Method for improving the storage stability and / or transport stability of polymers
The unnecessary crossover of the polymer during storage and transportation is solved by mixing ethylene and C4 to C12α olefin comonomers with the comonomers of hydrolyzable silane groups and combining them with specific stabilizers to form a stable polymer composition. The problem of connecting the material achieves long-term stability and characteristics maintenance.
Patent Information
- Application Number
- CN202080076357.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-06
- Filing Date
- 2020-09-02
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-09-02
AI Technical Summary
The prior art is difficult to effectively prevent unnecessary crosslinking of polymers containing hydrolyzable silane groups during storage and transportation, resulting in changes in material characteristics and reduced stability.
A mixture of ethylene and a copolymer of C4 to C12α olefin comonomer and a comonomer containing hydrolyzable silane groups is adopted, and stabilized with sterically hindered phenol, alkyl trialkoxysilane or alkenyl trialkoxysilane. The combination of agents forms a stable polymer composition stored in a container with a barrier layer to prevent penetration of moisture and oxygen.
It significantly improves the storage and transportation stability of polymers, extends the service life of the material, prevents unnecessary crosslinking and changes in characteristics, and ensures the stability of the material over a long period of time.
Smart Images

Figure BDA0003622542750000101 
Figure BDA0003622542750000111 
Figure BDA0003622542750000121
Abstract
Description
[0001] The present invention relates to a method for increasing the storage stability and / or transport stability of polymers containing hydrolyzable silane groups. In addition, the present invention relates to the use of specific stabilizers for increasing the storage stability and / or transport stability of these compositions in containers having a barrier layer.
[0002] Polymers containing hydrolyzable silane groups are in demand in a wide variety of applications, including cable jacketing, shoe soles and sealing materials. Hydrolyzable silane groups allow crosslinking of polymers and significantly change their properties. Often crosslinking is not carried out directly after production, but at a different location days or weeks later. Usually, crosslinking is initiated by a condensation catalyst, but in the absence of added catalysts crosslinking occurs slowly and leads to an unnecessary increase in melt viscosity and gel formation within the material, limiting the time the material remains available for further conversion. It is therefore necessary to prevent unwanted crosslinking after polymer production.
[0003] Methods for suppressing unwanted crosslinking directly during and after the manufacture of polymers comprising hydrolyzable groups are known in the art.
[0004] WO 90 / 07542 A1 relates to a crosslinkable polymer composition comprising an olefin copolymer or graft copolymer having hydrolyzable silane groups and a silanol condensation catalyst, and a silane compound having at least one hydrolyzable organic group. The polymer composition is characterized in that the silane compound has a compatibility with the polymer composition of at least 0.035 mol of hydrolyzable groups per 100 g of the polymer composition, and the silane compound is represented by the following general formula: R 1 (SiR 2 n X 3-n ) m , where R 1 is a monofunctional hydrocarbon group having 13 to 30 carbon atoms, or a difunctional hydrocarbon group having 4 to 24 carbon atoms, R 2 is a hydrocarbon group having 1 to 10 carbon atoms, X is a hydrolyzable organic group, n is 0, 1 or 2, and m is 1 or 2.
[0005] EP 0 193 317 A2 relates to a silane-crosslinkable polymer composition comprising (A) 100 parts by weight of a copolymer prepared by extensively polymerizing under high pressure a polymerizable monomer mixture consisting essentially of ethylene and an ethylenically unsaturated silane compound having a hydrolyzable organic group, and (B) 0.001 to 10 parts by weight of a silanol condensation catalyst, characterised in that the unsaturated silane compound is present in an amount of 0.1 to 5.
[0006] Known methods utilizing specific stabilizers are not suitable for long-term stabilization, and there remains a need for methods which allow stabilization of polymers comprising hydrolyzable groups over long periods of time.
[0007] It is an object of the present invention to provide a process which allows the storage and / or transport of polymers comprising hydrolysable silane groups.
[0008] This object has been solved by a method for improving the storage stability and / or transport stability of a polymer (A) according to claim 1 of the present invention, said method comprising at least the following steps:
[0009] a) providing a polymer (A) selected from the group consisting of ethylene and C4 to C 12 Copolymers of alpha-olefin comonomers, propylene copolymers and mixtures thereof which additionally contain comonomer units comprising hydrolyzable silane groups;
[0010] b) providing a stabilizer (B) selected from the group consisting of hindered phenols, alkyltrialkoxysilanes, alkenyltrialkoxysilanes, and mixtures thereof;
[0011] c) mixing the polymer (A) and the stabilizer (B) to obtain a stable polymer composition (I); and
[0012] d) transferring said stabilized polymer composition (I) obtained in step c) into a container comprising at least one barrier layer.
