A high temperature resistant polyamide-polyetherimide toughened polymer and preparation method thereof
By preparing polyamide-polyetherimide toughened micropowder with a specific molecular chain structure, the shortcomings of thermosetting matrix resin composites in terms of high heat resistance and high toughness were solved, achieving a high heat distortion temperature above 250℃ and a high unnotched impact strength of simply supported beams.
Patent Information
- Application Number
- CN202210269465.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2018-12-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2038-12-18
AI Technical Summary
Existing thermosetting matrix resin composites are insufficient in terms of high heat resistance and high toughness, and cannot simultaneously meet the requirements of high heat resistance and high toughness.
High-temperature resistant polyamide-polyetherimide toughening polymers with specific molecular chain structures are prepared by polymerizing in polar aprotic solvents and spray drying to produce polyamide-polyetherimide toughening micropowders. The particle size distribution and intrinsic viscosity are controlled to ensure high heat resistance and high toughness.
The prepared polyamide-polyetherimide toughened micro powder has a high heat distortion temperature and high unnotched impact strength of simply supported beam above 250℃, meeting the requirements of high heat resistance and high toughness.
Smart Images

Figure BDA0003554008880000021 
Figure BDA0003554008880000022 
Figure BDA0003554008880000023
Abstract
Description
[0001] This application is a divisional application of a patent application with an application date of December 18, 2018, application number 201811550448.5, and invention name “A high temperature resistant polyamide-polyetherimide toughened polymer and its preparation method”. Technical Field
[0002] The invention belongs to the technical field of polymer materials, and in particular relates to a high temperature resistant polyamide-polyetherimide toughened micropowder and a preparation method thereof. Background Art
[0003] Fiber-reinforced thermosetting matrix resin composites, such as carbon fiber-cyanate resin composites, have been widely used in high structural strength and light weight requirements due to their outstanding performance in terms of specific strength and specific modulus; however, such thermosetting matrix resins usually contain one or more "toughened" thermoplastic particles, such as polyetherimide ultrafine powder and polyamide-imide ultrafine powder. The commercialized "toughened" polyetherimide ultrafine powder, such as the Ultem 1000F3SP polyetherimide ultrafine powder of Saudi Arabia Sabic Company, has a simply supported beam unnotched impact strength representing its toughness that is several times higher than that of the non-toughened cyanate resin cured product. However, the heat deformation temperature (HDT, 1.82MPa) representing its long-term use temperature is only below 200℃, and the temperature resistance level is relatively low; the commercialized "toughened" polyamide-imide ultrafine powder, such as Torlon4000TF of Belgium Solvay Company, has a heat deformation temperature (HDT, 1.82MPa) representing its long-term use temperature above 240℃ and a high temperature resistance level, but the simply supported beam unnotched impact strength representing its toughness is much lower than that of the polyetherimide ultrafine powder. The long-term use temperature of thermosetting matrix resins, such as cyanate matrix resins or bismaleimide matrix resins after curing is generally above 230°C. Therefore, the use of polyetherimide ultrafine powder and polyamide-imide ultrafine powder as thermoplastic particles "toughened" by such matrix resins cannot simultaneously meet the requirements of high heat resistance and high toughness. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a high temperature resistant polyamide-polyetherimide toughened microparticles as thermoplastic particles "toughened" by a high temperature resistant thermosetting matrix resin (such as a cyanate matrix resin or a bismaleimide matrix resin, etc.), which can simultaneously meet the requirements of high heat resistance and high toughness.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0006] A high temperature resistant polyamide-polyetherimide toughened polymer, wherein the molecular chain of the polymer comprises repeating structural units as shown in formula (I) and / or formula (II) and / or formula (III):
[0007]
[0008] In Formula I and Formula II, X is a divalent functional group, and its structure is Formula (A) or (B):
[0009]
[0010] The diamine containing the X structure is any one of 4,4'-diaminobenzanilide, 3,3'-diaminobenzanilide, 3,4'-diaminobenzanilide, 4,3'-diaminobenzanilide; 1,4-bis(4-aminobenzoyl)phenylenediamine, 1,4-bis(3-aminobenzoyl)phenylenediamine, 1-(4-aminobenzoyl)-4-(3-aminobenzoyl)phenylenediamine; 1,3-bis(4-aminobenzoyl)phenylenediamine, 1,3-bis(3-aminobenzoyl)phenylenediamine, 1-(4-aminobenzoyl)-3-(3-aminobenzoyl)phenylenediamine;
[0011] In Formula III, Y is a tetravalent functional group, and its structure is shown in any one of Formulas (C) to (H):
[0012]
[0013] The dianhydride containing the Y structure is any one of 1,2,4,5-pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 4,4'-(4,4'-isopropyldiphenoxy)bis(phthalic anhydride) or 4,4'-(4,4'-hexafluoroisopropyldiphenoxy)bis(phthalic anhydride).
