Phase difference plate with optical compensation function
By using a specific design horizontally oriented liquid crystal cured film and a vertically oriented liquid crystal cured film laminate in the elliptical polarizer, the problem of insufficient optical compensation in the flexible display is solved, and optical performance compensation and reflection reduction in the folded state is achieved.
Patent Information
- Application Number
- CN202210265555.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2017-08-21
- Filing Date
- 2018-08-08
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2038-08-08
AI Technical Summary
The existing elliptical polarizer with optical compensation function cannot fully compensate for optical performance in the folded state of the flexible display, resulting in external light reflection and wrinkle problems.
Using a laminated body including a horizontally oriented liquid crystal cured film and a vertically oriented liquid crystal cured film, a phase difference plate that satisfies a specific relationship is designed by adjusting the difference between layers, film thickness and refractive index to achieve optical compensation function in the folded state. .
It effectively reduces the reflection hue changes during bending, avoids wrinkles, and ensures sufficient compensation of optical performance.
Smart Images

Figure BDA0003551660110000111 
Figure BDA0003551660110000431 
Figure BDA0003551660110000432
Abstract
Description
[0001] This application is a divisional application of the Chinese invention patent application with international application number PCT / JP2018 / 029757, application date August 8, 2018, national application number 201880053692.2, and invention name “Phase difference plate with optical compensation function”. Technical Field
[0002] The invention relates to a phase difference plate with optical compensation function. Background Art
[0003] An elliptically polarizing plate is an optical component obtained by laminating a polarizing plate and a phase difference plate. For example, in an organic EL image display device that displays an image in a planar state, an elliptically polarizing plate is used to prevent light reflection from occurring at the electrodes that constitute the device. Among the elliptically polarizing plates, a so-called λ / 4 plate is used as a phase difference plate.
[0004] As the phase difference plate used in the elliptically polarizing plate, a phase difference plate showing reverse wavelength dispersion is preferred from the aspect of exerting the same phase difference performance in a wide wavelength range of visible light. As a phase difference plate showing reverse wavelength dispersion, a phase difference plate formed only by the following horizontally oriented liquid crystal cured film is known, wherein the horizontally oriented liquid crystal cured film is obtained by polymerizing and curing a polymerizable liquid crystal compound showing reverse wavelength dispersion in a state oriented in a horizontal direction.
[0005] In addition, an elliptically polarizing plate with an optical compensation function is also required, which has a compensation function by exhibiting the same optical performance when observed from an oblique direction as when observed from a front direction. As a phase difference plate with an optical compensation function used in such an elliptically polarizing plate with an optical compensation function, Patent Document 1 (Japanese Patent Publication No. 2015-163935) proposes a phase difference plate having a horizontally oriented liquid crystal cured film with reverse wavelength dispersion and a vertically oriented liquid crystal cured film obtained by polymerizing and curing a polymerizable liquid crystal compound in a vertically oriented state. As for the vertically oriented liquid crystal cured film specifically disclosed in the document, it does not show reverse wavelength dispersion but shows normal positive wavelength dispersion, and fully exerts a compensation function in a normal image display device that displays images in a planar state.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2015-163935 Summary of the invention
[0009] Problems to be solved by the invention
[0010] However, with regard to the above-mentioned conventional elliptical polarizing plate with optical compensation function, when applied to a foldable so-called flexible display, when folded in a state where an image is displayed, in essence, the elevation angle of the folded portion (the angle between the film plane and the direction in which the observer observes the image) is very small, and therefore the optical performance cannot be fully compensated. It has been found that it will reflect external light in a colored state, produce wrinkles when folded, and other undesirable conditions.
[0011] Therefore, the purpose of the present invention is to develop a phase difference plate with optical compensation function used in an elliptically polarizing plate with optical compensation function, wherein the elliptically polarizing plate with optical compensation function is suitable for a flexible display and does not produce wrinkles or other undesirable conditions when folded in a state where an image is displayed, fully compensates for the optical performance, and does not reflect external light in a colored state.
[0012] Means for solving problems
[0013] The inventors of the present application have conducted intensive studies to solve the above-mentioned problems and have completed the present invention as a result.
[0014] That is, the present invention includes the following aspects.
[0015] [1] A phase difference plate with an optical compensation function, which is a laminate comprising a horizontally aligned liquid crystal cured film and a vertically aligned liquid crystal cured film,
[0016] The horizontally aligned liquid crystal cured film is formed by curing a composition containing a polymerizable liquid crystal compound in a state where the composition is aligned in a horizontal direction relative to the film surface.
[0017] The vertically aligned liquid crystal cured film is formed by curing a composition containing a polymerizable liquid crystal compound in a state where the composition is aligned in a vertical direction relative to the film surface.
[0018] The phase difference plate with optical compensation function satisfies the following relationships (1) to (4).
[0019] The interlayer distance between the horizontally aligned liquid crystal cured film and the vertically aligned liquid crystal cured film is 5 μm or less. ···(1)
[0020] A horizontal alignment film or a vertical alignment film is included between the layers of the horizontal alignment liquid crystal cured film and the vertical alignment liquid crystal cured film. ···(2)
[0021] ReA(450) / ReA(550)<1.00···(3)
[0022] [In the formula, ReA(λ) represents the in-plane phase difference value of the horizontally aligned liquid crystal cured film at a wavelength of λ nm.
[0023] The definition of the in-plane phase difference value ReA(λ) is as follows.
[0024] ReA(λ)=(nxA(λ)-nyA(λ))×dA
[0025] Here, nxA(λ) represents the principal refractive index within the film plane of the horizontally aligned liquid crystal cured film with respect to light of wavelength λ (nm),
[0026] nyA(λ) represents the refractive index for light of wavelength λ (nm) in a direction orthogonal to nxA(λ) in the same plane.
[0027] dA represents the thickness of the horizontally aligned liquid crystal cured film. 〕
[0028] RthC(450) / RthC(550)<1.00···(4)
[0029] [In the formula, RthC (λ) represents the phase difference value in the thickness direction at a wavelength of λ nm of the vertically aligned liquid crystal cured film. The phase difference value RthC (λ) is defined as follows.
[0030] RthC(λ)=((nxC(λ)+nyC(λ)) / 2-nzC(λ))×dC
[0031] Here, nxC(λ) represents the principal refractive index within the film plane of the vertically aligned liquid crystal cured film with respect to light of wavelength λ (nm),
[0032] nyC(λ) represents the refractive index for light of wavelength λ (nm) in a direction orthogonal to nxC(λ) in the same plane.
[0033] nzC(λ) represents the refractive index of the vertically aligned liquid crystal cured film in the thickness direction with respect to light of wavelength λ (nm),
[0034] dC represents the thickness of the vertically aligned liquid crystal cured film. 〕
[0035] It should be noted that, in the formula (4), when nxC=nyC, nxC can be set to the refractive index in any direction within the film surface.
[0036] [2] The phase difference plate with an optical compensation function as described in [1] above, which is a laminated body including a horizontally aligned liquid crystal cured film and a vertically aligned liquid crystal cured film, and satisfies the following relationship (5).
[0037] |R0(550)-R40(550)|<10nm···(5)
[0038] Here, R0(λ) represents the in-plane phase difference value of the phase difference plate with an optical compensation function including the horizontally aligned liquid crystal cured film and the vertically aligned liquid crystal cured film with respect to light of wavelength λ (nm).
[0039] In addition, R40(λ) represents the apparent phase difference value when the phase difference plate with optical compensation function including a horizontally oriented liquid crystal solid film and a vertically oriented liquid crystal solid film is rotated 40° around the direction (fast axis direction) orthogonal to the main refractive index direction in the film surface in the same plane, and is the phase difference value relative to the light of wavelength λ (nm).
[0040] [3] The phase difference plate with an optical compensation function as described in [1] or [2] above, which is a laminate comprising a horizontally aligned liquid crystal cured film and a vertically aligned liquid crystal cured film and satisfies the following relationship (6).
[0041] |R0(450)-R40(450)|<10nm···(6)
[0042] [Herein, R0(λ) represents the in-plane phase difference value of the phase difference plate with an optical compensation function including the horizontally aligned liquid crystal cured film and the vertically aligned liquid crystal cured film with respect to light of wavelength λ (nm).
[0043] In addition, R40 (λ) represents the apparent phase difference value when rotating 40° around the direction (fast axis direction) orthogonal to the main refractive index direction in the film surface in the phase difference plate with optical compensation function including the horizontally aligned liquid crystal cured film and the vertically aligned liquid crystal cured film, and is the phase difference value relative to light of wavelength λ (nm).
[0044] [4] The phase difference plate with an optical compensation function as described in any one of [1] to [3] above, which is a laminate comprising a horizontally aligned liquid crystal cured film and a vertically aligned liquid crystal cured film and satisfies the following relationship (7).
[0045] |{R0(450)-R40(450)}-{R0(550)-R40(550)}|<3nm···(7)
[0046] [Herein, R0(λ) represents the in-plane phase difference value of the phase difference plate with an optical compensation function including the horizontally aligned liquid crystal cured film and the vertically aligned liquid crystal cured film with respect to light of wavelength λ (nm).
[0047] In addition, R40 (λ) represents the apparent phase difference value when rotating 40° around the direction (fast axis direction) orthogonal to the main refractive index direction in the film surface in the phase difference plate with optical compensation function including the horizontally aligned liquid crystal cured film and the vertically aligned liquid crystal cured film, and is the phase difference value relative to light of wavelength λ (nm).
[0048] [5] The phase difference plate with optical compensation function as described in any one of [1] to [4] above, wherein the average refractive index difference of the horizontally aligned liquid crystal solid film, the vertically aligned liquid crystal solid film, and the horizontally aligned film or the vertically aligned film at a wavelength of 550 nm is 0.20 or less.
[0049] [6] The phase difference plate with an optical compensation function according to any one of [1] to [5] above, wherein a horizontal alignment film is included between the horizontal alignment liquid crystal cured film and the vertical alignment liquid crystal cured film, and the horizontal alignment film is a photo alignment film.
[0050] [7] The phase difference plate with an optical compensation function according to any one of [1] to [6] above, wherein a horizontal alignment film is included between the horizontal alignment liquid crystal cured film and the vertical alignment liquid crystal cured film, and the horizontal alignment film contains a cinnamoyl group.
[0051] [8] The phase difference plate with an optical compensation function as described in any one of [1] to [7] above, wherein a vertical alignment film is included between the horizontal alignment liquid crystal cured film and the vertical alignment liquid crystal cured film, and the film thickness of the vertical alignment film is greater than or equal to 30 nm and less than or equal to 1 μm.
[0052] [9] A phase difference plate with an optical compensation function as described in any one of [1] to [8] above, wherein a vertically oriented film is included between the horizontally oriented liquid crystal solid film and the vertically oriented liquid crystal solid film, and the vertically oriented film is a film formed by a compound containing Si, C and O elements in its constituent elements.
[0053]
[10] An elliptically polarizing plate, which is a laminate of the phase difference plate with an optical compensation function according to any one of [1] to [9] above and a polarizing plate.
[0054]
[11] An organic EL display device comprising the elliptically polarizing plate described in
[10] above.
[0055] Effects of the Invention
[0056] When the elliptically polarizing plate with optical compensation function using the phase difference plate with optical compensation function of the present invention is applied to a flexible display and then bent, the change in reflected hue is reduced. DETAILED DESCRIPTION
[0057] 〔Horizontally oriented liquid crystal cured film〕
[0058] A horizontally aligned liquid crystal cured film is a film having refractive index anisotropy in the film plane and is formed from a polymer containing a polymerizable liquid crystal compound. From the viewpoint of being able to arbitrarily design the thinning and wavelength dispersion characteristics of the horizontally aligned liquid crystal cured film, it is preferable to form the horizontally aligned liquid crystal cured film by the following method: applying a polymerizable liquid crystal composition onto a horizontally aligned film and polymerizing the composition containing the polymerizable liquid crystal compound in an oriented state by heating and / or light irradiation.
[0059] The three-dimensional refractive index ellipsoid formed by the horizontally aligned liquid crystal cured film may have biaxiality, but preferably has uniaxiality. For the horizontally aligned liquid crystal cured film, it may be a horizontally aligned liquid crystal cured film formed from a polymer of a polymerizable liquid crystal composition containing the following polymerizable liquid crystal compound, the polymerizable liquid crystal compound being in a state of being oriented in the horizontal direction with respect to the plane of the horizontally aligned liquid crystal cured film; it may also be a mixed-aligned liquid crystal cured film or an inclined-aligned liquid crystal cured film. For the refractive indices nx, ny, and nz in the three directions of the refractive index ellipsoid formed by the orientation of the polymerizable liquid crystal, they may have the relationship of nx > ny ≈ nz (referred to as a positive A plate) or nx < ny ≈ nz (referred to as a negative A plate). nx represents the principal refractive index in the direction parallel to the plane of the horizontally aligned liquid crystal cured film in the refractive index ellipsoid formed by the horizontally aligned liquid crystal cured film. ny represents the refractive index in the direction parallel to the plane of the horizontally aligned liquid crystal cured film and orthogonal to the direction of nx in the refractive index ellipsoid formed by the horizontally aligned liquid crystal cured film. nz represents the refractive index in the direction perpendicular to the plane of the horizontally aligned liquid crystal cured film in the refractive index ellipsoid formed by the horizontally aligned liquid crystal cured film.
[0060] The horizontally aligned liquid crystal cured film can use either rod-shaped polymerizable liquid crystal or disc-shaped polymerizable liquid crystal, but rod-shaped polymerizable liquid crystal is preferred. When the rod-shaped polymerizable liquid crystal forms a horizontally aligned liquid crystal cured film, the horizontally aligned liquid crystal cured film becomes a positive A plate.
[0061] When the horizontally aligned liquid crystal cured film has optical anisotropy in the plane of the film, the in-plane phase difference Re1(550) with respect to light of wavelength 550 nm preferably satisfies the optical characteristics shown by the following formula (21). In addition, for the horizontally aligned liquid crystal cured film, the in-plane phase difference Re1(450) with respect to light of wavelength 450 nm, the in-plane phase difference Re1(550) with respect to light of wavelength 550 nm, and the in-plane phase difference Re1(650) with respect to light of wavelength 650 nm also preferably satisfy the optical characteristics shown by formula (22) and formula (23). The horizontally aligned liquid crystal cured film more preferably satisfies the optical characteristics shown by the following formula (21), the following formula (22), and the following formula (23).
[0062] 120nm≤ReA(550)≤170nm···(21)
[0063] [In the formula, ReA(550) represents the in-plane phase difference value (in-plane retardation) of the horizontally aligned liquid crystal cured film relative to light of a wavelength of 550 nm.]
[0064] ReA(450) / ReA(550)≤1.0···(22)
[0065] 1.00≤ReA(650) / ReA(550)···(23)
[0066] [Wherein, ReA(450) represents the in-plane phase difference value of the horizontally aligned liquid crystal cured film relative to light of a wavelength of 450 nm, ReA(550) represents the in-plane phase difference value of the horizontally aligned liquid crystal cured film relative to light of a wavelength of 550 nm, and ReA(650) represents the in-plane phase difference value of the horizontally aligned liquid crystal cured film relative to light of a wavelength of 650 nm.]