[0013] Surprisingly, it has been found that the specific combination of two stabilization measures according to claim 1 , namely a barrier layer and a stabilizer, allows for effective long-term stabilization of polymers.
[0014] Advantageous embodiments of the method according to the invention are specified in dependent claims 2 to 13 .
[0015] Claim 14 of the present invention relates to the use of a stabilizer (B) selected from the group consisting of sterically hindered phenols, alkyltrimethoxysilanes, alkenyltrimethoxysilanes and mixtures thereof for improving the storage stability and / or transportation stability of a polymer (A), wherein the polymer (A) is selected from the group consisting of ethylene and C4 to C 12 Copolymers of alpha-olefin comonomers, propylene copolymers and mixtures thereof further comprising comonomer units comprising hydrolysable silane groups; whereby the transport or storage of polymer (A) is carried out in a container having at least one barrier layer against moisture.
[0016] Claims 15 and 16 specify preferred embodiments of the use according to the invention.
[0017] definition
[0018] The polymer composition according to the invention comprises components (A) (=polymer) and (B) (=stabilizer) and optionally further components, such as polymers different from component (A), additives, fillers or reinforcing agents. The requirement applicable here is that components (A) and (B) and further components (if present) add up to a total of 100 wt. %. Fixed ranges indicated for the quantities of the individual components (A) and (B) and optional further components are to be understood as such that any quantity of each individual component can be selected within the specified range, provided that the strict stipulation is met such that the sum of all components (A) and (B) and optional further components adds up to 100 wt. %. In addition, it is preferred that components (A) and (B) form at least 50 wt. %, more preferably at least 90 wt. % of the polymer composition.
[0019] For the purposes of this description and the subsequent claims, a barrier layer is a layer constructed to be a barrier to moisture and preferably to oxygen, preferably not more than 10 ppm and more preferably 0 to 5 ppm of water and / or oxygen can diffuse through the barrier layer.
[0020] Where the term "comprising" is used in the present description and claims, other non-specified elements of major or minor functional importance are not excluded. For the purposes of the present invention, the term "consisting of" is considered a preferred embodiment of the term "comprising..." If a group is defined hereinafter as comprising at least a certain number of embodiments, this is also to be understood as disclosing a group that preferably consists only of these embodiments.
[0021] Whenever the terms "including" or "having" are used, these terms are intended to be equivalent to "comprising" as defined above.
[0022] Where an indefinite or definite article is used when referring to a singular noun, for example "a", "an" or "the", this includes a plural of that noun unless something else is specifically stated.
[0023] method
[0024] In the following, preferred embodiments of the method according to the invention will be discussed.
[0025] A preferred embodiment of the method according to the invention provides that the container in step d) is selected from the group consisting of bags, sacks, big bags, boxes, bins, barrels, buckets, drums and cans, and is preferably a bag.
[0026] Preferably, step d) of the process according to the invention is carried out before transport and / or storage of the polymer composition (I).
[0027] The barrier layer of the container may be made of any material having a barrier effect against moisture and preferably also against oxygen. According to a preferred embodiment of the method according to the invention, the at least one barrier layer of the container comprises and preferably consists of a material selected from the group consisting of: metal, preferably aluminum or vacuum metallized polyester; HDPE; ethylene vinyl alcohol; polyvinyl chloride; polyvinylidene chloride and mixtures thereof; and more preferably consists of aluminum.
[0028] The barrier layer preferably has a thickness in the range of 1 to 300 μm and preferably 5 to 200 μm.
[0029] In a further preferred embodiment of the process according to the invention, polymer (A) is a copolymer of ethylene and 1-octene having a density measured according to ISO 1183 of 850 kg / m 3 Up to 920kg / m 3 In the range of 850 to 880 kg / m 3 and more preferably in the range of 855 to 870 kg / m 3 within the range.
[0030] Yet another preferred embodiment of the process according to the invention provides that polymer (A) is a copolymer of ethylene and 1-octene and a base polymer without hydrolyzable silane groups, having an MFR2 measured according to ISO 1133 at 190° C. and a loading of 2.16 kg in the range of 0.1 to 20.0 g / 10 min, preferably in the range of 0.1 to 5 g / 10 min, more preferably in the range of 0.5 to 4.0 g / 10 min and still more preferably in the range of 0.2 to 1.2 g / 10 min.