[0014] In formula III, Z is a divalent functional group, and its structure is shown in formula (I) to formula (R):
[0015]
[0016] Wherein, R1 is -OH, -COOH or -OCOR3 substituent; R2 is -H, -OH, -COOH, -OCOR3 substituent; R3 is a monovalent alkane or monovalent aromatic substituent;
[0017] In Formula I, Formula II and Formula III, l, m and n are natural numbers, but l and m cannot be 0 at the same time; and l, m and n in Formula I, Formula II and Formula III must simultaneously satisfy the following conditions: (l+m) / (l+m+n)≥0.6,
[0018] Among them, the diamine containing the Z structure is: 3,5-diaminobenzoic acid, 3,5-diaminophenol, carboxylic acid ester derivatives of 3,5-diaminophenol, 4,6-diamino-1,3-dihydroxybenzene, carboxylic acid ester derivatives of 4,6-diamino-1,3-dihydroxybenzene, 3,3'-diamino-4,4'-dihydroxybiphenyl, carboxylic acid ester derivatives of 3,3'-diamino-4,4'-dihydroxybiphenyl, 4,4'-diamino-3,3'-dihydroxybiphenyl, carboxylic acid ester derivatives of 4,4'-diamino-3,3'-dihydroxybiphenyl, 2,2-bis(3-amino-4-hydroxyphenyl)propane, carboxylic acid ester derivatives of 2,2-bis(3-amino-4-hydroxyphenyl)propane, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane or carboxylic acid ester derivatives of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane.
[0019] The preparation method of the above-mentioned high temperature resistant polyamide-polyetherimide toughened micropowder comprises the following steps:
[0020] (1) First, add diamine to a polar aprotic solvent, stir and dissolve completely at 25-50° C., preferably 35° C.; then cool to 10-20° C., preferably 15° C., add dianhydride, the molar ratio of dianhydride to diamine is 0.99-1.01, stir and polymerize for 10-15 hours to generate a polyamic acid resin;
[0021] (2) adding toluene, xylene or a mixture of the two in an amount of 0.2 to 0.55 times the volume of the solvent, then rapidly heating and refluxing with water for 12 to 24 hours, and finally distilling and heating to the boiling point of the polar aprotic solvent to separate the toluene, xylene or a mixture thereof to obtain a polyamide-polyetherimide turbid liquid; in the preparation process of the polyamide-polyetherimide turbid liquid, the mass fraction of the solids is 5 to 45%, preferably 15%, and the total mass of the dianhydride and the diamine / (the total mass of the solvent + the total mass of the dianhydride and the diamine) is the solid content of the polyamic acid, that is, the mass fraction of the polyamic acid solids;
[0022] (3) adjusting the solid content of the polyamide-polyetherimide turbid solution to 5-20% by mass using the polar aprotic solvent in step (1), and spray drying the solution in a centrifugal spray dryer to obtain polyamide-polyetherimide toughened micropowder.
[0023] In step (1), the polar aprotic solvent is one or a mixture of N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylacetamide, N,N-dimethylformamide, preferably N-methylpyrrolidone.