[0067] When the in-plane phase difference value ReA(550) of the horizontally oriented liquid crystal curing film exceeds the range of formula (21), the following problem will occur: the hue of the front of the display using an elliptically polarizing plate with an optical compensation function (which includes a phase difference plate with an optical compensation function) becomes red or blue. As a further preferred range of the in-plane phase difference value, 130nm≤ReA(550)≤160nm. When "ReA(450) / ReA(550)" of the horizontally oriented liquid crystal curing film exceeds 1.0, the ellipticity of the elliptically polarizing plate having the horizontally oriented liquid crystal curing film on the short wavelength side deteriorates. If the ellipticity of the elliptically polarizing plate on the short wavelength side deteriorates and is less than 1.0, there is a tendency that the function as an elliptically polarizing plate on the short wavelength side is impaired when observed from the front. The "ReA(450) / ReA(550)" is preferably 0.75 to 0.92, more preferably 0.77 to 0.87, and further preferably 0.79 to 0.85.
[0068] The in-plane phase difference of the horizontally oriented liquid crystal curing film can be adjusted by the thickness of the horizontally oriented liquid crystal curing film. Since the in-plane phase difference is determined by the following formula (24), in order to obtain the desired in-plane phase difference (ReA (λ): the in-plane phase difference of the horizontally oriented liquid crystal curing film at wavelength λ (nm)), the three-dimensional refractive index and the film thickness dA can be adjusted. It should be noted that the three-dimensional refractive index depends on the molecular structure and orientation state of the polymerizable liquid crystal compound described later.
[0069] ReA(λ)=(nxA(λ)-nyA(λ))×dA (24)
[0070] [In the formula, in the refractive index ellipsoid formed by the horizontally aligned liquid crystal curing film, there is a relationship of nxA(λ)>nyA(λ)≈nzA(λ), and nxA(λ) represents the principal refractive index of light with a wavelength of λ(nm) in a direction parallel to the plane of the horizontally aligned liquid crystal curing film. nyA(λ) represents the refractive index of light with a wavelength of λ(nm) in a direction parallel to the plane of the horizontally aligned liquid crystal curing film and orthogonal to the direction of nxA(λ) in the refractive index ellipsoid formed by the horizontally aligned liquid crystal curing film. dA represents the thickness of the horizontally aligned liquid crystal curing film.]
[0071] The horizontally oriented liquid crystal curing film is preferably a polymer of a composition of a polymerizable liquid crystal compound in an oriented state as described above. The polymerizable liquid crystal compound forming the horizontally oriented liquid crystal curing film is a liquid crystal compound having a polymerizable functional group, especially a photopolymerizable functional group. The so-called photopolymerizable functional group refers to a group that can participate in the polymerization reaction using active free radicals, acids, etc. generated by a photopolymerization initiator. As photopolymerizable functional groups, vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, acryloyloxy, methacryloyloxy, oxirane, oxetane, etc. can be cited. Among them, acryloyloxy, methacryloyloxy, vinyloxy, oxirane and oxetane are preferred, and acryloyloxy is more preferred. The liquid crystal can be a thermotropic liquid crystal or a lyotropic liquid crystal. As a phase sequence structure, it can be a nematic liquid crystal or a smectic liquid crystal.
[0072] In the present invention, from the viewpoint of exhibiting reverse wavelength dispersion and satisfying the relationship between the above formulas (21) and (22) or the relationship between (31) and (32) described later, the polymerizable liquid crystal compound is preferably a compound represented by the following formula (I):
[0073]
[0074] In formula (I), Ar represents a divalent aromatic group which may have a substituent. The aromatic group referred to herein refers to the following group, which is a group having a planar cyclic structure, and the number of π electrons possessed by the ring structure is counted as [4n+2] according to the Huckel rule. Here, n represents an integer. In the case where a ring structure is formed by including heteroatoms such as -N= and -S-, the case where the non-covalent bond electron pairs on these heteroatoms satisfy the Huckel rule and thus have aromaticity is also included. The divalent aromatic group preferably includes at least one of a nitrogen atom, an oxygen atom, and a sulfur atom.
[0075] G 1 and G 2 Each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group.
[0076] Here, the hydrogen atoms contained in the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted by a halogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group or a nitro group, and the carbon atoms constituting the divalent aromatic group or the divalent alicyclic hydrocarbon group may be replaced by an oxygen atom, a sulfur atom or a nitrogen atom.
[0077] L 1 , L 2 , B 1 and B 2 Each is independently a single bond or a divalent linking group.
[0078] k and l each independently represent an integer from 0 to 3, and satisfy the relationship 1≤k+1. Here, when 2≤k+1, B 1 and B 2 , G 1 and G 2 Each may be the same as or different from each other.
[0079] E 1 and E 2 Each independently represents an alkanediyl group having 1 to 17 carbon atoms, wherein the hydrogen atom contained in the alkanediyl group may be substituted with a halogen atom, and the -CH2- contained in the alkanediyl group may be replaced with -O-, -S-, or -Si-. 1 and P 2 Each independently represents a polymerizable group or a hydrogen atom, and at least one of them is a polymerizable group.
[0080] G 1 and G 2 Each of them is independently preferably 1,4-phenylenediyl which may be substituted with at least one substituent selected from the group consisting of halogen atoms and alkyl groups having 1 to 4 carbon atoms, 1,4-cyclohexanediyl which may be substituted with at least one substituent selected from the group consisting of halogen atoms and alkyl groups having 1 to 4 carbon atoms, more preferably 1,4-phenylene substituted with methyl, unsubstituted 1,4-phenylene, or unsubstituted 1,4-trans-cyclohexanediyl, and particularly preferably unsubstituted 1,4-phenylene or unsubstituted 1,4-trans-cyclohexanediyl. In addition, it is preferred that there are a plurality of G 1 and G 2 At least one of them is a divalent alicyclic hydrocarbon group, and more preferably, L 1 or L 2 Bonded G 1 and G 2 At least one of them is a divalent alicyclic hydrocarbon group.
[0081] L1 and L 2 Each of them is independently preferably a single bond, an alkylene group having 1 to 4 carbon atoms, -O-, -S-, -R a1 OR a2 -、-R a3 COOR a4 -、-R a5 OCOR a6 -、R a7 OC=OOR a8 -、-N=N-、-CR c =CR d -, or -C≡C-. Here, R a1 ~R a8 Each independently represents a single bond or an alkylene group having 1 to 4 carbon atoms, and R c and R d represents an alkyl group having 1 to 4 carbon atoms or a hydrogen atom. 1 and L 2 Each independently is more preferably a single bond, -OR a2-1 -、-CH2-、-CH2CH2-、-COOR a4-1 -, or -OCOR a6-1 -. Here, R a2-1 , R a4-1 , R a6-1 Each independently represents a single bond, -CH2-, or -CH2CH2-. 1 and L 2 Each independently is further preferably a single bond, -O-, -CH2CH2-, -COO-, -COOCH2CH2-, or -OCO-.
[0082] B 1 and B 2 Each of them is independently preferably a single bond, an alkylene group having 1 to 4 carbon atoms, -O-, -S-, -R a9 OR a10 -、-R a11 COOR a12 -、-R a13 OCOR a14 -, or R a15 OC=OOR a16 -. Here, R a9 ~R a16 Each independently represents a single bond or an alkylene group having 1 to 4 carbon atoms. 1 and B 2 Each independently is more preferably a single bond, -OR a10-1 -、-CH2-、-CH2CH2-、-COOR a12 -1-, or -OCOR a14-1 -. Here, R a10-1 , R a12-1 , R a14-1 Each independently represents any one of a single bond, -CH2-, and -CH2CH2-. 1 and B 2 Each independently is further preferably a single bond, -O-, -CH2CH2-, -COO-, -COOCH2CH2-, -OCO-, or -OCOCH2CH2-.
[0083] From the viewpoint of exhibiting reverse wavelength dispersion, k and l are preferably in the range of 2≤k+l≤6, preferably k+l=4, more preferably k=2 and l=2. When k=2 and l=2, a symmetrical structure is obtained, which is further preferred.
[0084] E 1 and E 2 Each independently is preferably an alkanediyl group having 1 to 17 carbon atoms, and more preferably an alkanediyl group having 4 to 12 carbon atoms.
[0085] As P 1 or P 2 The polymerizable group represented by , for example, epoxy, vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, acryloyloxy, methacryloyloxy, oxirane, and the like can be mentioned. Among these, acryloyloxy, methacryloyloxy, vinyloxy, oxirane, and oxirane are preferred, and acryloyloxy is more preferred.
[0086] Ar preferably has at least one selected from an aromatic hydrocarbon ring that may have a substituent, an aromatic heterocycle that may have a substituent, and an electron-withdrawing group. As the aromatic hydrocarbon ring, for example, benzene ring, naphthalene ring, anthracene ring, etc. can be cited, preferably benzene ring, naphthalene ring. As the aromatic heterocycle, furan ring, benzofuran ring, pyrrole ring, indole ring, thiophene ring, benzothiophene ring, pyridine ring, pyrazine ring, pyrimidine ring, triazole ring, triazine ring, pyrroline ring, imidazole ring, pyrazole ring, thiazole ring, benzothiazole ring, thienothiazole ring, oxazole ring, benzoxazole ring, and phenanthroline ring, etc. can be cited. Among these, preferably have thiazole ring, benzothiazole ring, or benzofuran ring, further preferably have benzothiazolyl. In addition, when Ar contains a nitrogen atom, the nitrogen atom preferably has π electrons.
[0087] In formula (I), the total number of π electrons N contained in the divalent aromatic group represented by Ar is π It is preferably 8 or more, more preferably 10 or more, further preferably 14 or more, and particularly preferably 16 or more. It is preferably 30 or less, more preferably 26 or less, and further preferably 24 or less.
[0088] Examples of the aromatic group represented by Ar include the following groups.
[0089]
[0090] In the formulas (Ar-1) to (Ar-22), the symbol * represents a connecting portion, and Z 0 , Z 1 and Z 2 Each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyano group, a nitro group, an alkylsulfinyl group having 1 to 12 carbon atoms, an alkylsulfonyl group having 1 to 12 carbon atoms, a carboxyl group, a fluoroalkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkylthio group having 1 to 12 carbon atoms, an N-alkylamino group having 1 to 12 carbon atoms, an N,N-dialkylamino group having 2 to 12 carbon atoms, an N-alkylsulfamoyl group having 1 to 12 carbon atoms, or an N,N-dialkylsulfamoyl group having 2 to 12 carbon atoms.
[0091] Q 1 and Q 2 Each independently represents -CR 2’ R 3’ -、-S-、-NH-、-NR 2’ -, -CO- or -O-, R 2’ and R 3’ Each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
[0092] J 1 , and J 2 Each independently represents a carbon atom or a nitrogen atom.
[0093] Y 1 , Y 2 and Y 3 Each independently represents an aromatic hydrocarbon group or an aromatic heterocyclic group which may be substituted.
[0094] W 1 and W 2 Each independently represents a hydrogen atom, a cyano group, a methyl group or a halogen atom, and m represents an integer of 0-6.
[0095] As Y 1 , Y 2 and Y 3The aromatic hydrocarbon group in the group includes aromatic hydrocarbon groups having 6 to 20 carbon atoms, such as phenyl, naphthyl, anthracenyl, phenanthrenyl, and biphenyl, preferably phenyl and naphthyl, and more preferably phenyl. The aromatic heterocyclic group includes aromatic heterocyclic groups having 4 to 20 carbon atoms, such as furanyl, pyrrolyl, thienyl, pyridyl, thiazolyl, and benzothiazolyl, and preferably furanyl, thienyl, pyridyl, thiazolyl, and benzothiazolyl.
[0096] Y 1 and Y 2 Each independently may be a substituted polycyclic aromatic hydrocarbon group or a polycyclic aromatic heterocyclic group. The polycyclic aromatic hydrocarbon group refers to a condensed polycyclic aromatic hydrocarbon group or a group derived from an aromatic ring collection. The polycyclic aromatic heterocyclic group refers to a condensed polycyclic aromatic heterocyclic group or a group derived from an aromatic ring collection.
[0097] Z 0 , Z 1 and Z 2 Each of Z is independently preferably a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyano group, a nitro group, or an alkoxy group having 1 to 12 carbon atoms. 0 More preferably, a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a cyano group. 1 and Z 2 More preferred are a hydrogen atom, a fluorine atom, a chlorine atom, a methyl group and a cyano group.
[0098] Q 1 and Q 2 Preferred are -NH-, -S-, -NR 2’ -、-O-,R 2’ A hydrogen atom is preferred, and -S-, -O-, and -NH- are particularly preferred.
[0099] Among formulae (Ar-1) to (Ar-22), formulae (Ar-6) and (Ar-7) are preferred from the viewpoint of molecular stability.
[0100] In the formulas (Ar-16) to (Ar-22), Y 1 The nitrogen atom and Z to which it can be bonded 0 Together, they form an aromatic heterocyclic group. Examples of the aromatic heterocyclic group include the aromatic heterocyclic groups described above as aromatic heterocyclic rings that Ar may have, such as pyrrole rings, imidazole rings, pyrroline rings, pyridine rings, pyrazine rings, pyrimidine rings, indole rings, quinoline rings, isoquinoline rings, purine rings, and pyrrolidine rings. The aromatic heterocyclic group may have a substituent. In addition, Y 1 The nitrogen atom and Z to which it can be bonded 0Together, they form the above-mentioned substituted polycyclic aromatic hydrocarbon group or polycyclic aromatic heterocyclic group. Examples thereof include benzofuran ring, benzothiazole ring, benzoxazole ring, etc. It should be noted that the compound represented by the above formula (I) can be manufactured, for example, according to the method described in Japanese Patent Publication No. 2010-31223.
[0101] The polymerizable liquid crystal compound can be used alone or in combination of two or more. When two or more are used, the content of the compound represented by the above formula (I) is preferably 50 parts by mass or more, more preferably 70 parts by mass or more, and further preferably 80 parts by mass or more relative to 100 parts by mass of the polymerizable liquid crystal compound.
[0102] The horizontal alignment liquid crystal cured film forming composition (hereinafter also referred to as polymerizable liquid crystal composition) used in the formation of the horizontal alignment liquid crystal cured film may further contain a solvent, a photopolymerization initiator, an inhibitor, a photosensitizer, a leveling agent, and an adhesion improver. These additives can be used alone or in combination of two or more.
[0103] The content of the polymerizable liquid crystal compound is, for example, 70 to 99.5 parts by mass, preferably 80 to 99 parts by mass, and more preferably 90 to 98 parts by mass, relative to 100 parts by mass of the solid content of the polymerizable liquid crystal composition. When the content is within the above range, there is a tendency for the orientation of the horizontally oriented liquid crystal cured film to be improved. Here, the solid content refers to the total amount of the components after removing the solvent from the composition.
[0104] As the solvent, a solvent capable of dissolving the polymerizable liquid crystal compound is preferred, and a solvent inactive to the polymerization reaction of the polymerizable liquid crystal compound is preferred. Examples of the solvent include alcohol solvents such as water, methanol, ethanol, ethylene glycol, isopropanol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, 1-methoxy-2-propanol, 2-butoxyethanol, and propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; alicyclic hydrocarbon solvents such as ethylcyclohexane; aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran, anisole, and dimethoxyethane; chlorinated solvents such as chloroform and chlorobenzene; amide solvents such as dimethylacetamide, dimethylformamide, N-methyl-2-pyrrolidone (NMP), and 1,3-dimethyl-2-imidazolidinone; and the like. These solvents can be used alone or in combination of two or more. However, the compound shown in the above formula (I) usually has a large conjugated system, so the solubility in the solvent is low. Among the solvents exemplified above, alcohol solvents, ester solvents, ketone solvents, chlorinated solvents, ether solvents, amide solvents and aromatic hydrocarbon solvents are preferably used, and ester solvents, ketone solvents, chlorinated solvents, ether solvents and amide solvents are more preferably used.
