A method for determining the work hardening behavior of a cylindrical indenter during repeated loading and unloading

By repeatedly adding and unloading the work hardening behavior of the cylindrical indenter, using the power function and bilinear model to fit the material parameters, the problem of the inability to judge the real work hardening behavior of the material in the existing technology is solved, and the test material is achieved The accurate judgment avoids calculation errors and is suitable for prediction of work hardening behaviors of various materials.

CN114519237BActive Publication Date: 2024-11-08SOUTHEAST UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210029228.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-11
Publication Date
2024-11-08
Estimated Expiration
2042-01-11

AI Technical Summary

Technical Problem

The existing cylindrical indentation head pressing detection technology cannot effectively judge the actual work hardening behavior of the tested material. Especially in engineering applications, when metal materials show obvious work hardening behavior, the existing method is not applicable, resulting in a single axis. There are huge calculation errors in the calculation of mechanical properties.

Method used

The process hardening behavior determination method of repeatedly adding and unloading cylindrical indenter heads is used to obtain the pressurized load-pressed displacement curve through shallow pressurized test, and the material parameters are fitted using power function model and bilinear model to calculate the strain proportion limit and processing Hardening index, combined with deep pressing test, determines the actual work hardening behavior of the material.

Benefits of technology

It can actively judge the actual work hardening behavior of the tested material and avoid inversion errors caused by the wrong selection of constitutive equations. It is suitable for the prediction of work hardening behavior of in-service equipment materials, additive manufacturing materials and new materials, and is universal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114519237B_ABST
    Figure CN114519237B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for determining the work hardening behavior of a cylindrical indenter by repeated loading and unloading, comprising: repeatedly loading and unloading the cylindrical indenter to perform a shallow indentation test on the material to be tested, and obtaining the loading segment of the load-displacement curve; using a power function model and a bilinear model to describe the work hardening behavior of the material to be tested, respectively, and calculating and obtaining the strain proportional limit and work hardening index of the material to be tested corresponding to power strengthening and the strain proportional limit and strengthening coefficient of the material to be tested corresponding to bilinear strengthening; performing a deep indentation test at the same position as the shallow indentation test, and obtaining the corresponding loading segment of the load-displacement curve; respectively obtaining the prediction errors of the indentation load corresponding to power strengthening and bilinear, and determining that the smaller of the prediction errors is the actual work hardening behavior of the material to be tested. The present invention can actively determine the actual work hardening behavior of the material in the indentation test, avoid the inversion error caused by the wrong selection of the constitutive equation, and has universal applicability to materials and occasions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of material property determination, and in particular to a method for determining work hardening behavior of repeatedly loading and unloading a cylindrical indenter. Background Art

[0002] As an alternative method to conventional uniaxial mechanical properties testing, cylindrical indenter indentation testing technology has the significant advantages of no sampling and being nearly non-destructive. It is particularly suitable for occasions with high microstructural heterogeneity such as welds, and is considered to be a mechanical properties testing method with broad application prospects.

[0003] In 2016, ARHMidawi et al. published a paper titled "Novel techniques for estimating yield strength from loads measured using nearly-flat instrumented indenters" in the journal Materials Science & Engineering A, Vol. 675, pp. 449-453. They used the expansion cavity model to study the cavity expansion behavior of ideal elastic-plastic materials when a cylindrical indenter was pressed in, and established a method for estimating the yield strength of the tested material. This method is only applicable to the estimation of elastic parameters and proportional limits of ideal elastic-plastic materials or materials with very insignificant work hardening. Metal materials in engineering applications usually show obvious work hardening behavior, so this method is not applicable.

[0004] In 2016, Cai Lixun and others applied for an invention patent titled "Method for Determining the Uniaxial Constitutive Relationship of Materials Predicted by Cylindrical Flat Head Indentation", and established an indentation control equation for power-hardened materials that correlates the cylindrical indentation load-indentation displacement curve and material parameters (work hardening index and proportional limit). This method is only applicable to materials that exhibit power-hardening work hardening behavior, and is not applicable to materials that exhibit work hardening behaviors such as linear strengthening.

