Negative electrode, electrochemical device and electronic device
By growing slip carbon materials in situ on the surface of hard carbon anode materials, combined with nitrogen elements and transition metal elements, the problems of high resistance of graphite materials and brittle fracture during processing of high gram capacity materials are solved, achieving high energy density and good cycle performance. electrochemical device.
Patent Information
- Application Number
- CN202180005821.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-06-21
AI Technical Summary
Existing negative electrode materials prepared from graphite have high diaphragm resistance and poor fast charging performance in electrochemical devices. Although high-gram capacity negative electrode materials increase energy density, they cause processing brittleness and cold pressing stripping problems, and cost If it is higher, the actual effect is not ideal.
Hard carbon is used as the negative active material, and slip carbon materials are grown in situ on its surface. Nitrogen and transition metal elements are introduced to form fibrous, flaky or granular carbon materials to enhance the negative active material layer and current collector. The bonding force between them improves the slippage and processing performance of hard carbon particles.
Significantly improves the bonding force between the negative active material layer and the current collector, reduces the diaphragm resistance, improves the cycle performance and processing stability of the electrochemical device, avoids the processing brittle fracture problem of hard carbon materials, and maintains the High energy density.
Smart Images

Figure BDA0003589263060000121 
Figure BDA0003589263060000131 
Figure BDA0003589263060000141
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrochemical energy storage, and in particular to negative electrodes, electrochemical devices and electronic devices. Background Art
[0002] With the development and progress of electrochemical devices (e.g., lithium-ion batteries), higher and higher requirements are placed on their cycle performance and energy density. The negative electrode prepared from graphite has a high film resistance and poor fast charging performance. At present, in order to improve the performance of electrochemical devices, some negative electrode materials with high gram capacity (e.g., silicon-based negative electrode materials, tin-based negative electrode materials, hard carbon materials, etc.) are usually used to replace the commonly used graphite. However, these high gram capacity negative electrode materials also bring some new problems, and further improvements are expected. Summary of the invention
[0003] Some embodiments of the present application provide a negative electrode, comprising a negative electrode current collector and a negative electrode active material layer, wherein the negative electrode active material layer comprises a negative electrode active material, and the bonding force between the negative electrode active material layer and the negative electrode current collector is greater than or equal to 7 N / m.
[0004] In some embodiments, the bonding force between the negative electrode active material layer and the negative electrode current collector is greater than or equal to 10 N / m.
[0005] In some embodiments, the negative electrode active material includes hard carbon.
[0006] In some embodiments, at least one of the conditions (a) to (d) is met: (a) carbon material is in situ grown on the surface of the negative electrode active material; (b) the Dv50 of the negative electrode active material is 6 μm to 20 μm; (c) the negative electrode active material also includes nitrogen and transition metal elements; (d) the cohesive force of the negative electrode active material is 5 N / m to 100 N / m.
[0007] In some embodiments, at least one of conditions (e) to (h) is met: (e) the carbon material includes at least one of a fibrous carbon material, a flaky carbon material or a granular carbon material; (f) the mass of the transition metal element in the negative electrode active material is 0.1% to 10%, and the mass of the nitrogen element in the negative electrode active material is 0.1% to 5%; (g) the transition metal element includes at least one of Co, Fe, Cr, Pt, Cu, Mn, Ag, Ni or Zn; (h) the mass percentage of the nitrogen element or the transition metal element in the negative electrode active material particle gradually decreases from the surface of the negative electrode active material particle to the center of the negative electrode active material particle.
[0008] In some embodiments, at least one of the conditions (i) to (k) is met: (i) the diameter of the fibrous carbon material is 50nm to 500nm, and the length is greater than 1μm; (j) the length of the flaky carbon material is greater than 1μm; (k) the average particle size of the granular carbon material is 50nm to 500nm.
[0009] Some embodiments of the present application provide an electrochemical device, which includes an electrolyte, a separator, a positive electrode and any one of the negative electrodes mentioned above, wherein the separator is disposed between the positive electrode and the negative electrode.
[0010] In some embodiments, the electrolyte includes at least one of fluoroether, fluoroethylene carbonate or ether nitrile. In some embodiments, the electrolyte includes a lithium salt, the lithium salt includes lithium bis(fluorosulfonyl)imide and lithium hexafluorophosphate, the concentration of the lithium salt is 1 mol / L to 2 mol / L, and the molar ratio of lithium bis(fluorosulfonyl)imide to lithium hexafluorophosphate is 0.05 to 4.
[0011] An embodiment of the present application further provides an electronic device, comprising the above-mentioned electrochemical device.
[0012] The embodiments of the present application improve the bonding force between the negative electrode active material layer and the negative electrode current collector, making the structure of the negative electrode more stable, which is beneficial to reducing the film resistance of the negative electrode and improving the performance of the electrochemical device. DETAILED DESCRIPTION
[0013] The following embodiments may enable those skilled in the art to more fully understand the present application, but do not limit the present application in any way.
[0014] Some embodiments of the present application provide a negative electrode, which includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector. In some embodiments, the negative electrode active material layer can be located on one side or both sides of the negative electrode current collector. In some embodiments, the negative electrode active material layer includes a negative electrode active material.