[0031] Another preferred embodiment of the process according to the invention provides that polymer (A) is a copolymer of ethylene and 1-octene and a polymer comprising hydrolyzable silane groups, having an MFR5 measured according to ISO 1133 at 190° C. and a loading of 5.0 kg in the range of 0.1 to 30.0 g / 10 min, preferably in the range of 0.1 to 20 g / 10 min and more preferably in the range of 0.2 to 10 g / 10 min.
[0032] According to a further preferred embodiment of the process according to the invention, polymer (A) comprises comonomer units of hydrolyzable silane groups which have been introduced by grafting or copolymerization and preferably by peroxide-initiated grafting.
[0033] In another preferred embodiment of the present invention, the hydrolyzable silane groups in polymer (A) are derived from alkenyl alkoxysilanes, preferably selected from the group consisting of vinyl trimethoxysilane, vinyl triethoxysilane, vinyl tripropoxysilane, γ-(meth)acryloxypropyl trimethoxysilane, γ-(meth)acryloxypropyl triethoxysilane and vinyl triacetoxysilane and mixtures thereof, of which vinyl trimethoxysilane is most preferred. Those skilled in the art will be fully aware that the raw materials used to introduce hydrolyzable silane groups in polymer (A) may at least partially change their structure during the introduction into polymer (A). For example, vinyl trimethoxysilane may be incorporated into polymer (A) via a free radical process and no vinyl group is present in the final polymer (A).
[0034] According to a further preferred embodiment of the present invention, the stabilizer (B) is an alkyltrialkoxysilane represented by the general formula (1):
[0035] R 1 (SiR 2 n X 3-n ) m (1)
[0036] in
[0037] R 1 is a monofunctional hydrocarbon group having 2 to 30 carbon atoms, preferably 6 to 30 carbon atoms and more preferably 13 to 30 carbon atoms or a difunctional hydrocarbon group having 4 to 24 carbon atoms, and is preferably a hexadecyl group;
[0038] R 2 may be the same or different and are hydrocarbon groups having 1 to 10 carbon atoms;
[0039] X may be the same or different and are alkoxy, preferably are the same alkoxy, and more preferably are the same and are methoxy;
[0040] n is 0, 1 or 2, and is preferably 0;
[0041] m is 1 or 2.
[0042] A particularly preferred stabilizer (B) is hexadecyltrimethoxysilane. A great advantage of this material is that it has a low vapor pressure and therefore does not disappear from the polymer composition by evaporation.
[0043] Yet another preferred embodiment of the present invention provides that the stabilizer (B) is a hindered phenol selected from the group consisting of pentaerythritol tetrakis(3-(3',5'-di-tert-butyl-4-hydroxyphenyl)-propionate, octadecyl 3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate, 2,2'-thiodiethylenebis-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionate, 1,3,5-tris(3',5'-di-tert-butyl-4'-hydroxybenzyl)isocyanurate, 4,4'-thiobis(2-tert-butyl-5-methylphenol) and mixtures thereof.
[0044] In a further preferred embodiment of the present invention, the amount of hydrolyzable silane groups in polymer (A) is in the range of 0.5 to 5.0 wt.-%, preferably in the range of 0.5 to 3.0 wt.-%, more preferably in the range of 1.0 to 2.0 wt.-% and still more preferably in the range of 1.2 to 1.8 wt.-%, based on the total weight of polymer (A). Lower amounts of hydrolyzable silane groups will make it difficult to achieve a high degree of crosslinking of the polymer, and for higher amounts of hydrolyzable silane groups it will be difficult to stabilize the polymer.
[0045] In another preferred embodiment of the present invention, the polymer composition (I) comprises 95.0 to 99.99% by weight, preferably 97.0 to 99.9% by weight of the polymer (A) and 0.01 to 5.0% by weight, preferably 0.1 to 3.0% by weight of the stabilizer (B); whereby the polymer (A) and the stabilizer (B) total 100% by weight.
[0046] Lower amounts of stabilizer (B) will not allow effective stabilization of polymer (A) and higher amounts will make it difficult to crosslink polymer (A).