[0005] In 2017, ARH Midawi et al. proposed a method for determining the parameters of power-hardened materials based on the finite element trial-and-error method in the journal "Internal Journal of Solids and Structures" Volume 104-105, pages 81-91. The material parameters of the tested power-hardened material in the finite element model (such as Young's modulus E, strain proportional limit ε0, and work hardening exponent n) are continuously adjusted until the indentation load-indentation displacement curve obtained in the test reaches the best consistency. This method is also only applicable to materials that exhibit power-hardening work hardening behavior, and for each indentation test, this method requires a large number of finite element calculations to determine the material parameters, which is difficult to promote in engineering under existing computing conditions.

[0006] In the prior art, the indentation control equations that relate the characteristic parameters of the cylindrical indenter (such as the indentation load-displacement curve) and the work hardening behavior of the material being tested are all established based on a single work hardening behavior. Therefore, the existing cylindrical indenter indentation test requires the work hardening behavior of the material being tested to be predicted before the test, and does not have the ability to judge the actual work hardening behavior of the material being tested. The situations where a cylindrical indenter is required for indentation are usually unable to predict the work hardening behavior of the material being tested, and misjudging the work hardening behavior of the material being tested will cause huge calculation errors in the indentation measurement of the uniaxial mechanical properties. For the target application scenarios of cylindrical indenter indentation tests such as service materials, welds, and new materials, the existing indentation detection technology is not applicable.

[0007] Therefore, it is necessary to design a method that can actively determine the actual work hardening behavior of the tested material in the cylindrical indenter penetration test. Summary of the invention

[0008] In view of the deficiencies in the prior art, the present invention provides a method for determining the work hardening behavior of repeatedly loading and unloading a cylindrical indenter, which solves the technical problem that the prior indentation method can only test a certain constitutive relationship material and cannot determine the true work hardening behavior of the tested material.

[0009] The technical solution adopted by the present invention is as follows:

[0010] A method for determining work hardening behavior of a cylindrical indenter subjected to repeated loading and unloading, comprising:

[0011] S1. Repeatedly load and unload the cylindrical indenter to perform shallow indentation test on the material being tested, using P = Ch m Describe the loading section of the indentation load-indentation displacement curve, where C and m are the fitting coefficient and fitting index, respectively, and P and h are the indentation load and indentation displacement, respectively;

[0012] S2. Use power function model Describes the work hardening behavior of the tested material, ε0 and n are the strain proportional limit and work hardening exponent of the tested material corresponding to power hardening, and E0 is the initial Young's modulus of the tested material;

[0013] The strain ratio limit ε0 and work hardening exponent n of the tested material corresponding to power hardening are determined by the following formula:

[0014]

[0015] Where W t (N) , and V p (N) are the total external work of the Nth indentation cycle of the shallow indentation test, the effective Young's modulus of the tested material, the maximum indentation depth and the volume of the plastic zone; ξ and ψ are the fitting coefficient function and the fitting exponential function respectively; N is the maximum number of cycles;

[0016] Calculate the equivalent stress-equivalent strain data points of the shallow indentation cycle, and use the power function model to fit, and obtain the optimal value of the work hardening exponent n and the corresponding optimal value of the strain proportional limit ε0 through iterative calculation;

[0017] S3. Using bilinear model Describes the work hardening behavior of the tested material, ε0, E p are the strain proportional limit and strengthening coefficient of the tested material corresponding to bilinear strengthening, E0 is the initial Young’s modulus of the tested material;

[0018] The strain proportional limit ε0 and strengthening coefficient E of the tested material corresponding to bilinear strengthening are determined by the following formula p :

[0019]

[0020] In the formula, α and β are the fitting coefficient function and the fitting exponential function respectively;

[0021] Calculate the equivalent stress-equivalent strain data points of the shallow indentation cycle, and use the bilinear model fitting to obtain the strengthening coefficient E through iterative calculation. p The optimal value of and the corresponding optimal value of strain proportional limit ε0;

[0022] S4. Monotonically load the cylindrical indenter to perform a deep penetration test on the same material at the same position as the shallow penetration test, and use P = Ch m Describing a loading segment of an indentation load-indentation displacement curve of a deep indentation test, wherein the indentation depth of the deep indentation test is greater than the maximum indentation depth of the shallow indentation test;