[0015] In some embodiments, the negative electrode active material includes hard carbon. By using hard carbon, on the one hand, the gram capacity of hard carbon is greater than the gram capacity of commonly used graphite, which can reach about twice the gram capacity of graphite, thereby improving the energy density of the electrochemical device. In addition, by using a negative electrode active material containing hard carbon, it is helpful to improve the bonding force between the negative electrode active material layer and the negative electrode current collector, thereby improving the structural stability of the negative electrode, which is conducive to improving the cycle performance of the electrochemical device prepared by the negative electrode.
[0016] In some embodiments, the bonding force between the negative electrode active material layer and the negative electrode current collector is greater than or equal to 7 N / m. The embodiments of the present application improve the bonding force between the negative electrode active material layer and the negative electrode current collector, making the structure of the negative electrode more stable, which is conducive to improving the cycle performance of the electrochemical device prepared by the negative electrode.
[0017] In some embodiments, the bonding force between the negative electrode active material layer and the negative electrode current collector is greater than or equal to 10 N / m. By using a negative electrode active material containing hard carbon, it is found that the bonding force between the negative electrode active material layer and the negative electrode current collector can be increased to greater than or equal to 10 N / m, which is much greater than 2 N / m to 6 N / m when graphite is used as the negative electrode active material.
[0018] In some embodiments, the surface of the hard carbon in the negative electrode active material has carbon material grown in situ. When pure hard carbon is used as the negative electrode active material, in addition to the advantages described above, there are also some disadvantages. For example, the edges and corners of the hard carbon particles are usually sharp, which may damage the negative electrode current collector during the cold pressing process, which is not conducive to the full play of the electrochemical performance of the electrochemical device; on the other hand, the sharp edges and corners of the hard carbon particles are not conducive to the slippage between the particles, resulting in brittle fracture during processing and cold pressing stripping and breaking.
[0019] One of the strategies to solve the above-mentioned unfavorable factors is to coat the surface of the hard carbon particles with a layer of material to cover the edges and corners of the hard carbon particles. However, the coating layer easily falls off from the surface of the hard carbon particles. Alternatively, the hard carbon can be mixed with graphite to utilize the good slip characteristics of graphite. However, this will sacrifice the high gram capacity of the hard carbon and affect the energy density of the electrochemical device. In addition, one-dimensional carbon tubes or two-dimensional graphene can also be added. They can largely cover the sharp edges and corners of the hard carbon and improve the situation where the hard carbon punctures the isolation film and copper foil during processing. At the same time, the lubricating effect of the carbon tubes or graphene can also increase the slip between the hard carbon particles and improve the problem of broken bands in the hard carbon processing. However, the carbon tubes or graphene are expensive, and the secondary addition is unevenly dispersed, resulting in the actual effect being less than expected.
[0020] The present application in situ grows carbon material that can increase slip on the surface of hard carbon to solve the sharp edges of hard carbon particles and increase the slip between hard carbon particles, while solving the problems of difficult slip and damage to negative electrode current collector that occur during the processing of hard carbon.
[0021] In some embodiments, the Dv50 of the hard carbon is 6 μm to 20 μm. The particle size test method refers to GB / T 19077-2016. The test equipment used is the Mastersizer 3000 produced by Malvern. During the test, when the laser beam passes through the dispersed particle sample, the particle size measurement is completed by measuring the intensity of the scattered light. The refractive index of the particles used in the test is 1.8. One sample is tested three times, and the particle size is finally measured by taking the average value of the three tests to obtain Dv50. If the Dv50 of the hard carbon is too small, the specific surface area of the hard carbon is large, and it is easy to have side reactions with the electrolyte. If the Dv50 of the hard carbon is too large, it is not conducive to the improvement of the rate performance.
[0022] In some embodiments, the negative electrode active material containing hard carbon also includes nitrogen and transition metal elements. In some embodiments, XPS analysis can be used to determine whether the negative electrode active material containing hard carbon includes nitrogen and transition metal elements. The carbon material of the present application is derived from the cracking of small molecules. Under normal circumstances, small molecules will directly volatilize without carbon residues during pyrolysis. In order to allow small molecule carbon to pyrolyze into carbon materials that increase slip on the surface of hard carbon particles, transition metal salts can be introduced and nitrogen-containing small molecule materials can be selected. By utilizing the combination of nitrogen elements in small molecules and d orbitals of transition metal elements, carbon materials with specific structures / morphologies are pyrolyzed in situ under the action of transition metals. Depending on the small molecules, fibrous, flaky or granular carbon materials can be pyrolyzed on the surface of hard carbon particles to improve the poor processing performance of hard carbon particles and the problems of puncturing the isolation membrane and the negative electrode current collector.
[0023] In some embodiments, the cohesive force between the negative electrode active materials is 5 N / m to 100 N / m. If the cohesive force between the negative electrode active materials is too small, it is not conducive to the stability of the structure of the negative electrode active materials; if the cohesive force between the negative electrode active materials is too large, it is not conducive to the improvement of the rate performance of the electrochemical device.
