A polymerizable electrolyte and its preparation method and application

By using boron trifluoride salt as an electrolyte additive or salt in secondary batteries, a stable passivation film and high conductivity electrolyte are formed, which solves the energy density and safety of liquid electrolytes, and improves the electrochemical performance and use of the battery. Lifespan, suitable for a variety of battery types.

CN114649570BActive Publication Date: 2024-11-26BEIJING WELION NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011491494.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-17
Publication Date
2024-11-26
Estimated Expiration
2040-12-17

AI Technical Summary

Technical Problem

The existing secondary batteries have low energy density and poor safety. The solid electrolyte still has shortcomings in taking into account high energy density, long cycle stability and safety, especially insufficient ionic conductivity and migration number.

Method used

Develop a polymerizable electrolyte containing a boron trifluoride salt structure, which is an additive or salt of the electrolyte, which can form a stable passivation film on the electrode surface, widen the electrochemical window, and provide high ionic conductivity as a single ion conductor, combined with Polymer groups form polymer frameworks to improve mechanical properties.

Benefits of technology

It significantly improves the discharge specific capacity, Coulomb efficiency and cycling performance of the battery, extends the service life of the battery, and improves the comprehensive performance of the battery through high ionic conductivity and mechanical properties. It is suitable for liquid, mixed solid-liquid, gel and all-solid state Battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114649570B_ABST
    Figure CN114649570B_ABST
Patent Text Reader

Abstract

The present application provides a polymerizable electrolyte and a preparation method and application thereof. The electrolyte includes a boron trifluoride salt, and the structure of the boron trifluoride salt is shown in general formula I. The electrolyte provided in the present application has a polymerizable group and a functionalized group, so that it has a variety of applications in batteries. It can be used as a functional additive to form a passivation film on the electrode surface to prevent the electrode from decomposing the components of the electrolyte; it can be used as a main salt, the main function of which is to provide the battery with transportable ions, and the secondary function is to form a passivation film on the electrode surface; it can be polymerized in situ / ex situ to form a single ion conductor polymer electrolyte and a polymer skeleton application, providing the battery with higher ionic conductivity, higher electrochemical stability, and better mechanical properties. Therefore, the battery prepared from the electrolyte has excellent long cycle stability, good battery life, and the raw material price is low, with good economic benefits. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a polymerizable electrolyte and a preparation method and application thereof. Background Art

[0002] Secondary batteries have been rapidly developed and their application scope is becoming wider and wider due to their advantages such as high energy density, long life and no memory effect. At present, secondary batteries are mainly liquid batteries, but liquid batteries have low energy density and poor safety. This is mainly because the electrochemical window of the liquid electrolyte currently used is narrow and cannot match the use of high-voltage positive electrode materials (such as high-voltage lithium cobalt oxide, lithium nickel manganese oxide, etc.); organic solvents have low boiling points and are prone to leakage, fire and explosion hazards; conventional salts are easy to decompose at high temperatures (such as lithium hexafluorophosphate), easily corrode aluminum foil (such as lithium bis(trifluoromethyl)sulfonyl imide, lithium bis(fluorosulfonyl imide), and easily produce gas (such as lithium difluoro oxalate phosphate), which affects the battery life.

[0003] There are currently two main solutions. One is to add some functional additives to the liquid electrolyte. The functional additives can form a passivation film on the electrode surface, which effectively alleviates the catalytic decomposition of the liquid electrolyte by the electrode. However, the passivation layer formed on the electrode surface by the conventional functional additives after decomposition is not dense, and the ions from the positive electrode are consumed in the process of forming the passivation layer, so the first-week efficiency and discharge specific capacity are low. The second is to develop solid-state batteries, that is, to replace the liquid electrolyte that transmits ions with solid electrolytes. Solid electrolytes greatly improve the safety of the battery, are not prone to thermal runaway, and have good high-temperature stability. Currently, commonly used solid electrolytes include oxide electrolytes, sulfide electrolytes, and polymer electrolytes. Among them, oxide electrolytes have a wide electrochemical window, but are too rigid; sulfide electrolytes are plastic, but have a narrow electrochemical window and are very easy to produce hydrogen sulfide gas; polymer electrolytes have good mechanical properties, but low ionic conductivity and low ion migration number. Worldwide, all-solid-state batteries are in their infancy and still cannot take into account high energy density, long cycle, and intrinsic safety. At present, hybrid solid-liquid and gel batteries are more developed, which can take into account the advantages of liquid batteries and all-solid-state batteries. However, the disadvantages of liquid electrolytes still determine the performance of batteries. Therefore, it is urgent to develop additives with good thermal stability, stable passivation layer, and self-providing ions, develop new salts with good stability and high conductivity, and develop single ion conductors with high ion conductivity and high migration number. Summary of the invention

[0004] In view of this, the embodiments of the present application provide a polymerizable electrolyte and a preparation method and application thereof to solve the technical defects existing in the prior art.

[0005] The present application provides a polymerizable electrolyte, the electrolyte comprising a boron trifluoride salt, the structure of the boron trifluoride salt being as shown in general formula I:

[0006]

[0007] Among them, R + Any one selected from monovalent positive metal cations, R1 selected from any one of a blank, a first ring or a chain containing a substituent or not containing a substituent, and R2 selected from a second ring containing a substituent or not containing a substituent capable of polymerization;

[0008] The first ring includes a ring composed of carbon atoms and a ring containing at least one heteroatom, the chain includes a chain composed only of carbon atoms and a chain containing at least one heteroatom, and the substituent includes a cyclic substituent, a chain substituent and a halogen atom.

[0009] Furthermore, R + Any one selected from sodium ion, lithium ion, and potassium ion;

[0010] The first ring is a three-membered ring to a sixteen-membered ring, the first ring includes a saturated carbocyclic ring, an unsaturated carbocyclic ring, a saturated heterocyclic ring, and an unsaturated heterocyclic ring, the chain is a chain composed of 1 to 20 atoms, the chain composed only of carbon atoms and the chain containing at least one heteroatom both include a saturated chain and an unsaturated chain containing an unsaturated bond, and the unsaturated bond includes a double bond and / or a triple bond;

[0011] The second ring is a three-membered ring to a ten-membered ring, and the second ring is selected from any one of cycloolefin, cyclic ether, cyclic acetal, cyclic ester, cyclic anhydride, cyclic carbonate, cyclic amide, cyclic amine, cyclic thioether, cyclic disulfide, cyclosiloxane, and cyclic phosphazene;

[0012] The cyclic substituents include substituted or unsubstituted three-membered rings to twenty-membered rings, and polycyclic substituents containing two or more ring structures at the same time;

[0013] The chain substituents include substituted or unsubstituted alkyl, heteroalkyl, alkenyl, heteroalkenyl, alkynyl, alkenynyl, alkylthio, C═O substituents, ═O, and ═S.