[0023] Substitute the strain proportional limit ε0 and the optimal value of the work hardening exponent n of the tested material corresponding to power hardening into the following two equations to determine the fitting coefficient C and the fitting exponent m, thereby obtaining the first set of indentation load-indentation displacement curves of the deep indentation test;

[0024] C=(i 00 +i 01 n+i 02 n 2 )+(i 10 +i 11 n+i 12 n 2 )ε0

[0025] m=j0+j1ε0+j2n+j3ε0n

[0026] Among them, i ij (i=0,1,j=0,1,2),j0,j1,j2,j3 are calibration coefficients;

[0027] The strain proportional limit ε0 and strengthening coefficient E of the tested material corresponding to the bilinear strengthening p The optimal value is substituted into the following two equations to determine the fitting coefficient C and the fitting index m, thereby obtaining the second set of indentation load-indentation displacement curves of the deep indentation test;

[0028]

[0029]

[0030] Among them, k0, k1, k2, k3, m0, m1, m2 are calibration coefficients;

[0031] S5. Calculate the indentation load prediction errors of the two sets of indentation load-indentation displacement curves of the deep indentation test respectively, and determine that the smaller one of the indentation load prediction errors corresponding to power hardening and bilinear hardening is the actual work hardening behavior of the tested material.

[0032] Further technical solutions are:

[0033] Step S1 further includes:

[0034] Pass-through Fit the unloading curve of the i-th (1≤i≤N) indentation cycle of the shallow indentation test to obtain the residual indentation depth and unloading slope S (i) ;

[0035] The effective Young's modulus of the i-th indentation cycle of the shallow indentation test is calculated by the following formula:

[0036]

[0037] Where R is the radius of the cylindrical indenter, v is the Poisson’s ratio of the material being tested, and E ind and v ind are Young’s modulus and Poisson’s ratio of the cylindrical indenter material, respectively;

[0038] Pass-through Calculate the total external work W of the i-th pressing cycle of the shallow pressing test t (i) , is the maximum penetration depth of the i-th penetration cycle of the shallow penetration test;

[0039] Pass-through Calculate the elastic external force work W of the i-th pressing cycle of the shallow pressing test e (i) , is the load-displacement curve during unloading of the i-th indentation cycle of the shallow indentation test;

[0040] pass Calculate the elastic external force work W of the i-th pressing cycle of the shallow pressing test p (i) .

[0041] In step S2 and step S3, the equivalent stress-equivalent strain data points of the shallow indentation cycle are calculated using the following two formulas:

[0042]

[0043]

[0044] In the formula, are the equivalent stress and equivalent strain, W e (i) , W p (i) , V p (i) are the elastic external force work, plastic external force work, effective Young's modulus of the tested material, maximum indentation load, maximum indentation depth, and plastic zone volume of the tested material in the i-th indentation cycle of the shallow indentation test; R is the radius of the cylindrical indenter, E ind and v ind are Young’s modulus and Poisson’s ratio of the cylindrical indenter material, respectively.

[0045] In step S2, the fitting coefficient function ξ and the fitting exponential function ψ are determined by the following two equations respectively:

[0046]

[0047] ψ=b0+b1n,where a ij(i=0, 1, 2, j=0, 1, 2), b0 and b1 are calibration coefficients.

[0048] In step S3, the fitting coefficient function α and the fitting exponential function β are determined by the following two equations:

[0049]

[0050] β=(d0+d1ε0), where c ij (i=0, 1, j=0, 1, 2), d0 and d1 are calibration coefficients.

[0051] Plastic zone volume V of the tested material in the Nth indentation cycle of the shallow indentation test p (N) Determined by the following formula:

[0052]

[0053] In step S5, the prediction error of the pressing load is calculated by the following formula:

[0054]

[0055] In the formula, and are the predicted value and tested value of the indentation load corresponding to the kth displacement sampling point, respectively, and M is the total number of sampling points.