[0024] In step (1), the diamine is one or a mixture of 4,4'-diaminobenzanilide, 2,2-bis(3-amino-4-hydroxyphenyl)propane; (1,4-phthalamide)bis(4-aminoaniline), 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane; 1,3-bis(4-aminobenzoyl)phenylenediamine, 1,3-bis(3-aminobenzoyl)phenylenediamine, 1,4-bis(4-aminobenzoyl)phenylenediamine.
[0025] In step (1), the dianhydride is one or a mixture of 4,4'-(4,4'-isopropyldiphenoxy)bis(phthalic anhydride), 4,4'-(4,4'-hexafluoroisopropyldiphenoxy)bis(phthalic anhydride), and 3,3',4,4'-benzophenonetetracarboxylic dianhydride.
[0026] In step (3), the drying conditions of the spray drying are: inlet air temperature 195-260°C; outlet air temperature 90-140°C; spray volume 5-50Kg / hr.
[0027] Beneficial Effects
[0028] The present invention discloses a polyamide-polyetherimide toughened micropowder, which has the following characteristics:
[0029] 1) Specific particle size distribution characteristics: D(05)≤1μm, D(50)≤35μm, D(95)≤75μm;
[0030] 2) Simply supported beam unnotched impact strength ≥160KJ / m 2 ;
[0031] 3) Heat deformation temperature (HDT, 1.82MPa) is above 250℃;
[0032] 4) Intrinsic viscosity ≥ 0.43dL / g;
[0033] The polyamide-polyetherimide toughened micropowder prepared by the invention can simultaneously meet the requirements of high heat resistance and high toughness, and has broad application prospects. DETAILED DESCRIPTION
[0034] The preparation process of polyamide-polyetherimide turbid solution is as follows:
[0035] In a polar aprotic solvent (such as N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylacetamide, N,N-dimethylformamide, etc. or any combination of any proportion of these mixed solvents), first add diamine, stir and dissolve completely at 25-50°C; then cool to 10-20°C, add dianhydride, stir and polymerize for 10-15 hours to generate polyamide acid resin; add toluene, xylene or a mixture thereof in an amount of 0.2-0.55 times the amount of solvent, then quickly heat and reflux with water for 12-24 hours, then distill and heat to the boiling point of the polar aprotic solvent, separate toluene, xylene or a mixture thereof, and obtain a polyamide-polyetherimide turbid liquid. In the preparation process of the polyamide-polyetherimide turbid liquid, the solid content is selected to be between 5% and 45% (wt.).
[0036] The turbid liquid spray drying process uses the same solvent to adjust the solid content of the above polyamide-polyetherimide turbid liquid to between 5% and 20%, and directly spray-dry it on a LPG-5-50 centrifugal spray dryer; the drying chamber inlet air temperature is between 195 and 260°C, the outlet air temperature is between 90 and 140°C, and the spray volume is between 5 and 50 kg / hr. The collected powder is the polyamide-polyetherimide toughened micropowder.
[0037] The sample test reference standards in the present invention are as follows:
[0038] 1. Laser particle size test: The particle size of the finished polyimide toughened particles was tested according to the wet method in the testing standard GB / T 19077.1-2003.
[0039] 2. Simply supported beam unnotched impact strength: According to the testing standard GB / T 1043.1-2008, all test samples are made into test specimens of specified size to test the simply supported beam unnotched impact strength.
[0040] 3. Heat deformation temperature: According to the testing standard GB / T 1634.1-2004, the heat deformation temperature of the sample is tested with a load of 1.82MPa.
[0041] 4. Intrinsic viscosity: According to the testing standard GB / T 1632.5-2008, NMP is used as the solvent and a Φ0.84mm Ubbelohde viscosity tube is selected to test the intrinsic viscosity of the sample.
