A composite lithium metal negative electrode material, preparation method thereof and metal lithium battery
By using composite lithium metal anode materials in lithium metal batteries, combined with skeleton materials, Li3N, LiNOx and metallic lithium, a dual conductive network is formed, which solves the problem of poor interface contact between the inorganic ceramic electrolyte and the lithium anode, and achieves high conductivity and long life. Cycling stability and simplified preparation process.
Patent Information
- Application Number
- CN202210465483.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-29
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-04-29
AI Technical Summary
The interface contact between the inorganic ceramic solid electrolyte and metallic lithium is poor, resulting in high interface resistance and uneven lithium ion flow, causing short-circuit failure of the battery. Existing improvement strategies have limitations in high temperature or corrosive environments.
Using composite lithium metal anode materials, including a combination of skeleton materials (such as carbon nanotubes, carbon cloth, three-dimensional porous copper films) and Li3N, LiNOx and metallic lithium, a dual-ion electronic conductive network is generated through in-situ chemical reactions to improve interface contact and Conductivity.
It improves the ion and electronic conductivity of the lithium anode, inhibits the formation of interface holes during battery cycling, achieves long-term cycle stability and stable interface, and simplifies the preparation process.
Smart Images

Figure HDA0003623836450000011 
Figure HDA0003623836450000012 
Figure HDA0003623836450000021
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of metal lithium batteries, and in particular relates to a composite lithium metal negative electrode material, a preparation method thereof and a metal lithium battery. Background Art
[0002] The metallic lithium anode has a high specific capacity (3680 mAh g -1 ), low electrode potential (-3.04 V vs standard hydrogen electrode) and low density (0.59 g cm -3 ), the inorganic solid electrolyte (LLZO) has the advantages of high ionic conductivity, wide electrochemical window, high thermal stability, high mechanical strength and chemical stability to lithium metal, so solid-state lithium metal batteries have become one of the research focuses of the next generation of lithium batteries.
[0003] However, the most critical problem is that the inorganic ceramic solid electrolyte will react chemically with the air to generate lithium carbonate, which will cover the surface of the solid electrolyte, resulting in poor wettability between LLZO and lithium. The poor contact between the electrolyte and metallic lithium will lead to high interface resistance and uneven lithium ion (Li + ) flow, further leading to the penetration of lithium dendrites, and ultimately causing the battery to short-circuit and fail. In order to improve the contact between LLZO and the lithium negative electrode, researchers usually use the following process approaches to solve the problem: high-temperature sintering or acid treatment is used to remove the lithium carbonate generated on the surface, and then a solid-state battery is prepared; or atomic layer deposition and magnetron sputtering are used to introduce metal elements, metal oxides, alloys and other intermediate layers to improve the interface contact. Although these methods can improve the interface contact between the solid electrolyte and the lithium negative electrode and reduce the interface impedance, these modification strategies are relatively strict and still have many limitations for practical applications, such as the high temperature or corrosive environment required to remove the impurity layer and the expensive equipment required to deposit the lithium-philic layer. Therefore, new improvement strategies need to be further developed. Summary of the invention
[0004] The present invention provides a composite lithium metal negative electrode material, a preparation method thereof and a metal lithium battery. The composite negative electrode of the present invention has good wettability with LLZO and can improve the ionic conductivity and electronic conductivity of the composite lithium negative electrode.
[0005] The present invention provides a composite lithium metal negative electrode material, comprising a skeleton material and Li3N, LiNO3 and LiN4 composited with the skeleton material. x and metallic lithium;
[0006] The skeleton material includes one or more of carbon nanotubes, carbon cloth, three-dimensional porous copper film, three-dimensional porous aluminum film and carbon nanotube film.
[0007] The present invention provides a method for preparing the composite lithium metal negative electrode material as described above, comprising the following steps:
[0008] A) mixing the framework material with a nitrate solution and drying to obtain an additive material;
[0009] B) mixing the additive material with molten metal lithium, and obtaining a composite lithium metal negative electrode material after cooling.