[0014] Further, in the case where R2 is selected from cycloolefin, R2 is a four-membered ring, a five-membered ring, a seven-membered ring, an eight-membered ring, a nine-membered ring or a ten-membered ring containing or not containing a substituent;

[0015] In the case where R2 is selected from cyclic ethers, R2 is a three-membered ring, a four-membered ring, a five-membered ring or a seven-membered ring which may or may not contain a substituent;

[0016] In the case where R2 is selected from cyclic acetals, R2 is a 6-membered ring or an 8-membered ring which may or may not contain a substituent;

[0017] In the case where R2 is selected from cyclic esters, R2 is a four-membered ring, a six-membered ring, a seven-membered ring or an eight-membered ring which may or may not contain a substituent;

[0018] In the case where R2 is selected from cyclic anhydrides, R2 is a 5-membered ring, a 7-membered ring or an 8-membered ring which may or may not contain a substituent;

[0019] In the case where R2 is selected from cyclic carbonates, R2 is a 6- to 8-membered ring which may be substituted or unsubstituted;

[0020] In the case where R2 is selected from cyclic amides, R2 is a four-membered to eight-membered ring containing or not containing a substituent;

[0021] In the case where R2 is selected from cyclic amines, R2 is a three-membered ring, a four-membered ring or a seven-membered ring containing or not containing a substituent;

[0022] In the case where R2 is selected from cyclic thioethers, R2 is a three-membered ring or a four-membered ring containing or not containing a substituent;

[0023] In the case where R2 is selected from cyclic disulfide, R2 is a four-membered to eight-membered ring containing or not containing a substituent;

[0024] In the case where R2 is selected from cyclosiloxane, R2 is a 6-membered ring, an 8-membered ring or a 10-membered ring which may or may not contain a substituent;

[0025] When R2 is selected from cyclic phosphazene, R2 is a six-membered ring which may be substituted or unsubstituted.

[0026] Further, in the case where R2 is selected from cycloolefin, the structure of Formula I comprises:

[0027]

[0028] In the case where R2 is selected from cyclic ethers, the structure of Formula I comprises:

[0029]

[0030]

[0031] In the case where R2 is selected from cyclic acetals, the structure of Formula I comprises:

[0032]

[0033] In the case where R2 is selected from cyclic esters, the structure of Formula I comprises:

[0034]

[0035] In the case where R2 is selected from cyclic anhydrides, the structure of Formula I comprises:

[0036]

[0037] In the case where R2 is selected from cyclic carbonates, the structure of Formula I comprises:

[0038]

[0039]

[0040] In the case where R2 is selected from cyclic amides, the structure of Formula I comprises:

[0041]

[0042] In the case where R2 is selected from cyclic amines, the structure of Formula I comprises:

[0043]

[0044] In the case where R2 is selected from cyclic thioethers, the structure of general formula I includes:

[0045]

[0046] In the case where R2 is selected from cyclic disulfide, the structure of Formula I includes:

[0047]

[0048] In the case where R2 is selected from cyclosiloxane, the structure of Formula I comprises:

[0049]

[0050] In the case where R2 is selected from cyclic phosphazene, the structure of general formula I includes:

[0051]

[0052] Among them, Q represents

[0053] R3, R4, R5, R6, R7, R8, R9, R 10 They are all selected from any one or a combination of hydrogen atoms, rings or chains with or without substituents, halogen atoms, and metal cations.

[0054] Further, the chain substituent includes hydrogen atom, halogen atom, ether oxygen bond / group, ether sulfur bond / group, nitro group, amide, sulfonamide group, sulfonyl group, sulfonic acid group, salt substituent, C=O substituent, N substituent, alkyl group, heteroalkyl group, alkenyl group, heteroalkenyl group, alkynyl group, alkenynyl group, =O, =S;

[0055] The cyclic substituents include three-membered rings, four-membered rings, five-membered rings, six-membered rings, seven-membered rings, eight-membered rings, and polycyclic substituents containing two or more ring structures at the same time;

[0056] The halogen atom includes a chlorine atom, a bromine atom, an iodine atom, and a fluorine atom.

[0057] Furthermore, the substituents include:

[0058] hydrogen atom, methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, n-pentyl, isopentyl, sec-pentyl, neopentyl, n-hexyl, isohexyl, sec-hexyl, neohexyl, n-heptyl, isoheptyl, sec-heptyl, neoheptyl, n-octyl, isooctyl, sec-octyl, neooctyl, vinyl, propenyl, butenyl, pentenyl, hexenyl, heptenyl, ethynyl, propynyl, butynyl, pentynyl, hexynyl, heptynyl, cyclohexyl, cyclopentyl, phenyl, ester group, sulfoalkane, amide group, sulfonamide group, sulfonyl, sulfonic acid group, aldehyde group, ether oxygen bond / group, ether sulfur bond / group, nitro group, -COOCH3, COOCH2CH3, -SCH3, =O, -N(CH3)2, -CO-N(CH3)2, -S-, -O-,

[0059] Furthermore, all or part of the hydrogen atoms on all carbon atoms in any one of the general formulas I are independently replaced by halogen atoms;

[0060] Preferably, all or part of the hydrogen atoms on all carbon atoms in any one of the general formulas I are independently replaced by fluorine atoms.

[0061] The present application also provides a method for preparing a polymerizable electrolyte according to any of the above paragraphs, the method comprising: preparing a monovalent structure containing a -OH group, a boron trifluoride compound and R + The product of the source reaction is a The structure of the boron trifluoride salt.

[0062] The present application also provides an application of a polymerizable electrolyte according to any of the above paragraphs in a secondary battery, wherein the application is as follows: the boron trifluoride salt can be used as an electrolyte additive and also as a salt, and the monomer containing a polymerizable group can also be used as a single ion conductor and polymer framework after polymerization.

