A forging method to overcome cracks in 4130 forgings

Through the forging method of slow heating and cooling and multiple treatments, the internal crack problems of 4130 forging during the forging process were solved. By removing bubbles and controlling temperature stress, the internal quality of the forging is significantly improved.

CN114603073BActive Publication Date: 2024-11-01NANJING DEV ADVANCED MFG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011420316.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-08
Publication Date
2024-11-01
Estimated Expiration
2040-12-08

AI Technical Summary

Technical Problem

In the prior art, 4130 forgings are prone to defect waves and cracks distributed through annularly distributed during forging, resulting in internal crack problems and is related to cooling speed. It is necessary to improve the forging process to overcome this problem.

Method used

The forging method is adopted for preheating and slow heating and cooling, including pre-working, pretreatment of the blank, heating to 1200 degrees and rotating and removing bubbles, performing three upsetting and rounding, austenitization and deep-cold quenching, and back-tempering. Control temperature and time to avoid cracks caused by temperature and tissue stress.

Benefits of technology

By strengthening the pretreatment of the blank and slowing up and down, the internal gaps and bubbles can be effectively removed, temperature stress can be reduced, cracks can be avoided, and the internal quality of the forgings can be improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114603073B_ABST
    Figure CN114603073B_ABST
Patent Text Reader

Abstract

The present invention discloses a forging method for overcoming cracks in 4130 forgings, including preparatory work, pretreatment of billets, reprocessing of billets, forging processing and forming, normalizing, austenitization and deep cold quenching, primary tempering, secondary tempering and other forging steps to obtain forgings. The present invention strengthens the pretreatment link of the billet, effectively removes the gaps and bubbles inside the billet; in the heating and cooling links, a slow heating and cooling process is adopted to avoid cracks caused by temperature stress. In addition, an inert gas is introduced to enhance the surface pressure to avoid surface cracks caused by changes in tissue stress.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a forging method for overcoming cracks of a 4130 forging, and belongs to the technical field of steel forging. Background Art

[0002] The smelted 4130 steel Ф500 continuous casting round ingot was forged into 74 forgings of different specifications by a 5t forging hammer. After normalizing and quenching and tempering, the forgings were inspected by ultrasonic flaw detection, and it was found that 11 of the forgings had a penetrating annular defect wave inside. The company's engineers immediately carried out ultrasonic flaw detection, dissected and sampled, analyzed the chemical composition, mechanical properties, and mechanical properties at the fracture, and conducted a series of tests such as low-power organization inspection, microstructure inspection, forging metallographic inspection, and non-metallic inclusion inspection. After research and analysis, it was found that the cracks in the sample were related to the internal defects of the forging blank and the cooling speed. Therefore, to overcome the cracks in the 4130 forgings, it is necessary to change the traditional forging process of 4130 forgings, and the forging method for overcoming the cracks in the 4130 forgings of this application is needed. Summary of the invention

[0003] In order to solve the above technical problems, the present invention discloses a forging method for overcoming cracks in 4130 forgings, and its specific technical solution is as follows:

[0004] Step 1, preparation: select 4130 billet, select a heating furnace of corresponding specifications and place it on the rotating mechanism, and preheat the heating furnace;

[0005] Step 2: Pretreatment of the blank: Place the blank in a heating furnace and heat it to 1200 degrees.

[0006] Step 3: Use a robotic arm to take out the blank, perform upsetting, stretching and rounding three times in the cross direction; then cool from the terminal temperature to room temperature;

[0007] Step 5, punching blind holes in the forgings, preliminary processing, and casting the forgings;

[0008] Step 6, normalizing: put the forging into a heating furnace at a temperature of 500±10℃, heat the furnace temperature to 900±10℃ within five hours, keep the temperature for more than 5.5h, then take out the forging and air cool it to room temperature;

[0009] Step 7, austenitization and deep cold quenching: put the forging into a heating furnace at a temperature of 400±10℃ and keep it warm for half an hour; heat the furnace temperature to 900±10℃ within three hours, keep it warm for at least three hours, and quench it with water;

[0010] Step 8, primary tempering: Place the forging in a heating furnace at a temperature of 250±10℃, heat the furnace temperature to 800±10℃ within three hours, keep the temperature for at least four hours, then take out the forging and air cool it to room temperature;

[0011] Step nine, secondary tempering: Place the forging into a heating furnace, start the heating furnace and heat the furnace temperature to 500±10℃ within two hours, keep it warm for at least two hours, then take out the forging and air cool it to room temperature.

[0012] Furthermore, the composition of the 4130 billet includes 0.11% to 0.15% carbon, 0.30% to 0.60% manganese, 0 to 0.5% silicon, 0 to 0.015% phosphorus, 0 to 0.010% sulfur, 2.00% to 2.50% chromium, 0 to 0.50% nickel, 0.87% to 1.13% molybdenum, 0 to 0.010% vanadium, 0 to 0.35% copper, 0 ~0.055% aluminum, 0~0.001% niobium, 0~0.0005% boron, 0~0010% titanium, 0~00.02% tin, 0~0.003% antimony, 0~0.002% arsenic, 0~0.010% lead, 0~0.010% bismuth, 0~0.005% calcium, 0~0.012% sodium, 0~2% hydrogen, 0~25% oxygen, and the rest is Fe.

