2D / 3D heterojunction-based blue light perovskite film, preparation method and light-emitting diode device

By forming a 2D/3D heterojunction structure in a blue light perovskite light emitting diode, the 3D perovskite layer is treated with cationic organic halide solution, which improves the luminous performance of deep blue, positive blue and sky blue light, and solves the existing blue light pertitanium The lack of brightness and color purity of mineral light-emitting diodes has achieved high-efficiency, ultra-narrow spectrum blue LEDs, meeting the wide color gamut requirements for future displays.

CN114566603BActive Publication Date: 2024-11-12FUJIAN NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210096221.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-26
Publication Date
2024-11-12
Estimated Expiration
2042-01-26

AI Technical Summary

Technical Problem

Existing blue light perovskite light emitting diodes are far less efficient and brighter than green and red in dark blue light, and it is difficult to meet the requirements of high brightness and high color purity, especially in display applications.

Method used

Using a blue light perovskite film based on 2D/3D heterojunction, the 2D perovskite surface cover layer is formed by spin-coating cationic organic halides on the surface of the 3D blue light perovskite layer to form a 2D/3D heterojunction structure to improve the film's Energy transfer efficiency and luminous performance.

Benefits of technology

Significantly improve the photoluminescence quantum yield and electroluminescence brightness of deep blue, positive blue and sky blue light, maximum external quantum efficiency improvement, and the color gamut area reaches 98% of the International Telecommunications Union BT.2020 standard, meeting ultra-high-definition display need.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114566603B_ABST
    Figure CN114566603B_ABST
Patent Text Reader

Abstract

The invention discloses a blue light perovskite film based on a 2D / 3D heterojunction, comprising a main 3D blue light perovskite layer located at a lower layer and a 2D perovskite surface covering layer formed by spin-coating an organic ion halide solution on the surface of the 3D blue light perovskite layer; a preparation method of a blue light perovskite film based on a 2D / 3D heterojunction, comprising the following steps: spin-coating the prepared perovskite precursor solution onto a substrate to prepare a stable 3D blue light perovskite film; taking the 3D blue light perovskite film as the main body, spin-coating the surface of the 3D blue light perovskite film again with an organic ion halide solution containing at least one cation to form a 2D perovskite surface covering layer, and finally forming a 2D / 3D heterojunction blue light perovskite film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention specifically relates to a 2D / 3D heterojunction-based blue light perovskite film, a preparation method and an application thereof, and belongs to the technical field of perovskite light-emitting diode manufacturing. Background Art

[0002] Metal halide perovskite is a new type of semiconductor material with the characteristics of tunable spectrum, high color saturation, low cost and easy preparation. It is one of the most promising luminescent materials in the field of future lighting and display. In recent years, the research and development of perovskite light-emitting diodes has been very rapid, and the performance of devices has been continuously improved. Among them, the external quantum efficiency of green, red and near-infrared perovskite light-emitting diodes has exceeded 20%, gradually narrowing the gap with organic light-emitting diodes. However, as one of the three primary colors, the efficiency, brightness and luminescence purity of blue light-emitting diodes are still far inferior to green and red, especially deep blue and blue, and still face the problem of low efficiency. To apply blue light-emitting diodes in large quantities, it is necessary to improve their brightness and luminescence purity. For display applications, brightness and luminescence purity are important indicators of display technology. High brightness can meet the requirements of outdoor display, and high color purity can better restore colors and meet the future display needs for wide color gamut display.

[0003] At present, among the many existing blue light perovskite light-emitting diodes, there are high-brightness or high-efficiency devices. The patent with application number CN202010234139.8 discloses "a blue light perovskite light-emitting diode and a preparation method thereof", which mainly regulates the phase distribution of blue light perovskite through the joint action of large-group organic halides and alkali metal halides, reduces the formation of two-dimensional perovskite phases with low exciton binding energy, and improves the formation of other low-dimensional perovskite phases with high exciton binding energy; the patent with application number CN202110788114.7 discloses "a blue light perovskite light-emitting diode and a preparation method thereof", which specifically discloses that when preparing a blue light perovskite light-emitting diode, a perovskite film is prepared by adding a perovskite precursor solution to a thiocyanate additive, so as to adjust the film morphology of the light-emitting layer by the thiocyanate additive; after the perovskite film is prepared, the perovskite film is passivated to improve the performance of the perovskite film, thereby improving the luminescence performance of the blue light perovskite light-emitting diode. At this stage, the performance of blue perovskite light-emitting diodes can barely meet the needs of display. The downside is that it is difficult to achieve high brightness and high efficiency requirements in deep blue and positive blue light. Summary of the invention