[0063] Further, the application includes application in liquid electrolyte, gel electrolyte, mixed solid-liquid electrolyte, quasi-solid electrolyte, and all-solid electrolyte, and the liquid electrolyte, gel electrolyte, mixed solid-liquid electrolyte, quasi-solid electrolyte, and all-solid electrolyte independently include the electrolyte described in any of the above paragraphs;

[0064] Preferably, the application also includes application as a battery or a battery pack, the battery includes the electrolyte as described in any of the above paragraphs and the positive electrode, the negative electrode and the packaging shell; the liquid electrolyte, gel electrolyte, mixed solid-liquid electrolyte, quasi-solid electrolyte, all-solid electrolyte can be applied to liquid batteries, mixed solid-liquid batteries, semi-solid batteries, gel batteries, quasi-solid batteries and all-solid batteries, and the battery pack includes the battery.

[0065] Technical effects:

[0066] The boron-containing organic compound provided in the present application can be used as an additive in a battery, which can form a stable and dense passivation film on the electrode surface of the battery, hindering the direct contact between the electrolyte and the electrode active material, inhibiting the decomposition of the various components of the electrolyte, and widening the electrochemical window of the entire electrolyte system, which can significantly improve the discharge capacity, coulomb efficiency and cycle performance of the battery; in addition, the boron-containing organic compound itself is an ion conductor. As an additive, it forms a passivation layer on the electrode surface while consuming less active ions released from the positive electrode, which can significantly improve the first coulomb efficiency and the first week discharge capacity of the battery. When the electrolyte containing the boron-containing organic compound and the existing high-voltage and high-specific-capacity positive electrode materials and low-voltage and high-specific-capacity negative electrode materials are compounded into a battery, the electrochemical performance of the battery is improved. In addition, the structure of the present application can also be mixed with conventional additives, that is, double additives or multiple additives, and the battery using double additives or multiple additives shows better electrochemical performance.

[0067] The boron-containing organic compound provided in the present application can be used as the main salt in the battery. The ions contained in the compound are easily dissociated, so the ionic conductivity is high and the assembled battery has excellent electrochemical performance.

[0068] If the boron-containing organic compound provided in the present application contains a polymerizable group, it can also form a single ion conductor and a polymer skeleton after polymerization, which can not only provide good ion conductivity, but also provide good mechanical properties, and the overall performance of the battery is good.

[0069] In addition, the boron trifluoride salt in the present application has abundant raw material sources, wide raw material selectivity, low cost, simple preparation process, simple reaction conditions and mild conditions, and has excellent industrial application prospects.

[0070] In addition, the present application can also use metals other than traditional lithium such as sodium and potassium to form salts, which provides more possibilities for the later application, cost control or raw material selection of the present application, which is of great significance.

[0071] Therefore, the polymerizable electrolyte provided in the present application can be applied to liquid batteries, hybrid solid-liquid batteries, gel batteries, quasi-solid-state batteries, and all-solid-state batteries, and can improve the electrochemical performance of the battery, including increasing the energy density of the battery, improving the cycle stability, and extending the service life of the battery. In addition, the synthesis process is simple, the raw material price is low, and it has good economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0072] Figures 1 to 12 is the H NMR spectrum of the products shown in Examples 1 to 12;

[0073] Figure 13 to Figure 16 The figures are respectively the effect comparison diagrams of the batteries 1 / 6 / 9 / 14 made by using the embodiments 1 / 6 / 9 / 14 as liquid electrolyte additives and the corresponding comparative batteries 1 / 4 / 7 / 11 not containing the embodiments of the present invention;

[0074] Figures 17-18 They are comparison diagrams of the effects of battery 1 / 7 made of Example 1 / 7 as liquid electrolyte salt and corresponding comparative battery 1 / 7 not containing the liquid electrolyte salt of the embodiment of the present invention;

[0075] Fig.19 This is a rendering of a polymer electrolyte battery 2 made using the monomer in Example 2 as a polymerized monomer;

[0076] Fig. 20 This is a diagram showing the effect of a polymer electrolyte battery 10 made by using the monomer in Example 10 as a polymerized monomer. DETAILED DESCRIPTION

[0077] The specific implementation of the present application is described below in conjunction with the accompanying drawings.

[0078] In the present invention, unless otherwise specified, the scientific and technical terms used herein have the meanings commonly understood by those skilled in the art. In addition, the reagents, materials and operating procedures used herein are reagents, materials and conventional procedures widely used in the corresponding fields. At the same time, in order to better understand the present invention, the definitions and explanations of the relevant terms are provided below.

[0079] In the present invention, if a group needs to be connected to two parts of the structure, it has two connecting bonds to be connected. If it is not clearly stated which two atoms are connected to the connected parts, any atom containing H can be connected.

[0080] In the present invention, if a C contains multiple H groups, any one or several of the multiple H groups may be substituted by a substituent, or all of the H groups may be substituted by a substituent. When two or more H groups are substituted by a substituent, the substituents may be the same or different. R 01 and R02 All of them indicate that the C to which they are connected can be substituted by one substituent or two substituents. For example, if R 01 is methyl, R 02 is F, then the above structure can be If R 01 For H, R 02 is methyl and F, then the above structure can be

[0081] In the present invention, if the chemical bond is not drawn on the atom, but drawn at the position where it intersects with the bond, such as Any H on cyclohexane can be replaced by a substituent R 04 Substitution can be substituted, and can replace one H or two or more H, and the substituents can be the same or different. If a C of cyclohexane contains two H, then both hydrogen H can be replaced by substituents, or only one can be replaced, such as both H can be replaced by methyl, or one can be replaced by methyl and the other by ethyl. In addition, the substituent can also be connected to the ring through a double bond. For example, in this structure, if R 04 is methyl, =O, F, then the above structure can be

[0082] The "Et" is an ethyl group, and the "Ph" is a phenyl group.

[0083] In the structural formula of the present invention, if a group in brackets "()" is behind an atom, it means that the group in brackets is connected to the atom in front of it. -CH(CH3)- is

[0084] The "boron trifluoride compound" refers to boron trifluoride, a compound containing boron trifluoride, a boron trifluoride complex, and the like.

[0085] The invention is to provide a monobasic organic boron trifluoride salt which can be used as an electrolyte additive, an electrolyte salt and a polymerizable monomer. Group, where R + Can be Li + 、Na + The boron trifluoride salt can be used in liquid batteries, hybrid solid-liquid batteries, semi-solid batteries, gel batteries, quasi-solid batteries and all-solid batteries. The preparation method of the compound is simple, ingenious and has a high yield. + The raw material is obtained by reacting with the source, specifically, the -OH in the raw material participates in the reaction, and other structures do not participate in the reaction. There are two specific preparation methods:

[0086] 1. Under nitrogen / argon atmosphere, R+ The source and the raw material are added to a solvent, mixed, reacted at 5-60° C. for 3-24 hours, and the obtained mixed solution is dried under reduced pressure at 20-80° C. and a vacuum degree of about -0.1 MPa to remove the solvent to obtain an intermediate; then a boron trifluoride compound is added, stirred at 5-60° C. and reacted for 6-24 hours, and the obtained mixed solution is dried under reduced pressure at 20-80° C. and a vacuum degree of about -0.1 MPa to obtain a crude product, and the crude product is washed, filtered, and dried to obtain a final product, a monobasic organic boron trifluoride salt, with a yield of 70-95%.

