A sol-type liquid disperse dye, its preparation and application
By using the super dispersant obtained by polycondensation of styrene-maleic anhydride copolymer and polyetheramine in the liquid dispersed dye, combining specific dispersed dye raw materials and auxiliary agents, a sol-type liquid dye with high viscosity and small particle size was prepared, and the solution was solved Poor storage stability and dyeing residual liquid problems have achieved efficient dyeing and energy saving and emission reduction.
Patent Information
- Application Number
- CN202111627806.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-28
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-12-28
AI Technical Summary
The existing liquid dispersed dyes have problems such as poor storage stability, short storage time, and easy to get coarse when temperature changes. The dyed residual liquid has high color and COD values, making it difficult to meet the requirements of energy conservation and emission reduction.
Using the superdispersant obtained by polycondensation of styrene-maleic anhydride copolymer and polyetheramine as components, combined with specific dispersed dye raw materials and additives, sol-type liquid dispersed dyes with high viscosity and small particle size are prepared by grinding. Suitable for dyeing of hydrophobic fiber materials.
It has achieved sol-type liquid dispersed dye with high dye strength, good fluidity and good storage stability, reduced the color and COD value of the dye residue, met the requirements of energy conservation and emission reduction, and is suitable for automated and intelligent printing and dyeing applications.
Abstract
Description
(I) Technical field
[0001] The invention relates to a sol-type liquid disperse dye and a preparation method thereof, as well as dyeing application on hydrophobic fiber materials, especially polyester and blended fabrics thereof. (II) Background technology
[0002] Conventional powdered disperse dyes contain a large amount of dispersants, which protect the disperse dyes during dyeing and enable the disperse dyes to be dyed smoothly. However, the dispersants themselves cannot dye the fibers and need to be washed after dyeing. Therefore, their concentration in the dyeing residual liquid is very high, resulting in high residual liquid chromaticity and COD values. At the same time, powdered disperse dyes have problems such as high energy consumption, dust pollution and VOCs emissions during the production process. Liquid dyes have the advantages of simple production and operation, good application performance, and significant energy-saving and emission reduction effects, so these drawbacks can be effectively avoided. At present, there are fewer varieties of liquid disperse dyes on the market, and there are many problems, such as poor storage stability, easy coarsening when stored for too long or when the temperature changes greatly, etc., which seriously affect the promotion and use of liquid disperse dyes. For example, the liquid dye in ZL201711428524.0 only uses conventional dispersants and has a short storage time. For example, the liquid dyes in ZL201811093922.6 and ZL201410854280.2 have problems such as low slurry strength and short storage time. (III) Summary of the invention
[0003] The present invention aims to provide a sol-type liquid disperse dye which has high dye strength, good fluidity, good storage stability, low dye residual liquid chromaticity and COD value and meets the requirements of energy conservation and emission reduction.
[0004] To achieve the purpose of the present invention, the technical solutions adopted are as follows:
[0005] A sol-type liquid disperse dye comprises the following components: 30% to 50% by weight of one or more disperse dyes, 1 to 8% by weight of a hyperdispersant, 2 to 11% by weight of an auxiliary agent, and 45 to 60% by weight of water; the hyperdispersant is obtained by polycondensing a styrene-maleic anhydride copolymer with a polyetheramine.
[0006] In the present invention, the disperse dye primary dye is preferably a combination of one or more of CI Disperse Yellow 114, CI Disperse Yellow 211, CI Disperse Yellow 163, CI Disperse Orange 25, CI Disperse Orange 30, CI Disperse Orange 44, CI Disperse Orange 73, CI Disperse Orange 288, CI Disperse Red 153, CI Disperse Red 167, CI Disperse Red 145, CI Disperse Violet 93, CI Disperse Blue 291, CI Disperse Blue 291:1, CI Disperse Blue 79, and CI Disperse Blue 60.
[0007] In the present invention, the styrene-maleic anhydride copolymer preferably has a molar ratio of styrene to maleic anhydride of 1 to 8:1 and a degree of polymerization of 1 to 12. The styrene-maleic anhydride copolymer can be a commercially available product, preferably a polymer with SMA grades of SMA1000, SMA2000, SMA3000, SMA4000, SMA6000, or SMA8000.
[0008] In the present invention, the molecular weight of the polyetheramine is preferably 500 to 5000. The polyetheramine can be commercially available, preferably polyetheramine products of models M-1000, M-2005, M-2070, and M3085.