[0004] To solve the problems in the prior art, the present invention provides a 2D / 3D heterojunction blue light perovskite film based on mixed halogen, a preparation method and an application thereof, which realizes high color purity blue light LEDs of deep blue, pure blue and sky blue, and can be applied to future high-definition displays.

[0005] The technical solution of the present invention is as follows:

[0006] The present invention provides a blue light perovskite film based on a 2D / 3D heterojunction, comprising a main 3D blue light perovskite layer located at a lower layer and a 2D perovskite surface covering layer formed by spin coating an organic ion halide solution on the surface of the 3D blue light perovskite layer.

[0007] The present invention also provides a method for preparing a 2D / 3D heterojunction blue light perovskite film, comprising the following steps:

[0008] (1) Spin coating the prepared perovskite precursor solution onto a substrate to prepare a stable 3D blue light perovskite film;

[0009] (2) Taking the 3D blue light perovskite film as the main body, an organic ion halide solution containing at least one cation is spin-coated on its surface again to form a 2D perovskite surface covering layer, and finally a 2D / 3D heterojunction blue light perovskite film is formed.

[0010] Furthermore, the preparation method of the 3D blue light perovskite film in the step (1) is: adding CsBr, FABr, PbBr2 and PbCl2 into a container and dissolving them in dimethyl sulfoxide, placing them on a magnetic stirring table and stirring them for 12 to 14 hours to obtain a transparent and clear perovskite precursor solution; dropping the perovskite precursor solution onto a substrate and rotating it at a speed of 3500 to 4500 r / min for 30 to 40 seconds to obtain a 3D blue light perovskite film, and placing the film on a heating table to dry the remaining solvent.

[0011] Furthermore, the organic ion halide solution in step (2) is prepared by using isopropanol as solvent to prepare an organic ion halide (AC1 x Br y ) solution; an organic ion halide solution is dropped onto the 3D blue light perovskite film and rotated at a speed of 3500 to 4500 r / min for 30 to 40 s to obtain a 2D / 3D heterojunction blue light perovskite film.

[0012] Furthermore, the molar ratio of CsBr, FABr, PbBr2 and PbCl2 is 1.2:0.3:(0.13-0.44):(0.56-0.87); CsBr, FABr, PbBr2 and PbCl2 are dissolved in dimethyl sulfoxide, and the molar concentration of the formed mixed solution is 0.11M.

[0013] Furthermore, the organic ion halide solution is PEABr and PEACl dissolved in an isopropanol solvent in a molar ratio of (0.52-0.68):(0.32-0.48).

[0014] Furthermore, the concentration of the organic ion halide solution is 2 mg / mL.

[0015] The present invention provides a light-emitting diode device, in which a prepared 2D / 3D heterojunction-based blue light perovskite film is placed as a light-emitting layer; the light-emitting diode device comprises an electron transport layer, a light-emitting layer and a hole transport layer which are sequentially arranged from top to bottom.

[0016] Furthermore, a buffer layer formed by spin coating of PVP is provided between the hole transport layer and the light emitting layer.

[0017] The present invention also provides a method for preparing a light emitting diode device, which specifically comprises the following steps:

[0018] S1. Spin-coating Poly-TPD (CB) and PVK (CB) on an ITO substrate, and annealing at 110-120° C. for 20-25 min to obtain a hole transport layer;

[0019] S2, spin-coating a PVP solution with ethanol as a solvent on the hole transport layer, and annealing at 70-80° C. for 10-20 min to form a buffer layer;

[0020] S3, spin coating the 2D / 3D heterojunction blue light perovskite film prepared according to the above method on the buffer layer to form a light-emitting layer;

[0021] S4, transfer the ITO substrate formed by spin coating into the hole transport layer, buffer layer and light-emitting layer into the vacuum evaporation system, and pump the vacuum evaporation box to 2×10 -4 Pa negative pressure, 50-60nm TPBi, 1-2nm LiF and 100-110nm Al were sequentially evaporated to finally prepare a blue light perovskite light-emitting diode device.