[0056] The beneficial effects of the present invention are as follows:

[0057] The present invention can judge the actual work hardening behavior of the tested material, actively determine the actual work hardening behavior of the tested material in a cylindrical indenter indentation test, and avoid inversion errors caused by incorrect selection of constitutive equations.

[0058] The present invention does not require additional acquisition of indentation characteristic parameters such as the indentation plastic zone radius and indentation profile, and is universal for test materials and test occasions. It can be widely used in the prediction of work hardening behavior of in-service equipment materials, additive manufacturing materials, new materials, and performance-degraded materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] Figure 1 This is a schematic diagram of the cylindrical indenter used in an embodiment of the present invention.

[0060] Figure 2 1 is a pressing load-pressing displacement curve of an embodiment of the present invention.

[0061] Figure 3 This is a diagram of the inversion results of the equivalent stress-equivalent strain power enhancement of the SA508 Gr.3 steel material according to an embodiment of the present invention.

[0062] Figure 4 This is a diagram of the equivalent stress-equivalent strain bilinear strengthening inversion result of the SA508 Gr.3 steel material according to an embodiment of the present invention.

[0063] Figure 5 This is the prediction of the deep indentation curve of the SA508 Gr.3 steel material according to the embodiment of the present invention.

[0064] Figure 6 This is a diagram of equivalent stress-equivalent strain inversion results of selected and discarded SA508Gr.3 steel materials according to an embodiment of the present invention.

[0065] Figure 1 In: 1. External load; 2. Cylindrical indenter; 3. Tested material. DETAILED DESCRIPTION

[0066] The specific implementation of the present invention is described below with reference to the accompanying drawings.

[0067] The present invention provides a method for determining work hardening behavior of a cylindrical indenter subjected to repeated loading and unloading, comprising:

[0068] S1. Repeatedly load and unload the cylindrical indenter to perform shallow indentation test on the material being tested, using P = Ch m Describe the loading section of the indentation load-indentation displacement curve, where C and m are the fitting coefficient and fitting index, respectively, and P and h are the indentation load and indentation displacement, respectively;

[0069] Specifically, it also includes:

[0070] Pass-through Fit the unloading curve of the i-th (1≤i≤N) indentation cycle of the shallow indentation test to obtain the residual indentation depth and unloading slope S (i) ;

[0071] The effective Young's modulus of the i-th indentation cycle of the shallow indentation test is calculated by the following formula:

[0072]

[0073] Where R is the radius of the cylindrical indenter, v is the Poisson’s ratio of the material being tested, and E ind and v ind are Young’s modulus and Poisson’s ratio of the cylindrical indenter material, respectively;

[0074] Pass-through Calculate the total external work W of the i-th pressing cycle of the shallow pressing test t (i) , is the maximum penetration depth of the i-th penetration cycle of the shallow penetration test;

[0075] Pass-through Calculate the elastic external force work W of the i-th pressing cycle of the shallow pressing test e (i) , is the load-displacement curve during unloading of the i-th indentation cycle of the shallow indentation test;

[0076] pass Calculate the elastic external force work W of the i-th pressing cycle of the shallow pressing test p (i) ;

[0077] S2. Use power function model Describes the work hardening behavior of the material being tested (i.e. stress σ eq - strain ε eq Relationship), ε0 and n are the strain proportional limit and work hardening index of the tested material corresponding to power hardening, and E0 is the initial Young's modulus of the tested material;

[0078] S21. Determine the strain ratio limit ε0 and work hardening exponent n of the tested material corresponding to power hardening by the following formula:

[0079]

[0080] Where W t (N) , and V p (N) are the total external work of the Nth indentation cycle of the shallow indentation test, the effective Young's modulus of the tested material, the maximum indentation depth and the volume of the plastic zone; ξ and ψ are the fitting coefficient function and the fitting exponential function respectively; N is the maximum number of cycles;

[0081]

[0082] The fitting coefficient function ξ and the fitting exponential function ψ are determined by the following two equations:

[0083]

[0084] Among them, a ij (i=0,1,2,j=0,1,2), b0, b1 are all known calibration coefficients;

[0085] In the first iteration calculation, n=0.1 is initialized, and the strain ratio limit ε0 of the tested power-hardened material is determined using formula (3);