[0087] 2. In a nitrogen / argon atmosphere, the raw materials and the boron trifluoride compound are added to the solvent, mixed evenly, and reacted at 5-60°C for 6-24 hours. The obtained mixed solution is dried under reduced pressure at 20-80°C and a vacuum degree of about -0.1 MPa to remove the solvent to obtain an intermediate; R + The source is added to the solvent, and then the R + The solvent of the source is added to the intermediate, and the reaction is stirred at 5-60° C. for 3-24 hours to obtain a crude product. The crude product is washed directly or washed after reduced pressure drying, and then filtered and dried to obtain the final product, monobasic organic boron trifluoride salt, with a yield of 70-95%.

[0088] In the above two specific preparation methods, the boron trifluoride compounds may include boron trifluoride ether complex, boron trifluoride tetrahydrofuran complex, boron trifluoride butyl ether complex, boron trifluoride acetic acid complex, boron trifluoride monoethylamine complex, boron trifluoride phosphate complex, and the like. + Sources include metallic lithium / sodium, lithium / sodium methoxide, lithium / sodium hydroxide, lithium / sodium ethoxide, butyl lithium / sodium, lithium / sodium acetate, etc. The solvents described in each place are independently alcohols (some liquid alcohol raw materials can also be solvents at the same time), ethyl acetate, DMF, acetone, hexane, dichloromethane, tetrahydrofuran, ethylene glycol dimethyl ether, etc. For washing, low polar solvents such as diethyl ether, n-butyl ether, n-hexane, diphenyl ether, etc. can be used.

[0089] Example 1

[0090] raw material

[0091] Preparation method: Under nitrogen atmosphere, mix the raw material (0.88g, 0.01mol) and lithium hydroxide (0.24g, 0.01mol) with 10ml methanol solution, and react at 15°C for 8 hours. The obtained mixed solution is dried under reduced pressure at 30°C and a vacuum degree of about -0.1MPa to remove the solvent to obtain an intermediate. Boron trifluoride ether complex (1.45g, 0.01mol) and 15ml THF (tetrahydrofuran) are added to the intermediate, stirred at 40°C for 6 hours, and the obtained mixed solution is dried under reduced pressure at 30°C and a vacuum degree of about -0.1MPa. The obtained crude product is filtered and dried with dichloromethane to obtain product A1. The yield is 86%, and the nuclear magnetic resonance is as follows Figure 1 shown.

[0092] Example 2

[0093] raw material

[0094] Preparation method: Under nitrogen atmosphere, mix the raw material (0.90g, 0.01mol) and boron trifluoride tetrahydrofuran complex (1.40g, 0.01mol) in 15ml of ethylene glycol dimethyl ether and react at room temperature for 10 hours. The obtained mixed solution is dried under reduced pressure at 40°C and a vacuum degree of about -0.1MPa to remove the solvent to obtain an intermediate. Lithium ethoxide (0.52g, 0.01mol) is dissolved in 10ml of ethanol and slowly added to the intermediate. Stir and react at 45°C for 8 hours. The obtained mixed solution is dried under reduced pressure at 45°C and a vacuum degree of about -0.1MPa. The obtained solid is washed three times with n-butyl ether, filtered and dried to obtain product A2. The yield is 80%, and the nuclear magnetic resonance is as follows Figure 2 shown.

[0095] Example 3

[0096] raw material

[0097] Preparation method: Under argon atmosphere, mix the raw material (1.15g, 0.01mol) and boron trifluoride ether complex (1.49g, 0.0105mol) in 15ml THF (tetrahydrofuran) and react at room temperature for 12 hours. The obtained mixed solution is dried under reduced pressure at 30°C and a vacuum degree of about -0.1MPa to remove the solvent to obtain an intermediate. Add 6.25ml of butyl lithium hexane solution (c=1.6mol / L) to the intermediate, stir and react at room temperature for 7 hours, and dry the obtained mixed solution under reduced pressure at 30°C and a vacuum degree of about -0.1MPa. The obtained crude product is washed 3 times with cyclohexane, filtered and dried to obtain product A3. The yield is 89%, and the nuclear magnetic resonance is as follows Figure 3 shown.

[0098] Example 4

[0099] raw material

[0100] Preparation method: Under nitrogen atmosphere, take a certain amount of raw material (0.74g, 0.01mol) and lithium methoxide (0.38g, 0.01mol), mix them evenly with 20ml methanol, and react at room temperature for 10 hours. The obtained mixed solution is dried under reduced pressure at 40°C and a vacuum degree of about -0.1MPa to remove the solvent to obtain an intermediate. Boron trifluoride tetrahydrofuran complex (1.40g, 0.01mol) and 15ml THF (tetrahydrofuran) are added to the intermediate, stirred at room temperature for 6 hours, and the obtained mixed solution is dried under reduced pressure at 40°C and a vacuum degree of about -0.1MPa. The obtained solid is washed three times with isopropyl ether, filtered, and dried to obtain product A4. The yield is 81%, and the nuclear magnetic resonance is as follows Figure 4 shown.

[0101] Example 5

[0102] raw material

[0103] Preparation method: Under nitrogen atmosphere, mix the raw material (0.91g, 0.01mol) and lithium hydroxide (0.24g, 0.01mol) with 10ml methanol solution and react at room temperature for 8 hours. The obtained mixed solution is dried under reduced pressure at 40°C and a vacuum degree of about -0.1MPa to remove the solvent to obtain an intermediate. Add boron trifluoride phosphate complex (1.66g, 0.01mol) and 15mlTHF to the intermediate, stir and react at 45°C for 6 hours, and dry the obtained mixed solution under reduced pressure at 60°C and a vacuum degree of about -0.1MPa. The obtained crude product is filtered and dried with dichloromethane to obtain product A5. The yield is 85%, and the nuclear magnetic resonance is as follows Figure 5 shown.