[0009] Preferably, the hyperdispersant is prepared by the following steps: adding styrene-maleic anhydride copolymer and polyetheramine in a molar ratio of 1:1 to 6, stirring and mixing evenly, heating to 150-200°C, performing a dehydration reaction for 3-6 hours under nitrogen protection, and after dehydration, cooling to obtain a hyperdispersant.
[0010] Preferably, the auxiliary agent is a dye dispersant or a combination of a dye dispersant and one or more of a wetting agent, a thickener, a defoaming agent, a preservative and bactericide, a pH adjuster, an emulsifier, and a hygroscopic agent.
[0011] As further preferred, the dye dispersant is at least one of methylnaphthalenesulfonic acid formaldehyde condensate, benzylnaphthalenesulfonic acid formaldehyde condensate, alkylnaphthalenesulfonate formaldehyde condensate, and lignin sulfonate.
[0012] As a further preference, the wetting agent is at least one of alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, sodium salt of dioctyl sulfonate succinate, and silanol nonionic surfactant.
[0013] As further preferred, the hygroscopic agent is at least one of glycerol, diethylene glycol monobutyl ether, polyethylene glycol, ethylene glycol, polyethylene glycol oleate, and urea.
[0014] As further preferred, the thickener is at least one of sodium polyacrylate, xanthan gum, carboxymethyl cellulose, sodium alginate, organic bentonite and carbomer.
[0015] As a further preference, the preservative and bactericidal agent is at least one of methyl-4-isothiazoline-3-one (MIT), 5-chloro-2-methyl-4-isothiazoline-3-one (CIT), 2-benzisothiazol-3-one (BIT), and sodium benzoate.
[0016] As further preferred, the defoaming agent is tributyl phosphate.
[0017] As further preferred, the pH adjuster is aqueous ammonia, liquid ammonia or soda ash.
[0018] As a further preference, the emulsifier is Quick T.
[0019] Preferably, the solid content of the sol-type liquid disperse dye is 40% to 55%.
[0020] Preferably, the viscosity of the sol-type liquid disperse dye is 100 to 400 cP, more preferably 150 to 250 cP.
[0021] In a second aspect, the present invention provides a method for preparing the sol-type liquid disperse dye, comprising the following steps:
[0022] According to the components and their contents, the original dye, superdispersant, auxiliary agent and water are weighed and added to the grinding device to grind and disperse the raw materials. The mixture is ground to a particle size of 0.1 to 2 μm and filtered with a 200 to 300 mesh filter to obtain a liquid disperse dye.
[0023] Preferably, the grinding is performed by sand milling, and the sand milling medium is zirconium beads with a particle size of 0.2 to 2 mm, zirconium oxide beads with a particle size of 0.2 to 2 mm, glass sand of 14 to 20 meshes, or quartz sand of 14 to 20 meshes. The sand milling time is 1 to 10 hours, and the sand milling speed is 1000 to 3000 rpm. The weight ratio of the zirconium beads or zirconium oxide beads to the dried raw materials (the weight of the dried raw materials, i.e., the total weight of the solid components in the raw materials) is 30 to 50:1, and the weight ratio of the glass sand or quartz sand to the dried raw materials is 5 to 15:1.
[0024] Preferably, the viscosity of the sol-type liquid disperse dye is 100-400 cP, more preferably 150-250 cP; when the viscosity of the sol-type liquid disperse dye is lower than 100 cP, a proper amount of thickener is added to the filtered liquid disperse dye to make the viscosity of the liquid disperse dye meet the requirements.
[0025] In a third aspect, the present invention provides the use of the sol-type liquid disperse dye in dyeing hydrophobic fiber materials.
[0026] The hydrophobic fiber material is preferably polyester or a blended fabric material thereof.
[0027] The dyeing can be a conventional dip dyeing method, a high temperature and high pressure dyeing method, a hot melt dyeing method and a pad dyeing method.
[0028] In the sol-type liquid disperse dye of the present invention, the original dye, the superdispersant and the auxiliary agent are all known compounds and can be purchased on the market, or can be prepared by existing methods.