[0086] S22. Calculate the equivalent stress-equivalent strain data points of the shallow indentation cycle using equations (5) and (6):

[0087]

[0088]

[0089] In the formula, are the equivalent stress and equivalent strain, W e (i) , W p (i) , V p (i) are the elastic external force work, plastic external force work, effective Young's modulus of the tested material, maximum indentation load, maximum indentation depth, and plastic zone volume of the tested material in the i-th indentation cycle of the shallow indentation test; R is the radius of the cylindrical indenter, E ind and v ind are Young’s modulus and Poisson’s ratio of the cylindrical indenter material, respectively;

[0090] S23, using the power function model (2) to fit the equivalent stress-equivalent strain data points calculated in S22, determine the new work hardening index n New , calculate the calculation error Error(n) of the work hardening index: n New is the newly calculated work hardening index, n is the assumed work hardening index;

[0091] S24. If the calculation error Error(n) is less than the allowable error δ(customized), the calculation is completed and the proportional limit and work hardening index of the power hardening material are output; otherwise, the new work hardening index n is used. nNew Alternative assumption of work hardening exponent n (n = n New ), and repeat steps S21 to S24 until the work hardening index calculation error Error(n) is less than the allowable error δ;

[0092] So far, the optimal value of the work hardening exponent n and the corresponding optimal value of the strain proportional limit ε0 are obtained;

[0093] S3. Using bilinear model Describes the work hardening behavior of the tested material, ε0, E p are the strain proportional limit and strengthening coefficient of the tested material corresponding to bilinear strengthening, E0 is the initial Young’s modulus of the tested material;

[0094] S31, determine the strain ratio limit ε0 and strengthening coefficient E of the tested material corresponding to bilinear strengthening by the following formula p :

[0095]

[0096] In the formula, α and β are the fitting coefficient function and the fitting exponential function respectively; the meanings of other parameters are the same as those in formula (3). Determined by formula (4);

[0097] The fitting coefficient function α and the fitting exponential function β are determined by the following two formulas:

[0098]

[0099] Among them, c ij (i=0,1,j=0,1,2), d0 and d1 are known calibration coefficients;

[0100] In the first calculation, the initial strengthening coefficient Ep = 2000MPa is set, and the strain proportional limit ε0 of the tested power-hardened material is determined using formula (8);

[0101] S32, using equations (5) and (6) to calculate the equivalent stress-equivalent strain data points of the shallow compression cycle;

[0102] S33, using the bilinear model (7) to fit the equivalent stress-equivalent strain data points obtained by S32, and determine the new strengthening coefficient E PNew . The calculation error of the reinforcement coefficient Error (E P ): E pNew is the newly calculated reinforcement coefficient, E P is the hypothesized reinforcement coefficient;

[0103] S34、If the calculation error Error(E P ) is less than the allowable error δ (customized), the calculation is completed and the proportional limit and strengthening coefficient of the bilinear strengthening material are output. Otherwise, the new strengthening coefficient E is used. PNew The reinforcement coefficient E of the alternative hypothesis P (E P =E PNew ), and repeat steps S31 to S34 until the enhancement coefficient calculation error Error (E P ) is less than the allowable error δ.

[0104] So far, we have obtained the reinforcement coefficient E p The optimal value of and the corresponding optimal value of strain proportional limit ε0;

[0105] S4. Monotonically load the cylindrical indenter to perform a deep penetration test on the same material at the same position as the shallow penetration test, and use P = Ch m Describing a loading segment of an indentation load-indentation displacement curve of a deep indentation test, wherein the indentation depth of the deep indentation test is greater than the maximum indentation depth of the shallow indentation test;

[0106] Substitute the strain proportional limit ε0 and the optimal value of the work hardening exponent n of the tested material corresponding to power hardening into the following two equations to determine the fitting coefficient C and the fitting exponent m, thereby obtaining the first set of indentation load-indentation displacement curves of the deep indentation test;

[0107] C=(i 00 +i 01 n+i 02 n 2 )+(i 10 +i 11 n+i 12 n 2 )ε0 (9)