[0010] Preferably, the nitrate includes one or more of aluminum nitrate, magnesium nitrate, lithium nitrate, zinc nitrate, copper nitrate, silver nitrate, nickel nitrate, tin nitrate, bismuth nitrate, antimony nitrate and iron nitrate.
[0011] Preferably, in step A), the mass ratio of nitrate to framework material is 1:(10-30).
[0012] Preferably, the concentration of the nitrate solution is 0.05-0.2 mol / L.
[0013] Preferably, the framework material is mixed with the nitrate solution under ultrasonic conditions; the ultrasonic time is 10 to 60 minutes.
[0014] Preferably, the mass of the additive material accounts for 0.5-5% of the mass of the metallic lithium.
[0015] The present invention provides a lithium metal battery, comprising the composite lithium metal negative electrode material described above.
[0016] Preferably, the lithium metal battery is one or more of a liquid metal lithium battery, a liquid lithium-sulfur battery, a liquid lithium-air battery, an all-solid-state metal lithium battery, an all-solid-state lithium-ion battery and an all-solid-state lithium-sulfur battery.
[0017] The present invention provides a composite lithium metal negative electrode material, comprising a skeleton material and Li3N, LiNO and the like composited with the skeleton material. x and metallic lithium; the skeleton material comprises one or more of carbon nanotubes, carbon cloth, three-dimensional porous copper film, three-dimensional porous aluminum film and carbon nanotube film. The present invention mixes the skeleton material, nitrate and molten metallic lithium to generate the skeleton material, lithium nitride, nitrogen oxide and the like through in-situ chemical reaction, and has CNT / Li3N / LiNO x / lithium dual ion electronic conductive network, to obtain a composite lithium negative electrode with interface stability and high ionic conductivity and high electronic conductivity dual conductive network; at the same time, the formation of interface holes during battery cycling can be inhibited to achieve long-cycle stability of solid-state batteries. The method of the present invention can effectively regulate the viscosity, surface energy and surface tension of the metal lithium negative electrode, effectively improve the interface contact between the solid electrolyte and the lithium negative electrode, and achieve long-cycle stability of the symmetrical battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0019] Figure 1 The interfacial impedance curves of the composite lithium negative electrode with different additive contents in Example 1 of the present invention;
[0020] Figure 2 The cycle performance of the unmodified lithium negative electrode symmetrical battery in Example 1 of the present invention at room temperature;
[0021] Figure 3 The symmetrical lithium battery containing 1% of the composite lithium / / LLZTO / / composite lithium in Example 1 of the present invention has a current density of 0.3 mA cm at room temperature. -2 Time cycle performance;
[0022] Figure 4 The rate performance of the composite lithium / / LLZTO / / lithium iron phosphate solid-state battery at 1C in Example 1 of the present invention;
[0023] Figure 5 The cycle performance of the composite lithium / / LLZTO / / NCM811 solid-state battery at 0.2C in Example 1 of the present invention;
[0024] Figure 6 The LNO-CC / / LE / / LNO-CC symmetric battery in Example 2 of the present invention is at a current density of 1 mA cm -2 Cycle performance;
[0025] Figure 7 The cycle performance of LNO-CNT / / LE / / NCM811 and Li / / LE / / NCM811 full lithium batteries at 1C in Example 3 of the present invention;
[0026] Figure 8 This is the cycle performance of the Li / / LLZTO / / lithium iron phosphate solid-state battery at 0.1C in Example 1 of the present invention. DETAILED DESCRIPTION
[0027] The present invention provides a composite lithium metal negative electrode material, comprising a skeleton material and Li3N, LiNO and the like composited with the skeleton material. x and metallic lithium;
[0028] The skeleton material includes one or more of carbon nanotubes, carbon cloth, three-dimensional porous copper film, three-dimensional porous aluminum film and carbon nanotube film.
[0029] In the present invention, the skeleton material in the composite lithium metal negative electrode material has a skeleton effect, which can alleviate the volume change during the charge and discharge process and maintain close contact of the interface during the cycle; secondly, it improves the electronic conductivity of the composite electrode. Carbon nanotubes, carbon cloth, three-dimensional porous copper film, and three-dimensional porous aluminum film all have high conductivity. Li3N / LiNO x It has a high ionic conductivity, so the composite electrode prepared in this application has dual ionic and electronic conductivity.