[0104] Example 6

[0105] raw material

[0106] Preparation method: Under argon atmosphere, mix the raw material (0.88g, 0.01mol) and boron trifluoride acetic acid complex (1.92g, 0.0102mol) in 15ml THF (tetrahydrofuran) and react at room temperature for 12 hours. The obtained mixed solution is dried under reduced pressure at 40°C and a vacuum degree of about -0.1MPa to remove the solvent to obtain an intermediate. Lithium acetate (0.68g, 0.0102mol) is dissolved in 10ml of N,N-dimethylformamide and added to the intermediate. Stir and react at 50°C for 8 hours. The obtained mixed solution is dried under reduced pressure at 80°C and a vacuum degree of about -0.1MPa. The obtained solid is washed three times with diphenyl ether, filtered and dried to obtain product A6. The yield is 78%, and the nuclear magnetic resonance is as follows: Figure 6 shown.

[0107] Example 7

[0108] raw material

[0109] Preparation method: Under argon atmosphere, lithium methoxide (0.38 g, 0.01 mol) was dissolved in 15 ml of methanol, mixed evenly, added to the raw material (1.04 g, 0.01 mol) and mixed evenly, reacted at 45°C for 12 hours, and the resulting mixed solution was dried under reduced pressure at 45°C and a vacuum degree of about -0.1 MPa to remove the solvent to obtain an intermediate. Boron trifluoride ether complex (1.45 g, 0.01 mol) and 15 ml of THF were added to the intermediate, stirred at room temperature for 24 hours, and the resulting mixed solution was dried under reduced pressure at 40°C and a vacuum degree of about -0.1 MPa. The obtained solid was washed three times with dichloromethane, filtered, and dried to obtain the product A7. The yield was 75%, and the NMR was as follows Figure 7 shown.

[0110] Example 8

[0111] raw material

[0112] Preparation method: Under nitrogen atmosphere, mix the raw material (1.04g, 0.01mol) and lithium hydroxide (0.24g, 0.01mol) with 10ml methanol solution and react at 10℃ for 8 hours. The obtained mixed solution is dried under reduced pressure at 40℃ and a vacuum degree of about -0.1MPa to remove the solvent to obtain an intermediate. Boron trifluoride ether complex (1.45g, 0.01mol) is added to the intermediate, and 10ml of ethylene glycol dimethyl ether solvent is added. Stir at room temperature for 24 hours, and the obtained mixed solution is dried under reduced pressure at 40℃ and a vacuum degree of about -0.1MPa. The obtained solid is washed three times with dichloromethane, filtered and dried to obtain product A8. The yield is 82%, and the nuclear magnetic resonance is as follows: Figure 8 shown.

[0113] Example 9

[0114] raw material

[0115] Preparation method: Under argon atmosphere, mix the raw material (1.36g, 0.01mol) and boron trifluoride ether complex (1.45g, 0.01mol) in 15ml THF (tetrahydrofuran) and react at room temperature for 12 hours. The obtained mixed solution is dried under reduced pressure at 30°C and a vacuum degree of about -0.1MPa to remove the solvent to obtain an intermediate. Add 6.25ml of butyl lithium hexane solution (c=1.6mol / L) to the intermediate, stir at room temperature for 6 hours, and dry the obtained mixed solution under reduced pressure at 40°C and a vacuum degree of about -0.1MPa. The obtained crude product is washed 3 times with cyclohexane, filtered and dried to obtain product A9. The yield is 85%, and the nuclear magnetic resonance is as follows Fig. 9 shown.

[0116] Example 10

[0117] raw material

[0118] Preparation method: Under argon atmosphere, add 10 ml of THF to the raw material (0.84 g, 0.01 mol), slowly drop 6.25 ml of butyl lithium hexane solution (c = 1.6 mol / L) into the THF solution of 1-cyclobutene-1-methanol, stir at room temperature for 6 hours, and dry the resulting mixture under reduced pressure at 40°C and a vacuum degree of about -0.1 MPa to obtain an intermediate. Add boron trifluoride ether complex (1.45 g, 0.01 mol) and 15 ml of THF to the intermediate and react at room temperature for 12 hours. Dry the resulting mixture under reduced pressure at 30°C and a vacuum degree of about -0.1 MPa to remove the solvent. The crude product is washed 3 times with cyclohexane, filtered and dried to obtain product A10. The yield is 85%, and the nuclear magnetic resonance is as follows Fig.10 shown.

[0119] Embodiment 11

[0120] raw material

[0121] Preparation method: Under nitrogen atmosphere, mix the raw material (1.12g, 0.01mol) and lithium hydroxide (0.24g, 0.01mol) with 10ml methanol solution and react at 10°C for 8 hours. The obtained mixed solution is dried under reduced pressure at 40°C and a vacuum degree of about -0.1MPa to remove the solvent to obtain an intermediate. Boron trifluoride ether complex (1.45g, 0.01mol) is added to the intermediate, and 10ml of ethylene glycol dimethyl ether solvent is added, stirred at room temperature for 24 hours, and the obtained mixed solution is dried under reduced pressure at 40°C and a vacuum degree of about -0.1MPa. The obtained solid is washed three times with dichloromethane, filtered and dried to obtain the product A11. The yield is 79%, and the nuclear magnetic resonance is as follows Fig.11 shown.

[0122] Example 12

[0123] raw material

[0124] Preparation method: Under argon atmosphere, mix the raw material (1.30g, 0.01mol) and boron trifluoride ether complex (1.45g, 0.01mol) in 15ml THF (tetrahydrofuran) and react at room temperature for 12 hours. The obtained mixed solution is dried under reduced pressure at 30°C and a vacuum degree of about -0.1MPa to remove the solvent to obtain an intermediate. Add 6.25ml of butyl lithium hexane solution (c=1.6mol / L) to the intermediate, stir and react at room temperature for 6 hours, and dry the obtained mixed solution under reduced pressure at 40°C and a vacuum degree of about -0.1MPa. The obtained crude product is washed 3 times with cyclohexane, filtered and dried to obtain product A12. The yield is 83%, and the nuclear magnetic resonance is as follows Fig.12 shown.

[0125] Test Example 1

[0126] The boron trifluoride organic salt protected by the present invention mainly plays three roles: 1. It is used as an additive in electrolytes (including liquid and solid), mainly to generate a passivation layer, and because it can dissociate ions, it can replenish the consumed ions, so the first-week efficiency, first-week discharge capacity, long-cycle stability, and rate performance of the battery are greatly improved; 2. It is used as a salt in electrolytes (including liquid and solid), mainly to provide ion transport and passivate the electrode, and it is effective when used alone as a salt or in combination with traditional salts as a double salt; 3. After polymerization, it is used as a single-ion conductor polymer electrolyte in gel batteries and all-solid-state batteries. The performance of this application is illustrated in an experimental manner below.