[0029] The sol-type liquid disperse dye of the present invention has the following beneficial effects compared with conventional powder / liquid black:
[0030] (1) It has a certain viscosity, small particle size, high strength, excellent stability, and can be stored for more than 6 months at 50°C;
[0031] (2) The depth of the dyeing residual liquid is shallow, and the COD value brought in by the dye is reduced by 38-70%;
[0032] (3) It has good fluidity and is easy to measure. It is suitable for automated and intelligent printing and dyeing applications and has good application prospects. (IV) Specific implementation methods
[0033] The present invention is further described in detail below in conjunction with specific implementation modes.
[0034] Embodiment 1:
[0035] Styrene maleic anhydride copolymer (brand name SMA4000) and polyetheramine (M2070) are added in a 1:1 molar ratio, stirred and mixed evenly, heated to 190°C, and dehydrated for 3 hours under nitrogen protection. After dehydration, the temperature is lowered to obtain a super dispersant. At room temperature, 17.4g CI Disperse Blue 291:1 dye, 11.8g C.I. Disperse Violet 93 dye, 20.8g C.I. Disperse Orange 288 dye (40%), 4.5g super dispersant (3.6%), 6.5g dispersant MF, 1g Quick T, 0.5g glycerol (6.5%) are weighed, and 62.0g water (50%) is added to quickly beat the mixture evenly. The slurry was put into a sand mill and sanded with quartz sand (15 mesh) for 3 hours at a sand milling speed of 1500 rpm. The weight ratio of the quartz sand to the raw material (dry basis) was 10:1. The dispersed black liquid dye with a solid content of 50% was obtained by filtration.
[0036] Embodiment 2:
[0037] Styrene maleic anhydride copolymer (brand name SMA3000) and polyetheramine (M2005) are added in a molar ratio of 1:2, stirred and mixed evenly, heated to 150°C, and dehydrated for 6 hours under nitrogen protection. After dehydration, the temperature is lowered to obtain a super dispersant. At room temperature, 22g of C.I. Disperse Blue 291:1 dye, 17.5g of C.I. Disperse Violet 93 dye, 22.4g of C.I. Disperse Orange 288 dye (42.7%), 5.5g of super dispersant (3.8%), 5g of dispersant MF, 0.1g of tributyl phosphate defoamer (3.5%) are weighed, and 72.4g of water (50%) is added to quickly beat the mixture evenly. The slurry was put into a sand mill and sanded with glass sand (20 mesh) for 4 hours at a sand milling speed of 1000 rpm. The weight ratio of the glass sand to the raw material (dry basis) was 5:1. The dispersed black liquid dye with a solid content of 50% was obtained by filtration.
[0038] Embodiment 3:
[0039] Styrene maleic anhydride copolymer (brand name SMA6000) and polyetheramine (M3085) were added in a 1:1 molar ratio, stirred and mixed evenly, heated to 180°C, and dehydrated for 4 hours under nitrogen protection. After dehydration, the temperature was lowered to obtain a super dispersant. At room temperature, 70g C.I. Disperse Red 167 dye (50%), 1.5g super dispersant (1.1%), 4g dispersant NNO, 1g Peregal O-25, 0.5g polyethylene glycol 600 (3.9%) were weighed, and 63g water (45%) was added to quickly beat the mixture evenly. The slurry enters a sand mill and is sand-milled with glass sand (20 mesh) for 1 h at a sand mill speed of 2000 rpm. The weight ratio of the glass sand to the raw material (dry basis) is 10:1. The disperse red liquid dye with a solid content of 55% is obtained by filtration. 0.7 g (0.5%) of sodium polyacrylate thickener is added to the filtered slurry.
[0040] Embodiment 4:
[0041] SMA resin (styrene maleic anhydride copolymer) (brand name SMA2000) and polyetheramine (M1000) are added in a 1:3 molar ratio, stirred and mixed evenly, heated to 200°C, and dehydrated for 3 hours under nitrogen protection. After dehydration, the temperature is lowered to obtain a super dispersant. At room temperature, 53g C.I. Disperse Blue 79 dye (43.2%), 1.5g super dispersant (1.2%), 12.5g dispersant CNF, 0.5g glycerol (10.6%) are weighed, and 55.2g water (45%) is added to quickly beat the pulp evenly. The slurry enters the sand mill and is sanded with zirconium beads (0.8mm) for 2h, the sand milling speed is 2000rpm, the weight ratio of the zirconium beads to the raw materials (dry) is 30:1, and the disperse blue liquid dye with a solid content of 55% is obtained by filtration. 0.25g sodium polyacrylate thickener is added to the filtered slurry.