[0108] m=j0+j1ε0+j2n+j3ε0n (10)

[0109] Among them, i ij (i=0,1,j=0,1,2), j0, j1, j2, j3 are known calibration coefficients;

[0110] The strain proportional limit ε0 and strengthening coefficient E of the tested material corresponding to the bilinear strengthening p The optimal value is substituted into the following two equations to determine the fitting coefficient C and the fitting index m, thereby obtaining the second set of indentation load-indentation displacement curves of the deep indentation test;

[0111]

[0112]

[0113] Among them, k0, k1, k2, k3, m0, m1, m2 are known calibration coefficients;

[0114] S5, respectively calculating the indentation load prediction errors of the two sets of indentation load-indentation displacement curves of the deep indentation test, and determining that the smaller one of the indentation load prediction errors corresponding to power hardening and bilinear hardening is the actual work hardening behavior of the tested material;

[0115] Specifically, the loading section of the indentation load P-indentation displacement h curve is divided into M equal parts (M is preferably not less than 10) and the indentation load prediction error is calculated by the following formula:

[0116]

[0117] In the formula, and are the predicted value and tested value of the indentation load corresponding to the kth displacement sampling point respectively.

[0118] If the deep indentation load prediction error of the power hardening material parameters is not greater than the deep indentation load prediction error of the bilinear hardening material parameters, the power hardening is determined to be the actual work hardening behavior of the tested material; otherwise, the bilinear hardening is determined to be the actual work hardening behavior of the tested material.

[0119] The technical solution of the present application is further illustrated by specific embodiments below.

[0120] The determination method of this embodiment is used to determine the work hardening behavior of SA508 Gr.3 steel material, including the following steps:

[0121] (1) Calibration of material parameters for power hardening and bilinear hardening based on repeated loading and unloading of a cylindrical indenter with shallow penetration depth;

[0122] like Figure 1 As shown, a carbide cylindrical indenter 2 with a radius R of 0.38 mm is used, and the tested material 3 is a rectangular parallelepiped specimen with a size of 50 mm long×10 mm wide×10 mm thick.

[0123] First, the surface of the tested SA508 Gr.3 steel material was simply polished to meet the test conditions, requiring the roughness of the test surface to be less than 0.32 μm and the area covered by the cylindrical indenter to be flat.

[0124] Secondly, under the action of external load 1, a carbide cylindrical indenter 2 (tungsten carbide, elastic modulus E ind =710GPa, Poisson's ratio v ind =0.21) A shallow indentation test including 10 loading and unloading cycles was performed on the smooth surface of the tested material (the maximum indentation depth of the 10th loading Obtain the indentation load P-indentation displacement h curve of the shallow indentation test.

[0125] Next, the indentation load P-indentation displacement h curve of the cylindrical indenter with shallow indentation depth is respectively brought into the inversion model established based on power hardening and bilinear hardening behavior to complete the material parameter calibration. The specific steps of material parameter calibration are as follows from step S1 to step S3 above.

[0126] Among them, the power enhancement inversion results of equivalent stress-equivalent strain of SA508 Gr.3 steel material are as follows: Figure 3 The bilinear strengthening inversion results of equivalent stress-equivalent strain of SA508 Gr.3 steel material are shown in Figure 4 shown.

[0127] (2) Determination of work hardening behavior based on the deep penetration depth of a cylindrical indenter under monotonic loading.

[0128] First, use the same carbide cylindrical indenter (tungsten carbide, elastic modulus Eind =710GPa, Poisson's ratio v ind =0.21) After the 10th loading of the shallow indentation test is completed, a deep indentation test with monotonic loading is performed on the same position of the tested sample, with the maximum loading depth being 0.26R, and the indentation load P-indentation displacement h curve of the deep indentation test is obtained. The indentation load-displacement curve of the entire indentation test is shown in Figure 2 shown.