[0024] In some embodiments, the carbon material grown in situ on the surface of the hard carbon includes at least one of a fibrous carbon material, a flaky carbon material, or a granular carbon material. In some embodiments, the diameter of the fibrous carbon material is 50nm to 500nm, and the length is greater than 1μm. If the diameter of the fibrous carbon material is too small, the stability of the fibrous carbon material is relatively weak; if the diameter of the fibrous carbon material is too large, the coating flexibility of the fibrous carbon material will be relatively weak. In addition, if the length of the fibrous carbon material is too small, the effect of the carbon material on improving the slip between the hard carbon particles is relatively limited. The diameter and length test of the fibrous carbon material is performed by photographing and observing the material powder through a SEM scanning electron microscope, and then, using image analysis software, 50 fibrous carbon materials are randomly selected from each of the 10 SEM photos, and the diameter and length of each of these fibrous carbon materials are measured, and then the average value of the diameter and length of 10×50 carbon nanotubes is calculated, which is the diameter and length of the fibrous carbon material (the length and diameter are similar to the measurement method of the length and diameter of carbon nanotubes).
[0025] In some embodiments, the length of the flaky carbon material is greater than 1 μm. If the length of the flaky carbon material is too small, the effect of the carbon material on improving the slip between hard carbon particles is relatively limited. The length of the flaky carbon material is measured by photographing the material powder using a SEM scanning electron microscope, and then, using image analysis software, 50 flaky carbon materials are randomly selected from 10 SEM photos, the longest length of these flaky carbon materials is measured, and then the average value of the longest length of 10×50 flaky carbon materials is calculated, which is the length of the flaky carbon material.
[0026] In some embodiments, the average particle size of the granular carbon material is 50 nm to 500 nm. If the average particle size of the granular carbon material is too small, it is not conducive to the full coating of the hard carbon particles; if the average particle size of the granular carbon material is too large, it will affect the effect of the granular carbon material on improving the slip between the hard carbon particles. The average particle size test of the granular carbon material is to photograph and observe the material powder through a SEM scanning electron microscope, and then, using image analysis software, 10 granular carbon materials are randomly selected from the SEM photos to calculate the area of each of these material particles. Then, assuming that the material particles are spherical, the respective particle sizes R (diameter) are calculated by the following formula: R = 2 × (S / π) 1 / 2 ; Wherein, S is the area of the material particles; 10 SEM images are processed to obtain the particle size R of the material particles, and the particle sizes of 100 (10×10) material particles obtained are arithmetic averaged to obtain the average particle size of the matrix.
[0027] In some embodiments, the mass of the transition metal element in the negative electrode active material is 0.1% to 10%, and the mass of the nitrogen element in the negative electrode active material is 0.1% to 5%. If the mass percentage of the transition metal element or the nitrogen element is too small, it is not conducive to the in-situ growth of the carbon material on the surface of the hard carbon particles; if the mass percentage of the transition metal element or the nitrogen element is too large, the effect of increasing the amount of residual carbon in the in-situ growth process is no longer significantly increased, and it is not conducive to the improvement of the energy density of the electrochemical device. In some embodiments, the transition metal element includes at least one of Co, Fe, Cr, Pt, Cu, Mn, Ag, Ni or Zn.
[0028] In some embodiments, the mass percentage of nitrogen and transition metal elements in the negative electrode active material gradually decreases from the surface of the negative electrode active material to the center of the negative electrode active material. The mass percentage of nitrogen and transition metal elements is tested by linear scanning of the scanning electron microscope energy spectrum. During the test, the electrode sheet of the negative electrode active material is first cut along the cross section by ion polishing or liquid nitrogen brittle fracture, and the negative electrode active material particle cut in the center is found in the scanning electron microscope. A straight line is drawn from the inside of the particle to the surface and a linear scanning energy spectrum test is performed along the straight line. The test elements are selected as N element and transition metal element.
[0029] In some embodiments, if the average length from the volume center to the surface of the negative electrode active material is set to L, the mass of the nitrogen element and the transition metal element on the surface of the negative electrode active material is n, the mass percentage of the nitrogen element or the transition metal element at any point inside the negative electrode active material with a distance of l from the surface is m, m = (n × l) / L, and satisfies: 0 ≤ m ≤ 1. In this way, a gradient distribution of the in-situ grown carbon material can be achieved, which is beneficial to increase the slip effect of the hard carbon particles.
[0030] The preparation process of the negative electrode active material is briefly described below to better understand the present application, but this is only exemplary and not intended to limit the present application. In some embodiments, the preparation method of the negative electrode active material containing hard carbon includes the following steps: dispersing the hard carbon material in a first solvent to prepare a first solution; adding the nitrogen-containing raw material of the carbon material and the transition metal nitrate to the first solution to obtain a uniform second solution; stirring the second solution, evaporating it to dryness, and heat-treating it under an inert gas to obtain a negative electrode active material. In some embodiments, the first solvent includes at least one of distilled water, ethanol, dimethylformamide or tetrahydrofuran. In some embodiments, the nitrogen-containing raw material of the carbon material includes at least one of melamine, dicyandiamide, methylimidazole, dipyridylamine, o-phenylenediamine, bipyridine, dibromobipyridine, pyrimidine, o-phenanthroline, dibromophenanthroline or imidazolylpyridine. In some embodiments, the transition metal nitrate includes at least one of Co(NO3)2, Fe(NO3)3, Cr(NO3)3, H2PtCl6, Mn(NO3)2, AgNO3, Ni(NO3)2, or Zn(NO3)2. It should be understood that the preparation method is only exemplary, and other suitable preparation methods may also be used.