[0127] 1. As an additive in liquid electrolyte

[0128] First, in a glove box with a moisture content of less than 10 ppm, organic solvents, salts, and conventional additives are added in sequence and mixed thoroughly to prepare basic liquid electrolytes L1 to L10.

[0129] It should be noted that the organic solvents used in this test example include ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethylene carbonate (EC), conventional additives include fluoroethylene carbonate (FEC), vinylene carbonate (VC), trimethyl phosphate (TMP), and vinyl sulfate (DTD), and salts include lithium bis(oxalatoborate) (LiBOB), lithium difluorooxalatoborate (LiODFB), lithium bis(fluorosulfonyl)imide (LiFSI), lithium hexafluorophosphate (LiPF6), lithium bis(trifluoromethyl)sulfonylimide (LiTFSI), lithium tetrafluoroborate (LiBF4), and lithium perchlorate (LiClO4). The details are shown in Table 1.

[0130] Table 1 Basic liquid electrolyte formula

[0131]

[0132] The organic substances A1-A12 obtained in Examples 1-12 and the basic liquid electrolytes L1-L10 were fully mixed to obtain a series of liquid electrolytes E1-E15. The specific components and proportions are shown in Table 2.

[0133] Table 2 Liquid electrolytes E1 to E15 prepared from organic matter in Examples 1 to 12

[0134] Liquid electrolyte Basic liquid electrolyte additive Additive ratio E1 L1 A1 0.5% E2 L1 A1 1% E3 L1 A1 2% E4 L1 A2 1% E5 L2 A3 1% E6 L3 A4 1% E7 L4 A5 1% E8 L5 A6 1% E9 L6 A7 1% E10 L7 A7 1% E11 L8 A8 1% E12 L9 A9 2% E13 L10 A10 1% E14 L10 A11 1% E15 L10 A12 1%

[0135] The basic liquid electrolytes L1 to L10 and series liquid electrolytes E1 to E15 obtained above were respectively assembled into button batteries, as follows: the negative electrode shell, the negative electrode pole piece, the PE / Al2O3 separator, the electrolyte, the positive electrode pole piece, the stainless steel sheet, the spring sheet, and the positive electrode shell were assembled into a button battery, and a long cycle test was carried out at room temperature, wherein the cycle mode was 0.1C / 0.1C for 1 week, 0.2C / 0.2C for 5 weeks, and 1C / 1C for 44 weeks (C represents the rate), the positive electrode pole piece was a round piece with a diameter of 12 mm, the negative electrode pole piece was a round piece with a diameter of 14 mm, and the separator was a round piece with a diameter of 16.2 mm, which was a commercial Al2O3 / PE porous separator, as shown in Tables 4 and 5.

[0136] Among them, the preparation process of the positive and negative electrode sheets of the battery is as follows:

[0137] (1) Positive electrode

[0138] The positive electrode main material active material, conductive additive, and binder are added to the solvent in a ratio of 95:2:3, with the solvent accounting for 68% of the total slurry. The mixture is stirred evenly to obtain a positive electrode slurry with a certain fluidity; the positive electrode slurry is coated on aluminum foil, dried, and compacted to obtain a usable positive electrode sheet. The active materials used here are lithium cobalt oxide (LiCoO2, abbreviated as LCO), lithium nickel cobalt manganese oxide (NCM811), and lithium nickel cobalt aluminum oxide (LiNi 0.8 Co 0.15 Al 0.05 O2, abbreviated as NCA), lithium nickel manganese oxide (LiNi 0.5 Mn 1.5 O4, abbreviated as LNMO), carbon nanotubes (CNT) and SuperP are used as conductive additives, polyvinylidene fluoride (PVDF) is used as binder, and N-methylpyrrolidone (NMP) is used as solvent.

[0139] (2) Negative electrode

[0140] The negative electrode main material active material (except metal lithium), conductive additives, and binders are added to the solvent deionized water at a ratio of 95:2:3, with the solvent accounting for 45% of the total slurry, and mixed and stirred evenly to obtain a negative electrode slurry with a certain fluidity; the negative electrode slurry is coated on copper foil, and dried and compacted to obtain a usable negative electrode sheet. The active materials here are graphite (C), silicon oxygen carbon (SiOC450), and metal lithium (Li), the conductive agents are carbon nanotubes (CNT) and SuperP, and the binders are carboxymethyl cellulose (CMC) and styrene butadiene rubber (SBR).

[0141] The selected positive and negative electrode systems are shown in Table 3:

[0142] Table 3 Positive and negative electrode system

[0143] Battery positive and negative electrode system Positive electrode material Negative electrode material X1 LCO SiOC450 X2 NCM811 SiOC450 X3 NCA C X4 NCM811 Li X5 LNMO C

[0144] The first-week efficiency, first-week discharge specific capacity, and 50-cycle capacity retention rate of batteries 1 to 16 and comparative batteries 1 to 12 at room temperature were tested. The configuration and test method of the embodiment and comparative example batteries are shown in Table 4, and the test results are shown in Table 5.

[0145] Table 4 Configuration and testing methods of the battery of the embodiment and the comparative example

[0146]

[0147] Table 5 Comparison of test results of first-week efficiency, first-week discharge specific capacity, and 50-week capacity retention rate

[0148]

[0149]

[0150] It can be seen that the battery with the material provided by the present application as an additive has a higher first-week discharge capacity, a higher first-week efficiency, and a higher capacity retention rate after 50 cycles than the control battery without the material added, and the performance is better than the current conventional additives. In addition, in the presence of conventional additives, the battery using the boron salt additive shows more excellent electrochemical performance.

[0151] 2. As a salt in liquid electrolyte

[0152] (1) Preparation of liquid electrolyte

[0153] A1, A5, A6, A7, A12 are mixed evenly with organic solvents, conventional additives, and conventional salts to obtain a series of liquid electrolytes R1, R5, R6, R7, and R12. Conventional salts, organic solvents, and conventional additives are mixed evenly to obtain a series of conventional liquid electrolytes Q1, Q5, Q6, Q7, and Q12. The solvents and conventional additives used are all included in the solvents and conventional additives described in this test example "1". The specific composition and proportion of the liquid electrolyte are shown in Table 6.

[0154] Table 6 Synthesized boron-containing organic matter as liquid electrolyte prepared as salt

[0155]

[0156] Note: 1M means 1mol / L.