[0013] Furthermore, in step 2, heating to 1200 degrees includes step a of first heating to 500±10°C and keeping warm for at least 300 minutes, then heating with the furnace to 950±10°C and keeping warm for at least 600 minutes, and finally heating with the furnace to 1500±10°C and keeping warm for 300 minutes, with a heating rate of 50±10 degrees / hour.

[0014] Furthermore, in the step 2, the rotation speed of the heating furnace is maintained at 30 rpm.

[0015] Furthermore, in step three, heating the billet to 1200 degrees includes the steps of first heating it to 400±10°C and keeping it warm for at least 300 minutes, then heating it to 800±10°C with the furnace and keeping it warm for at least 600 minutes, and finally heating it to 1200±10°C with the furnace and keeping it warm for 300 minutes, with a heating rate of 50±10 degrees / hour; during quenching, it is first water-cooled to a surface temperature not higher than 400 degrees, and the water temperature at the beginning of quenching does not exceed 40 degrees.

[0016] Furthermore, the upsetting aspect ratios of the three upsettings in step three are all 1.5, and the upsetting aspect ratio in step four is 2.

[0017] Beneficial effects: The present invention strengthens the pretreatment process of the blank, effectively removes the gaps and bubbles inside the blank; in the heating and cooling process, a slow heating and cooling process is adopted to avoid cracks caused by temperature stress. In addition, inert gas is introduced to enhance the surface pressure and avoid surface cracks caused by changes in tissue stress. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 is a cross-sectional view of a forging of the prior art;

[0019] Figure 2 The figure is a cross-sectional view of a forging obtained by using the method of the present application. DETAILED DESCRIPTION

[0020] The present invention is further explained below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art all fall within the scope defined by the claims attached to this application.

[0021] Embodiment 1, a forging method for overcoming cracks in 4130 forgings, comprising:

[0022] Step 1, preparation: select 4130 billet, the billet composition includes 0.11% to 0.15% carbon, 0.30% to 0.60% manganese, 0 to 0.5% silicon, 0 to 0.015% phosphorus, 0 to 0.010% sulfur, 2.00% to 2.50% chromium, 0 to 0.50% nickel, 0.87% to 1.13% molybdenum, 0 to 0.010% vanadium, 0 to 0.35% Copper, 0-0.055% aluminum, 0-0.001% niobium, 0-0.0005% boron, 0-0010% titanium, 0-00.02% tin, 0-0.003% antimony, 0-0.002% arsenic, 0-0.010% lead, 0-0.010% bismuth, 0-0.005% calcium, 0-0.012% sodium, 0-2% hydrogen, 0-25% oxygen, and the rest is Fe. Select a heating furnace of corresponding specifications and place it on the rotating mechanism, and preheat the heating furnace to 300 degrees.

[0023] Step 2: Pretreatment of the blank: placing the blank in a heating furnace and heating it to 1200 degrees to make the blank molten;

[0024] The process of heating to 1200 is as follows: first heat to 500±10℃ and keep warm for at least 300 minutes, then heat up with the furnace to 950±10℃ and keep warm for at least 600 minutes, and finally heat up with the furnace to 1200±10℃ and keep warm for 300 minutes, and the heating rate is 50±10 degrees / hour. At this time, the billet is in a molten state. Start the rotating mechanism to rotate the heating furnace for 30 minutes, and the heating furnace rotation speed is maintained at 30 rpm. Under the action of centrifugal force, the internal bubbles and gaps are squeezed out to reduce the generation of internal cracks; the heating furnace stops rotating, and the billet cools to room temperature. The cooling time is maintained for 10 hours, and the cooling rate is 100 degrees / hour.

[0025] Step three, billet reprocessing: heating the billet to 1200 degrees, including the steps of first heating to 400±10℃ and keeping warm for at least 300 minutes, then heating with the furnace to 800±10℃ and keeping warm for at least 600 minutes, and finally heating with the furnace to 1200±10℃ and keeping warm for 300 minutes, with a heating rate of 50±10 degrees / hour; then quenching, first water cooling to a surface temperature not higher than 400 degrees, and the water temperature at the beginning of quenching does not exceed 38 degrees.

[0026] The blank is placed in a heating furnace for the third heating to 1200 degrees. The heating process is the same as the second heating. The blank is taken out by a robotic arm and subjected to three times of upsetting, drawing and rounding in a cross direction. Then it is cooled from the final stage temperature to room temperature.

[0027] Step five, punching blind holes in the forgings, preliminary processing, and casting the forgings.