[0105] Relative to 100 parts by mass of the polymerizable liquid crystal composition, the content of the solvent is preferably 50 to 98 parts by mass, more preferably 70 to 95 parts by weight. Therefore, the solid content shared in 100 parts by mass of the composition is preferably 2 to 50 parts by mass. When the solid content of the composition is less than 50 parts by mass, the viscosity of the composition decreases, so the thickness of the horizontally oriented liquid crystal cured film becomes roughly uniform, and there is a tendency that it is not easy to produce unevenness in the horizontally oriented liquid crystal cured film. The above-mentioned solid content can be appropriately determined considering the thickness of the horizontally oriented liquid crystal cured film to be manufactured.
[0106] A polymerization initiator is a compound that generates a reactive substance by the participation of heat or light, and can initiate a polymerization reaction of a polymerizable liquid crystal, etc. As the reactive substance, active substances such as free radicals, cations, or anions can be cited. Among them, from the viewpoint of easy control of the reaction, a photopolymerization initiator that reacts by light irradiation is preferred.
[0107] Examples of the photopolymerization initiator include photoradical polymerization initiators, photocationic polymerization initiators, etc. Examples of the photoradical polymerization initiator include benzoin compounds, benzophenone compounds, benzyl ketal compounds, α-hydroxyketone compounds, α-aminoketone compounds, triazine compounds, etc. Examples of the photocationic polymerization initiator include onium salts such as aromatic diazonium salts, aromatic iodonium salts, aromatic sulfonium salts, and iron-arene complexes.
[0108] Specific examples thereof include Irgacure (registered trademark) 907, Irgacure 184, Irgacure 651, Irgacure 819, Irgacure 250, Irgacure 369, Irgacure 379, Irgacure 127, Irgacure 2959, Irgacure 754, and Irgacure 379EG (all manufactured by BASF Japan Co., Ltd.), SEIKUOL BZ, SEIKUOL Z, and SEIKUOL BEE (all manufactured by Seiko Chemical Industries, Ltd.), Kayacure BP100 (manufactured by Nippon Kayaku Co., Ltd.), Kayacure UVI-6992 (manufactured by DOW), ADEKA Optomer SP-152, ADEKA Optomer SP-170, ADEKA Optomer N-1717, and ADEKA Optomer N-1919, ADEKA ARKLS NCI-831, ADEKA ARKLS NCI-930 (above are made by ADEKA Co., Ltd.), TAZ-A, TAZ-PP (above are made by Japan Siber Hegner Co., Ltd.) and TAZ-104 (made by Sanwa Chemical Co., Ltd.), KAYARAD (registered trademark) series (made by Nippon Kayaku Co., Ltd.), CYRACUREUVI series (made by Dow Chemical Co., Ltd.), CPI series (made by SAN-APRO Co., Ltd.), TAZ, BBI and DTS (above are made by Midori Chemical Co., Ltd.), RHODORSIL (registered trademark) (made by Rhodia Co., Ltd.), etc. The photopolymerization initiator can be used alone or in combination of two or more. Among these, from the viewpoint of easy control of the reaction, a photoradical polymerization initiator that generates free radicals by light irradiation is preferred.
[0109] As for the photopolymerization initiator, from the viewpoint of being able to fully utilize the energy emitted by the light source and achieving excellent productivity, it is preferred that the maximum absorption wavelength exists in the range of 300nm to 400nm, and more preferably exists in the range of 300nm to 380nm. In addition, from the same viewpoint, α-acetophenone-based polymerization initiators and oxime-based photopolymerization initiators are preferred.
[0110] Examples of the α-acetophenone-based polymerization initiator include 2-methyl-2-morpholino-1-(4-methylthiophenyl)-1-propanone, 2-dimethylamino-1-(4-morpholinophenyl)-2-benzyl-1-butanone, and 2-dimethylamino-1-(4-morpholinophenyl)-2-(4-methylphenylmethyl)-1-butanone, and more preferably 2-methyl-2-morpholino-1-(4-methylthiophenyl)-1-propanone and 2-dimethylamino-1-(4-morpholinophenyl)-2-benzyl-1-butanone. Examples of commercially available α-acetophenone compounds include Irgacure 369, 379EG, and 907 (all manufactured by BASF Japan Co., Ltd.) and SEIKUOL BEE (manufactured by Seiko Chemical Co., Ltd.).
[0111] Oxime-based photopolymerization initiators generate free radicals by irradiating light. Through the free radicals, the polymerization of the polymerizable liquid crystal compound in the deep part of the horizontally aligned liquid crystal curing film is well carried out. In addition, from the perspective of making the polymerization reaction in the deep part of the horizontally aligned liquid crystal curing film more efficient, it is preferred to use a photopolymerization initiator that can efficiently utilize ultraviolet rays with a wavelength of more than 350nm. As a photopolymerization initiator that can efficiently utilize ultraviolet rays with a wavelength of more than 350nm, triazine compounds and oxime ester carbazole compounds are preferred. From the perspective of sensitivity, oxime ester carbazole compounds are more preferred. As oxime ester carbazole compounds, for example, 1,2-octanedione, 1-[4-(phenylthio)-2-(O-benzoyl oxime)], O-acetyl-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-1-(acetone oxime) and the like can be cited. Examples of commercially available products of oxime ester type carbazole compounds include Irgacure OXE-01, Irgacure OXE-02, and Irgacure OXE-03 (all manufactured by BASF Japan Co., Ltd.), ADEKA Optomer N-1919, and ADEKA ARKLS NCI-831 (all manufactured by ADEKA Corporation).
[0112] The amount of the photopolymerization initiator added is usually 0.1 to 30 parts by mass, preferably 1 to 20 parts by mass, and more preferably 1 to 15 parts by mass relative to 100 parts by mass of the polymerizable liquid crystal compound. Within the above range, the reaction of the polymerizable group proceeds sufficiently and the alignment of the polymerizable liquid crystal compound is less likely to be disturbed.
[0113] By adding a polymerization inhibitor, the polymerization reaction of the polymerizable liquid crystal compound can be controlled. As the polymerization inhibitor, hydroquinone and hydroquinones having substituents such as alkyl ethers; butyl catechol and other catechols having substituents such as alkyl ethers; pyrogallols, 2,2,6,6-tetramethyl-1-piperidinyloxy radicals and other radical scavengers; thiophenols; β-naphthylamines and β-naphthols. In order to polymerize the polymerizable liquid crystal compound without disturbing the orientation of the polymerizable liquid crystal compound, the content of the polymerization inhibitor is generally 0.01 to 10 parts by mass, preferably 0.1 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass relative to 100 parts by mass of the polymerizable liquid crystal compound. The polymerization inhibitor can be used alone or in combination of two or more.
[0114] In addition, by using a photosensitizer, the photopolymerization initiator can be made highly sensitive. Examples of photosensitizers include xanthone, thioxanthone and other xanthones; anthracenes and anthracenes having substituents such as alkyl ethers; phenothiazines; and rubrene. Photosensitizers can be used alone or in combination of two or more. The content of the photosensitizer is generally 0.01 to 10 parts by mass, preferably 0.05 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound.
[0115] The so-called leveling agent refers to an additive having the function of adjusting the fluidity of the polymerizable liquid crystal composition and making the layer obtained by coating the composition flatter. Examples of leveling agents include silicone-based leveling agents such as silane coupling agents, polyacrylate-based leveling agents, and perfluoroalkyl-based leveling agents. Specific examples include DC3PA, SH7PA, DC11PA, SH28PA, SH29PA, SH30PA, ST80PA, ST86PA, SH8400, SH8700, FZ2123 (all manufactured by Toray Dow Corning Co., Ltd.), KP321, KP323, KP324, KP326, KP340, KP341, X22-161A, KF6001, KBM-1003, KBE-1003, KBM-303, KBM-402, KBM-403, KBE-402, KBE-403, KBM-1403, KBM-502, KBM-503, KBE-502, KBE-503, K BM-5103, KBM-602, KBM-603, KBM-903, KBE-903, KBE-9103, KBM-573, KBM-575, KBE-585, KBM-802, KBM-802, KBM-803, KBE-846, KBE-9007 (all manufactured by Shin-Etsu Chemical Co., Ltd.), TSF400, TSF401, TSF410, TSF4300, TSF4440, TSF4445, TSF-4446, TSF4452, TSF4460 (all manufactured by Momentive Materials Japan Co., Ltd.), Fluorinert (registered trademark) FC-72, Fluorinert FC-40, Fluorinert FC-43, Fluorinert FC-3283 (all manufactured by Sumitomo 3M Co., Ltd.), MEGAFAC (registered trademark) R-08, MEGAFAC R-30, MEGAFAC R-90, MEGAFAC F-410, MEGAFAC F-411, MEGAFAC F-443, MEGAFAC F-445, MEGAFAC F-470, MEGAFAC F-477, MEGAFAC F-479, MEGAFAC F-482, MEGAFAC F-483 (all manufactured by DIC Corporation), EFTOP (trade name) EF301, EFTOP EF303, EFTOP EF351, EFTOP EF352 (all manufactured by Mitsubishi Materials Electronic Chemicals Co., Ltd.), Surflon (registered trademark) S-381, Surflon S-382, Surflon S-383, Surflon S-393, Surflon SC-101, SurflonSC-105, KH-40, SA-100 (all manufactured by AGC Seimi Chemical Co., Ltd.), trade name E1830, trade name E5844 (manufactured by Daikin Fine Chemicals Laboratories), BM-1000, BM-1100, BYK-352, BYK-353 and BYK-361N (all trade names: manufactured by BM Chemie Co., Ltd.), etc. The leveling agent may be used alone or in combination of two or more.
[0116] The content of the leveling agent is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. When the content of the leveling agent is within the above range, the obtained horizontally aligned liquid crystal cured film tends to be smoother, which is preferred.
[0117] The polymerizable liquid crystal composition can be obtained by stirring a polymerizable liquid crystal compound and components other than the polymerizable liquid crystal compound such as additives at a predetermined temperature.
[0118] The horizontally aligned liquid crystal cured film can be obtained by applying the above polymerizable liquid crystal composition onto the horizontally aligned film described later, removing the solvent, and curing the polymerizable liquid crystal composition containing the aligned polymerizable liquid crystal compound by heating and / or active energy rays.
[0119] As a method for coating a polymerizable liquid crystal composition on a horizontally aligned film (hereinafter, sometimes referred to as coating method A), for example, extrusion coating, direct gravure coating, reverse gravure coating, CAP coating, slit coating, micro gravure, die coating, inkjet, etc. can be cited. In addition, a method for coating using a coating machine such as a dip coater, a rod coater, a spin coater, etc. can also be cited. Among them, in the case of continuous coating in a roll-to-roll manner, a coating method based on a micro gravure method, an inkjet method, a slit coating method, and a die coating method is preferably used.
[0120] As a method for removing the solvent (hereinafter, sometimes referred to as solvent removal method A), for example, natural drying, ventilation drying, heating drying, reduced pressure drying and a combination thereof can be mentioned. Among them, natural drying or heating drying is preferred. The drying temperature is preferably in the range of 0 to 200° C., more preferably in the range of 20 to 150° C., and further preferably in the range of 50 to 130° C. The drying time is preferably 10 seconds to 20 minutes, more preferably 30 seconds to 10 minutes.
[0121] As the active energy ray for irradiation, it can be appropriately selected according to the type of polymerizable liquid crystal compound (especially, the type of photopolymerizable functional group possessed by the polymerizable liquid crystal compound), the type of photopolymerization initiator (when including a photopolymerization initiator), and their amount. Specifically, one or more lights selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α rays, β rays, and γ rays can be cited. Among them, from the aspect of easy control of the progress of the polymerization reaction and the aspect of being able to use a device that has been widely used in the art as a photopolymerization device, ultraviolet light is preferred, and the type of polymerizable liquid crystal compound is preferably selected in a manner that can be photopolymerized by ultraviolet light.
[0122] As the light source of the above-mentioned active energy rays, for example, there can be mentioned a low-pressure mercury lamp, a medium-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a xenon lamp, a halogen lamp, a carbon arc lamp, a tungsten lamp, a gallium lamp, an excimer laser, an LED light source emitting light in the wavelength range of 380 to 440 nm, a chemical lamp, a black light lamp, a microwave-excited mercury lamp, a metal halide lamp, and the like.
[0123] UV radiation intensity is usually 10 to 3,000 mW / cm 2 The ultraviolet irradiation intensity is preferably an intensity in a wavelength region effective for activating a photocationic polymerization initiator or a photoradical polymerization initiator. The irradiation time is usually 0.1 second to 10 minutes, preferably 0.1 second to 5 minutes, more preferably 0.1 second to 3 minutes, and further preferably 0.1 second to 1 minute.
[0124] When irradiated once or multiple times with such ultraviolet irradiation intensity, the cumulative light intensity is 10 to 3,000 mJ / cm 2 , preferably 50 to 2,000 mJ / cm 2 , more preferably 100 to 1,000 mJ / cm 2 When the accumulated light amount is below the above lower limit, the curing of the polymerizable liquid crystal compound becomes insufficient, and sometimes good transferability cannot be obtained. On the contrary, when the accumulated light amount is above the above upper limit, sometimes the phase difference plate with optical compensation function including the horizontally oriented liquid crystal cured film is colored.
[0125] From the viewpoint of thin film formation of the functional film, the film thickness of the horizontally aligned liquid crystal cured film is preferably 5 μm or less, more preferably 3 μm or less, and further preferably 2.5 μm or less. In addition, the lower limit of the film thickness of the horizontally aligned liquid crystal cured film is preferably 0.1 μm or more, more preferably 0.5 μm or more, and further preferably 1.0 μm or more. The film thickness of the horizontally aligned liquid crystal cured film can be measured using an ellipsometer or a contact film thickness meter.
[0126] 〔Horizontal alignment film〕
[0127] The alignment film is a film having an alignment control force that orients the polymerizable liquid crystal compound of the liquid crystal curing film in a predetermined direction. In addition, various alignments such as vertical alignment, horizontal alignment, mixed alignment, and tilted alignment can be controlled by the type of alignment film, rubbing conditions, and light irradiation conditions. Among them, the horizontal alignment film is an alignment film having an alignment control force that orients the polymerizable liquid crystal compound of the liquid crystal curing film in a horizontal direction. Therefore, by using the horizontal alignment film, a horizontally aligned liquid crystal film can be formed.
[0128] The alignment film preferably has solvent resistance such that the polymerizable liquid crystal composition does not dissolve due to coating or the like, and has heat resistance against a heating treatment for removing the solvent and aligning the polymerizable liquid crystal compound.
[0129] As the horizontal alignment film that exhibits an alignment control force that orients the horizontal alignment liquid crystal cured film in the horizontal direction, there can be cited a rubbing alignment film, a photo alignment film, and a groove alignment film having a concave-convex pattern and a plurality of grooves on the surface, etc. When applied to, for example, a long roll film, a photo alignment film is preferred from the aspect that the alignment direction can be easily controlled.
[0130] In the case of a rubbed oriented film, a composition comprising an oriented polymer and a solvent (hereinafter also referred to as a rubbed oriented film forming composition) is usually applied to a substrate, etc., the solvent is removed to form a coating film, and the coating film is rubbed to impart an orientation control force.