[0047] According to a further preferred embodiment of the present invention, the polymer composition (I) comprises 97.0 to 99.5 wt %, preferably 98.0 to 99.5 wt %, and more preferably 98.5 to 99.0 wt % of the polymer (A) and 0.5 to 3.0 wt %, preferably 0.5 to 2.0 wt %, and more preferably 1.0 to 1.5 wt % of the stabilizer (B), the stabilizer (B) being an alkyltrialkoxysilane represented by the general formula (1):
[0048] R 1 (SiR 2 n X 3-n ) m (1)
[0049] in
[0050] R 1 is a monofunctional hydrocarbon group having 2 to 30 carbon atoms or a difunctional hydrocarbon group having 4 to 24 carbon atoms, and is preferably a hexadecyl group;
[0051] R 2 may be the same or different and are hydrocarbon groups having 1 to 10 carbon atoms;
[0052] X may be the same or different and are alkoxy, preferably are the same alkoxy, and more preferably are the same and are methoxy;
[0053] n is 0, 1 or 2, and is preferably 0;
[0054] m is 1 or 2;
[0055] And preferably the stabilizer (B) is hexadecyltrimethoxysilane; whereby the polymer (A) and the stabilizer (B) add up to 100% by weight.
[0056] A further preferred embodiment of the present invention provides that the polymer composition (I) comprises 97.0 to 99.99% by weight, preferably 99.0 to 99.95% by weight and more preferably 99.50 to 99.90% by weight of polymer (A) and 0.01 to 3.0% by weight, preferably 0.05 to 1.0% by weight and more preferably 0.1 to 0.5% by weight of at least one sterically hindered phenol as stabilizer (B), the sterically hindered phenol being preferably selected from the group consisting of: tetrakis(3-(3',5'-diol) tert-butyl-4-hydroxyphenyl)-propionic acid pentaerythritol ester, 3-(3',5'-di-tert-butyl-4-hydroxyphenyl) propionic acid octadecyl ester, 2,2'-thiodiethylenebis-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionate, 1,3,5-tris(3',5'-di-tert-butyl-4'-hydroxybenzyl) isocyanurate, 4,4'-thiobis(2-tert-butyl-5-methylphenol) and mixtures thereof; whereby the polymer (A) and the stabilizer (B) together amount to 100% by weight.
[0057] According to a further preferred embodiment of the present invention, polymer (A) is grafted with a compound having hydrolyzable silane groups and step c) is carried out before / during or after the grafting step, preferably step c) is carried out on an extruder during the grafting step.
[0058] Another preferred embodiment of the present invention provides that the MFR5 of the polymer composition (I) measured according to ISO 1133 at 190°C and a load of 5.00 kg after 60 days of storage and / or transport is not more than 25%, preferably not more than 15% and more preferably between 0.01% and 10% or 0.01% to 30% lower than the MFR5 of the same polymer composition (I) measured according to ISO 1133 at 190°C and a load of 5.00 kg before storage or transport.
[0059] According to another preferred embodiment of the present invention, the MFR5 of the polymer composition (I) measured at 190°C and a load of 5.00 kg according to ISO 1133 after 120 days of storage and / or transportation is not more than 50%, preferably not more than 40% and more preferably between 1% and 40% lower than the MFR5 of the same polymer composition (I) measured at 190°C and a load of 5.00 kg according to ISO 1133 before storage or transportation.
[0060] A preferred polymer composition (I) comprises or preferably consists of: 97.0 to 99.5 wt. % of a polymer (A), based on the total weight of the polymer composition (I), said polymer (A) being a copolymer of ethylene and 1-octene grafted with vinyltrimethoxysilane, having a density of 850 kg / m2 as measured according to ISO 1183. 3 Up to 920kg / m 3 and an MFR2 measured according to ISO 1133 at 190°C and a load of 2.16 kg in the range of 0.1 to 20.0 g / 10 min; and
[0061] 0.50 to 3.0 wt. % of a stabilizer (B), based on the total weight of the polymer composition (I), the stabilizer (B) being selected from the group consisting of hexadecyltrimethoxysilane, pentaerythritol tetrakis(3-(3',5'-di-tert-butyl-4-hydroxyphenyl)-propionate, octadecyl 3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate, and mixtures thereof;
[0062] wherein the polymer (A) and the stabilizer (B) add up to 100% by weight; and wherein the container has a moisture-blocking barrier layer made of aluminum.