[0031] In some embodiments, different small molecule carbon sources are added to obtain carbon materials with different morphologies. For example, using dicyandiamide as the carbon source and cobalt nitrate as the transition metal salt, fibrous carbon materials can be grown in situ on the surface of hard carbon particles. The fibrous carbon materials are located on the surface of hard carbon particles, which can not only effectively improve the contact problem between hard carbon particles, prevent hard carbon from stabbing the isolation membrane and the negative electrode current collector, but also effectively increase the slip between hard carbon particles and improve the brittle fracture problem. For example, when o-phenylenediamine is used as the carbon source and cobalt nitrate is used as the transition metal salt, flaky carbon materials can be grown in situ on the surface of hard carbon particles. The flaky carbon materials are located on the surface of hard carbon particles, which can also effectively improve the contact problem between hard carbon particles, prevent hard carbon from stabbing the isolation membrane and the negative electrode current collector, and effectively increase the slip between hard carbon particles. In addition, different contents of transition metal salts also result in different residual carbon rates of carbon materials cracked by small molecule carbon sources. For example, taking o-phenylenediamine as the carbon source and cobalt nitrate as the transition metal salt, when the content of cobalt nitrate is 1%, the residual carbon rate is 10%, while when the content of cobalt nitrate is 10%, the residual carbon rate can reach 50%.
[0032] In some embodiments, the negative electrode active material layer may further include a conductive agent and a binder. In some embodiments, the conductive agent in the negative electrode active material layer may include at least one of conductive carbon black, Ketjen black, lamellar graphite, graphene, carbon nanotubes or carbon fibers. In some embodiments, the binder in the negative electrode active material layer may include at least one of carboxymethyl cellulose (CMC), polyacrylic acid, polyvinyl pyrrolidone, polyaniline, polyimide, polyamide-imide, polysiloxane, styrene-butadiene rubber, epoxy resin, polyester resin, polyurethane resin or polyfluorene. In some embodiments, the mass ratio of the negative electrode active material, the conductive agent and the binder in the negative electrode active material layer may be (78 to 98.5): (0.1 to 10): (0.1 to 10). The negative electrode active material may be a negative electrode active material containing hard carbon. It should be understood that the above is only an example, and any other suitable material and mass ratio may be used. In some embodiments, the negative electrode current collector may use at least one of copper foil, nickel foil or a carbon-based current collector.
[0033] The embodiments of the present application also provide an electrochemical device, which includes an electrode assembly, wherein the electrode assembly includes a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode. In some embodiments, the negative electrode is any of the negative electrodes described above.
[0034] In some embodiments, the electrochemical device includes a lithium ion battery, but the present application is not limited thereto. In some embodiments, the electrochemical device may further include an electrolyte. The electrolyte may be one or more of a gel electrolyte, a solid electrolyte, and an electrolyte solution.
[0035] In some embodiments, the electrolyte includes at least one of fluoroether, fluoroethylene carbonate or ether nitrile. In some embodiments, the electrolyte also includes a lithium salt, the lithium salt includes lithium bis(fluorosulfonyl)imide and lithium hexafluorophosphate, the concentration of the lithium salt is 1 mol / L to 2 mol / L, and the molar ratio of lithium bis(fluorosulfonyl)imide to lithium hexafluorophosphate is 0.05 to 4.
[0036] In some embodiments, the electrolyte may further include a non-aqueous solvent, which may be a carbonate compound, a carboxylate compound, an ether compound, other organic solvents, or a combination thereof.
[0037] The carbonate compound may be a linear carbonate compound, a cyclic carbonate compound, a fluorinated carbonate compound or a combination thereof.
[0038] Examples of chain carbonate compounds are diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC) and combinations thereof. Examples of cyclic carbonate compounds are ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinyl ethylene carbonate (VEC) or combinations thereof. Examples of fluorocarbonate compounds are fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate or combinations thereof.
[0039] Examples of the carboxylic acid ester compound are methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolide, valerolactone, mevalonolactone, caprolactone, methyl formate, or a combination thereof.
[0040] Examples of the ether compound are dibutyl ether, tetraglyme, diglyme, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, or a combination thereof.
[0041] Examples of other organic solvents are dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, trioctyl phosphate, and phosphoric acid esters or combinations thereof.
[0042] In some embodiments, the positive electrode includes a current collector and a positive electrode active material layer disposed on the current collector, and the positive electrode active material layer may include a positive electrode active material. In some embodiments, the positive electrode active material includes at least one of lithium cobaltate, lithium iron phosphate, lithium manganese iron phosphate, sodium iron phosphate, lithium vanadium phosphate, sodium vanadium phosphate, lithium vanadium phosphate, sodium vanadium phosphate, lithium vanadate, lithium manganate, lithium nickelate, lithium nickel cobalt manganate, lithium-rich manganese-based materials, or lithium nickel cobalt aluminum oxide. In some embodiments, the positive electrode active material layer may also include a conductive agent. In some embodiments, the conductive agent in the positive electrode active material layer may include at least one of conductive carbon black, ketjen black, lamellar graphite, graphene, carbon nanotubes, or carbon fibers. In some embodiments, the positive electrode active material layer may also include a binder, and the binder in the positive electrode active material layer may include at least one of carboxymethyl cellulose (CMC), polyacrylic acid, polyvinyl pyrrolidone, polyaniline, polyimide, polyamide-imide, polysiloxane, styrene-butadiene rubber, epoxy resin, polyester resin, polyurethane resin, or polyfluorene. In some embodiments, the mass ratio of the positive electrode active material, the conductive agent, and the binder in the positive electrode active material layer may be (80 to 99): (0.1 to 10): (0.1 to 10). In some embodiments, the thickness of the positive electrode active material layer may be 10 μm to 500 μm. It should be understood that the above description is only an example, and the positive electrode active material layer may adopt any other suitable material, thickness, and mass ratio.