[0131] As the oriented polymer, for example, polyamides having amide bonds, gelatins, polyimides having imide bonds and their hydrolyzates, i.e., polyamic acid, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinyl pyrrolidone, polyacrylic acid and polyacrylates can be cited. These oriented polymers can be used alone or in combination of two or more.
[0132] The concentration of the oriented polymer in the rubbed oriented film-forming composition may be within a range in which the oriented polymer is completely dissolved in the solvent. The content of the oriented polymer is preferably 0.1 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, based on 100 parts by mass of the composition.
[0133] The rubbed alignment film-forming composition is commercially available, and examples of commercially available products include SUNEVER (registered trademark, manufactured by Nissan Chemical Industries, Ltd.) and OPTMER (registered trademark, manufactured by JSR Corporation).
[0134] The solvent may be any of the solvents listed in the horizontal alignment liquid crystal cured film. The coating method A may be used as a method for coating the rubbed alignment film-forming composition on a substrate, and the solvent removal method A may be used as a method for removing the solvent.
[0135] As a method of rubbing treatment, for example, a method of bringing the coating film into contact with a rubbing roller wound with a rubbing cloth and rotating can be mentioned. During the rubbing treatment, if masking is performed, a plurality of regions (patterns) with different alignment directions can be formed on the alignment film.
[0136] The photo-alignment film can be generally obtained by applying a composition containing a polymer or monomer having a photoreactive group and a solvent (also referred to as a photo-alignment film-forming composition) on a substrate, etc., removing the solvent, and irradiating the substrate with polarized light (preferably polarized UV light). For the photo-alignment film, the direction of the orientation control force can be arbitrarily controlled by selecting the polarization direction of the irradiated polarized light.
[0137] The so-called photoreactive group refers to a group that generates an orientation ability by light irradiation. Specifically, there can be cited groups that participate in photoreactions that become the source of orientation ability, such as orientation-induced reactions, isomerization reactions, photodimerization reactions, photocrosslinking reactions, or photodecomposition reactions of molecules that occur by light irradiation. As a photoreactive group, a group having an unsaturated bond, especially a double bond, is preferred, and a group having at least one selected from the group consisting of a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond), and a carbon-oxygen double bond (C=O bond) is particularly preferred.
[0138] As photoreactive groups having C=C bonds, for example, vinyl, polyene, stilbene, stilbazole, stilbazolium, chalcone and cinnamoyl groups can be cited. As photoreactive groups having C=N bonds, for example, groups having structures such as aromatic Schiff bases and aromatic hydrazones can be cited. As photoreactive groups having N=N bonds, for example, azophenyl, azonaphthyl, aromatic heterocyclic azo, bisazo, formazan, and groups having an oxidized azobenzene structure can be cited. As photoreactive groups having C=O bonds, for example, benzophenone, coumarin, anthraquinone and maleimide groups can be cited. These groups may have substituents such as alkyl, alkoxy, aryl, allyloxy, cyano, alkoxycarbonyl, hydroxyl, sulfonic acid, and halogenated alkyl. From the perspective of excellent orientation, a group that participates in a photodimerization reaction or a photocrosslinking reaction is preferred. Among them, a photoreactive group that participates in a photodimerization reaction is preferred. From the perspective of less polarized light irradiation required for orientation and easy acquisition of a photoalignment film having excellent thermal stability and temporal stability, a cinnamoyl group and a chalcone group are preferred. As a polymer having a photoreactive group, a polymer having a cinnamoyl group such that the terminal portion of the polymer side chain becomes a cinnamic acid structure or a cinnamate structure is particularly preferred.
[0139] The content of the polymer or monomer having a photoreactive group can be adjusted according to the type of the polymer or monomer and the thickness of the target photoalignment film, and is preferably at least 0.2 parts by mass, more preferably in the range of 0.3 to 10 parts by mass, relative to 100 parts by mass of the photoalignment film-forming composition.
[0140] The solvent may be any of the solvents listed in the horizontal alignment liquid crystal cured film. The method for applying the photoalignment film-forming composition to a substrate or the like may include the coating method A, and the method for removing the solvent may include the solvent removal method A.
[0141] In order to irradiate polarized light, for example, it can be a method of directly irradiating polarized light to the product obtained by removing the solvent from the composition for forming a photo-alignment film applied to a substrate, etc. In addition, it is preferred that the polarized light is substantially parallel light. The wavelength of the irradiated polarized light is preferably a wavelength in the wavelength region where the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy. Specifically, UV (ultraviolet light) in the range of 250 to 400 nm is particularly preferred. As a light source for irradiating the polarized light, xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, ultraviolet lasers such as KrF and ArF can be cited. Among them, high-pressure mercury lamps, ultra-high-pressure mercury lamps and metal halide lamps are preferred because of the high luminous intensity of ultraviolet rays with a wavelength of 313 nm. Polarized UV light can be irradiated by passing light from the above-mentioned light source through an appropriate polarizing element. As a polarizing element, polarizing filters, polarizing prisms such as Glan-Thompson and Glan-Taylor, and wire grids can be cited. Among them, a wire grid type polarizing element is preferred from the viewpoint of increasing the area and the resistance to heat.
[0142] It should be noted that, by shielding during rubbing or polarized light irradiation, a plurality of regions (patterns) in which the directions of liquid crystal alignment are different can be formed.
[0143] The groove oriented film is a film having a concave-convex pattern or multiple grooves (grooves) on the film surface. When a polymerizable liquid crystal compound is applied to a film having multiple linear grooves arranged at equal intervals, the liquid crystal molecules will be oriented in the direction along the grooves.
[0144] As methods for obtaining a grooved oriented film, there are: a method of exposing the surface of a photosensitive polyimide film through an exposure mask having a slit in a pattern shape, and then developing and rinsing to form a concave-convex pattern; a method of forming a layer of a UV-curable resin before curing on a plate-like original plate having grooves on its surface, transferring the formed resin layer to a substrate, etc., and then curing it; and a method of pressing a roll original plate having a plurality of grooves against a film of a UV-curable resin before curing formed on a substrate, etc., thereby forming concave-convex, and then curing it; and the like.
[0145] The horizontal alignment film-forming composition such as the rubbed alignment film-forming composition and the photo-alignment film-forming composition may contain the additives exemplified in the horizontal alignment liquid crystal cured film in addition to the solvent.
[0146] From the viewpoint of thinning the retardation plate with an optical compensation function, the film thickness of the horizontal alignment film is preferably 1 μm or less, more preferably 0.5 μm or less, and still more preferably 0.3 μm or less. In addition, the film thickness of the horizontal alignment film is preferably 1 nm or more, more preferably 5 nm or more, still more preferably 10 nm or more, and particularly preferably 30 nm or more. The film thickness of the horizontal alignment film can be measured using an ellipsometer or a contact type film thickness meter.
[0147] [Vertically aligned liquid crystal cured film]
[0148] The horizontally aligned liquid crystal cured film is a film having refractive index anisotropy in a direction perpendicular to the film plane and is formed of a polymer containing a polymerizable liquid crystal compound. From the aspect of being able to arbitrarily design the thinning and wavelength dispersion characteristics of the vertically aligned liquid crystal cured film, it is preferable to form the vertically aligned liquid crystal cured film by the following method: applying a polymerizable liquid crystal composition onto a vertically aligned film and polymerizing the polymerizable liquid crystal composition containing the polymerizable liquid crystal compound in an oriented state by heating and / or light irradiation.
[0149] The three-dimensional refractive index ellipsoid formed by the vertically aligned liquid crystal cured film may have biaxiality, but preferably has uniaxiality. For the vertically aligned liquid crystal cured film, it may be a vertically aligned liquid crystal cured film formed of a polymer of a polymerizable liquid crystal composition containing the following polymerizable liquid crystal compound, wherein the polymerizable liquid crystal compound is in a state of being oriented in a direction perpendicular to the plane of the liquid crystal cured film; it may also be a mixed alignment liquid crystal cured film or an inclined alignment liquid crystal cured film. For the refractive indices nx, ny, and nz in the three directions of the refractive index ellipsoid formed by the orientation of the polymerizable liquid crystal, the relationship of nz>nx≈ny (referred to as a positive C-plate) or nz<nx≈ny (referred to as a negative C-plate) may be present. nx represents the principal refractive index in the direction parallel to the plane of the vertically aligned liquid crystal cured film in the refractive index ellipsoid formed by the vertically aligned liquid crystal cured film. ny represents the refractive index in the direction parallel to the plane of the vertically aligned liquid crystal cured film and orthogonal to the direction of nx in the refractive index ellipsoid formed by the vertically aligned liquid crystal cured film. It should be noted that when nx = ny, nx can take any direction within the plane of the vertically aligned liquid crystal cured film. nz represents the refractive index in the direction perpendicular to the plane of the vertically aligned liquid crystal cured film in the refractive index ellipsoid formed by the vertically aligned liquid crystal cured film.
[0150] The vertically aligned liquid crystal cured film can use either a rod-shaped polymerizable liquid crystal or a disc-shaped polymerizable liquid crystal, but a rod-shaped polymerizable liquid crystal is preferred. When the rod-shaped polymerizable liquid crystal forms a vertically aligned liquid crystal cured film, the vertically aligned liquid crystal cured film becomes a positive C-plate.
[0151] When the vertically aligned liquid crystal cured film is a positive C plate, the phase difference value in the thickness direction relative to the light of wavelength λnm, i.e., RthC(λ), preferably satisfies the optical properties shown in the following formula (31). In addition, it is also preferred to satisfy the optical properties shown in the following formulas (32) and (33). The vertically aligned liquid crystal cured film more preferably satisfies the optical properties shown in the following formulas (31), (32), and (33).
[0152] -100nm≤RthC(550)≤-50nm···(31)
[0153] (Wherein, RthC(550) represents the phase difference in the thickness direction relative to light with a wavelength of 550 nm.)
[0154] RthC(450) / RthC(550)≤1.0···(32)
[0155] 1.00≤RthC(650) / RthC(550)···(33)
[0156] (In the formula, RthC(450) represents the phase difference value in the thickness direction relative to light with a wavelength of 450 nm, RthC(550) represents the phase difference value in the thickness direction relative to light with a wavelength of 550 nm, and RthC(650) represents the phase difference value in the thickness direction relative to light with a wavelength of 650 nm.)
[0157] When the phase difference value RthC(550) in the thickness direction of the vertically oriented liquid crystal curing film exceeds the range of formula (31), the following problem will arise: the oblique hue of the display using an elliptically polarizing plate with optical compensation function (which includes a phase difference plate with optical compensation function) becomes red or blue. As a more preferred range of the phase difference value in the thickness direction, -95nm≤RthC(550)≤-55nm, as a further preferred range, -90nm≤RthC(550)≤-60nm. When "RthC(450) / RthC(550)" of the vertically oriented liquid crystal curing film exceeds 1.0, the ellipticity of the elliptically polarizing plate having the vertically oriented liquid crystal curing film deteriorates when observed from an oblique direction on the short wavelength side. If the ellipticity of the elliptically polarizing plate on the short wavelength side deteriorates and is less than 1.0, there is a tendency that the function of the elliptically polarizing plate on the short wavelength side is impaired. "RthC(450) / RthC(550)" is preferably 0.75 to 0.92, more preferably 0.77 to 0.87, and further preferably 0.79 to 0.85.
[0158] The phase difference value in the thickness direction of the vertically oriented liquid crystal curing film can be adjusted by the thickness of the vertically oriented liquid crystal curing film. Since the phase difference value in the thickness direction is determined by the following formula (34), in order to obtain the desired phase difference value in the thickness direction (RthC (λ): the phase difference value in the thickness direction of the vertically oriented liquid crystal curing film at wavelength λ (nm)), it is sufficient to adjust the three-dimensional refractive index and the film thickness dC. It should be noted that the three-dimensional refractive index depends on the molecular structure and orientation of the polymerizable liquid crystal compound described later.
[0159] RthC(λ)=[(nxC(λ)+nyC(λ)) / 2-nzC(λ)]×dC···(34)
[0160] (In the formula, in the refractive index ellipsoid formed by the vertically aligned liquid crystal curing film, there is a relationship of nzC(λ)>nxC(λ)≈nyC(λ), wherein nzC(λ) represents the refractive index of light with a wavelength of λ(nm) in the direction perpendicular to the plane of the vertically aligned liquid crystal curing film in the refractive index ellipsoid formed by the vertically aligned liquid crystal curing film. nxC(λ) represents the maximum refractive index of light with a wavelength of λ(nm) in the direction parallel to the plane of the vertically aligned liquid crystal curing film in the refractive index ellipsoid formed by the vertically aligned liquid crystal curing film. nyC(λ) represents the refractive index of light with a wavelength of λ(nm) in the direction parallel to the plane of the vertically aligned liquid crystal curing film and orthogonal to the above-mentioned direction of nxC in the refractive index ellipsoid formed by the vertically aligned liquid crystal curing film. However, when nxC(λ)=nyC(λ), nxC(λ) represents the refractive index in any direction parallel to the plane of the vertically aligned liquid crystal curing film. Here, dC represents the thickness of the vertically aligned liquid crystal curing film.)
[0161] The vertically oriented liquid crystal cured film is preferably a polymer of a polymerizable liquid crystal composition containing a polymerizable liquid crystal compound in a vertically oriented state as described above. The polymerizable liquid crystal compound forming the vertically oriented liquid crystal cured film is a liquid crystal compound having a polymerizable functional group, especially a photopolymerizable functional group. The so-called photopolymerizable functional group refers to a group that can participate in the polymerization reaction using active free radicals, acids, etc. generated by a photopolymerization initiator. As photopolymerizable functional groups, vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, acryloyloxy, methacryloyloxy, oxirane, oxetane, etc. can be cited. Among them, acryloyloxy, methacryloyloxy, vinyloxy, oxirane and oxetane are preferred, and acryloyloxy is more preferred. Liquid crystal can be a thermotropic liquid crystal or a lyotropic liquid crystal. As a phase sequence structure, it can be a nematic liquid crystal or a smectic liquid crystal.
[0162] The polymerizable liquid crystal compound used in forming the vertically aligned liquid crystal cured film is preferably a compound represented by the above formula (I). By using the compound represented by the formula (I), reverse wavelength dispersion can be exhibited and the above relationships (31) and (32) can be satisfied.
[0163] The polymerizable liquid crystal compound used in the vertically aligned liquid crystal cured film can be used alone or in combination of two or more. When two or more are used, the content of the compound represented by the above formula (I) is preferably 50 parts by mass or more, more preferably 70 parts by mass or more, and further preferably 80 parts by mass or more relative to 100 parts by mass of the polymerizable liquid crystal compound.
[0164] The composition for forming a vertically aligned liquid crystal cured film (hereinafter also referred to as a polymerizable liquid crystal composition) used in the vertically aligned liquid crystal cured film may further contain a solvent, a photopolymerization initiator, an inhibitor, a photosensitizer, a leveling agent, and an adhesion improver. These additives may be used alone or in combination of two or more.
[0165] The content of the polymerizable liquid crystal compound is, for example, 70 to 99.5 parts by mass, preferably 80 to 99 parts by mass, and more preferably 90 to 98 parts by mass, relative to 100 parts by mass of the solid content of the polymerizable liquid crystal composition. When the content is within the above range, there is a tendency for the orientation of the vertically oriented liquid crystal cured film to be improved. Here, the solid content refers to the total amount of the components after removing the solvent from the composition.