[0028] Step 6, normalizing: put the forging into a heating furnace at a temperature of 500±10℃, heat the furnace temperature to 900±10℃ within five hours, keep the temperature for more than 5.5h, then take out the forging and air cool it to room temperature;

[0029] Step 7, austenitization and deep cold quenching: put the forging into a heating furnace at a temperature of 400±10℃ and keep it warm for half an hour; heat the furnace temperature to 900±10℃ within three hours, keep it warm for at least three hours, and quench it with water;

[0030] Step 8, primary tempering: Place the forging in a heating furnace at a temperature of 250±10℃, heat the furnace temperature to 800±10℃ within three hours, keep the temperature for at least four hours, then take out the forging and air cool it to room temperature;

[0031] Step nine, secondary tempering: Place the forging into a heating furnace, start the heating furnace and heat the furnace temperature to 500±10℃ within two hours, keep it warm for at least two hours, then take out the forging and air cool it to room temperature.

[0032] The upsetting aspect ratios of the three upsettings in step three are all 1.5, and the upsetting aspect ratio in step four is 2.

[0033] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A forging method for overcoming cracks in 4130 forgings, characterized in that: include Step 1, preparation: select 4130 billet, select a heating furnace of corresponding specifications and place it on the rotating mechanism, and preheat the heating furnace; The composition of the 4130 blank includes 0.11% to 0.15% carbon, 0.30% to 0.60% manganese, 0 to 0.5% silicon, 0 to 0.015% phosphorus, 0 to 0.010% sulfur, 2.00% to 2.50% chromium, 0 to 0.50% nickel, 0.87% to 1.13% molybdenum, 0 to 0.010% vanadium, 0 to 0.35% copper, 0 to 0.055% aluminum, 0 to 0.001% niobium, 0 to 0.0005% boron, 0 to 0010% titanium, 0 to 00.02% tin, 0 to 0.003% antimony, 0 to 0.002% arsenic, 0 to 0.010% lead, 0 to 0.010% bismuth, 0 to 0.005% calcium, 0 to 0.012% sodium, 0 to 2% hydrogen, 0 to 25% oxygen, and the rest is Fe; Step 2: Pretreatment of the blank: Place the blank in a heating furnace and heat it to 1200 degrees; In the step 2, heating to 1200 degrees includes the steps of first heating to 500±10°C and keeping warm for at least 300 minutes, then heating to 950±10°C with the furnace and keeping warm for at least 600 minutes, and finally heating to 1200±10°C with the furnace and keeping warm for 300 minutes, with a heating rate of 50±10 degrees / hour; At this time, the blank is in a molten state, and the rotating mechanism is started to rotate the heating furnace for 30 minutes. The heating furnace rotation speed is maintained at 30 rpm. Under the action of centrifugal force, the internal bubbles and gaps are squeezed out to reduce the generation of internal cracks. The heating furnace stops rotating, and the blank is cooled to room temperature. The cooling time is maintained for 10 hours, and the cooling rate is 100 degrees / hour. Step 3, billet reprocessing: heating the billet to 1200 degrees, including the steps of first heating to 400±10°C and keeping it warm for at least 300 minutes, then heating it to 800±10°C with the furnace and keeping it warm for at least 600 minutes, and finally heating it to 1200±10°C with the furnace and keeping it warm for 300 minutes, with a heating rate of 50±10 degrees / hour; then quenching, first water cooling to a surface temperature not higher than 400 degrees during quenching, and the water temperature at the beginning of quenching does not exceed 38 degrees; The blank is placed in a heating furnace for the third heating to 1200 degrees. The heating process is the same as the second heating. The blank is taken out by a robotic arm and subjected to three upsetting, drawing and rounding processes in the cross direction. Then the blank is cooled from the final forging temperature to room temperature. The upsetting aspect ratios of the three upsettings in step 3 are all 1.5, and the upsetting aspect ratio in step 4 is 2; Step 4: Punch blind holes in the forgings for preliminary processing to shape the forgings; Step 5, normalizing: put the forging into a heating furnace at a temperature of 500±10℃, heat the furnace temperature to 900±10℃ within five hours, keep the temperature for more than 5.5h, then take out the forging and air cool it to room temperature; Step 6, austenitization and deep cold quenching: put the forging into a heating furnace at a temperature of 400±10℃ and keep it warm for half an hour; heat the furnace temperature to 900±10℃ within three hours, keep it warm for at least three hours, and quench it with water; Step 7, primary tempering: Place the forging in a heating furnace at a temperature of 250±10℃, heat the furnace temperature to 800±10℃ within three hours, keep the temperature for at least four hours, then take out the forging and air cool it to room temperature; Step 8, secondary tempering: Place the forging into a heating furnace, start the heating furnace and heat the furnace temperature to 500±10℃ within two hours, keep it warm for at least two hours, then take out the forging and air cool it to room temperature.

2. The forging method for overcoming cracks in 4130 forgings according to claim 1, characterized in that: In the step 2, the rotation speed of the heating furnace is maintained at 30 rpm.