[0043] In some embodiments, the positive electrode current collector may be Al foil, and of course, other current collectors commonly used in the art may also be used. In some embodiments, the thickness of the positive electrode current collector may be 1 μm to 50 μm. In some embodiments, the positive electrode active material layer may be coated only on a partial area of the positive electrode current collector.
[0044] In some embodiments, the separator includes at least one of polyethylene, polypropylene, polyvinylidene fluoride, polyethylene terephthalate, polyimide or aramid. For example, polyethylene includes at least one selected from high-density polyethylene, low-density polyethylene or ultra-high molecular weight polyethylene. In particular, polyethylene and polypropylene have a good effect on preventing short circuits and can improve the stability of the battery through the shutdown effect. In some embodiments, the thickness of the separator is in the range of about 5 μm to 50 μm.
[0045] In some embodiments, the surface of the isolation membrane may further include a porous layer, the porous layer is disposed on at least one surface of the isolation membrane, the porous layer includes inorganic particles and a binder, the inorganic particles are selected from at least one of aluminum oxide (Al2O3), silicon oxide (SiO2), magnesium oxide (MgO), titanium oxide (TiO2), hafnium dioxide (HfO2), tin oxide (SnO2), cerium dioxide (CeO2), nickel oxide (NiO), zinc oxide (ZnO), calcium oxide (CaO), zirconium oxide (ZrO2), yttrium oxide (Y2O3), silicon carbide (SiC), boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate. In some embodiments, the pores of the isolation membrane have a diameter in the range of about 0.01 μm to 1 μm. The binder of the porous layer is selected from at least one of polyvinylidene fluoride, copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, sodium carboxymethyl cellulose, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene or polyhexafluoropropylene. The porous layer on the surface of the separator can improve the heat resistance, oxidation resistance and electrolyte wetting performance of the separator, and enhance the adhesion between the separator and the pole piece.
[0046] In some embodiments of the present application, the electrode assembly of the electrochemical device is a wound electrode assembly, a stacked electrode assembly, or a folded electrode assembly. In some embodiments, the positive electrode and / or the negative electrode of the electrochemical device can be a multi-layer structure formed by winding or stacking, or a single-layer structure in which a single-layer positive electrode, a separator, and a single-layer negative electrode are stacked.
[0047] In some embodiments of the present application, taking a lithium-ion battery as an example, a positive electrode, a separator, and a negative electrode are wound or stacked in sequence to form an electrode component, and then encapsulated in, for example, an aluminum-plastic film, injected with an electrolyte, formed, and encapsulated to form a lithium-ion battery. Then, the prepared lithium-ion battery is subjected to a performance test.
[0048] Those skilled in the art will appreciate that the above-described method for preparing an electrochemical device (eg, a lithium-ion battery) is only an example, and other methods commonly used in the art may be used without departing from the disclosure of the present application.
[0049] Embodiments of the present application also provide an electronic device including the above-mentioned electrochemical device. The electronic device of the embodiment of the present application is not particularly limited, and it can be any electronic device known in the prior art. In some embodiments, the electronic device may include, but is not limited to, a laptop computer, a pen-input computer, a mobile computer, an e-book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a drone, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery and a lithium-ion capacitor, etc.
[0050] Some specific embodiments and comparative examples are listed below to better illustrate the present application, wherein a lithium-ion battery is used as an example.
[0051] Example 1
[0052] Preparation of positive electrode: Mix the positive electrode active materials lithium cobalt oxide, conductive carbon black (Super P), and polyvinylidene fluoride (PVDF) in a weight ratio of 97:1.4:1.6, add N-methylpyrrolidone (NMP) as a solvent, and stir evenly. The slurry (solid content of 72wt%) is evenly coated on the positive electrode current collector aluminum foil with a coating thickness of 80μm, dried at 85℃, and then cold pressed, cut, and slit, and dried under vacuum conditions at 85℃ for 4 hours to obtain the positive electrode.
[0053] Preparation of negative electrode: Commercial artificial hard carbon, binder styrene butadiene rubber and sodium carboxymethyl cellulose (CMC) were dissolved in deionized water at a weight ratio of 97:2:1 to form a negative electrode slurry (solid content of 40wt%). A 10μm thick copper foil was used as the negative electrode current collector, and the negative electrode slurry was coated on the negative electrode current collector with a coating thickness of 50μm, dried at 85°C, and then cold pressed, cut and slit, and dried under vacuum conditions at 120°C for 12 hours to obtain the negative electrode.
[0054] Preparation of isolation film: The isolation film is 7 μm thick polyethylene (PE).
[0055] Preparation of electrolyte: In a dry argon atmosphere glove box, ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) were mixed in a mass ratio of EC:EMC:DEC=30:50:20, and then 1.5wt% of 1,3-propane sultone and 2wt% of fluoroethylene carbonate were added. After dissolving and stirring thoroughly, lithium salt LiPF6 was added and mixed evenly to obtain an electrolyte in which the concentration of LiPF6 was 1 mol / L.