[0022] Compared with the prior art, the beneficial effects of the present invention are:

[0023] 1. The 2D / 3D heterojunction blue light perovskite film provided by the present invention includes a main 3D blue light perovskite layer located in the lower layer and a 2D perovskite surface covering layer formed by spin-coating a cationic organic halide on the surface of the 3D blue light perovskite layer, wherein the 2D perovskite surface covering layer capped on the surface of the 3D blue light perovskite can passivate the surface defects of the single-layer 3D perovskite film, thereby increasing the non-compound radiation probability of the 2D / 3D heterojunction blue light perovskite film, realizing the energy funnel effect of energy transfer from the 2D phase to the 3D phase, improving the energy transmission efficiency, and significantly improving the photoluminescence and electroluminescence performance of the film.

[0024] 2. The photoluminescence quantum yields of the 2D / 3D heterojunction blue perovskite film prepared by the present invention in deep blue (465nm), pure blue (475nm) and sky blue (485nm) are increased from 2.1%, 4.1% and 6.9% to 8.4%, 20.1% and 36.4%, respectively, and the maximum electroluminescent devices reach 928cd / m 2 、6727cd / m 2 and 9424cd / m 2 , the maximum external quantum efficiency reached 2.11%, 6.29% and 8.57%.

[0025] 3. In the present invention, the prepared 2D / 3D heterojunction blue light perovskite film is used as the light-emitting layer of the light-emitting diode device. The three-color blue light obtained by the prepared light-emitting diode has high brightness and ultra-narrow half-width (<15nm). Its color gamut area reaches 98% of the BT.2020 standard issued by the International Telecommunication Union for ultra-high-definition television. It has ultra-high color purity, meets the future display demand for wide color gamut display, and shows great potential in the display industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 (a) is an electron microscope scanning image of a 2D / 3D heterojunction blue light perovskite film in the present invention, and (b) is an electron microscope scanning image of a 3D blue light perovskite film in a comparative example that has not been treated with an organic ion halide;

[0027] Figure 2 (a) is a schematic diagram of XRD of the 2D / 3D heterojunction blue perovskite film of the present invention, (b) is a GIWAXS spectrum of the 3D blue perovskite film without organic ion halide treatment in the comparative example, (c) is a GIWAXS spectrum of the 2D / 3D heterojunction blue perovskite film of the present invention;

[0028] Figure 3 The temperature curve of the 2D / 3D heterojunction blue perovskite film in the present invention after being cooled down and gradually heated up by liquid nitrogen treatment;

[0029] Figure 4 (a) is a schematic diagram of the structure of the light-emitting diode device of the present invention, (b) is an illustration of the device and the ultra-narrow electroluminescence spectrum of the light-emitting diode device of deep blue, pure blue and sky blue light at a voltage of 4.6 V;

[0030] Figure 5 This is the (dashed line) color gamut in CIE of the 2D / 3D heterojunction blue perovskite film used as the light-emitting layer of the light-emitting diode in the present invention. DETAILED DESCRIPTION

[0031] In order to better understand the present invention, the present invention is further described below by way of examples. The examples are only used to explain the present invention and do not constitute any limitation to the present invention.

[0032] In the following examples, unless otherwise specified, the technical means used are conventional means well known to those skilled in the art, and the raw materials used are all commercially available products; phenylethylamine bromide (PEABr), phenylethylamine chloride (PEACl), poly[(4,4′-(N-(4-sec-butylphenyl)diphenylamine)](poly-TPD), poly(9-vinylcarbazole) (PVK), 1,3,5-tri(1-phenyl-1H-benzimidazol-2-yl)benzene (TPBi) were purchased from Xi'an Biolight Optoelectronics Technology Co., Ltd.; anhydrous dimethyl sulfoxide (DMSO), anhydrous dimethylformamide (DMF) and polyvinylpyrrolidone (PVP) were purchased from Inokai Technology Co., Ltd.