[0063] use
[0064] The present invention also relates to the use of a stabilizer (B) selected from the group consisting of sterically hindered phenols, alkyltrimethoxysilanes, alkenyltrimethoxysilanes and mixtures thereof for improving the storage stability and / or transport stability of a polymer (A) selected from the group consisting of ethylene and C4 to C 12 Copolymers of alpha-olefin comonomers, propylene copolymers and mixtures thereof further comprising comonomer units comprising hydrolysable silane groups, whereby the transport and / or storage of polymer (A) is carried out in a container having at least one barrier layer.
[0065] According to a preferred embodiment of the use of the present invention, based on the total weight of the polymer (A) and the stabilizer (B), 0.50 to 3.0 wt. % of the stabilizer (B) is a compound represented by the general formula (1):
[0066] R1 (SiR 2 n X 3-n ) m (1)
[0067] in
[0068] R 1 is a monofunctional hydrocarbon group having 2 to 30 carbon atoms, 6 to 30 carbon atoms and more preferably 13 to 30 carbon atoms or a difunctional hydrocarbon group having 4 to 24 carbon atoms, and is preferably a hexadecyl group;
[0069] R 2 may be the same or different and are hydrocarbon groups having 1 to 10 carbon atoms;
[0070] X may be the same or different and are alkoxy, preferably are the same alkoxy and more preferably are the same and are methoxy;
[0071] n is 0, 1 or 2, and is preferably 0;
[0072] m is 1 or 2;
[0073] The stabilizer (B) is used to improve the storage stability and / or transportation stability of 97.0 to 99.5% by weight of the polymer (A), based on the total weight of the polymer (A) and the stabilizer (B), wherein the polymer (A) is a copolymer of ethylene and 1-octene grafted with vinyltrimethoxysilane and has a density of 850 kg / m3 as measured according to ISO 1183. 3 Up to 920kg / m 3 The MFR2 measured according to ISO 1133 at 190°C and a loading of 2.16 kg is in the range of 0.1 to 20.0 g / 10 min.
[0074] Yet another preferred embodiment of the use according to the invention provides that the stabilizer (B) is selected from the group consisting of hexadecyltrimethoxysilane, pentaerythritol tetrakis(3-(3',5'-di-tert-butyl-4-hydroxyphenyl)-propionate, octadecyl 3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate and mixtures thereof.
[0075] According to another preferred embodiment of the use according to the invention, the barrier layer comprises or consists of a material selected from the group consisting of: metals, preferably aluminum; HDPE; ethylene vinyl alcohol; polyvinyl chloride; polyvinylidene chloride and mixtures thereof; and more preferably consists of aluminum.
[0076] All preferred aspects and embodiments as described above for the method according to the invention shall also apply to the use according to the invention.
[0077] The invention will now be described with reference to the following non-limiting examples.
[0078] Experimental Section
[0079] A. Measurement Method
[0080] Unless defined otherwise, the following definitions of terms and assay methods apply to the above general description of the invention as well as to the following examples.
[0081] Melt flow rate (MFR)
[0082] For PE copolymers, MFR5 is measured according to ISO 1133 at 190°C under a loading of 5.00 kg.
[0083] For PE copolymers, MFR2 is measured according to ISO 1133 at 190°C under a loading of 2.16 kg.
[0084] density
[0085] The density of the material is measured according to ISO 1183-1.
[0086] Quantification of VTMS in PE-g-VTMS Copolymer
[0087] Quantitative nuclear magnetic resonance (NMR) spectroscopy was used to quantify the VTMS content of the polymers.
[0088] Quantitative data were recorded in the melt using a Bruker Avance III 500 NMR spectrometer operating at 500.13 MHz. 1 H NMR spectra. All spectra were obtained using 13 A C-optimized 7 mm magic angle spinning (MAS) probe was used at 150 °C using nitrogen for all gas dynamic recordings. Approximately 200 mg of material was loaded into a 7 mm outer diameter zirconium oxide MAS rotor and spun at 4 kHz. This setup was chosen primarily for the high sensitivity required for rapid identification and accurate quantification (see references klimke06, parkinson07 and castignolles09 as specified below). Standard single pulse excitation was used, with a short recycle delay of 2 s applied. A total of 128 transients were acquired per spectrum. Quantification was performed using a custom-made automated procedure for spectral analysis. 1 H NMR spectra were processed, integrated and quantitatively characterized. All chemical shifts were internally referenced to the poly(ethylene) signal at 1.33 ppm.