[0157] (2) Battery assembly

[0158] The obtained series of liquid electrolytes R (shown in Table 6) and conventional liquid electrolytes Q (shown in Table 6) were assembled into button batteries, and the positive and negative electrodes, the size of the separator, the assembly method, and the battery cycle mode were the same as the button batteries shown in the experimental example "I", namely, batteries (ie, embodiments) 1, 5, 6, 7, 12 and the corresponding comparative batteries. The specific configuration, cycle mode and voltage range of the batteries are shown in Table 7, and the first week discharge specific capacity, first week efficiency, and 50-week cycle capacity retention rate of the batteries (ie, the embodiments in Table 7 or 8) and the comparative batteries (ie, the comparative examples in Table 7 or 8) at room temperature are shown in Table 8.

[0159] Table 7 Configuration and testing method of button cells in the embodiment and comparative example

[0160]

[0161]

[0162] Table 8 Comparison of the test results of the button-type batteries of the embodiments and comparative examples shown in Table 7

[0163]

[0164] In summary, the boron trifluoride salt provided by the present invention is used alone as a salt for transporting ions or forms a double salt with a conventional salt in a non-aqueous solvent, and the ions are easily solvated, providing a higher ionic conductivity for the battery, and has high stability and excellent comprehensive performance. In a liquid battery system with LCO and NCM811 as the positive electrode and SiOC450 and Li as the negative electrode, it shows very excellent electrochemical performance, and the first-week efficiency, first-week discharge specific capacity, and capacity retention rate are all relatively high, and the performance is comparable to or slightly better than that of the battery corresponding to the traditional salt.

[0165] 3. Single-ion conductor polymer electrolyte

[0166] (1) Preparation of electrolytes

[0167] The monomers (compounds A1, A2, A4, A5, A9, A10, A11, A12 in the examples of the present application), plasticizers, battery additives, salts, and initiators were uniformly stirred to form a precursor solution, and precursors S1, S2, S4, S5, S9, S10, S11, and S12 were obtained. The specific composition is shown in Table 9. The initiators used were azobisisobutyronitrile (AIBN), benzoyl peroxide (BPO), and stannous isooctanoate (Sn(Oct)2).

[0168] Table 9 Precursor solution composition

[0169]

[0170] (2) Battery assembly

[0171] The electrolyte precursor solutions S1, S2, S4, S5, S9, S10, S11, and S12 obtained from Table 9 are respectively assembled into soft-pack batteries, namely batteries 1, 2, 4, 5, 9, 10, 11, and 12; specifically as follows: a positive electrode sheet with a size of 64 mm × 45 mm, a negative electrode sheet with a size of 65 mm × 46 mm, and a separator are assembled into a 2Ah soft-pack battery cell, and a secondary battery is obtained through stacking, baking, injection, and formation processes. The battery assembly system is X2 in Table 3, and a commercial PE / Al2O3 porous membrane is used as the separator.

[0172] (3) Battery test

[0173] After the secondary batteries prepared with electrolyte precursor solutions S1, S2, S4, S5, S9, S10, S11, and S12 were completely cured in situ, the first-week discharge capacity, first-week efficiency, and 50-cycle capacity retention rate of the batteries were tested at room temperature. The test voltage range was 3.0 to 4.2 V, and the cycle modes were 0.1C / 0.1C for 2 weeks and 0.3C / 0.3C for 48 weeks (C represents the rate). The test results are shown in Table 10.

[0174] Table 10 Test results of the battery of the embodiment

[0175] Battery First week discharge capacity (Ah) First week efficiency (%) Capacity retention rate after 50 cycles (%) Battery 1 1.74 86.8 79.6 Battery 2 1.90 94.6 89.8 Battery 4 1.94 96.5 90.3 Battery 5 1.92 95.8 90.1 Battery 9 1.88 93.3 89.9 Battery 10 1.73 86.0 79.1 Battery 11 1.76 87.4 80.0 Battery 12 1.89 94.2 90.4

[0176] As shown in Table 10, the test data in the examples show that the precursor solution composed of polymerizable monomers A1, A2, A4, A5, A9, A10, A11, and A12 is used as a polymer electrolyte after in-situ curing in the NCM811 / SiOC450 solid-state battery system, showing very excellent electrochemical performance, with relatively high first-week efficiency, first-week discharge capacity, and capacity retention rate. After polymerization of Examples 1, 10, and 11 (as shown in Table 10, no conventional salt is added to the system), a solid electrolyte with excellent performance can be obtained; when additional conventional salt is used, the battery exhibits more excellent electrochemical performance due to the increase in the number of dissociated ions.

[0177] In addition, this application also shows some embodiments of the present invention as additives, salts and polymer electrolytes. Figure 13 to Figure 16 The figures are respectively a comparison of the effects of batteries 1 / 6 / 9 / 14 made by using embodiments 1 / 6 / 9 / 14 as liquid electrolyte additives and corresponding comparative batteries 1 / 4 / 7 / 11 not containing the embodiments of the present invention. Figures 17-18 They are comparison diagrams of the effects of battery 1 / 7 made with Example 1 / 7 as liquid electrolyte salt and corresponding comparison battery 1 / 7 not containing the example of the present invention. Fig.19 This is a rendering of a polymer electrolyte battery 2 made using the monomer in Example 2 as a polymerized monomer; Fig. 20 This is a diagram showing the effect of a polymer electrolyte battery 10 made by using the monomer in Example 10 as a polymerized monomer.

[0178] In summary, the first-week efficiency, first-week discharge specific capacity, first-week discharge capacity, capacity retention rate and other performance have a direct and significant impact on the overall performance of the battery, which directly determines whether the battery can be used. Therefore, improving these performances is the goal or direction of many researchers in this field, but in this field, it is very difficult to improve these performances. Generally, it is a big progress to improve them by about 3-5%. In the preliminary test data of this application, it was pleasantly surprised to find that these data are greatly improved compared with the conventional data. When used as a liquid electrolyte additive, the battery performance is improved by about 5-35%, and the additives in this application are also used in combination with conventional additives. The material provided by the present invention is very effective as a salt in the electrolyte, and it has a better effect when matched with conventional salts. It can also be used at a higher concentration (such as 1.5M, 2M) to obtain a high-salt system electrolyte, which also has a very outstanding effect on the electrochemical performance of the battery, which will not be repeated here; the material provided by the present invention can also initiate polymerization to form a single-ion conductor polymer electrolyte, which is used in gel batteries, quasi-solid-state batteries and all-solid-state batteries. Moreover, the structural type of the present application is also greatly different from the conventional structure, which provides a new direction and idea for the research and development in this field, and also brings a lot of space for further research. Moreover, the material in the present application can have multiple uses with one structure; it is of great significance.