[0033] Example 1

[0034] Based on a 2D / 3D heterojunction blue light perovskite film, it includes a main 3D blue light perovskite layer located at the bottom layer and a 2D perovskite surface covering layer formed by spin-coating a cationic organic halide on the surface of the 3D blue light perovskite layer.

[0035] Example 2

[0036] Based on a 2D / 3D heterojunction blue light perovskite film, it includes a main 3D blue light perovskite layer located at the bottom layer and a 2D perovskite surface covering layer formed by spin-coating a cationic organic halide on the surface of the 3D blue light perovskite layer;

[0037] The above-mentioned method for preparing a 2D / 3D heterojunction blue light perovskite film specifically comprises the following steps:

[0038] (1) Spin coating the prepared perovskite precursor solution onto a substrate to prepare a stable 3D blue light perovskite film; adding CsBr, FABr, PbBr2 and PbCl2 into a glass sample bottle and dissolving them in dimethyl sulfoxide, placing them on a magnetic stirring table and stirring them for 12 to 14 hours to obtain a transparent and clear perovskite precursor solution; dropping the perovskite precursor solution onto a substrate and rotating it at a speed of 3500 to 4500 r / min for 30 to 40 seconds to obtain a 3D blue light perovskite film, placing the film on a heating table, heating it at 80°C for 10 minutes, and drying the remaining solvent to obtain a 3D blue light perovskite film;

[0039] (2) With the 3D blue light perovskite film as the main body, 75 μL of an organic ion halide solution containing at least one cation is spin-coated on the surface of the 3D blue light perovskite film at a speed of 3500-4500 r / min for 30-40 s to form a 2D perovskite surface covering layer, and finally a 2D / 3D heterojunction blue light perovskite film is formed; in this embodiment, the organic ion halide solution containing at least one cation is an organic ion halide (AC1) with the same chlorine and bromine ratio prepared using isopropanol as a solvent. x Br y ) solution, the concentration of the organic ion halide solution is 2 mg / mL;

[0040] When preparing 2D / 3D heterojunction deep blue perovskite film, the molar ratio of CsBr, FABr, PbBr2 and PbCl2 in the prepared perovskite precursor solution is 1.2:0.3:0.16:0.84, CsBr, FABr, PbBr2 and PbCl2 are dissolved in 1 mL of DMSO solvent, and the molar concentration of the formed mixed solution is 0.11 M; the molar ratio of PEABr and PEACl in the prepared organic ion halide is 0.52:0.48;

[0041] When preparing a 2D / 3D heterojunction positive blue perovskite film, the molar ratio of CsBr, FABr, PbBr2 and PbCl2 in the prepared perovskite precursor solution is 1.2:0.3:0.13:0.87, CsBr, FABr, PbBr2 and PbCl2 are dissolved in 1 mL of DMSO solvent, and the molar concentration of the formed mixed solution is 0.11 M; the molar ratio of PEABr and PEACl in the prepared organic ion halide is 0.6:0.4;

[0042] When preparing 2D / 3D heterojunction sky blue perovskite film, the molar ratio of CsBr, FABr, PbBr2 and PbCl2 in the prepared perovskite precursor solution is 1.2:0.3:0.44:0.56, CsBr, FABr, PbBr2 and PbCl2 are dissolved in 1 mL of DMSO solvent, and the molar concentration of the formed mixed solution is 0.11 M; the molar ratio of PEABr and PEACl in the prepared organic ion halide is 0.68:0.32.