[0166] The solvent is preferably a solvent capable of dissolving the polymerizable liquid crystal compound and preferably a solvent inactive to the polymerization reaction of the polymerizable liquid crystal compound. The same solvent as used in the horizontal alignment liquid crystal cured film-forming composition can be used as the solvent.
[0167] Relative to 100 parts by mass of the polymerizable liquid crystal composition, the content of the solvent is preferably 50 to 98 parts by mass, more preferably 70 to 95 parts by weight. Therefore, the solid content occupied in 100 parts by mass of the composition is preferably 2 to 50 parts by mass. When the solid content of the composition is less than 50 parts by mass, the viscosity of the composition decreases, so the thickness of the vertically aligned liquid crystal cured film becomes roughly uniform, and there is a tendency that it is not easy to produce unevenness in the vertically aligned liquid crystal cured film. The above-mentioned solid content can be appropriately determined considering the thickness of the vertically aligned liquid crystal cured film to be manufactured.
[0168] The polymerization initiator is a compound that generates a reactive substance by the participation of heat or light and can initiate a polymerization reaction of a polymerizable liquid crystal or the like. As the reactive substance, active substances such as free radicals, cations, or anions can be cited. Among them, from the viewpoint of easy control of the reaction, a photopolymerization initiator that reacts by light irradiation is preferred. The photopolymerization initiator can use the same initiator as the photopolymerization initiator used in the composition for forming a horizontally aligned liquid crystal cured film.
[0169] The amount of the photopolymerization initiator added is usually 0.1 to 30 parts by mass, preferably 1 to 20 parts by mass, and more preferably 1 to 15 parts by mass relative to 100 parts by mass of the polymerizable liquid crystal compound. Within the above range, the reaction of the polymerizable group proceeds sufficiently and the alignment of the polymerizable liquid crystal compound is less likely to be disturbed.
[0170] By combining a polymerization inhibitor, the polymerization reaction of the polymerizable liquid crystal compound can be controlled. As a polymerization inhibitor, the same polymerization inhibitor as that used in the horizontally aligned liquid crystal curing film forming composition can be used. In order to polymerize the polymerizable liquid crystal compound without disturbing the orientation of the polymerizable liquid crystal compound, the content of the polymerization inhibitor is usually 0.01 to 10 parts by mass, preferably 0.1 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass relative to 100 parts by mass of the polymerizable liquid crystal compound. The polymerization inhibitor can be used alone or in combination of two or more.
[0171] In addition, by using a photosensitizer, the photopolymerization initiator can be highly sensitive. As a photosensitizer, the same photosensitizer as that used in the horizontal alignment liquid crystal cured film forming composition can be used. The content of the photosensitizer is usually 0.01 to 10 parts by mass, preferably 0.05 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass relative to 100 parts by mass of the polymerizable liquid crystal compound.
[0172] The leveling agent is an additive having the function of adjusting the fluidity of the polymerizable liquid crystal composition and making the layer obtained by coating the composition flatter, and the same leveling agent as that used for the horizontal alignment liquid crystal cured film-forming composition can be used.
[0173] The content of the leveling agent is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. When the content of the leveling agent is within the above range, the resulting vertically aligned liquid crystal cured film tends to be smoother, which is preferred.
[0174] The polymerizable liquid crystal composition used for forming the vertically aligned liquid crystal cured film can be obtained by stirring a polymerizable liquid crystal compound and components other than the polymerizable liquid crystal compound such as additives at a predetermined temperature.
[0175] The vertically aligned liquid crystal cured film can be obtained by applying the above-mentioned polymerizable liquid crystal composition on the vertically aligned film described later, then removing the solvent, and curing the polymerizable liquid crystal composition containing the polymerizable liquid crystal compound in an aligned state by heating and / or active energy rays.
[0176] The method for coating the polymerizable liquid crystal composition on the vertical alignment film can be the same method as that used in forming the horizontal alignment liquid crystal cured film.
[0177] The method of removing the solvent can use the same method as in the case of forming the horizontal alignment liquid crystal cured film.
[0178] As the active energy ray for irradiation, it can be appropriately selected according to the type of polymerizable liquid crystal compound (especially, the type of photopolymerizable functional group possessed by the polymerizable liquid crystal compound), the type of photopolymerization initiator (when including a photopolymerization initiator), and their amount. Specifically, one or more lights selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α rays, β rays, and γ rays can be cited. Among them, from the aspect of easy control of the progress of the polymerization reaction and the aspect of being able to use a device that has been widely used in the art as a photopolymerization device, ultraviolet light is preferred, and the type of polymerizable liquid crystal compound is preferably selected in a manner that can be photopolymerized by ultraviolet light.
[0179] As the light source of the above-mentioned active energy ray, the same light source as that used when forming the horizontally aligned liquid crystal cured film can be used.
[0180] UV radiation intensity is usually 10 to 3,000 mW / cm 2 The ultraviolet irradiation intensity is preferably an intensity in a wavelength region effective for activating a photocationic polymerization initiator or a photoradical polymerization initiator. The irradiation time is usually 0.1 second to 10 minutes, preferably 0.1 second to 5 minutes, more preferably 0.1 second to 3 minutes, and further preferably 0.1 second to 1 minute.
[0181] When irradiated once or multiple times with such ultraviolet irradiation intensity, the cumulative light intensity is 10 to 3,000 mJ / cm 2 , preferably 50 to 2,000 mJ / cm 2 , more preferably 100 to 1,000 mJ / cm 2 When the accumulated light amount is below the above lower limit, the curing of the polymerizable liquid crystal compound becomes insufficient, and sometimes good transferability cannot be obtained. On the contrary, when the accumulated light amount is above the above upper limit, sometimes the phase difference plate with optical compensation function including the vertically aligned liquid crystal cured film is colored.
[0182] From the viewpoint of thin film of functional film, the film thickness of vertically aligned liquid crystal cured film is preferably 3 μm or less, more preferably 2 μm or less, and further preferably 1.5 μm or less. In addition, the lower limit of the film thickness of vertically aligned liquid crystal cured film is preferably 0.1 μm or more, more preferably 0.3 μm or more, and further preferably 0.5 μm or more. The film thickness of vertically aligned liquid crystal cured film can be measured using an ellipsometer or a contact film thickness meter.
[0183] [Vertical Alignment Film]
[0184] The alignment film is a film having an alignment control force that orients the polymerizable liquid crystal compound of the liquid crystal curing film in a predetermined direction. In addition, various alignments such as vertical alignment, horizontal alignment, mixed alignment, and tilted alignment can be controlled by the type of alignment film, rubbing conditions, and light irradiation conditions. Among them, the vertical alignment film is an alignment film having an alignment control force that orients the polymerizable liquid crystal compound of the liquid crystal curing film in a vertical direction. Therefore, by using the vertical alignment film, a vertically aligned liquid crystal film can be formed.
[0185] As a vertical alignment film, it is preferred to use a material that reduces the surface tension of the surface of a substrate, etc. As such a material, the above-mentioned oriented polymers, such as polyimide, polyamide, its hydrolyzate, i.e., polyamic acid, perfluoroalkyl and other fluorine-based polymers, and silane compounds and polysiloxane compounds obtained by their condensation reaction can be cited. The vertical alignment film can be obtained by applying a composition (hereinafter also referred to as a vertical alignment film forming composition) containing such a material and a solvent, such as a solvent exemplified in the vertical alignment liquid crystal film, to a substrate, etc., and after removing the solvent, heating the coated film, etc.
[0186] When a silane compound is used in the vertical alignment film, from the viewpoint of easily reducing the surface tension and easily improving the adhesion with the layer adjacent to the vertical alignment film, the vertical alignment film is preferably a film formed by a compound containing Si element and C element in the constituent elements, and the silane compound can be used appropriately. In the present invention, when a vertical alignment film is configured between the horizontal alignment liquid crystal curing film and the vertical alignment liquid crystal curing film, the vertical alignment film, the horizontal alignment liquid crystal curing film and the vertical alignment liquid crystal curing film show high adhesion, and can effectively suppress or prevent peeling at the interface between the layers in the phase difference plate with optical compensation function.
[0187] As the silane compound, the above-mentioned silane coupling agent and other organic silicon-based compounds can be preferably used, for example, vinyl trimethoxysilane, vinyl triethoxysilane, vinyl tri(2-methoxyethoxy)silane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylene)propylamine, 3-glycidoxypropyltrimethoxysilane, Methoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-chloropropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropyldimethoxymethylsilane, 3-glycidoxypropylethoxydimethylsilane, etc.
[0188] The silane compound may be a silicone monomer type or a silicone oligomer (polymer) type. When the silicone oligomer is shown in the form of a (monomer)-(monomer) copolymer, examples include: copolymers containing mercaptopropyl groups such as 3-mercaptopropyltrimethoxysilane-tetramethoxysilane copolymer, 3-mercaptopropyltrimethoxysilane-tetraethoxysilane copolymer, 3-mercaptopropyltriethoxysilane-tetramethoxysilane copolymer, and 3-mercaptopropyltriethoxysilane-tetraethoxysilane copolymer; and copolymers containing mercaptopropyl groups such as mercaptomethyltrimethoxysilane-tetramethoxysilane copolymer, mercaptomethyltrimethoxysilane-tetraethoxysilane copolymer, mercaptomethyltriethoxysilane-tetramethoxysilane copolymer, and mercaptomethyltriethoxysilane-tetraethoxysilane copolymer. 3-methacryloxypropyl trimethoxysilane-tetramethoxysilane copolymer, 3-methacryloxypropyl trimethoxysilane-tetraethoxysilane copolymer, 3-methacryloxypropyl triethoxysilane-tetramethoxysilane copolymer, 3-methacryloxypropyl triethoxysilane-tetraethoxysilane copolymer, 3-methacryloxypropyl methyl dimethoxysilane-tetramethoxysilane copolymer, 3-methacryloxypropyl methyl dimethoxysilane-tetraethoxysilane copolymer, 3-methacryloxypropyl methyl diethoxysilane-tetramethoxysilane copolymer, and 3-methacryloxypropyl methyl 3-acryloxypropyl trimethoxysilane-tetramethoxysilane copolymer, 3-acryloxypropyl trimethoxysilane-tetraethoxysilane copolymer, 3-acryloxypropyl triethoxysilane-tetramethoxysilane copolymer, 3-acryloxypropyl triethoxysilane-tetraethoxysilane copolymer, 3-acryloxypropyl methyldimethoxysilane-tetramethoxysilane copolymer, 3-acryloxypropyl methyldimethoxysilane-tetraethoxysilane copolymer, 3-acryloxypropyl methyldiethoxysilane-tetramethoxysilane copolymer, and Copolymers containing an acryloxypropyl group such as 3-acryloxypropylmethyldiethoxysilane-tetraethoxysilane copolymer; copolymers containing a vinyl group such as vinyltrimethoxysilane-tetramethoxysilane copolymer, vinyltrimethoxysilane-tetraethoxysilane copolymer, vinyltriethoxysilane-tetramethoxysilane copolymer, vinyltriethoxysilane-tetraethoxysilane copolymer, vinylmethyldimethoxysilane-tetramethoxysilane copolymer, vinylmethyldimethoxysilane-tetraethoxysilane copolymer, vinylmethyldiethoxysilane-tetramethoxysilane copolymer, and vinylmethyldiethoxysilane-tetraethoxysilane copolymer;3-aminopropyltrimethoxysilane-tetramethoxysilane copolymer, 3-aminopropyltrimethoxysilane-tetraethoxysilane copolymer, 3-aminopropyltriethoxysilane-tetramethoxysilane copolymer, 3-aminopropyltriethoxysilane-tetraethoxysilane copolymer, 3-aminopropylmethyldimethoxysilane-tetramethoxysilane copolymer, 3-aminopropylmethyldimethoxysilane-tetraethoxysilane copolymer, 3-aminopropylmethyldiethoxysilane-tetramethoxysilane copolymer, and 3-aminopropylmethyldiethoxysilane-tetraethoxysilane copolymer, etc., which contain amino groups. The silane compound can be used alone or in combination of two or more. In addition, silane coupling agents, which are sometimes used as leveling agents, can also be used. ;
[0189] Among these, silane compounds having an alkyl group at the molecular terminal are preferred, and silane compounds having an alkyl group having 3 to 30 carbon atoms are more preferred.
[0190] From the viewpoint of easier improvement of adhesion, the viewpoint of coating property of the composition for forming a vertically oriented liquid crystal curing film, and the viewpoint that the layer disposed in the lower layer in the manufacturing method of the phase difference plate with optical compensation function described later is not easily dissolved, the vertically oriented film is preferably a film formed by a compound containing Si element, C element and O element in the constituent elements. In addition, the number of carbon atoms of the substituent (preferably alkyl or alkoxy) including the C atom bonded to the Si atom of the silane compound forming the vertically oriented film is preferably 1 to 30, more preferably 2 to 25, and further preferably 3 to 20. That is, the ratio of Si element to C element (Si / C, molar ratio) is preferably 0.03 to 1.00, more preferably 0.04 to 0.50, and further preferably 0.05 to 0.33. When the Si / C ratio is above the above lower limit, the coating property of the composition for forming a vertically oriented liquid crystal curing film is improved, and when the Si / C ratio is below the above upper limit, the adhesion with the adjacent layer can be improved.
[0191] The solvent may be any of the solvents listed in the horizontal alignment liquid crystal cured film. The coating method A may be used as a method for coating the vertical alignment film-forming composition, and the solvent removal method A may be used as a method for removing the solvent.
[0192] The composition for forming a vertical alignment film may contain the additives exemplified in the section of the horizontal alignment liquid crystal cured film, in addition to the solvent.
[0193] From the perspective of the thin film of the phase difference plate with optical compensation function and the presentation of the orientation control force, the film thickness of the vertical alignment film is preferably less than 1 μm, more preferably less than 0.3 μm, and more preferably less than 0.1 μm. In addition, the film thickness of the vertical alignment film is preferably more than 1 nm, more preferably more than 5 nm, more preferably more than 10 nm, and particularly preferably more than 30 nm. The film thickness of the vertical alignment film can be measured using an ellipsometer or a contact film thickness meter.
[0194] 〔Base material〕
[0195] The substrate is a material used when applying an oriented film forming composition or a liquid crystal curing film forming composition. It can be a design in which the film applied to the substrate is transferred by peeling the substrate, or it can be a design in which the film cannot be transferred because the substrate is given adhesion to the substrate. From the viewpoint of thin filmization, it is preferably a design in which the substrate can be transferred to the transfer body and the substrate can be peeled off. As such a substrate, a glass substrate and a film substrate can be cited. From the viewpoint of processability, a film substrate is preferably a film substrate. From the viewpoint of continuous manufacture, a long roll film is more preferably cited. As a resin constituting the film substrate, for example, polyolefins such as polyethylene, polypropylene, and norbornene polymers can be cited; cyclic olefin resins; polyvinyl alcohol; polyethylene terephthalate; polymethacrylate; polyacrylate; cellulose esters such as triacetyl cellulose, diacetyl cellulose, and cellulose acetate propionate; polyethylene naphthalate; polycarbonate; polysulfone; polyether sulfone; polyether ketone; plastics such as polyphenylene sulfide and polyphenylene ether. The surface of the substrate can be subjected to a demolding treatment such as silicone treatment. Examples of commercially available cellulose ester substrates include "FUJITACFILM" (manufactured by Fuji Photo Film Co., Ltd.); "KC8UX2M", "KC8UY" and "KC4UY" (manufactured by Konica Minolto Opto Co., Ltd.). Such resins can be made into films by known means such as solvent casting and melt extrusion to form substrates.