[0089] Characteristic signals resulting from grafting of vinyltrimethylsiloxane with various comonomer sequences were observed. Vinyltrimethylsiloxane grafting was quantified using the signal integration at 3.52 ppm assigned to the 1VTMS site (see reference brandolini01), interpreting the reported number of nuclei for each comonomer:
[0090] gVTMS=l 1VT M s / 9
[0091]
[0092] Ethylene content (E) is quantified using the integration of the volumetric aliphatic (volume) signal between 0.00 and 3.00 ppm. This integral must be compensated by subtracting 4 gVTMS (2 methylenes, 2VTMS and 3VTMS) and adding one gVTMS (*VTMS lacks 1 proton), for a total of 3 gVTMS subtractions.
[0093] E=(volume – 3*gVTMS) / 4
[0094] It should be noted that insignificant errors are introduced due to the inability to compensate for saturated chain ends that have no associated branching sites.
[0095] The total mole fraction of vinyl trimethylsiloxane in the polymer is calculated as follows:
[0096] fVTMS=gVTMS / (E+gVTMS)
[0097] The total comonomer incorporation of vinyltrimethylsiloxane in weight percent is calculated in the standard manner from the mole fractions:
[0098] cVTMS[weight%]=[100*(fVTMS*148.23)] / [(fVTMS*148.23)+((1-fVTMS)*28.05)]
[0099] As described by 1 Quantification of grafted vinyltrimethylsiloxane by H NMR as weight percent cVTMS [wt %] is independent of additional α-coolefins with an even number of carbons (eg C4, C6 or C8) that may be incorporated into the polyethylene chain.
[0100] References:
[0101] brandolini01
[0102] AJBrandolini, DDHills, "NMR spectra of polymers and polymeradditives", Marcel Deker Inc., 2000.
[0103] klimke06
[0104] Klimke, K., Parkinson, M., Piel, C., Kaminsky, W., Spiess, HW, Wilhelm, M., Macromol. Chem. Phys. 2006; 207:382.
[0105] parkinson07
[0106] Parkinson, M., Klimke, K., Spiess, HW, Wilhelm, M., Macromol. Chem. Phys. 2007; 208:2128.
[0107] castignolles09
[0108] Castignolles,P.,Graf,R.,Parkinson,M.,Wilhelm,M.,Gaborieau,M.,Polymer50(2009)2373.
[0109] B. Materials used
[0110] Table 1 summarizes the materials used to make the polymer compositions.
[0111] Table 1: Raw materials.
[0112]
[0113]
[0114] C. Preparation of Polymer Compositions
[0115] The polymer compositions according to the inventive examples (IE1 and IE2) and comparative examples (CE1 to CE3) were prepared by mixing and grafting Queo 6200-01 with the amounts of peroxide and VTMS given in Table 2 below and reacting them in a co-rotating twin-screw extruder (Werner & Pfleiderer ZSK 30) at a temperature of 200° C. with a residence time of 60 seconds to obtain the grafted polymer (A). Stabilizer (B) was additionally added in the co-rotating twin-screw extruder for IE1 and IE2 and calcium stearate was additionally added in the co-rotating twin-screw extruder for CE2 and CE3.
[0116] Table 2 summarizes the composition of the prepared polymer compositions comprising the grafted polymer (A) and optionally the stabilizer (B) or calcium stearate.
[0117] Table 2: Composition of the prepared polymer compositions.
[0118]
[0119] *: Based on the total amount of the polymer composition;
[0120] **: based on the total amount of polymer (A);
[0121] ***: The amount of VTMS has been calculated based on the NMR signal of the methoxy groups (1.98 wt% (determined by NMR) - (0.95 wt% * 0.428 (molar weight ratio of VTMS to HDTMS)) determined by NMR under the assumption that all the HDTMS added is in the polymer composition.
[0122] The aging of the polymer compositions was studied by storing pellets of each polymer composition in LDPE bags and aluminum lined bags, both of which were opened to the atmosphere when the polymer was transferred thereto. The MFR5 of the samples was measured after different storage times and the results are summarized in Tables 3 and 4 below and Figure 1 and Figure 2 (relative MFR versus time is shown). For CE1a to CE3a and CE1b and CE3b, polymer compositions according to CE1 to CE3 or CE1 and CE3, respectively, were used.
[0123] Table 3: Summary of aging tests in LDPE bags.
[0124]
[0125] a) using pellets made from polymer composition IE1 according to Table 2;
[0126] b) using pellets made from polymer composition IE2 according to Table 2;
[0127] nm = not measured.