[0179] Test Example 2

[0180] This test example sets up test groups 1-3 and control groups 1-3. Among them, test group 1 uses the electrolyte provided in the above embodiment 1, test group 2 uses the electrolyte provided in the above embodiment 2, and test group 3 uses the electrolyte provided in the above embodiment 3.

[0181] Control group 1 used an electrolyte with the following structure:

[0182]

[0183] Control group 2 used an electrolyte with the following structure:

[0184]

[0185] Control group 3 used an electrolyte with the following structure:

[0186]

[0187] The test groups 1-3 and the control groups 1-3 were prepared using the following method:

[0188] (1) Preparation of positive electrode sheet: After the positive electrode active material, conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) are mixed evenly at a mass ratio of 80:10:10, a certain amount of solvent N-methyl-2-pyrrolidone (NMP) is added, and the mixture is fully ground in a mixer for 1 hour. Then, a film of a certain thickness is coated on the current collector aluminum foil through an automatic coating machine, and the film is placed in an 80°C forced air drying oven for 30 minutes, and then placed in a 120°C vacuum drying oven for 12 hours. The dried electrode sheet is rolled by a roller machine to tightly combine the active material with the current collector. After the pressed electrode sheet is cut into Φ12mm discs, it is vacuum dried again and stored for later use.

[0189] (2) Preparation of negative electrode sheet, liquid electrolyte and diaphragm: The negative electrode sheet is a lithium metal sheet with a thickness of 1.5 mm and a diameter of 14 mm. The liquid electrolyte is prepared by dissolving the electrolyte of each group in a solution of EC:DEC:EMC=1:1:1 (volume ratio) (the solid content of each group of electrolyte is 20%) and adding 1% AIBN or Sn(Oct)2 initiator. The diaphragm is a commercial Al2O3 / PE porous diaphragm, which is cut into Φ16 mm discs by a slicer.

[0190] (3) Battery assembly: The battery assembly is carried out in a glove box filled with argon. The oxygen content and water content in the glove box must be less than 1ppm. After the dried positive and negative electrodes are moved into the glove box, the negative electrode shell, negative electrode sheet, PE / Al2O3 diaphragm, liquid electrolyte, positive electrode sheet, stainless steel sheet, spring sheet, and positive electrode shell are assembled into button cells in sequence and sealed with a sealing machine. The button cells are then heated in an oven at 60°C for 12 hours. The battery assembly system is X4 in Table 3, and the diaphragm uses a commercial PE / Al2O3 porous membrane. The first week discharge specific capacity, first week efficiency, and 50-week capacity retention rate of the test group 1-3 and the control group 1-3 batteries were tested and recorded respectively. The results are shown in Table 11.

[0191] Table 11 Comparison of battery test results between the experimental group and the control group

[0192]

[0193]

[0194] It can be seen that the first-week discharge specific capacity, first-week efficiency and 50-week capacity retention rate of control groups 1-3 are all lower than those of test groups 1-3. This may be because when the electrolyte solid content is the same, the relative number of lithium ions in control group 1 is lower, and the transmission of lithium ions is poor; although the monomers in control group 2 can be free radical polymerized, their stability to Li is slightly poor; control group 3 is a small molecule that cannot be polymerized, and it is impossible to form a stable passivation protective layer on the surface of metallic lithium, so it is impossible to prevent the side reaction between metallic lithium and the electrolyte, and the viscosity is slightly larger, and the ion transmission performance is slightly lower. In summary, the electrolyte provided in this application can effectively improve battery performance, extend battery life, and improve battery safety through its in-situ polymerization in the battery.

[0195] In the present invention, the structures in Examples 1-12 are selected as representatives to illustrate the preparation method and effect of the present application. Other structures not listed can be prepared by the method described in any one of Examples 1-12. The preparation method is to prepare the raw materials, boron trifluoride compounds and R + The product boron trifluoride organic salt is obtained by the reaction of the raw material, that is, the -OH in the raw material becomes R + Can be Li + 、Na + In addition, the research team of the applicant has conducted serial effect tests on many other structures, and the effects are very good, similar to those in the above embodiments, but due to space constraints, only some structures are recorded.

[0196] In the present invention, only some structures are selected as representatives in the examples to illustrate the preparation method and effects of the present application, and other structures not listed have similar effects. For example:

[0197]

[0198] wait.

[0199] The raw materials used in the examples can all be purchased or prepared simply, and the preparation processes are all prior art, so they are not described in detail in the specification.

[0200] It should also be noted that the applicant has conducted a large number of tests on this series of structures. Sometimes, in order to better compare with the existing system, the same structure and system have been tested more than once. Therefore, there may be certain errors in different tests.

[0201] Finally, it should be noted that the above-described embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A polymerizable electrolyte, characterized in that The electrolyte comprises a boron trifluoride salt, The boron trifluoride salt is selected from: At least one of .

2. A method for preparing a polymerizable electrolyte according to claim 1, characterized in that: The method comprises the following steps: using a monovalent structure containing a -OH group, a boron trifluoride compound and R + The product of the source reaction is a The structure of boron trifluoride salt, where R + For lithium ion.

3. Use of the polymerizable electrolyte according to claim 1 in a secondary battery, characterized in that: The application is: the boron trifluoride salt is used as an additive of an electrolyte, or as a salt, or is used as a single ion conductor and polymer framework after polymerization of a monomer containing a polymerizable group.

4. The use according to claim 3, characterized in that: The application includes application in liquid electrolyte, gel electrolyte, mixed solid-liquid electrolyte, quasi-solid electrolyte, and all-solid electrolyte, and the liquid electrolyte, gel electrolyte, mixed solid-liquid electrolyte, quasi-solid electrolyte, and all-solid electrolyte independently include the electrolyte described in claim 1.

5. The application according to claim 4, wherein the application also includes application as a battery or a battery pack, wherein the battery comprises the electrolyte according to claim 1 and a positive electrode, a negative electrode and a packaging shell; the liquid electrolyte, gel electrolyte, mixed solid-liquid electrolyte, quasi-solid electrolyte, and all-solid-state electrolyte are applied to liquid batteries, gel batteries, mixed solid-liquid batteries, quasi-solid-state batteries and all-solid-state batteries, and the battery pack comprises the battery.