[0196] Examples of commercially available cyclic olefin resins include "Topas" (registered trademark) (manufactured by Ticona (Germany)), "ARTON" (registered trademark) (manufactured by JSR Corporation), "ZEONOR" (registered trademark), "ZEONEX" (registered trademark) (manufactured by Japan ZEON Co., Ltd.), and "Apel" (registered trademark) (manufactured by Mitsui Chemicals, Inc.). Commercially available cyclic olefin resin substrates may also be used. Examples of commercially available cyclic olefin resin substrates include "Escena" (registered trademark), "SCA40" (registered trademark) (manufactured by Sekisui Chemical Co., Ltd.), "ZEONORFILM" (registered trademark) (manufactured by OPTES Co., Ltd.), and "ARTONFILM" (registered trademark) (manufactured by JSR Corporation).
[0197] The substrate preferably has a thickness that allows easy lamination of the horizontal alignment liquid crystal cured film, the horizontal alignment film, the vertical alignment liquid crystal cured film, and the vertical alignment film, and is easily peeled off. The thickness of such a substrate is usually 5 to 300 μm, preferably 20 to 200 μm.
[0198] [Phase difference plate with optical compensation function]
[0199] The retardation plate with an optical compensation function of the present invention comprises a horizontal alignment liquid crystal cured film, a horizontal alignment film or a vertical alignment film, and a vertical alignment liquid crystal cured film in this order, and satisfies the following requirements (1) to (4).
[0200] The interlayer distance between the horizontally aligned liquid crystal cured film and the vertically aligned liquid crystal cured film is 5 μm or less. ···(1)
[0201] A horizontal alignment film or a vertical alignment film is included between the layers of the horizontal alignment liquid crystal cured film and the vertical alignment liquid crystal cured film. ···(2)
[0202] Satisfies the following relationship
[0203] ReA(450) / ReA(550)<1.00···(3).
[0204] Here, ReA(λ) represents the in-plane phase difference value at the wavelength λ nm of the horizontally aligned liquid crystal cured film.
[0205] The definition of the phase difference value is as follows.
[0206] ReA(λ)=(nxA-nyA)×dA
[0207] Here, nxA represents the principal refractive index in the film plane of the horizontally aligned liquid crystal cured film, nyA represents the refractive index in the direction orthogonal to nxA in the same plane, and dA represents the thickness of the horizontally aligned liquid crystal cured film.
[0208] Satisfies the following relationship
[0209] RthC(450) / RthC(550)<1.00···(4).
[0210] Here, RthC(λ) represents the phase difference value in the thickness direction at the wavelength λ nm of the vertically aligned liquid crystal cured film. The definition of the phase difference value is as follows.
[0211] RthC(λ)=((nxC+nyC) / 2-nzC)×dC
[0212] Among them, nxC represents the principal refractive index in the film plane of the vertically aligned liquid crystal cured film, nyC represents the refractive index in the direction orthogonal to nxC in the same plane, nzC represents the refractive index in the thickness direction of the vertically aligned liquid crystal cured film, and dC represents the thickness of the vertically aligned liquid crystal cured film.
[0213] It should be noted that, when nxC=nyC, nxC can be set to the refractive index in any direction within the film surface.
[0214] In addition, the interlayer distance between the horizontally aligned liquid crystal solidified film and the vertically aligned liquid crystal solidified film is 5 μm or less, preferably 1 μm or less, more preferably 0.5 μm or less, and further preferably 0.3 μm or less, as in formula (1). In addition, the film thickness of the horizontally aligned film is preferably 1 nm or more, more preferably 5 nm or more, further preferably 10 nm or more, and particularly preferably 30 nm or more.
[0215] The phase difference plate with optical compensation function preferably satisfies the following relationship (5). In order to reduce the amount of light leakage near the oblique wavelength of 550nm when the elliptically polarizing plate with optical compensation function using the phase difference plate with optical compensation function is applied to the display, the smaller the value of |R0(550)-R40(550)|, the better. The value of |R0(550)-R40(550)| is preferably less than 10nm, more preferably less than 5nm, further preferably less than 3nm, and particularly preferably less than 2nm.
[0216] |R0(550)-R40(550)|<10nm···(5)
[0217] Here, R0(λ) represents the in-plane phase difference value of the phase difference plate with optical compensation function including the horizontally oriented liquid crystal curing film and the vertically oriented liquid crystal curing film. In addition, R40 represents the apparent phase difference value when the phase difference plate with optical compensation function including the horizontally oriented liquid crystal curing film and the vertically oriented liquid crystal curing film is rotated 40° around the direction (fast axis direction) orthogonal to the main refractive index direction in the film surface in the same plane.
[0218] The phase difference plate with optical compensation function preferably satisfies the following relationship (6). In order to reduce the amount of light leakage near the oblique wavelength of 450nm when the elliptically polarizing plate with optical compensation function using the phase difference plate with optical compensation function is used for a display, the smaller the value of |R0(450)-R40(450)|, the better. The value of |R0(450)-R40(450)| is preferably less than 10nm, more preferably less than 5nm, further preferably less than 3nm, and particularly preferably less than 2nm.
[0219] |R0(450)-R40(450)|<10nm···(6)
[0220] Among them, R0(λ) represents the in-plane phase difference value of the phase difference plate with optical compensation function including the horizontally oriented liquid crystal cured film and the vertically oriented liquid crystal cured film. In addition, R40 represents the apparent phase difference value when the phase difference plate with optical compensation function including the horizontally oriented liquid crystal cured film and the vertically oriented liquid crystal cured film is rotated 40° around the direction (fast axis direction) orthogonal to the main refractive index direction in the film surface in the same plane.
[0221] Furthermore, the difference between the values shown in relational expressions (5) and (6) preferably satisfies the following relational expression (7).
[0222] |{R0(450)-R40(450)}-{R0(550)-R40(550)}|<3nm···(7)
[0223] When the relationship (7) is satisfied, when an elliptically polarizing plate with optical compensation function using a phase difference plate with optical compensation function is applied to a display, the front and oblique reflected hue is close to black. Therefore, the value of (7) is preferably less than 3nm, more preferably less than 2nm, and further preferably less than 1nm.
[0224] In addition, when the average refractive index difference of each layer (i.e., the average refractive index of each layer of the phase difference plate with optical compensation function of the present invention, and the difference between the average refractive index of other layers adjacent to the layer) is large, light leakage sometimes occurs due to the influence of the interface reflection occurring between the layers. The average refractive index difference at a wavelength of 550nm of each layer is preferably less than 0.20, more preferably less than 0.15, further preferably less than 0.10, and particularly preferably less than 0.05. In this range, the occurrence of light leakage caused by interface reflection can be suppressed.
[0225] Specific examples of the difference in average refractive index between the layers include:
[0226] (1) The difference between the average refractive index of the horizontally aligned liquid crystal cured film and the average refractive index of the vertically aligned liquid crystal cured film;
[0227] (2) When a horizontal alignment film is included between the horizontal alignment liquid crystal cured film and the vertical alignment liquid crystal cured film,
[0228] (2-a) the difference between the average refractive index of the horizontally aligned liquid crystal cured film and the average refractive index of the horizontally aligned film,
[0229] (2-b) the difference between the average refractive index of the horizontally aligned film and the average refractive index of the vertically aligned liquid crystal cured film;
[0230] (3) When a vertical alignment film is included between the horizontal alignment liquid crystal cured film and the vertical alignment liquid crystal cured film,
[0231] (3-a) the difference between the average refractive index of the horizontally aligned liquid crystal cured film and the average refractive index of the vertically aligned film,
[0232] (3-b) the difference between the average refractive index of the vertically aligned film and the average refractive index of the vertically aligned liquid crystal cured film;
[0233] etc.
[0234] The phase difference plate with optical compensation function of the present invention may include layers other than horizontally oriented liquid crystal curing film, horizontally oriented film, vertically oriented liquid crystal curing film, and vertically oriented film, and specific examples thereof include other oriented liquid crystal curing films, other oriented films, protective layers, etc. As other oriented liquid crystal curing films, vertically oriented liquid crystal curing films and horizontally oriented liquid crystal curing films exemplified above can be cited, and as other oriented films, oriented films exemplified above can be cited.
[0235] The protective layer is preferably formed by the following protective layer-forming composition, which generally contains: a water-soluble polymer, i.e., an acrylic oligomer or polymer formed by multifunctional acrylates (methacrylates), urethane acrylates, polyester acrylates, epoxy acrylates, etc., polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polyvinyl pyrrolidone, starch, methyl cellulose, carboxymethyl cellulose, sodium alginate, etc.; and a solvent.
[0236] The solvent contained in the protective layer forming composition can include the same solvents as those exemplified above, wherein, from the aspect of not dissolving the layer forming the protective layer, it is preferably at least one solvent selected from the group consisting of water, alcohol solvents and ether solvents. As alcohol solvents, methanol, ethanol, butanol, ethylene glycol, isopropanol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether and propylene glycol monomethyl ether can be mentioned. As ether solvents, ethylene glycol monomethyl ether acetate and propylene glycol monomethyl ether acetate can be mentioned. Among them, ethanol, isopropanol, propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate are preferred.
[0237] The film thickness of the protective layer is 0.1 μm to 10 μm, more preferably 0.1 μm to 3 μm.
[0238] [Method for manufacturing a phase difference plate with an optical compensation function]
[0239] The manufacturing method of the phase difference plate with optical compensation function of the present invention is not particularly limited as long as it is a method that can stack horizontally oriented liquid crystal curing film, horizontally oriented film or vertically oriented film, and vertically oriented liquid crystal curing film in sequence, preferably: stacking a horizontally oriented film on a substrate, then stacking a horizontally oriented liquid crystal curing film, and then stacking a vertically oriented film, and then stacking a vertically oriented liquid crystal curing film (hereinafter referred to as manufacturing method A); or, stacking a vertically oriented film on a substrate, then stacking a vertically oriented liquid crystal curing film, and then stacking a horizontally oriented film, and then stacking a horizontally oriented liquid crystal curing film (hereinafter referred to as manufacturing method B). The stacking method of horizontally oriented liquid crystal curing film, horizontally oriented film, vertically oriented liquid crystal curing film, and vertically oriented film can use the above-mentioned formation method of each layer.
[0240] When manufacturing a phase difference plate with an optical compensation function using manufacturing method A or manufacturing method B, poor orientation and orientation defects may occur due to the orientation of the liquid crystal curing film disposed in the lower layer. That is, in the case of manufacturing method A, since the vertically oriented liquid crystal curing film is stacked after the horizontally oriented liquid crystal curing film is stacked in the lower layer, when the vertically oriented liquid crystal curing film is formed, it may be affected by the horizontally oriented liquid crystal curing film of the lower layer and produce poor orientation and orientation defects; in the case of manufacturing method B, similarly, the horizontally oriented liquid crystal curing film is stacked after the vertically oriented liquid crystal curing film is stacked in the lower layer, so when the horizontally oriented liquid crystal curing film is formed, it may be affected by the vertically oriented liquid crystal curing film of the lower layer and produce poor orientation and orientation defects. Therefore, according to the type of solvent used for the composition (horizontally oriented film forming composition, horizontally oriented liquid crystal curing film forming composition, vertically oriented film forming composition, vertically oriented liquid crystal curing film forming composition) to form each layer to be stacked, there is also the following situation: the lower layer is dissolved to produce changes in optical properties, poor orientation, orientation defects, etc. Therefore, it is necessary to appropriately select materials, solvents, solid content concentration, coating methods, film thickness, etc. contained in the composition used to form each layer to be laminated.
[0241] [Elliptical polarizing plate with optical compensation function]
[0242] With regard to the phase difference plate with optical compensation function of the present invention, it is transferred by being attached to the transfer body and peeling off the substrate, or being laminated by an adhesive in a state with a substrate, so that the function of the phase difference plate with optical compensation function, that is, its optical properties, can be given to the transfer body, and an optical laminate having optical properties of the phase difference plate with optical compensation function can be manufactured. Wherein, in the case of being laminated with a polarizing plate, an elliptical polarizing plate with optical compensation function can be prepared. In an embodiment of the present invention, it is preferred to laminate in such a way that the slow axis (optical axis) of the horizontally oriented liquid crystal curing film and the absorption axis of the polarizing plate are substantially 45°. By laminating in such a way that the slow axis (optical axis) of the optical film of the present invention and the absorption axis of the polarizing plate are substantially 45°, it is possible to obtain a function as a circular polarizing plate. It should be noted that the so-called substantially 45° is generally in the range of 45±5°.
[0243] [Transfer object]
[0244] As the transferred body, it can be enumerated: an optical film of a single-layer structure, such as a polarizing plate, a phase difference plate, a brightness enhancement film, an anti-glare film, an anti-reflection film, a diffusion film, a light-gathering film, etc.; an optical film of a multilayer structure, such as a phase difference plate, an elliptically polarizing plate, among which, a phase difference plate, a phase difference plate, a polarizing plate, an elliptically polarizing plate can be preferably used. The optical laminate in the present invention can be used for an image display device, such as a liquid crystal display device, an organic electroluminescent (EL) display device, an inorganic electroluminescent (EL) display device, a touch panel display device, an electron emission display device (field emission display device (FED, etc.), a surface field emission display device (SED)), an electronic paper (a display device using electronic ink, an electrophoretic element), a plasma display device, a projection type display device (grating light valve (grating light valve) (GLV) display device, a display device with a digital micromirror device (DMD), etc.) and a piezoelectric ceramic display, etc., can be particularly suitably used in an organic EL display device and a touch panel display device, etc.
[0245] [Polarizing plate]
[0246] As polarizing plate, it is formed by polarizing sheet with polarizing function. As polarizing sheet, a stretched film adsorbed with a pigment with absorption anisotropy or a film coated with a pigment with absorption anisotropy can be enumerated. As the pigment with absorption anisotropy, a dichroic pigment can be enumerated.
[0247] The stretched film adsorbed with a pigment having absorption anisotropy is usually manufactured by the following steps: a process of uniaxially stretching a polyvinyl alcohol resin film; a process of dyeing the polyvinyl alcohol resin film with a dichroic pigment so that it adsorbs the dichroic pigment; a process of treating the polyvinyl alcohol resin film adsorbed with a dichroic pigment with an aqueous boric acid solution; and a process of washing with water after treatment with an aqueous boric acid solution. A polarizing plate can be obtained by laminating the polarizer obtained in this way with a transparent protective film. As dichroic pigments, iodine and dichroic organic dyes can be cited. As dichroic organic dyes, dichroic direct dyes formed by disazo compounds such as CI Direct Red 39 and dichroic direct dyes formed by compounds such as triazo and tetrazo can be cited. As described above, the thickness of the polarizer obtained by uniaxially stretching the polyvinyl alcohol resin film, dyeing based on dichroic pigments, boric acid treatment, washing with water and drying is preferably 5μm to 40μm.
[0248] [Binder]
[0249] Examples of the adhesive include pressure-sensitive adhesives, dry-curable adhesives, and chemical-reaction adhesives. Examples of the chemical-reaction adhesive include active energy ray-curable adhesives.
[0250] Pressure-sensitive adhesives usually contain polymers and may contain solvents. Examples of polymers include acrylic polymers, silicone polymers, polyesters, polyurethanes, and polyethers. Among them, acrylic adhesives containing acrylic polymers have excellent optical transparency, appropriate wettability, cohesive force, excellent adhesion, and excellent weather resistance and heat resistance, and are not prone to floating or peeling under heating or humidification conditions, so they are preferred.