[0042] Embodiment 5:
[0043] SMA resin (styrene maleic anhydride copolymer) (brand name SMA2000) and polyetheramine (M2070) were added in a 1:1 molar ratio, stirred and mixed evenly, heated to 180°C, and dehydrated for 5 hours under nitrogen protection. After dehydration, the temperature was lowered to obtain a super dispersant. At room temperature, 45g C.I. Disperse Yellow 114 dye (30.2%), 11.2g super dispersant (7.5%), 2.6g dispersant MF, 0.8g emulsifier TX-15 (2.3%) were weighed, and 89.4g water (60%) was added to quickly beat the mixture evenly. The slurry enters a sand mill and is sand-milled with zirconium beads (1.0 mm) for 3 h at a sand mill speed of 1500 rpm. The weight ratio of the zirconium beads to the raw material (dry basis) is 50:1. The disperse yellow liquid dye having a solid content of 40% is obtained by filtration. 0.28 g of Carbomer 2020 thickener (0.2%) is added to the filtered slurry.
[0044] Embodiment 6:
[0045] SMA resin (styrene maleic anhydride copolymer) (brand name SMA8000) and polyetheramine (M2070) are added in a 1:2 molar ratio, stirred and mixed evenly, heated to 170°C, and dehydrated for 6 hours under nitrogen protection. After dehydration, the temperature is lowered to obtain a super dispersant. At room temperature, 60g CI disperse blue 56 dye (46.8%), 5g super dispersant (3.9%), 3g conventional lignin (2.3%) are weighed, and 60.3g water (47%) are added to quickly beat the pulp evenly. The slurry enters a sand mill and is sanded with quartz sand (15 mesh) for 3 hours. The sand milling speed is 1500rpm. The weight ratio of the quartz sand to the raw material (dry) is 10:1. Filter to obtain a disperse blue liquid dye with a solid content of 53%.
[0046] Embodiment 7:
[0047] SMA resin (styrene maleic anhydride copolymer) (brand name SMA4000) and polyetheramine (M2070) were added in a molar ratio of 1:4, stirred and mixed evenly, heated to 150°C, and dehydrated for 5 hours under nitrogen protection. After dehydration, the temperature was lowered to obtain a super dispersant. At room temperature, 50g C.I. Disperse Red 153 dye (33.6%), 2g super dispersant (1.3%), 10g dispersant NNO, 0.5g diethylene glycol monobutyl ether (auxiliary agent: 7.1%) were weighed, and 86.3g water (58%) was added to quickly beat the mixture evenly. The slurry enters a sand mill and is sand-milled with quartz sand (15 mesh) for 3 h. The sand-milling speed is 1500 rpm. The weight ratio of the quartz sand to the raw material (dry basis) is 15:1. The disperse red liquid dye with a solid content of 42% is obtained by filtration. 0.45 g (0.3%) of Carbomer 2020 thickener is added to the filtered slurry.
[0048] Embodiment 8:
[0049] SMA resin (styrene maleic anhydride copolymer) (brand name SMA2000) and polyetheramine (M2070) are added in a molar ratio of 1:3, stirred and mixed evenly, heated to 160°C, and dehydrated for 6 hours under nitrogen protection. After dehydration, the temperature is lowered to obtain a super dispersant. At room temperature, 40g C.I. Disperse Orange 30 dye (40.4%), 4g super dispersant (4.0%), 2g dispersant CNF, 2g conventional lignin, 0.5g fast penetrant T (4.5%) are weighed, and 50.5g water (51%) is added to quickly beat the pulp evenly. The slurry enters a sand mill and is sanded with quartz sand (15 mesh) for 1.5 hours. The sand milling speed is 1500rpm. The weight ratio of the quartz sand to the raw material (dry) is 12:1. Filter to obtain a disperse orange liquid dye with a solid content of 49%.
[0050] Embodiment 9:
[0051] SMA resin (styrene maleic anhydride copolymer) (brand name SMA3000) and polyetheramine (M2070) are added in a 1:4 molar ratio, stirred and mixed evenly, heated to 160°C, and dehydrated for 5 hours under nitrogen protection. After dehydration, the temperature is lowered to obtain a super dispersant. At room temperature, 55g C.I. Disperse Orange 44 dye (41.9%), 5.5g super dispersant (4.2%), 7.0g dispersant MF, 0.5g fast penetrant T, 0.2g urea (auxiliary agent: 5.9%) are weighed, and 63.0g water (48%) is added to quickly beat the pulp evenly. The slurry enters a sand mill and is sanded with quartz sand (15 mesh) for 1.5 hours. The sand milling speed is 1600rpm. The weight ratio of the quartz sand to the raw material (dry) is 12:1. Filter to obtain a disperse orange liquid dye with a solid content of 52%.