[0129] Then, the indentation load P-indentation displacement h curve extrapolated based on the power hardening behavior and the bilinear hardening behavior is matched with the deep indentation test result to determine the actual work hardening behavior of the tested material. The specific steps for determining the actual work hardening behavior of the material are as shown in the above steps S4 and S5, wherein the known calibration coefficients involved in formula (9)-formula (12) are taken according to Table 1-Table 4 respectively:

[0130] Table 1 Calibration coefficients in the power hardening material fitting coefficient C function

[0131] coefficient <![CDATA[i 00 ]]> <![CDATA[i 01 ]]> <![CDATA[i 02 ]]> <![CDATA[i 10 ]]> <![CDATA[i 11 ]]> <![CDATA[i 12 ]]> Numeric 3.11E+00 -2.90E+02 1.29E+04 4.50E+05 2.05E+06 6.17E+06

[0132] Table 2 Calibration coefficients in the fitting index m function of power hardened materials

[0133] coefficient <![CDATA[j0]]> <![CDATA[j1]]> <![CDATA[j2]]> <![CDATA[j3]]> Numeric 9.28E-02 8.43E+00 7.66E-01 2.58E+01

[0134] Table 3 Calibration coefficients in the bilinear strengthening material fitting coefficient C function

[0135] coefficient <![CDATA[k0]]> <![CDATA[k1]]> <![CDATA[k2]]> <![CDATA[k3]]> Numeric 3.27E+01 4.47E+05 1.67E+05 1.74E+06

[0136] Table 4 Calibration coefficients in the bilinear strengthening material fitting index m function

[0137] coefficient <![CDATA[m0]]> <![CDATA[m1]]> <![CDATA[m2]]> Numeric 2.83E+00 -6.24E+02 7.66E+04

[0138] The indentation curve of this embodiment is predicted as Figure 5 As shown. In step S5, the loading section of the deep indentation test indentation load P-indentation displacement h curve (0.08R≤h≤0.26R part) is divided into 10 equal parts, and the indentation load prediction error is calculated by formula (13). In this embodiment, for the tested SA508 Gr.3 steel material, the power hardening and bilinear hardening indentation load prediction errors Error are 0.021 and 1.78 respectively, so the power hardening is determined to be the actual work hardening behavior of the tested SA508 Gr.3 steel material. The equivalent stress-equivalent strain inversion results of the SA508 Gr.3 steel material selected and discarded in this embodiment are shown in Figure 6 The determination method of the present application can make a judgment on the actual work hardening behavior of the tested material and avoid the inversion error caused by the wrong selection of the constitutive equation.

[0139] Those skilled in the art can understand that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions recorded in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for determining the work hardening behavior of a cylindrical indenter by repeated loading and unloading, characterized in that: include: S1. Repeatedly load and unload the cylindrical indenter to perform shallow indentation test on the material being tested, using P = Ch m Describe the loading section of the indentation load-indentation displacement curve, where C and m are the fitting coefficient and fitting index, respectively, and P and h are the indentation load and indentation displacement, respectively; S2. Use power function model Describes the work hardening behavior of the tested material, ε0 and n are the strain proportional limit and work hardening exponent of the tested material corresponding to power hardening, and E0 is the initial Young's modulus of the tested material; The strain ratio limit ε0 and work hardening exponent n of the tested material corresponding to power hardening are determined by the following formula: In the formula, and are the total external work of the Nth indentation cycle of the shallow indentation test, the effective Young's modulus of the tested material, the maximum indentation depth and the volume of the plastic zone; ξ and ψ are the fitting coefficient function and the fitting exponential function respectively; N is the maximum number of cycles; Calculate the equivalent stress-equivalent strain data points of the shallow indentation cycle, and use the power function model to fit, and obtain the optimal value of the work hardening exponent n and the corresponding optimal value of the strain proportional limit ε0 through iterative calculation; S3. Using bilinear model Describes the work hardening behavior of the tested material, ε0, E p are the strain proportional limit and strengthening coefficient of the tested material corresponding to bilinear strengthening, E0 is the initial Young’s modulus of the tested material; The strain proportional limit ε0 and strengthening coefficient E of the tested material corresponding to bilinear strengthening are determined by the following formula p : In the formula, α and β are the fitting coefficient function and the fitting exponential function respectively; Calculate the equivalent stress-equivalent strain data points of the shallow indentation cycle, and use the bilinear model fitting to obtain the strengthening coefficient E through iterative calculation. p The optimal value of and the corresponding optimal value of strain proportional limit ε0; S4. Monotonically load the cylindrical indenter to perform a deep penetration test on the same material at the same position as the shallow penetration test, and use P = Ch m Describing a loading segment of an indentation load-indentation displacement curve of a deep indentation test, wherein the indentation depth of the deep indentation test is greater than the maximum indentation depth of the shallow indentation test; Substitute the strain proportional limit ε0 and the optimal value of the work hardening exponent n of the tested material corresponding to power hardening into the following two equations to determine the fitting coefficient C and the fitting exponent m, thereby obtaining the first set of indentation load-indentation displacement curves of the deep indentation test; C=(i 00 +i 01 n+i 02 n 2 )+(i 10 +i 11 n+i 12 n 2 )ε0 m=j0+j1ε0+j2n+j3ε0n Among them, i 00 ,i 01 ,i 02 ,i 10 ,i 11 ,i 12 , j0, j1, j2, j3 are all calibration coefficients; The strain proportional limit ε0 and strengthening coefficient E of the tested material corresponding to the bilinear strengthening p The optimal value is substituted into the following two equations to determine the fitting coefficient C and the fitting index m, thereby obtaining the second set of indentation load-indentation displacement curves of the deep indentation test; Among them, k0, k1, k2, k3, m0, m1, m2 are calibration coefficients; S5. Calculate the indentation load prediction errors of the two sets of indentation load-indentation displacement curves of the deep indentation test respectively, and determine that the smaller one of the indentation load prediction errors corresponding to power hardening and bilinear hardening is the actual work hardening behavior of the tested material.