[0043] Example 3

[0044] like Figure 4As shown in (a), a light-emitting diode device, wherein the 2D / 3D heterojunction-based deep blue light perovskite film, the 2D / 3D heterojunction-based positive blue light perovskite film and the 2D / 3D heterojunction-based sky blue light perovskite film prepared in Example 2 are placed in the light-emitting diode device as a light-emitting layer; the photoelectric light-emitting diode device comprises an electron transport layer, a light-emitting layer and a hole transport layer arranged in sequence from top to bottom; a buffer layer formed by PVP spin coating is also arranged between the hole transport layer and the light-emitting layer. In this embodiment, the buffer layer formed by PVP spin coating does not have the function of transport and light emission, so the buffer layer formed by PVP spin coating is attributed to the hole transport layer located below, above the light-emitting layer; under this structure, as shown in FIG. Figure 4 As shown in (b), the device illustrations and ultra-narrow electroluminescence spectra of the deep blue, bright blue and sky blue light-emitting diode devices at a voltage of 4.6 V meet the needs of ultra-wide display in future displays.

[0045] Example 3

[0046] The method for preparing a light emitting diode device specifically comprises the following steps:

[0047] S1. Spin-coat a 6 mg / mL Poly-TPD solution in which the solvent is chlorobenzene and a PVK solution in which the solvent is chlorobenzene on an ITO substrate at 4000 r / min for 40 seconds, and anneal at 110 to 120° C. for 20 to 25 minutes to obtain a hole transport layer;

[0048] S2, spin-coating a PVP solution with ethanol as a solvent on the hole transport layer, and annealing at 70-80° C. for 10-20 min to form a buffer layer;

[0049] S3, spin coating the 2D / 3D heterojunction-based deep blue perovskite film, the 2D / 3D heterojunction-based positive blue perovskite film, and the 2D / 3D heterojunction-based sky blue perovskite film prepared according to Example 2 on the buffer layer to finally form a light-emitting layer;

[0050] S4, transfer the ITO substrate formed by spin coating into the hole transport layer, buffer layer and light-emitting layer into the vacuum evaporation system, and pump the vacuum evaporation box to 2×10 -4 Pa negative pressure, 50-60nm TPBi, 1-2nm LiF and 100-110nm Al are sequentially evaporated. In this embodiment, TPBi is evaporated to form an electron transport layer, LiF and Al constitute electrodes located above the electron transport layer, and finally a blue light perovskite light-emitting diode device is prepared.

[0051] Comparative Example 1

[0052] The difference from Example 1 is that the 3D heterojunction blue light perovskite film is a single layer and is not post-treated with a cationic organic halide solution during the specific preparation process.

[0053] Performance Testing

[0054] See also Figure 1 From the electron microscope scanning image of the 3D blue light perovskite film without organic ion halide treatment in the comparative example, it can be seen that the 3D blue light perovskite film forms submicron platelet structure crystals in terms of mechanism, and there are large vacancies; however, after the 3D blue light perovskite film is treated with an organic ion halide solution containing cations to form a 2D / 3D heterojunction blue light perovskite film, more small clusters appear, indicating that the perovskite morphology has changed after the organic ion halide solution treatment. Figure 2 , it can be found that the XRD diffraction peak of the blue light perovskite film based on the 2D / 3D heterojunction has the emission peak of the 2D perovskite due to the post-treatment of the organic cation halide solution; from the GIWAXS spectrum, it can be seen that the 2D perovskite only grows on the surface of the 3D perovskite and grows horizontally;

[0055] The 2D / 3D heterojunction blue perovskite film was cooled from room temperature to 80K by liquid nitrogen, and then gradually raised to room temperature at intervals of 30K. Its temperature curve was monitored, as shown in Figure 2. Figure 3 As shown, since the 2D perovskite covers the surface of the 3D perovskite to form a 2D / 3D heterojunction blue perovskite film, it exhibits low-dimensional peak emission at 404nm and 432nm. At the same time, through the fitting calculation of the exciton binding energy, it is obtained that the 2D / 3D structure has a relatively high exciton binding energy and a higher probability of radiative recombination.

[0056] Figure 5 The (dashed line) color gamut in CIE based on 2D / 3D heterojunction blue perovskite film as the light-emitting layer of the light-emitting diode. The CIE figure is the BT.2020 standard color gamut released by the International Telecommunication Union for ultra-high-definition television. By comparing the color gamut area, the color gamut area of ​​the light-emitting diode prepared by the present invention reaches 98% of the BT.2020 standard, with very high color display, which is sufficient to meet the needs of wide color gamut display.