[0052] Embodiment 10:
[0053] SMA resin (styrene maleic anhydride copolymer) (brand name SMA3000) and polyetheramine (M2005) are added in a 1:3 molar ratio, stirred and mixed evenly, heated to 190°C, and dehydrated for 4 hours under nitrogen protection. After dehydration, the temperature is lowered to obtain a super dispersant. At room temperature, 46g C.I. Disperse Violet 93 dye (42.9%), 2.8g super dispersant (2.6%), 7.5g dispersant NNO, 0.5g emulsifier TX-15 (auxiliary agent: 7.5%) are weighed, and 50.4g water (47%) is added to quickly beat the pulp evenly. The slurry enters a sand mill and is sanded with quartz sand (15 mesh) for 1 hour. The sand milling speed is 1500rpm. The weight ratio of the quartz sand to the raw material (dry) is 10:1. Filter to obtain a disperse orange liquid dye with a solid content of 53%.
[0054] Comparative Example 1: The powdered disperse black dye prepared in Example 35 of ZL99104177.1 is used as Comparative Example 1.
[0055] Comparative Example 2: The liquid disperse dye prepared in Example 1 in ZL201711428524.0 is used as Comparative Example 2.
[0056] Comparative Example 3: The liquid disperse dye prepared in Example 1 in ZL201811093922.6 is used as Comparative Example 3.
[0057] Comparative Example 4: The liquid disperse dye prepared in Example 1 in ZL201410854280.2 is used as Comparative Example 4.
[0058] The viscosity of the dyes provided in Examples 1 to 10 and Comparative Examples 1 to 4 was tested using a DVS+ viscometer and placed in a 50° C. oven to observe the stratification and precipitation of the dyes. The results are shown in Table 1:
[0059] Table 1 Basic performance test of liquid disperse dyes
[0060] Example Dry strength / % Slurry strength / % Viscosity / cP Storage days / days Example 1 194.2 97.1 206.8 180-200 Example 2 207.2 103.6 228.3 180-200 Example 3 295.6 162.6 348.2 150-180 Example 4 182.2 100.2 206.2 180-200 Example 5 228.2 91.3 266.5 180-200 Example 6 291.5 154.5 180.6 150-180 Example 7 276.2 116.0 216.0 150-180 Example 8 261.2 128.0 186.1 180-200 Example 9 235.9 122.7 221.7 180-200 Example 10 208.3 110.4 239.5 180-200 Comparative Example 1 85.5 powder powder dust Comparative Example 2 190.8 95.4 <50 60-80 Comparative Example 3 184.6 72.0 50-100 60-90 Comparative Example 4 265.1 66.3 <50 60-90
[0061] Dyeing Example
[0062] The dyes provided in Examples 1-10 and Comparative Examples 1-4 were dyed with a dyeing depth of 6% omf, and the specific dyeing formula and process were as follows: the pH of the dye bath was adjusted to 4-5 with acetic acid and sodium acetate solution, and then the temperature was raised to 130°C within 40 minutes, and the temperature was lowered to 80°C after keeping the temperature for 40 minutes. The fabric sample (polyester fabric) was washed, reduced cleaned, acid washed and neutralized, washed, dried and shaped to obtain the finished dyed fabric. The absorption area of the dyeing residual liquid within a wavelength of 380-700nm was tested by UV-2600, an ultraviolet visible spectrophotometer, to characterize the residual liquid depth. The COD value of the dyeing residual liquid was determined by using GB / T 11914-1989 "Determination of Chemical Oxygen Demand of Water Quality - Dichromate Method". The dye-in COD refers to the COD value of the dyeing residual liquid minus the COD value of the blank dye bath without dye. The test data are shown in Table 2.