[0042] Example 1
[0043] Preparation process of polyamide-polyetherimide turbid solution: First, add 36.362 g of 4,4'-diaminobenzanilide and 10.333 g of 2,2-bis(3-amino-4-hydroxyphenyl)propane to 878.96 g of N-methylpyrrolidone, stir and dissolve completely at 25-50°C; then cool to between 10 and 20°C, add 83.278 g of 4,4'-(4,4'-isopropyldiphenyloxy)bis(phthalic anhydride) and 25 .137g 4,4'-(4,4'-hexafluoroisopropyldiphenoxy)bis(phthalic anhydride), stirred and polymerized for 14 hours to generate polyamide acid resin; 439.48g toluene was added, and the temperature was rapidly raised and refluxed with water for 22 hours, and finally the temperature was raised to the boiling point of N-methylpyrrolidone and the distillation was stopped, and 512.62g toluene fraction was separated, and 73.14g N-methylpyrrolidone was added to the reaction system to keep the solid content of the system at 15% (wt.). A polyamide-polyetherimide turbid liquid was obtained.
[0044] The turbid liquid spray drying process uses the same solvent to adjust the solid content of the above polyamide-polyetherimide turbid liquid to between 15%, and directly spray-dry it on a LPG-15 centrifugal spray dryer; the drying chamber inlet air temperature is between 250°C and the outlet air temperature is between 135°C, and the spray volume is between 12Kg / hr. The collected powder is the polyamide-polyetherimide toughened micropowder.
[0045] The samples are subjected to performance inspection or testing in accordance with the aforementioned testing standards.
[0046] Example 2
[0047] Except for the formula, the preparation process of the polyamide-polyetherimide toughened particles in this embodiment is exactly the same as that in Example 1. The formula of this embodiment is as follows: 952.36 grams of N-methylpyrrolidone, 36.362 grams of 4,4'-diaminobenzanilide and 10.333 grams of 2,2-bis(3-amino-4-hydroxyphenyl)propane, 20.820 grams of 4,4'-(4,4'-isopropyldiphenoxy)bis(phthalic anhydride) and 100.549 grams of 4,4'-(4,4'-hexafluoroisopropyldiphenoxy)bis(phthalic anhydride). 476.18 grams of toluene were added before reflux, 559.76 grams of toluene fraction were separated, and 83.58 grams of N-methylpyrrolidone were added.
[0048] The samples are subjected to performance inspection or testing in accordance with the aforementioned testing standards.
[0049] Example 3
[0050] Except for the formula, the preparation process of the polyamide-polyetherimide toughened particles in this embodiment is exactly the same as that in Example 1. The formula of this embodiment is as follows: 911.69 grams of N-methylpyrrolidone, 45.029 grams of (1,4-phthaloyl)bis(4-aminoaniline) and 25.638 grams of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 67.664 grams of 4,4'-(4,4'-isopropyldiphenyloxy)bis(phthalic anhydride) and 22.555 grams of 3,3',4,4'-benzophenonetetracarboxylic dianhydride. Before reflux, 455.84 grams of toluene were added, 535.85 grams of toluene fraction were separated, and 80.01 grams of N-methylpyrrolidone were added.
[0051] The samples are subjected to performance inspection or testing in accordance with the aforementioned testing standards.
[0052] Example 4
[0053] Except for the formula, the preparation process of the polyamide-polyetherimide toughened particles in this embodiment is exactly the same as that in Example 1. The formula of this embodiment is as follows: 982.45 grams of N-methylpyrrolidone, 69.276 grams of 1,3-bis(4-aminobenzoyl)phenylenediamine, and 104.098 grams of 4,4'-(4,4'-isopropyldiphenyloxy)bis(phthalic anhydride). 491.23 grams of toluene are added before reflux, 577.45 grams of toluene fraction are separated, and 86.22 grams of N-methylpyrrolidone is added.
[0054] The samples are subjected to performance inspection or testing in accordance with the aforementioned testing standards.
[0055] Example 5
[0056] Except for the formula, the preparation process of the polyamide-polyetherimide toughened particles in this embodiment is exactly the same as that in Example 1. The formula of this embodiment is as follows: 828.59 grams of N-methylpyrrolidone, 51.957 grams of 1,4-bis(4-aminobenzoyl)phenylenediamine, and 94.265 grams of 4,4'-(4,4'-hexafluoroisopropyldiphenoxy)bis(phthalic anhydride). 414.30 grams of toluene are added before reflux, 487.02 grams of toluene fraction are separated, and 72.72 grams of N-methylpyrrolidone is added.