[0251] Preferred acrylic polymers include copolymers of (meth)acrylates in which the alkyl group in the ester portion is an alkyl group having 1 to 20 carbon atoms, such as methyl, ethyl or butyl, and (meth)acrylic acid, hydroxyethyl (meth)acrylate and other (meth)acrylic acid monomers having a functional group.
[0252] A pressure-sensitive adhesive containing such a copolymer is preferred because it has excellent adhesiveness and can be easily removed without leaving adhesive residue on the transfer object when it is removed after being attached to the transfer object. The glass transition temperature of the acrylic polymer is preferably 25° C. or less, more preferably 0° C. or less. The mass average molecular weight of such an acrylic polymer is preferably 100,000 or more.
[0253] As the solvent, the solvents listed above as solvents and the like can be cited. The pressure-sensitive adhesive may contain a light diffuser. The light diffuser is an additive that imparts light diffusivity to the adhesive, as long as it is microparticles having a refractive index different from the refractive index of the polymer contained in the adhesive. As the light diffuser, microparticles formed of inorganic compounds and microparticles formed of organic compounds (polymers) can be cited. Since most polymers contained in the adhesive as an effective ingredient, including acrylic polymers, have a refractive index of about 1.4 to 1.6, it is preferred to appropriately select from light diffusers with a refractive index of 1.2 to 1.8. The difference in refractive index between the polymer contained in the adhesive as an effective ingredient and the light diffuser is usually 0.01 or more, and is preferably 0.01 to 0.2 from the perspective of the brightness and display properties of the display device. The microparticles used as the light diffuser are preferably spherical and nearly monodisperse microparticles, and more preferably microparticles with an average particle size of 2 to 6 μm. The refractive index can be measured using a conventional minimum deflection angle method or an Abbe refractometer.
[0254] As microparticles formed of inorganic compounds, aluminum oxide (refractive index 1.76) and silicon oxide (refractive index 1.45) can be cited. As microparticles formed of organic compounds (polymers), melamine beads (refractive index 1.57), polymethyl methacrylate beads (refractive index 1.49), methyl methacrylate / styrene copolymer resin beads (refractive index 1.50-1.59), polycarbonate beads (refractive index 1.55), polyethylene beads (refractive index 1.53), polystyrene beads (refractive index 1.6), polyvinyl chloride beads (refractive index 1.46), and silicone resin beads (refractive index 1.46) can be cited. The content of the light diffusing agent is usually 3 to 30 parts by mass relative to 100 parts by mass of the polymer.
[0255] The thickness of the pressure-sensitive adhesive can be determined according to its adhesion, etc., and is therefore not particularly limited, and is generally 1 μm to 40 μm. In terms of processability and durability, the thickness is preferably 3 μm to 25 μm, and more preferably 5 μm to 20 μm. By making the thickness of the adhesive layer formed by the adhesive 5 μm to 20 μm, the brightness of the display device when viewed from the front and when viewed from an oblique direction can be maintained, and it is not easy to produce stains or blurs on the displayed image.
[0256] The dry curing adhesive may contain a solvent. As the dry curing adhesive, the following compositions can be cited, which contain a polymer of a monomer having a protic functional group such as a hydroxyl group, a carboxyl group or an amino group and an ethylenically unsaturated group, or a carbamate polymer as a main component, and also contain a crosslinking agent or curing compound such as a polyaldehyde, an epoxy compound, an epoxy resin, a melamine compound, a zirconium oxide compound, and a zinc compound. As the polymer of a monomer having a protic functional group such as a hydroxyl group, a carboxyl group or an amino group and an ethylenically unsaturated group, ethylene-maleic acid copolymers, itaconic acid copolymers, acrylic acid copolymers, acrylamide copolymers, saponified products of polyvinyl acetate, and polyvinyl alcohol resins can be cited.
[0257] Examples of the polyvinyl alcohol-based resin include polyvinyl alcohol, partially saponified polyvinyl alcohol, completely saponified polyvinyl alcohol, carboxyl-modified polyvinyl alcohol, acetoacetyl-modified polyvinyl alcohol, methylol-modified polyvinyl alcohol, and amino-modified polyvinyl alcohol. The content of the polyvinyl alcohol-based resin in the aqueous binder is usually 1 to 10 parts by mass, preferably 1 to 5 parts by mass, relative to 100 parts by mass of water.
[0258] Examples of the polyurethane resin include polyester-based ionomer-type polyurethane resins and the like.
[0259] The polyester ionomer polyurethane resin referred to herein refers to a polyurethane resin having a polyester skeleton and into which a small amount of ionic components (hydrophilic components) are introduced. Since the ionomer polyurethane resin is emulsified in water without using an emulsifier to form an emulsion, it can be made into a water-based adhesive. When using the polyester ionomer polyurethane resin, it is effective to add a water-soluble epoxy compound as a crosslinking agent.
[0260] As epoxy resin, polyamide epoxy resin obtained by reacting polyamide polyamine (polyamide polyamine) (which is obtained by reacting polyalkylene polyamine such as diethylenetriamine or triethylenetetramine with dicarboxylic acid such as adipic acid) with epichlorohydrin, etc. can be mentioned. Commercially available products of the polyamide epoxy resin include "SUMIREZRESIN (registered trademark) 650" and "SUMIREZRESIN 675" (both manufactured by SumikaChemtex Co., Ltd.), "WS-525" (manufactured by PMC Co., Ltd., Japan), etc. When epoxy resin is added, the amount thereof added is usually 1 to 100 parts by mass, preferably 1 to 50 parts by mass, relative to 100 parts by mass of the polyvinyl alcohol resin.
[0261] The thickness of the adhesive layer formed of a drying-curing adhesive is usually 0.001 to 5 μm, preferably 0.01 to 2 μm, and more preferably 0.01 to 0.5 μm. If the adhesive layer formed of a drying-curing adhesive is too thick, the appearance is likely to be poor.
[0262] The active energy ray-curable adhesive may contain a solvent. The so-called active energy ray-curable adhesive refers to an adhesive that is cured by being irradiated with active energy rays. Examples of active energy ray-curable adhesives include cationic polymerizable adhesives containing epoxy compounds and cationic polymerization initiators; free radical polymerizable adhesives containing acrylic curing components and free radical polymerization initiators; adhesives containing both cationic polymerizable curing components such as epoxy compounds and free radical polymerizable curing components such as acrylic compounds, and also containing cationic polymerization initiators and free radical polymerization initiators; and adhesives that do not contain these polymerization initiators and are cured by irradiation with electron beams.
[0263] Among them, free radical polymerizable active energy ray-curable adhesives containing acrylic curing components and photo-free radical polymerization initiators, and cationic polymerizable active energy ray-curable adhesives containing epoxy compounds and photo-cationic polymerization initiators are preferred. As acrylic curing components, (meth)acrylates such as methyl (meth)acrylate and hydroxyethyl (meth)acrylate and (meth)acrylic acid can be cited. The active energy ray-curable adhesive containing epoxy compounds can also contain compounds other than epoxy compounds. As compounds other than epoxy compounds, oxetane compounds, acrylic compounds, etc. can be cited.
[0264] Examples of the photoradical polymerization initiator and the photocationic polymerization initiator include the above-mentioned photoradical polymerization initiators and the photocationic polymerization initiators. The content of the radical polymerization initiator and the cationic polymerization initiator is usually 0.5 to 20 parts by mass, preferably 1 to 15 parts by mass, relative to 100 parts by mass of the active energy ray-curable adhesive.
[0265] The active energy ray-curable adhesive may further contain an ion trapping agent, an antioxidant, a chain transfer agent, a tackifier, a thermoplastic resin, a filler, a flow regulator, a plasticizer, a defoaming agent, and the like.
[0266] In this specification, the so-called active energy ray is defined as an energy ray that can decompose a compound that can generate active species to generate active species. Such active energy rays include visible light, ultraviolet rays, infrared rays, X-rays, α rays, β rays, γ rays and electron beams, preferably ultraviolet rays and electron beams. The preferred ultraviolet irradiation conditions are the same as those for the polymerization of the above-mentioned polymerizable liquid crystal compound.
[0267] Example
[0268] Hereinafter, the present invention will be described in more detail using examples. It should be noted that the "%" and "parts" in the examples refer to mass % and mass parts unless otherwise specified. In addition, in the following examples, the film thickness is measured using an ellipsometer M-220 manufactured by JASCO Corporation, or a contact film thickness meter (MH-15M, Counter TC101, MS-5C manufactured by Nikon Corporation). In addition, the phase difference value Rth (λ) in the thickness direction, the in-plane phase difference value Re (λ), and the apparent phase difference value R40 (λ) when measured from the 40° direction are measured and calculated using KOBRA-WPR manufactured by Oji Testing Instruments Co., Ltd. or an ellipsometer M-220 manufactured by JASCO Corporation. In addition, the Si / C ratio can be calculated by elemental analysis of the vertically oriented film, by measuring the surface constituent elements using X-ray photoelectric spectroscopy; or, when the structural formula of the compound used to form the vertically oriented film is fully known, it can be calculated from the structural formula. The corona treatment apparatus used was AGF-B10 manufactured by Kasuga Electric Co., Ltd. The corona treatment can be appropriately performed when the composition is applied to the substrate. The corona treatment apparatus was used and the treatment was performed once under the conditions of an output of 0.3 kW and a treatment speed of 3 m / min.
[0269] [Example 1]
[0270] [Preparation of composition for forming horizontal alignment film]
[0271] As components, 5 parts of a photo-alignment material having the following structure (weight average molecular weight: 30,000) and 95 parts of cyclopentanone (solvent) were mixed, and the obtained mixture was stirred at 80° C. for 1 hour to obtain a composition for forming a horizontal alignment film.
[0272]
[0273] [Preparation of a composition for forming a vertical alignment film]
[0274] A silane coupling agent "KBE-9103" manufactured by Shin-Etsu Chemical Co., Ltd. was dissolved in a mixed solvent of ethanol and water at a ratio of 9:1 (mass ratio) to obtain a vertical alignment film-forming composition having a solid content of 0.5%.
[0275] [Preparation of a composition for forming a horizontally aligned liquid crystal cured film and a composition for forming a vertically aligned liquid crystal cured film]
[0276] To a mixture obtained by mixing the polymerizable liquid crystal compound A and the polymerizable liquid crystal compound B shown below in a mass ratio of 90:10, 1.0 part of a leveling agent (F-556; manufactured by DIC Corporation) and 6 parts of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)-1-butanone ("Irgacure 369 (Irg369)", manufactured by BASF JAPAN Co., Ltd.) as a polymerization initiator were added.
[0277] Furthermore, N-methyl-2-pyrrolidone (NMP) was added so that the solid content concentration might become 13%, and it stirred at 80 degreeC for 1 hour, and obtained the horizontal alignment liquid crystal cured film formation composition and the vertical alignment liquid crystal cured film formation composition.
[0278] The polymerizable liquid crystal compound A was produced by the method described in Japanese Unexamined Patent Publication No. 2010-31223. The polymerizable liquid crystal compound B was produced by the method described in Japanese Unexamined Patent Publication No. 2009-173893. The molecular structures of each are shown below.
[0279] [Polymerizable liquid crystal compound A]
[0280]
[0281] [Polymerizable liquid crystal compound B]
[0282]
[0283] 〔Manufacturing of polarizing plates〕
[0284] After immersing a polyvinyl alcohol film having an average degree of polymerization of about 2,400, a saponification degree of 99.9 mol% or more, and a thickness of 75 μm in pure water at 30°C, it is immersed in an aqueous solution having a mass ratio of iodine / potassium iodide / water of 0.02 / 2 / 100 at 30°C for iodine dyeing (iodine dyeing process). The polyvinyl alcohol film that has undergone the iodine dyeing process is immersed in an aqueous solution having a mass ratio of potassium iodide / boric acid / water of 12 / 5 / 100 at 56.5°C for boric acid treatment (boric acid treatment process). After washing the polyvinyl alcohol film that has undergone the boric acid treatment process with pure water at 8°C, it is dried at 65°C to obtain a polarizer with iodine adsorbed and oriented in polyvinyl alcohol (the thickness after stretching is 27 μm). At this time, stretching is performed in the iodine dyeing process and the boric acid treatment process. The total stretching ratio in this stretching is 5.3 times. The polarizer obtained is bonded to a saponified triacetyl cellulose film (KC4UYTAC 40μm manufactured by Konica Minolto) using a clamping roller via an aqueous adhesive. While the tension of the obtained bond is maintained at 430N / m, it is dried at 60°C for 2 minutes to obtain a polarizer having a triacetyl cellulose film as a protective film on one side. It should be noted that the aqueous adhesive is prepared by adding 3 parts of carboxyl-modified polyvinyl alcohol (manufactured by Kuraray, "Kuraray PovalKL318") and 1.5 parts of a water-soluble polyamide epoxy resin (manufactured by Sumika Chemtex, "Sumirez Resin 650", an aqueous solution with a solid content concentration of 30%) to 100 parts of water.
[0285] The optical properties of the obtained polarizing plate were measured. The measurement was carried out using a spectrophotometer ("V7100", manufactured by JASCO Corporation) with the polarizer surface of the polarizing plate obtained above as the incident surface. The absorption axis of the polarizing plate was consistent with the stretching direction of the polyvinyl alcohol. The visibility-corrected single transmittance of the obtained polarizing plate was 42.1%, the visibility-corrected polarization degree was 99.996%, the single hue a was -1.1, and the single hue b was 3.7.
[0286] [Manufacturing of a laminate comprising a substrate, a horizontal alignment film, and a horizontal alignment liquid crystal cured film]
[0287] After corona treatment on a COP film (ZF-14-50) manufactured by ZEON Co., Ltd. of Japan, the horizontal alignment film forming composition was applied by a bar coater, dried at 80°C for 1 minute, and irradiated with a polarized UV light device ("SPOT CURE SP-9", manufactured by Ushio Electric Co., Ltd.) at a wavelength of 313 nm with a cumulative light intensity of 100 mJ / cm 2 Polarized UV exposure was performed at an axis angle of 45° under the conditions of . The film thickness of the obtained horizontally oriented film was measured with an ellipsometer and found to be 100 nm.
[0288] Next, the horizontal alignment liquid crystal curable film-forming composition was applied onto the horizontal alignment film using a bar coater, dried at 120° C. for 1 minute, and then irradiated with ultraviolet light (under a nitrogen atmosphere, cumulative light intensity at a wavelength of 365 nm: 500 mJ / cm 2 ), thereby forming a horizontally aligned liquid crystal cured film, and obtaining a laminate including a substrate, a horizontally aligned film, and a horizontally aligned liquid crystal cured film. The film thickness of the horizontally aligned liquid crystal cured film was measured with an ellipsometer, and the result was 2.3 μm.
[0289] 〔Re measurement of horizontally aligned liquid crystal cured film〕
[0290] The in-plane retardation value ReA(λ) of the horizontally aligned liquid crystal cured film manufactured by the above method was measured by a measuring machine ("KOBRA-WPR", manufactured by Oji Instruments Co., Ltd.) after bonding to glass via an adhesive. The retardation value ReA(λ) at each wavelength was measured as follows: ReA(450) = 121 nm, ReA(550) = 142 nm, ReA(650) = 146 nm, ReA(450) / ReA(550) = 0.85.