[0063] Table 2: Residual liquid depth and COD value test
[0064] Example Residual liquid depth Dye brought into COD / ppm Example 1 180.2 432 Example 2 156.3 386.0 Example 3 138.6 374.3 Example 4 189.1 459 Example 5 196.8 439.5 Example 6 155.5 368.5 Example 7 192.1 441.6 Example 8 172.6 401.2 Example 9 191.8 451 Example 10 198.5 462 Comparative Example 1 386.6 1580 Comparative Example 2 224.1 608 Comparative Example 3 201.2 516.2 Comparative Example 4 220.5 615
[0065] It can be seen that the liquid dye of the present invention has high strength, good storage stability, low chroma of the dyeing residual liquid, and greatly reduced COD value in the dyeing residual liquid. The liquid dye of the present invention has good fluidity, is easy to measure, is suitable for automated and intelligent printing and dyeing applications, and has good application prospects.
Claims
1. A sol-type liquid disperse dye, comprising the following components: 30% to 50wt% of one or more disperse dyes, 1 to 8wt% of a hyperdispersant, 2 to 11wt% of an auxiliary agent, and 45 to 60wt% of water; the hyperdispersant is obtained by polycondensing a styrene-maleic anhydride copolymer and a polyetheramine, wherein the molar ratio of styrene to maleic anhydride in the styrene-maleic anhydride copolymer is 1 to 8:1, and the degree of polymerization is 1 to 12; the molecular weight of the polyetheramine is 500 to 5000.
2. The sol-type liquid disperse dye according to claim 1, characterized in that: The super dispersant is prepared by the following steps: adding styrene-maleic anhydride copolymer and polyetheramine in a molar ratio of 1:1-6, stirring and mixing evenly, heating to 150-200° C., performing a dehydration reaction for 3-6 hours under nitrogen protection, and cooling after the dehydration is completed to obtain the super dispersant.
3. The sol-type liquid disperse dye according to claim 1 or 2, characterized in that: The styrene-maleic anhydride copolymer is a styrene-maleic anhydride copolymer with the brand of SMA1000, SMA2000, SMA3000, SMA4000, SMA6000 or SMA8000.
4. The sol-type liquid disperse dye according to claim 1 or 2, characterized in that: The polyetheramine is a polyetheramine product with model number M-1000, M-2005, M-2070 or M3085.
5. The sol-type liquid disperse dye according to claim 1 or 2, characterized in that: The disperse dye primary dye is a combination of one or more of CI Disperse Yellow 114, CI Disperse Yellow 211, CI Disperse Yellow 163, CI Disperse Orange 25, CI Disperse Orange 30, CI Disperse Orange 44, CI Disperse Orange 73, CI Disperse Orange 288, CI Disperse Red 153, CI Disperse Red 167, CI Disperse Red 145, CI Disperse Violet 93, CI Disperse Blue 291, CI Disperse Blue 291:1, CI Disperse Blue 79, and CI Disperse Blue 60.
6. The sol-type liquid disperse dye according to claim 1 or 2, characterized in that: The auxiliary agent is a dye dispersant or a combination of a dye dispersant and one or more of a wetting agent, a thickener, a defoaming agent, a preservative and bactericide, a pH adjuster, an emulsifier, and a hygroscopic agent.
7. The sol-type liquid disperse dye according to claim 1 or 2, characterized in that: The solid content of the sol-type liquid disperse dye is 40% to 55%.
8. The sol-type liquid disperse dye according to claim 1 or 2, characterized in that: The viscosity of the sol-type liquid disperse dye is 100-400 cP.
9. The sol-type liquid disperse dye according to claim 8, characterized in that: The viscosity of the sol-type liquid disperse dye is 150-250 cP.
10. A method for preparing a sol-type liquid disperse dye as claimed in claim 1 or 2, comprising the following steps: According to the components and their contents, the original dye, superdispersant, auxiliary agent and water are weighed and added into a grinding device to grind and disperse the raw materials. The mixture is ground to a particle size of 0.1 to 2 μm and filtered with a 200 to 300 mesh filter to obtain a liquid disperse dye.
11. Use of the sol-type liquid disperse dye according to claim 1 in dyeing hydrophobic fiber materials.
Citation Information
Patent Citations
Blue liquid disperse dye and preparation method and application thereof
CN104497631A
Disperse azo dye mixtures
CN1230575A
Novel modified polyether type dispersing agent and preparation method thereof
CN106220799A
Energy-saving emission-reduction type high-intensity liquid dispersion dye as well as preparation method and application thereof
CN108219532A
Waterless-dyeing dispersed liquid dye and preparation method and application thereof
CN109135334A