (B) in the resin composition is 100% by mass, and b1 is defined as b1, the ratio of b1 / c1 is 5 or less.
22. The resin composition according to claim 1, wherein, When the content of component (B) in the resin composition is 100% by mass, and b1 is defined as b1, the ratio of b1 / c1 is 3 or less.
23. The resin composition according to claim 1, wherein, When the non-volatile component in the resin composition is set to 100% by mass, the content of component (D) is 70% by mass or more.
24. The resin composition according to claim 1, wherein, When the non-volatile component in the resin composition is set to 100% by mass, the content of component (D) is 75% by mass or more.
25. The resin composition according to claim 1, wherein, When the non-volatile component in the resin composition is set to 100% by mass, the content of component (D) is 95% by mass or less.
26. The resin composition according to claim 1, wherein, When the non-volatile component in the resin composition is set to 100% by mass, the content of component (D) is 90% by mass or less.
27. The resin composition according to claim 1, wherein, When the non-volatile component in the resin composition is set to 100% by mass, the content of component (D) is 85% by mass or less.
28. The resin composition according to claim 1, used as a sealing layer.
29. A resin sheet comprising: Support body, and A resin composition layer comprising the resin composition according to any one of claims 1 to 28 is disposed on the support.
30. A circuit board comprising a cured layer formed using a cured resin composition according to any one of claims 1 to 28.
31. A semiconductor chip package comprising: The circuit board according to claim 30, and Semiconductor chips mounted on the circuit board.
32. A semiconductor chip package comprising a semiconductor chip sealed with a resin composition according to any one of claims 1 to 28 or a resin sheet according to claim 29.
33. A semiconductor device comprising the semiconductor chip package of claim 32.
Citation Information
Patent Citations
Resin composition for mold underfill
JP2017008312A
Sealing sheet
WO2016035577A1
Liquid resin composition for encapsulation and electronic component / device
CN109071919A
Epoxy resin curing agent, epoxy resin composition, epoxy resin cured product and optical member using the same
JP2007308683A
Epoxy resin composition, prepreg, and method for producing fiber-reinforced composite material
JP2017122205A