[0057] The samples are subjected to performance inspection or testing in accordance with the aforementioned testing standards.
[0058] In the present invention, commercialized polyamide-imide ultrafine powder (such as Torlon 4000TF, etc.) is selected as the sample of Comparative Example 1, and commercialized polyetherimide ultrafine powder (such as ULTEM 1000F3SP, etc.) is selected as the sample of Comparative Example 2. The samples are also tested or tested for performance according to the above-mentioned test standards.
[0059] The sample performance detection or test results of all embodiments and comparative examples are shown in Table 1.
[0060] As can be seen from Table 1, the polyamide-polyetherimide toughened particles provided by the present invention have higher temperature resistance and toughness. As thermoplastic particles "toughened" by thermosetting matrix resins (such as cyanate matrix resins or bismaleimide matrix resins, etc.), they have a better performance basis for meeting high heat resistance and high toughness.
[0061] Table 1 Sample test results
[0062]
Claims
1. A high temperature resistant polyamide-polyetherimide toughened polymer particle, It is characterized in that The molecular chain of the polymer includes a repeating structural unit as shown in formula (I), or includes a repeating structural unit as shown in formula (II), or includes repeating structural units shown in formula (I), formula (II) and formula (III) at the same time: In formula (I) and formula (II), X is a divalent functional group, and its structure is formula (A) or (B): In formula (III), Y is a tetravalent functional group, and its structure is shown in any one of formulas (F) to (H): In formula (III), Z is a divalent functional group, and its structure is shown in formula (M) or formula (O): Among them, R 1 , R 2 is a -OH substituent; When the molecular chain of the polymer contains repeating structural units represented by formula (I), formula (II) and formula (III) at the same time, the following conditions must be met: (l+m) / (l+m+n)≥0.6, When the molecular chain of the polymer contains only the repeating structural unit represented by formula (I) or formula (II), X in formula (I) and formula (II) is a structure represented by formula (B); The particle size distribution characteristics of the microparticles are: D(05)≤1μm, D(50)≤35μm, D(95)≤75μm; The simply supported beam unnotched impact strength of the particles is ≥160KJ / m 2 ; The thermal deformation temperature of the particles under a load of 1.82 MPa is greater than 250°C.
2. The method for preparing the high temperature resistant polyamide-polyetherimide toughened polymer particles according to claim 1, It is characterized in that The steps include: (1) First, add diamine to a polar aprotic solvent, stir and dissolve completely at 25-50° C.; then cool to 10-20° C., add dianhydride, the molar ratio of dianhydride to diamine is 0.99-1.01, stir and polymerize for 10-15 hours to generate a polyamic acid resin; (2) adding 0.2 to 0.55 times the volume of the solvent of toluene, xylene or a mixture of the two, then rapidly heating and refluxing with water for 12 to 24 hours, and finally distilling and heating to the boiling point of the polar aprotic solvent to separate toluene and xylene to obtain a polyamide-polyetherimide turbid liquid; during the preparation process of the polyamide-polyetherimide turbid liquid, the mass fraction of the solids is 5 to 45%; (3) adjusting the solid content of the polyamide-polyetherimide turbid solution to 5-20% by mass using the polar aprotic solvent in step (1), and spray drying the solution in a centrifugal spray dryer to obtain polyamide-polyetherimide toughened micropowder.
3. The method for preparing the high temperature resistant polyamide-polyetherimide toughened polymer particles according to claim 2, It is characterized in that The polar aprotic solvent is one of N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylacetamide, N,N-dimethylformamide or a mixture of several thereof.
4. The method for preparing the high temperature resistant polyamide-polyetherimide toughened polymer particles according to claim 2, It is characterized in that In step (3), the drying conditions of the spray drying are: inlet air temperature 195-260°C, outlet air temperature 90-140°C, and spray volume 5-50 Kg / hr.