[0057] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing a 2D / 3D heterojunction blue light perovskite film, characterized in that: The following steps are involved: (1) Spin coating the prepared perovskite precursor solution onto a substrate to prepare a stable 3D blue light perovskite film; adding CsBr, FABr, PbBr2 and PbCl2 into a container and dissolving them in dimethyl sulfoxide, placing the container on a magnetic stirring table and stirring for 12 to 14 hours to obtain a transparent and clear perovskite precursor solution; Drop the perovskite precursor solution onto the substrate and rotate it at a speed of 3500-4500 r / min for 30-40 seconds to obtain a 3D blue light perovskite film, and place the film on a heating table to dry the remaining solvent; (2) Taking the 3D blue light perovskite film as the main body, an organic ion halide solution containing at least one cation is spin-coated on its surface again to form a 2D perovskite surface covering layer, and finally a 2D / 3D heterojunction blue light perovskite film is formed.

2. The method for preparing a 2D / 3D heterojunction blue light perovskite film according to claim 1, characterized in that: The molar ratio of CsBr, FABr, PbBr2 and PbCl2 is 1.2:0.3:(0.13-0.44):(0.56-0.87); CsBr, FABr, PbBr2 and PbCl2 are dissolved in dimethyl sulfoxide, and the molar concentration of the formed mixed solution is 0.11M.

3. The method for preparing a 2D / 3D heterojunction blue light perovskite film according to claim 1, characterized in that: The organic ion halide solution in step (2) is prepared by using isopropanol as solvent to prepare an organic ion halide (ACl) with the same chlorine and bromine ratio. x Br y ) solution; an organic ion halide solution is dropped onto the 3D blue light perovskite film and rotated at a speed of 3500 to 4500 r / min for 30 to 40 s to obtain a 2D / 3D heterojunction blue light perovskite film.

4. The method for preparing a 2D / 3D heterojunction blue light perovskite film according to claim 3, characterized in that: The organic ion halide solution is prepared by dissolving PEABr and PEACl in an isopropanol solvent in a molar ratio of (0.52-0.68):(0.32-0.48).

5. The method for preparing a 2D / 3D heterojunction blue light perovskite film according to claim 4, characterized in that: The concentration of the organic ion halide solution is 2 mg / mL.

6. The 2D / 3D heterojunction blue light perovskite film prepared by the preparation method according to claim 1, characterized in that: It includes a main 3D blue light perovskite layer located at the bottom layer and a 2D perovskite surface covering layer formed by spin coating an organic ion halide solution on the surface of the 3D blue light perovskite layer.

7. A light emitting diode device, characterized in that: The light-emitting diode device places the 2D / 3D heterojunction-based blue light perovskite film as described in claim 6 in the light-emitting diode device as a light-emitting layer; the light-emitting diode device includes an electron transport layer, a light-emitting layer and a hole transport layer arranged in sequence from top to bottom.

8. The light emitting diode device according to claim 7, characterized in that: A buffer layer formed by spin coating of PVP is also arranged between the hole transport layer and the light emitting layer.

9. The method for preparing a light emitting diode device according to claim 7, characterized in that: The specific steps include: S1. Spin-coating Poly-TPD (CB) and PVK (CB) on an ITO substrate, and annealing at 110-120° C. for 20-25 min to obtain a hole transport layer; S2, spin-coating a PVP solution with ethanol as a solvent on the hole transport layer, and annealing at 70-80° C. for 10-20 min to form a buffer layer; S3, spin coating the 2D / 3D heterojunction blue light perovskite film prepared according to the above method on the buffer layer to form a light-emitting layer; S4, transfer the ITO substrate formed by spin coating into the hole transport layer, buffer layer and light-emitting layer into the vacuum evaporation system, and pump the vacuum evaporation box to 2×10 -4 Pa negative pressure, 50-60nm TPBi, 1-2nm LiF and 100-110nm Al were sequentially evaporated to finally prepare a blue light perovskite light-emitting diode device.