[0030] In the present invention, the Li3N, LiNO x The ratio between metallic lithium and the skeleton material is preferably 1:1:(10-30), and more preferably 1:1:(15-25).
[0031] The present invention also provides a method for preparing a composite lithium metal negative electrode material, comprising the following steps:
[0032] A) mixing the framework material with a nitrate solution and drying to obtain an additive material;
[0033] B) mixing the additive material with molten metal lithium, and obtaining a composite lithium metal negative electrode material after cooling.
[0034] The present invention first prepares a nitrate solution, wherein the nitrate is preferably one or more of aluminum nitrate, magnesium nitrate, lithium nitrate, zinc nitrate, copper nitrate, nickel nitrate, tin nitrate, bismuth nitrate, antimony nitrate and iron nitrate; the concentration of the nitrate solution is preferably 0.05-0.2 mol / L, more preferably 0.1-0.15 mol / L.
[0035] Then the framework material is added into the nitrate solution, ultrasonicated, and dried to obtain the additive material.
[0036] In the present invention, the types of the skeleton material are consistent with the types of the skeleton material described above, and will not be repeated here.
[0037] The mass ratio of the nitrate to the framework material is preferably 1:(10-30), more preferably 1:(15-25), such as 1:10, 1:15, 1:20, 1:25, 1:30, preferably a range value with any of the above values as the upper or lower limit.
[0038] In the present invention, the frequency of the ultrasound is preferably 30 to 80 kHz, preferably 40 to 70 kHz, such as 30 kHz, 40 kHz, 50 kHz, 60 kHz, 70 kHz, 80 kHz, preferably a range value with any of the above values as the upper or lower limit; the time of the ultrasound is preferably 10 to 60 min, more preferably 20 to 50 min, and most preferably 30 to 40 min. The ultrasound can fully and evenly mix the nitrate and the carbon nanotube skeleton, so as to facilitate the later acquisition of a composite lithium metal negative electrode with better performance.
[0039] In the present invention, the drying temperature is preferably 60-100°C, more preferably 70-90°C, such as 60°C, 70°C, 80°C, 90°C, 100°C, preferably a range value with any of the above values as the upper or lower limit; in the present invention, too high or too low drying temperature will affect the effect of the additive, if the temperature is too low, the solvent cannot be completely volatilized, and if the temperature is too high, it may cause the decomposition of the lower nitrate.
[0040] After obtaining the additive material, the present invention heats the metallic lithium to a molten state, and then adds the additive material described above into the molten metallic lithium.
[0041] In the present invention, it is preferred to heat metallic lithium to about 200°C to achieve a molten state, and the mass of the additive material accounts for 0.5-5% of the mass of the metallic lithium, preferably 1-4%, such as 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, preferably a range value with any of the above values as the upper or lower limit.
[0042] Then the additive material and the molten lithium metal are stirred or adsorbed at a constant temperature for 3 to 8 minutes, and after cooling to room temperature, a skeleton material / Li3N / LiNO is obtained. x / Lithium dual ion electronic conductive network composite lithium metal anode material.
[0043] In this process, molten metallic lithium reacts in situ with nitrate to form a lithium alloy-lithium nitride / lithium nitrogen oxide mixed phase to improve the interfacial contact between the carbon material and the lithium matrix. The excellent lithium affinity of the lithium alloy-lithium nitride / lithium nitrogen oxide mixed phase formed by nitrate conversion is utilized to achieve lithium loading, which is easy to prepare on a large scale and the technology is much simpler.
[0044] The present invention also provides a lithium metal battery, wherein the negative electrode is made of the composite lithium metal negative electrode material described above, and the positive electrode and electrolyte can use the positive electrode and electrolyte commonly used by technicians in this field in lithium metal batteries, which will not be described in detail in the present invention.