[0128] Table 4: Summary of aging tests in aluminum lined bags.
[0129]
[0130] nm = not measured.
[0131] D. Discussion of Results
[0132] For samples according to CE1a, CE2a and CE3a, no stabilization measures were used, while for samples according to CE4 and CE5, stabilizers were added. As can be gathered from Table 3, for samples without any stabilization measures, the MFR5 dropped to less than 50% of the original value after only 15 days. Adding stabilizers allowed the material to be used for at least 8 days after removal from the barrier bag / exposure to the atmosphere with only a minimal decrease in MFR (<16%), since the stabilizers slowed down the decrease in the initial MFR. However, the MFR of the stabilized compositions did continue to drop, which means that adding stabilizers alone is not sufficient to stabilize the polymer in the long term.
[0133] For samples according to CE1b and CE2b, a barrier layer was used as a stabilization measure, and samples according to the invention IE1 and IE2 were stabilized with a barrier layer and a stabilizer. As can be seen from Table 4, the MFR5 of the invention is quite stable after more than 50 days. The MFR5 of comparative examples CE1 and CE3 starts to drop after 35 days and the values measured after 253 days are less than 60% of the original value. For samples according to the invention IE1 and IE2, the MFR5 is still at an acceptable level after 125 days, and even after more than 250 days the MFR5 measured is around 50% of the original value.
[0134] In general, only the specific combination of two stabilization measures, namely barrier layer and stabilizer according to claim 1, allows effective long-term stabilization of polymers. The method according to the invention also allows to extend the processing time, which means the time after the material is taken out of the container with the barrier layer and exposed to the atmosphere.
Claims
1. A method for improving the storage stability and / or transportation stability of a polymer (A), the method comprising the following steps: a) providing a polymer (A) containing additional comonomer units containing hydrolyzable silane groups selected from the group consisting of ethylene and C4 to C 12 Copolymers of alpha-olefin comonomers, propylene copolymers and mixtures thereof; b) providing a stabilizer (B); c) mixing the polymer (A) and the stabilizer (B) to obtain a stable polymer composition (I); and d) transferring said stabilized polymer composition (I) obtained in step c) into a container comprising at least one barrier layer, Wherein, the stabilizer (B) is an alkyltrialkoxysilane represented by the general formula (1): R 1 (SiX3) m (1) in R 1 is a monovalent alkyl group having 2 to 30 carbon atoms or a divalent alkyl group having 4 to 24 carbon atoms; X are the same or different and are alkoxy; m is 1 or 2.
2. The method according to claim 1, characterized in that: The container is selected from the group consisting of a bag, a sack, a box, a case, a barrel, a bucket, a can and a jar.
3. The method according to claim 1, characterized in that The at least one barrier layer of the container comprises a material selected from the group consisting of: metal or vacuum metallized polyester; HDPE; ethylene vinyl alcohol; polyvinyl chloride; polyvinylidene chloride, and mixtures thereof.
4. The method according to claim 3, characterized in that The at least one barrier layer consists of aluminum.
5. The method according to claim 1, characterized in that: Polymer (A) is a copolymer of ethylene and 1-octene containing additional comonomer units containing hydrolyzable silane groups, and has a density measured according to ISO 1183 of 850 kg / m 3 Up to 920kg / m 3 within the range.
6. The method according to claim 5, characterized in that Polymer (A) is a copolymer of ethylene and 1-octene containing additional comonomer units containing hydrolyzable silane groups, having a density measured according to ISO 1183 of 850 to 880 kg / m 3 within the range.
7. The method according to claim 1, characterized in that The polymer (A) comprising hydrolyzable silane groups has an MFR5 measured according to ISO 1133 at 190° C. and a loading of 5.0 kg in the range of 0.1 to 30.0 g / 10 min.
8. The method according to claim 7, characterized in that The polymer (A) comprising hydrolyzable silane groups has an MFR5 measured according to ISO 1133 at 190° C. and a loading of 5.0 kg in the range of 0.1 to 20 g / 10 min.
9. The method according to claim 1, characterized in that: The base polymer of the polymer (A) having no hydrolyzable silane groups has an MFR2 measured according to ISO 1133 at 190° C. and a loading of 2.16 kg in the range of 0.1 to 20.0 g / 10 min.