[0056] Preparation of lithium-ion battery: stack the positive electrode, separator and negative electrode in order, so that the separator is between the positive electrode and the negative electrode to play a role of isolation, and wind them to obtain the electrode assembly. Place the electrode assembly in the outer packaging aluminum plastic film, remove moisture at 80°C, inject the above electrolyte and package, and obtain the lithium-ion battery through the process of formation, degassing, trimming and other processes.
[0057] Other embodiments and comparative examples are based on the steps of embodiment 1 with parameter changes, and the specific changed parameters are as follows.
[0058] The difference between Example 2 and Example 1 is that the negative electrode active material is a negative electrode active material containing hard carbon. The other parts are the same as Example 1. The preparation method of the negative electrode active material containing hard carbon is as follows:
[0059] 20g of hard carbon material was dispersed in 100mL of solvent to prepare solution A, wherein the solvent was distilled water; then, 2g of small molecule material (small molecule material was dihydrogen diamine) and a certain proportion of transition metal salt (Co(NO3)2·6H2O) were added to solution A to obtain a uniform solution B, wherein the mass ratio of transition metal in nitrate to small molecule material was 20%; solution B was stirred at 25° for 2h, then the temperature was raised to evaporate the solvent, and the obtained sample was calcined at 900 degrees in a N2 atmosphere for 2h. After cooling, the powder was passed through a 300 standard sieve to obtain a negative active material containing hard carbon.
[0060] Examples 3 to 7 are substantially the same as Example 2, except that the mass ratio of the transition metal to the small molecule material in the nitrate is different. The mass ratio of the transition metal to the small molecule material in the nitrate of Examples 3 to 7 is 10%, 5%, 2%, 1%, and 0%, respectively. Comparative Example 1 is the same as Example 1 except that the hard carbon in Example 1 is replaced with graphite.
[0061] The mass ratio of the small molecule material and the transition metal in the nitrate to the small molecule material in Examples 8 to 13 is different from that in Example 2, and the other aspects are the same as Example 2. The small molecule material in Examples 8 to 13 is replaced with o-phenylenediammonium. The mass ratio of the transition metal in the nitrate to the small molecule material in Examples 8 to 13 is 20%, 10%, 5%, 2%, 1%, and 0%, respectively.
[0062] The small molecule materials, nitrate types and / or the mass ratio of transition metals in nitrates to small molecule materials in Examples 14 to 33 are different from those in Example 2, and other aspects are the same as Example 2. Please refer to the table below for details.
[0063] The small molecule material, the mass ratio of the transition metal in the nitrate to the small molecule material, the Dv50 of the hard carbon particles, and the morphology and size of the carbon material in Example 34 are different from those in Example 5, and other aspects are the same as those in Example 5.
[0064] The test methods for various parameters of this application are described below.
[0065] Adhesion test:
[0066] The hard carbon negative electrode active material, styrene butadiene rubber (SBR) and sodium carboxymethyl cellulose (CMC) were fully stirred and mixed in an appropriate amount of deionized water at a weight ratio of 97:2:1 to form a uniform negative electrode slurry, wherein the solid content of the negative electrode slurry was 40wt%. The slurry was coated on the negative electrode current collector (6μm copper foil) on both sides, with a coating weight of 5mg / cm 2 Up to 8mg / cm 2 After coating, it is dried at 85°C, and then after cold pressing, cutting and slitting, it is dried under vacuum conditions at 120°C for 12 hours to obtain the negative electrode.
[0067] Use the negative electrode sheet obtained above (width 30 mm, length 100 mm to 160 mm), fix it on the steel plate with double-sided tape (model: 3M9448A, width 20 mm, length 90 mm to 150 mm), stick the tape on the surface of the negative active material layer, one side of the tape is connected to a paper tape of the same width, adjust the limit block of the tensile testing machine to a suitable position, fold the paper tape upward and slide 40 mm, the sliding rate is 50 mm / min, and test the bonding force between the negative active material layer and the negative current collector at 180° (i.e., stretching in the opposite direction).
[0068] Test of cohesion of negative electrode active materials:
[0069] The test was carried out using an Instron (model 33652) tester: take the negative electrode (width 30 mm, length 100 mm to 160 mm), fix it on a steel plate with double-sided tape (model: 3M9448A, width 20 mm, length 90 mm to 150 mm), stick the tape on the surface of the negative electrode active material layer, and connect one side of the tape to a paper tape of the same width. Adjust the limit block of the tensile testing machine to a suitable position, fold the paper tape upward and slide 40 mm, with a sliding rate of 50 mm / min, and test the polymerization strength between the negative electrode active materials inside the negative electrode active material layer at 180° (i.e., stretching in the opposite direction).
[0070] Diaphragm resistance test:
[0071] The area is 154mm 2The negative electrode disc is tested at room temperature, 0.4T and 26MPa. Ten points at different positions are taken for each test and the average value is taken.
[0072] Belt break test:
[0073] The tape breakage mentioned here refers to the brittle breakage of the negative electrode during the process of passing through the cold pressing roller and before winding. The negative electrode current collector is 6μm copper foil, and the single-sided coating weight of the negative electrode is between 5mg / cm 2 Up to 8mg / cm 2 The negative electrode material in the negative electrode is a hard carbon material, and its 5-ton powder compaction density is between 0.9g / cm 3 Up to 1.2g / cm 3 ; The cold pressing density of the negative electrode during the cold pressing process is between 0.9g / cm 3 Up to 1.2g / cm 3 The tension of the winding device of the cold pressing equipment is between 3N and 10N.