2. The method according to claim 1, characterized in that Step S1 further includes: Pass-through Fit the unloading curve of the i-th indentation cycle of the shallow indentation test, 1≤i≤N, and obtain the residual indentation depth and unloading slope S (i) ; The effective Young's modulus of the i-th indentation cycle of the shallow indentation test is calculated by the following formula: Where R is the radius of the cylindrical indenter, v is the Poisson’s ratio of the material being tested, and E ind and v ind are Young’s modulus and Poisson’s ratio of the cylindrical indenter material, respectively; Pass-through Calculate the total external work W of the i-th pressing cycle of the shallow pressing test t (i) , is the maximum penetration depth of the i-th penetration cycle of the shallow penetration test; Pass-through Calculate the elastic external force work of the i-th indentation cycle in the shallow indentation test is the load-displacement curve during unloading of the i-th indentation cycle of the shallow indentation test; pass Calculate the elastic external force work of the i-th indentation cycle in the shallow indentation test 3. The method according to claim 2, characterized in that In step S2 and step S3, the equivalent stress-equivalent strain data points of the shallow indentation cycle are calculated using the following two formulas: In the formula, are the equivalent stress and equivalent strain, respectively. are the elastic external force work, plastic external force work, effective Young's modulus of the tested material, maximum indentation load, maximum indentation depth, and plastic zone volume of the tested material in the i-th indentation cycle of the shallow indentation test; R is the radius of the cylindrical indenter, E ind and v ind are Young’s modulus and Poisson’s ratio of the cylindrical indenter material, respectively.

4. The method according to claim 2, characterized in that: In step S2, the fitting coefficient function ξ and the fitting exponential function ψ are determined by the following two equations respectively: ψ=b0+b1n, Among them, a ij , i=0,1,2, j=0,1,2, b0, b1 are calibration coefficients.

5. The method according to claim 2, characterized in that: In step S3, the fitting coefficient function α and the fitting exponential function β are determined by the following two equations: β=(d0+d1ε0), Among them, c ij , i=0,1,j=0,1,2, d0 and d1 are calibration coefficients.

6. The method according to claim 2, characterized in that Plastic zone volume of the tested material in the Nth indentation cycle of the shallow indentation test Determined by the following formula:

7. The method according to claim 1, characterized in that In step S5, the prediction error of the pressing load is calculated by the following formula: In the formula, and are the predicted value and tested value of the indentation load corresponding to the kth displacement sampling point, respectively, and M is the total number of sampling points.