10. The method according to claim 9, characterized in that The base polymer of the polymer (A) having no hydrolyzable silane groups has an MFR2 measured according to ISO 1133 at 190° C. and a loading of 2.16 kg in the range of 0.1 to 5 g / 10 min.
11. The method according to claim 1, characterized in that: The comonomer units comprising hydrolyzable silane groups in polymer (A) are introduced by grafting.
12. The method according to claim 1, characterized in that The hydrolyzable silane groups in polymer (A) are derived from alkenyl alkoxy silanes.
13. The method according to claim 12, characterized in that The alkenyl alkoxysilane is selected from the group consisting of vinyl trimethoxysilane, vinyl triethoxysilane, vinyl tripropoxysilane, γ-(meth)acryloxypropyl trimethoxysilane and γ-(meth)acryloxypropyl triethoxysilane, and mixtures thereof.
14. The method according to claim 1, characterized in that The stabilizer (B) is hexadecyltrimethoxysilane.
15. The method according to claim 1, characterized in that The amount of the hydrolyzable silane group in the polymer (A) is in the range of 0.5 to 5.0 wt %, based on the total weight of the polymer (A).
16. The method according to claim 1, characterized in that The polymer composition (I) comprises 95.0 to 99.99 wt. % of polymer (A); and 0.01 to 5.0% by weight of stabilizer (B); thereby The total amount of the polymer (A) and the stabilizer (B) is 100% by weight.
17. The method according to claim 1, characterized in that The polymer composition (I) comprises 97.0 to 99.5 wt. % of polymer (A); and 0.5 to 3.0 wt. % of a stabilizer (B); thus The total amount of the polymer (A) and the stabilizer (B) is 100% by weight.
18. The method according to claim 1, characterized in that The polymer (A) is obtained by grafting the copolymer with a compound having a hydrolyzable silane group and step c) is carried out after the grafting step.
19. The method according to claim 1, characterized in that The MFR5 of the polymer composition (I) after 60 days of storage and / or transportation measured at 190°C and a load of 5.00 kg according to ISO 1133 is not more than 25% lower or 0.01% to 30% higher than the MFR5 of the same polymer composition (I) measured at 190°C and a load of 5.00 kg according to ISO 1133 before storage or transportation; and / or The MFR5 of the polymer composition (I) measured at 190°C and a load of 5.00 kg according to ISO 1133 after 120 days of storage and / or transportation is not more than 50% lower than the MFR5 of the same polymer composition (I) measured at 190°C and a load of 5.00 kg according to ISO 1133 before storage or transportation.
20. The method according to claim 1, characterized in that The polymer composition (I) comprises: 97.0 to 99.5 wt. % of polymer (A), based on the total weight of the polymer composition (I), wherein the polymer (A) is a copolymer of ethylene and 1-octene grafted with vinyltrimethoxysilane, and has a density of 850 kg / m 3 Up to 920kg / m 3 In the range of 0.1 to 20.0 g / 10 min, MFR2 measured according to ISO 1133 at 190°C and a load of 2.16 kg is in the range of 0.1 to 20.0 g / 10 min; and 0.50 to 3.0 wt % of a stabilizer (B), based on the total weight of the polymer composition (I), wherein the stabilizer (B) is hexadecyltrimethoxysilane; wherein the polymer (A) and the stabilizer (B) together account for 100% by weight; and wherein The container has a moisture barrier layer made of aluminum.
21. Use of a stabilizer (B) as defined in claim 1 for improving the storage stability and / or transport stability of a polymer (A) containing additional comonomer units containing hydrolyzable silane groups, selected from the group consisting of ethylene and C4 to C 12 Copolymers of alpha-olefin comonomers, propylene copolymers and mixtures thereof; whereby the transport and / or storage of polymer (A) is carried out in a container having at least one barrier layer.
22. The use according to claim 21, characterized in that 0.50 to 3.0 wt. % of stabilizer (B), based on the total weight of polymer (A) and stabilizer (B); Based on the total weight of polymer (A) and stabilizer (B), 97.0 to 99.5% by weight of polymer (A), polymer (A) is a copolymer of ethylene and 1-octene grafted with vinyltrimethoxysilane, and has a density of 850 kg / m3 as measured according to ISO 1183. 3 Up to 920kg / m 3 The MFR2 measured according to ISO 1133 at 190°C and a loading of 2.16 kg is in the range of 0.1 to 20.0 g / 10 min.
23. The use according to claim 22, characterized in that The stabilizer (B) is hexadecyltrimethoxysilane.