[0074] The belt breakage is divided into severe belt breakage, moderate belt breakage, and mild belt breakage according to the degree of the belt breakage; during the cold pressing process of every 10 meters of negative electrode, if the negative electrode has 4 or more brittle breaks, it is a severe belt break, if it has 2 to 3 brittle breaks, it is a moderate belt break, and if it has 1 brittle break, it is a mild belt break.
[0075] Capacity retention rate of lithium-ion battery after 400 cycles:
[0076] Place the lithium-ion battery in a 45℃ constant temperature box and let it stand for 30 minutes. After the lithium-ion battery reaches a constant temperature, test the initial thickness of the battery. Charge the lithium-ion battery that has reached a constant temperature at a constant current of 0.5C to a voltage of 4.2V, then charge it at a constant voltage of 4.2V to a current of 0.05C, and then discharge it at a constant current of 1C to a voltage of 3.0V. This is a charge and discharge cycle. With the capacity of the first discharge as 100%, repeat the charge and discharge cycle for 400 times, stop the test, record the cycle capacity retention rate, and measure the battery thickness at the same time. The capacity retention rate and thickness expansion rate are used as indicators to evaluate the cycle performance of lithium-ion batteries.
[0077] Cycle capacity retention rate = capacity at 400 cycles / capacity at first discharge × 100%.
[0078] The thickness expansion rate of lithium-ion batteries is calculated as follows:
[0079] Thickness change of lithium-ion battery after 400 cycles = (battery thickness after 400 cycles - initial battery thickness) / initial battery thickness × 100%.
[0080] The calculation formula for the compaction density described in the article is: compaction density = mass of negative electrode material / force-bearing area of negative electrode material / thickness of sample; the calculation formula for the cold pressing compaction density is: cold pressing compaction density = mass of negative electrode material / force-bearing area of negative electrode material / thickness of sample.
[0081] Table 1 shows various parameters and evaluation results of Examples 1 to 13 and Comparative Example 1.
[0082] Table 1
[0083]
[0084]
[0085] Table Notes: The mass content of transition metal elements and nitrogen elements refer to the mass ratio of transition metal elements to nitrogen elements in the whole negative electrode active material in the calcined sample. The mass ratio of transition metal elements to small molecule materials in nitrate refers to the ratio of the weight of transition metals to the weight of small molecule materials in the whole nitrate. For example, in Example 3, the weight of the added nitrate is 2g, of which the weight of Co element is (2g×59) / 291=0.4g, and the weight of the added small molecule material is 2g, so the ratio of transition metals to small molecules in nitrate is 0.4g / 2g=20% (the calculation method of other embodiments is the same). In this application, theoretically all diamines can be used (all carbon-containing small molecules with amino groups can be used), because small molecules contain N and can combine with transition metal elements.
[0086] By comparing Example 1 and Comparative Example 1, it can be seen that by using hard carbon as the negative electrode active material, the bonding force between the negative electrode active material layer and the negative electrode current collector is significantly increased. In addition, compared with graphite materials, the smaller the film resistance of the hard carbon material, the better its rapid charge and discharge performance.
[0087] By comparing Examples 1, 2 and 3, it can be seen that by using the modified hard carbon composite particles as the negative electrode active material, the bonding force between the negative electrode active material layer and the negative electrode current collector can be further increased compared to using hard carbon. There is basically no band breakage in Examples 2 and 3. The content of transition metal nitrate cannot be too high. If it is too high, the content of transition metal in the composite particles will be too high, and the transition metal will agglomerate into small particles, which will affect the contact between the small molecule converted carbon material and the hard carbon substrate.
[0088] Graphite materials are soft and will not break during processing. In comparison, hard carbon materials are hard and have sharp edges and corners, which will cause serious band breaking. The reason why the hard carbon in Example 1 breaks seriously due to its hardness and sharp edges and corners is that there is no slip and buffer space between particles during processing due to its hardness, which leads to large stress between particles and brittle fracture. Examples 2 to 6 and 8 to 12 grow carbon materials that can assist slip and buffer stress between particles in situ on the surface of hard carbon, wrapping the sharp edges and corners of the hard carbon substrate, thereby improving the problem of sharp edges and corners of the hard carbon substrate, enhancing the bonding force between the particles and the current collector, and at the same time improving the situation of band breaking during processing, so its processing performance is improved and there is no situation of band breaking during processing. However, since only small molecules are added but no transition metal salts are added in Examples 7 and 13, the small molecules are completely volatilized during the calcination process, and carbon materials cannot be grown on the surface of the hard carbon, so the problem of band breaking during processing is not solved.
[0089] Comparative Example 1 is graphite that has not been modified with small molecules and nitrates. Its bonding force is lower than that of hard carbon, but because graphite is soft and has a layered structure, it can slip during the cold pressing process so that no band breakage occurs. However, compared with hard carbon, especially modified hard carbon, the film resistance of graphite is larger, which is not conducive to the output of fast charge and discharge performance.
[0090] Table 2 shows various parameters and evaluation results of Examples 14 to 33 and Comparative Example 1.