[0291] [Manufacturing of a laminate comprising a substrate, a horizontal alignment film, a horizontal alignment liquid crystal cured film, a vertical alignment film, and a vertical alignment liquid crystal cured film]
[0292] After corona treatment was performed on the laminate including the substrate, the horizontal alignment film and the horizontal alignment liquid crystal cured film produced by the above method, a vertical alignment film-forming composition was applied by a bar coater and dried at 80° C. for 1 minute to obtain a vertical alignment film. The film thickness of the obtained vertical alignment film was measured by an ellipsometer and found to be 50 nm.
[0293] Furthermore, the vertical alignment film was coated with a composition for forming a vertical alignment liquid crystal curable film using a bar coater, dried at 120° C. for 1 minute, and then irradiated with ultraviolet rays (in a nitrogen atmosphere, the cumulative light amount at a wavelength of 365 nm: 500 mJ / cm 2 ), thereby forming a vertically oriented liquid crystal cured film, and obtaining a laminate comprising a substrate, a horizontally oriented film, a horizontally oriented liquid crystal cured film, a vertically oriented film, and a vertically oriented liquid crystal cured film. The film thickness of the vertically oriented liquid crystal cured film was measured by an ellipsometer, and the result was 1.2 μm. In addition, the interlayer distance between the horizontally oriented liquid crystal cured film and the vertically oriented liquid crystal cured film was 50 nm. In addition, the constituent element ratio of the vertically oriented film was Si / C=0.33.
[0294] [Rth measurement of vertically aligned liquid crystal cured film]
[0295] In order to measure the Rth of the vertically oriented liquid crystal curing film, the same steps as above are used to manufacture the vertically oriented film and the vertically oriented liquid crystal curing film on the COP film (ZF-14-50) made by ZEON Co., Ltd. of Japan, and the vertically oriented liquid crystal curing film is bonded to the glass via an adhesive (pressure-sensitive adhesive 15μm made by Lintec). After confirming that there is no phase difference in COP, the phase difference value is measured by changing the incident angle of light to the sample using an ellipsometer. In addition, the average refractive index at the wavelength λ of 450nm and 550nm is measured using a refractometer (made by Atago Co., Ltd., "Multi-wavelength Abbe Refractometer DR-M4"). The ReC calculated based on the obtained film thickness, average refractive index, and the measurement results of the ellipsometer are:
[0296] RthC(450)=-63nm, RthC(550)=-73nm, RthC(450) / RthC(550)
[0297] =0.85.
[0298] [Measurement of R0 and R40 of a laminate (retardation plate with optical compensation function) comprising a horizontally aligned liquid crystal cured film, a vertically aligned film, and a vertically aligned liquid crystal cured film]
[0299] Through an adhesive (pressure-sensitive adhesive 15 μm manufactured by Lintec), a laminate comprising a substrate, a horizontally oriented film, a horizontally oriented liquid crystal curing film, a vertically oriented film, and a vertically oriented liquid crystal curing film manufactured by the above method was bonded to glass, and the COP was peeled off to prepare a sample for measurement. Then, after confirming that there was no phase difference between the horizontally oriented film and the vertically oriented film, the phase difference value R0 (λ) in the front direction of the phase difference plate with an optical compensation function and the phase difference value R40 (λ) when tilted 40° with the fast axis of the horizontally oriented liquid crystal curing film as the center were measured using KOBRA-WPR. |R0(550)-R40(550)|, |R0(450)-R40(450)|, and |{R0(450)-R40(450)}-{R0(550)-R40(550)}| were calculated based on the obtained values of R0(λ) and R40(λ), and the obtained results are shown in Table 1.
[0300] [Difference in average refractive index of each layer in the plane]
[0301] Each layer was coated on glass according to the above method, and the average refractive index of each layer was calculated using a refractometer ("Multi-wavelength Abbe Refractometer DR-M4" manufactured by Atago Co., Ltd.) or ellipsometry, and it was confirmed that the difference in the average refractive index in the plane of each layer was 0.2 or less.
[0302] 〔Flexibility test〕
[0303] A 0.7 mm thick glass plate was placed on the coating surface side of the laminate comprising a substrate, a horizontal alignment film, a horizontal alignment liquid crystal cured film, a vertical alignment film, and a vertical alignment liquid crystal cured film prepared by the above method, and the laminate was bent 180 degrees in a manner of lying on the glass plate, and then a 10x magnifying glass was used to transmit light from a fluorescent lamp, and the bent portion was observed to confirm the presence or absence of wrinkles. The results are shown in Table 1.
[0304] [Confirmation of the reflected color of the curved part]
[0305] After the coating surface side of the laminate comprising a substrate, a horizontal alignment film, a horizontal alignment liquid crystal curing film, a vertical alignment film, and a vertical alignment liquid crystal curing film prepared by the above method is subjected to corona treatment, the absorption axis of the polarizing plate and the slow axis of the horizontal alignment film are made to form an angle of 45°, and the substrate is peeled off by an adhesive to prepare an elliptically polarizing plate with an optical compensation function. Afterwards, it is attached to the aluminum foil via an adhesive, and the polarizing plate side is bent 180° in a manner of a radius of 1 cm, and the reflected hue of the bent portion is visually observed. The results are shown in Table 1. It should be noted that the polarizing plate used in this test is prepared as follows.
[0306] (Examples 2 and 3)
[0307] A retardation plate with an optical compensation function was prepared in the same manner as in Example 1 except that the thickness of the vertical alignment film was changed as described in Table 1, and retardation value measurement, bendability test, and reflection hue confirmation of the bent portion were carried out.
[0308] (Example 4)
[0309] 0.5 wt % of polyimide ("SUNEVER SE-610", manufactured by Nissan Chemical Industry Co., Ltd.), 72.3 wt % of N-methyl-2-pyrrolidone, 18.1 wt % of 2-butoxyethanol, 9.1 wt % of ethylcyclohexane, and 0.01 wt % of DPHA (manufactured by Shin-Nakamura Chemical) were mixed to prepare a vertically oriented film-forming composition B. The vertically oriented film-forming composition B was used. In addition, a phase difference plate with an optical compensation function was prepared in the same manner as in Example 1, and phase difference value measurement, bending test, and reflection hue confirmation of the bent portion were performed. The results are shown in Table 1. It should be noted that the film thickness of the vertically oriented film was measured with an ellipsometer, and the result was 0.2 μm. It can be seen that the interlayer distance between the horizontally oriented liquid crystal curing film and the vertically oriented liquid crystal curing film is 0.2 μm. In addition, it was confirmed that when the vertically oriented liquid crystal curing film-forming composition was applied, the vertically oriented film was eroded by the solvent, and orientation defects and poor orientation were locally generated.
[0310] (Example 5)
[0311] The substrate was changed to a polyethylene terephthalate film (SP-PLR382050 manufactured by Lintec (Strain), hereinafter referred to as "diaphragm") to which a demolding treatment was implemented, and the stacking order was changed to the order of vertically oriented film, vertically oriented liquid crystal curing film, horizontally oriented film, and horizontally oriented liquid crystal curing film. In addition, a phase difference plate with an optical compensation function was prepared in the same manner as in Example 1, and phase difference value measurement, bending test, and reflection hue confirmation of the bent portion were performed. The results are shown in Table 1. It should be noted that the film thickness of the horizontally oriented film was measured with an ellipsometer, and the result was 0.2 μm. It can be seen that the interlayer distance between the horizontally oriented liquid crystal curing film and the vertically oriented liquid crystal curing film is 0.2 μm.
[0312] (Comparative Example 1)
[0313] The composition for forming a vertically aligned liquid crystal cured film was changed to the composition for forming a vertically aligned liquid crystal cured film (B) described below, and the drying temperature after applying the composition for forming a vertically aligned liquid crystal cured film (B) was changed from 120°C to 80°C. A phase difference plate with an optical compensation function was prepared in the same manner as described in Example 1, and a phase difference value measurement, a bendability test, and a reflection hue confirmation of a bent portion were performed. The results are shown in Table 1.
[0314] (Preparation of a Homeotropically Aligned Liquid Crystal Cured Film-Forming Composition (B))
[0315] To the following liquid crystal compound LC242: Paliocolor LC242 (registered trademark of BASF), 0.1 parts of leveling agent F-556 and 3 parts of polymerization initiator Irg369 were added, and cyclopentanone was added in such a way that the solid content concentration became 13%, thereby obtaining a composition (B) for forming a vertically aligned liquid crystal cured film. The obtained liquid crystal composition was named "Composition V".
[0316] Liquid crystal compound LC242: Paliocolor LC242 (registered trademark of BASF)
[0317]
[0318] After manufacturing a laminate of a horizontally oriented film and a horizontally oriented liquid crystal curing film by the method described in Example 1, a laminate of a vertically oriented film and a vertically oriented liquid crystal curing film (manufactured by Lintec) was prepared on COP by the same method as in Example. The obtained laminates were bonded to each other with an adhesive (pressure-sensitive adhesive 15 μm manufactured by Lintec) to prepare a phase difference plate with an optical compensation function. Phase difference value measurement, bendability test, and reflection hue confirmation of the bent portion were performed. The results are shown in Table 1.
[0319] [Table 1]
[0320]
[0321] It is found that when the elliptically polarizing plate with optical compensation function using the phase difference plate with optical compensation function of Examples 1 to 5 is applied to a flexible display and then bent, the change in reflection hue at the bent portion is reduced.
Claims
1. A phase difference plate with an optical compensation function, which is a laminate comprising a horizontally aligned liquid crystal cured film and a vertically aligned liquid crystal cured film, The horizontally aligned liquid crystal cured film is formed by curing a composition containing a polymerizable liquid crystal compound in a state where the composition is aligned in a horizontal direction relative to the film surface. The vertically aligned liquid crystal cured film is formed by curing a composition containing a polymerizable liquid crystal compound in a state where the composition is aligned in a vertical direction relative to the film surface. The phase difference plate with optical compensation function satisfies the following relations (1) to (4) and (23): The interlayer distance between the horizontally aligned liquid crystal cured film and the vertically aligned liquid crystal cured film is 5 μm or less. (1) A vertical alignment film is included between the layers of the horizontal alignment liquid crystal cured film and the vertical alignment liquid crystal cured film. (2) ReA(450) / ReA(550)<1.00 · · · (3) RthC(450) / RthC(550)<1.00 ··· (4) 1.00≤ReA(650) / ReA(550) ··· (23) In formula (3), ReA(λ) represents the in-plane phase difference value of the horizontally aligned liquid crystal cured film at a wavelength of λ nm, The definition of the in-plane phase difference value ReA(λ) is as follows: ReA(λ)=(nxA(λ)-nyA(λ))×dA in, nxA(λ) represents the principal refractive index within the film surface of the horizontally aligned liquid crystal cured film with respect to light of wavelength λ (nm), nyA(λ) represents the refractive index for light of wavelength λ (nm) in a direction orthogonal to nxA(λ) in the same plane. dA represents the thickness of the horizontally aligned liquid crystal cured film; In formula (4), RthC(λ) represents the phase difference value in the thickness direction at a wavelength of λ nm of the vertically aligned liquid crystal cured film. The phase difference value RthC(λ) is defined as follows: RthC(λ)=((nxC(λ)+nyC(λ)) / 2-nzC(λ))×dC Here, nxC(λ) represents the principal refractive index within the film plane of the vertically aligned liquid crystal cured film with respect to light of wavelength λ (nm), nyC(λ) represents the refractive index for light of wavelength λ (nm) in a direction orthogonal to nxC(λ) in the same plane. nzC(λ) represents the refractive index of the vertically aligned liquid crystal cured film in the thickness direction with respect to light of wavelength λ (nm), dC represents the thickness of the vertically aligned liquid crystal cured film, The vertical alignment film disposed between the horizontal alignment liquid crystal cured film and the vertical alignment liquid crystal cured film is a film formed of a compound containing Si, C and O as constituent elements, and the molar ratio of Si to C, i.e. Si / C, is 0.03 to 1.
00.
2. The phase difference plate with optical compensation function according to claim 1, which is a laminate comprising a horizontally aligned liquid crystal cured film and a vertically aligned liquid crystal cured film, and satisfies the following relationship (5): |R0(550)-R40(550)|<10nm ··· (5) in, R0(λ) represents the in-plane phase difference value of the phase difference plate with an optical compensation function including the horizontal alignment liquid crystal cured film and the vertical alignment liquid crystal cured film with respect to light of wavelength λ (nm), In addition, R40(λ) represents the apparent phase difference value when the phase difference plate with optical compensation function including a horizontally oriented liquid crystal solid film and a vertically oriented liquid crystal solid film is rotated 40° around the direction orthogonal to the main refractive index direction in the film surface in the same plane, that is, the fast axis direction, and is the phase difference value relative to the light of wavelength λ (nm).
3. The phase difference plate with optical compensation function according to claim 1 or 2, which is a laminate comprising a horizontally aligned liquid crystal cured film and a vertically aligned liquid crystal cured film, and satisfies the relationship (6) shown below, |R0(450)-R40(450)|<10nm ··· (6) in, R0(λ) represents the in-plane phase difference value of the phase difference plate with an optical compensation function including the horizontal alignment liquid crystal cured film and the vertical alignment liquid crystal cured film with respect to light of wavelength λ (nm), In addition, R40(λ) represents the apparent phase difference value when the phase difference plate with optical compensation function including a horizontally oriented liquid crystal solid film and a vertically oriented liquid crystal solid film is rotated 40° around the direction orthogonal to the main refractive index direction in the film surface in the same plane, that is, the fast axis direction, and is the phase difference value relative to the light of wavelength λ (nm).
4. The phase difference plate with optical compensation function according to claim 1 or 2, which is a laminate comprising a horizontally aligned liquid crystal cured film and a vertically aligned liquid crystal cured film, and satisfies the following relationship (7), |{R0(450)-R40(450)}-{R0(550)-R40(550)}|<3nm···(7) in, R0(λ) represents the in-plane phase difference value of the phase difference plate with an optical compensation function including the horizontal alignment liquid crystal cured film and the vertical alignment liquid crystal cured film with respect to light of wavelength λ (nm), In addition, R40(λ) represents the apparent phase difference value when the phase difference plate with optical compensation function including a horizontally oriented liquid crystal solid film and a vertically oriented liquid crystal solid film is rotated 40° around the direction orthogonal to the main refractive index direction in the film surface in the same plane, that is, the fast axis direction, and is the phase difference value relative to the light of wavelength λ (nm).
5. The phase difference plate with optical compensation function according to claim 1 or 2, wherein: The average refractive index difference at a wavelength of 550 nm of the horizontal alignment liquid crystal cured film, the vertical alignment liquid crystal cured film, and the horizontal alignment film or the vertical alignment film is 0.20 or less.
6. The phase difference plate with optical compensation function according to claim 1 or 2, wherein: A horizontal alignment film is included between the horizontal alignment liquid crystal cured film and the vertical alignment liquid crystal cured film, and the horizontal alignment film is a photo alignment film.
7. The phase difference plate with optical compensation function according to claim 1 or 2, wherein: A horizontal alignment film is included between the horizontal alignment liquid crystal cured film and the vertical alignment liquid crystal cured film, and the horizontal alignment film includes a cinnamoyl group.
8. The phase difference plate with optical compensation function according to claim 1 or 2, wherein: A vertical alignment film is included between the horizontal alignment liquid crystal cured film and the vertical alignment liquid crystal cured film, and the film thickness of the vertical alignment film is 30 nm or more and 1 μm or less. 9 . An elliptically polarizing plate, comprising a laminate of the phase difference plate with an optical compensation function according to claim 1 and a polarizing plate. 10 . An organic EL display device comprising the elliptically polarizing plate according to claim 9 .