[0091] Table 2
[0092]
[0093] Table 2 expands the cobalt nitrate in Table 1 to other nitrates such as iron nitrate and zinc nitrate. By expanding the transition metal elements in the transition metal nitrate from Co to Fe and Zn, the purpose of improving processing performance and reducing membrane resistance can still be achieved, and the band breaking situation of the electrode composed of the obtained negative electrode active material is improved. By comparing Examples 14 to 18, it can be seen that as the content of the transition metal salt gradually increases, the bonding force and cohesive strength of the electrode composed of the obtained negative electrode active material are improved, and the processing band breaking situation is also improved. By comparing Examples 14 to 18 with 19 to 23, it can be seen that by using different types of small molecule materials, the same rules as Examples 14 to 18 can be obtained. Similarly, by comparing Examples 24 to 28 and Comparative Examples 29 to 33, it can be seen that by using different types of transition metal salts, the same rules as Examples 14 to 18 can also be obtained.
[0094] Table 3 shows various parameters and evaluation results of Examples 1, 3, 9, 34 and Comparative Example 1.
[0095] Table 3
[0096]
[0097] It can be seen from Table 3 that by fixing the transition metal nitrate and changing the type of small molecule material, different morphologies can be grown on the surface of the hard carbon particles, and the purpose of improving the processing performance can be achieved. The band breaking condition of the electrode composed of the obtained negative active material is improved, and its membrane resistance is reduced, and the overall performance of the battery is better.
[0098] Table 4 shows various parameters and evaluation results of Examples 35 to 37 and Example 1.
[0099]
[0100]
[0101] Table Notes: Compared with Example 3, Examples 35 to 37 differ only in that the electrolyte compositions are different as shown in Table 4.
[0102] As shown in Table 4, by comparing Example 1 with Comparative Example 1, the graphite material forms a LiC6 intercalation compound after lithium insertion, and has a certain volume expansion. Therefore, as the number of cycles of the lithium-ion battery increases, the thickness of the lithium-ion battery increases. After 400 cycles, the thickness increases by 12%. 002 The large interplanar spacing (about 0.36nm to 0.4nm), the presence of a large number of micropores and their isotropic properties make the hard carbon material almost unchanged in volume after lithium insertion, and the electrode thickness change after 400 cycles is small, less than or equal to 5%. Especially after being modified with small molecule carbon materials, the buffer between its particles is increased and the volume expansion change is smaller.
[0103] On the other hand, Examples 35 to 37 show that by changing the lithium salt concentration and composition of the electrolyte, the thickness expansion is suppressed, and the cycle performance and thickness expansion performance are better.
[0104] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of disclosure involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but also should cover other technical solutions formed by any combination of the above technical features or their equivalent features. For example, the above features are replaced with the technical features with similar functions disclosed in the present application.
Claims
1. A negative electrode, comprising a negative electrode current collector and a negative electrode active material layer, wherein the negative electrode active material layer comprises a negative electrode active material, and the bonding force between the negative electrode active material layer and the negative electrode current collector is greater than or equal to 7 N / m; The negative electrode active material includes hard carbon, a carbon material is in situ grown on the surface of the hard carbon, the carbon material includes at least one of a flaky carbon material or a granular carbon material, the length of the flaky carbon material is greater than 1 μm, and the average particle size of the granular carbon material is 50 nm to 500 nm.
2. The negative electrode according to claim 1, wherein The bonding force between the negative electrode active material layer and the negative electrode current collector is greater than or equal to 10 N / m.
3. The negative electrode according to claim 1, wherein Satisfies at least one of conditions (b) to (d): (b) the Dv50 of the negative electrode active material is 6 μm to 20 μm; (c) the negative electrode active material further comprises nitrogen and a transition metal element; (d) The cohesive force of the negative electrode active material is 5 N / m to 100 N / m.
4. The negative electrode according to claim 3, wherein Satisfy at least one of conditions (e) to (h): (e) the carbon material grown in situ on the surface also includes fibrous carbon material; (f) the mass percentage of the transition metal element in the negative electrode active material is 0.1% to 10%, and the mass percentage of the nitrogen element in the negative electrode active material is 0.1% to 5%; (g) the transition metal element comprises at least one of Co, Fe, Cr, Pt, Cu, Mn, Ag, Ni or Zn; (h) The mass percentage of the nitrogen element or the transition metal element in the particles of the negative electrode active material gradually decreases from the surface of the particles of the negative electrode active material to the center of the particles of the negative electrode active material.
5. The negative electrode according to claim 4, wherein The diameter of the fibrous carbon material is 50 nm to 500 nm, and the length is greater than 1 μm. 6 . An electrochemical device comprising an electrolyte, a separator, a positive electrode, and the negative electrode according to claim 1 , wherein the separator is disposed between the positive electrode and the negative electrode.
7. The electrochemical device according to claim 6, wherein: The electrolyte includes at least one of fluoroether, fluoroethylene carbonate or ether nitrile.
8. The electrochemical device according to claim 6, wherein: The electrolyte includes a lithium salt, wherein the lithium salt includes lithium bis(fluorosulfonyl)imide and lithium hexafluorophosphate, the concentration of the lithium salt is 1 mol / L to 2 mol / L, and the molar ratio of the lithium bis(fluorosulfonyl)imide to the lithium hexafluorophosphate is 0.05 to 4.
9. An electronic device comprising the electrochemical device according to any one of claims 6 to 8.
Citation Information
Patent Citations
Negative electrode piece and secondary battery
CN109494349A
KR20200078397A