[0045] The lithium metal battery is one or more of a liquid metal lithium battery, a liquid lithium-sulfur battery, a liquid lithium-air battery, an all-solid-state metal lithium battery, an all-solid-state lithium ion battery and an all-solid-state lithium-sulfur battery.
[0046] The present invention provides a composite lithium metal negative electrode material, comprising a skeleton material and Li3N, LiNO and the like composited with the skeleton material. x and metallic lithium; the skeleton material comprises one or more of carbon nanotubes, carbon cloth, three-dimensional copper foil, three-dimensional aluminum foil and carbon nanotube film. The present invention mixes the skeleton material, nitrate and molten metallic lithium to generate the skeleton material, lithium nitride, nitrogen oxide and the like through in-situ chemical reaction, and has CNT / Li3N / LiNO x / lithium dual ion electronic conductive network, to obtain a composite lithium negative electrode with interface stability and high ionic conductivity and high electronic conductivity dual conductive network; at the same time, the formation of interface holes during battery cycling can be inhibited to achieve long-cycle stability of solid-state batteries. The method of the present invention can effectively regulate the viscosity, surface energy and surface tension of the metal lithium negative electrode, effectively improve the interface contact between the solid electrolyte and the lithium negative electrode, and achieve long-cycle stability of the symmetrical battery.
[0047] In order to further illustrate the present invention, a composite lithium metal negative electrode material, a preparation method thereof and a metal lithium battery provided by the present invention are described in detail below in combination with embodiments, but it should not be understood as limiting the scope of protection of the present invention.
[0048] Example 1
[0049] A 0.1 mol / L nitrate aqueous solution was prepared, and then CNTs were added to the solution at a mass ratio of nitrate:CNT=1:20, and ultrasonicated for 30 minutes. Finally, the solution was dried to obtain CNT / nitrate powder.
[0050] Lithium metal was heated to 200°C to a molten state, and then additives (CNT / nitrate powder) of different mass ratios (0.5%, 1%, and 5%) were added to the molten lithium.
[0051] The nitrate additive and molten lithium are stirred at a constant temperature for 5 minutes until they are evenly mixed, and then cooled to room temperature to obtain a modified composite lithium negative electrode material.
[0052] (1) LLZO was placed in a glove box, and composite metal lithium was used as the electrode to assemble a composite lithium / / LLZTO / / composite lithium symmetric lithium battery, and its interfacial impedance and cycle stability were evaluated.
[0053] The results are as follows Figure 1 As shown by Figure 1 It can be seen that when 1% CNT / nitrate powder is added to molten lithium, the symmetrical battery has the smallest single-side interface resistance at room temperature, which is 5Ωcm2 A symmetrical cell can be operated at 0.3 mA cm -2 ((0.15mAh cm -2 ) has been cycled for 2000 hours at current density ( Figure 3 ), the comparative experiment shows that the single-side interface resistance of the symmetrical battery constructed with mechanically polished lithium metal is 527.5Ωcm 2 , can only be 0.1mA / cm 2 Cycle several times ( Figure 2 ).
[0054] (2) The prepared lithium iron phosphate positive electrode was placed in a glove box, and a composite lithium metal was used as the negative electrode and lithium iron phosphate was used as the positive electrode to assemble a composite lithium / / LLZTO / / lithium iron phosphate solid-state battery, and its cycle stability was evaluated;
[0055] like Figure 4 As shown in the figure, the solid-state lithium metal battery can be stably cycled at 1C, and the lithium iron phosphate-based solid-state lithium metal battery can be stably cycled at 1C for 200 cycles, with a capacity retention rate of up to 77.4% after 200 cycles. Figure 8 ), that is, the full battery constructed with mechanically polished solid electrolyte cannot cycle normally;
[0056] (3) The prepared NCM811 cathode was placed in a glove box, and a composite lithium metal was used as the anode and NCM811 as the cathode to assemble a composite lithium / / LLZTO / / NCM811 solid-state battery, and its cycle stability was evaluated;
[0057] The resulting solid-state lithium metal battery can be stably cycled at 0.2C ( Figure 5 ), NCM811-based solid-state lithium metal batteries can be stably cycled for 50 cycles at 0.2C. Figure 8 ), that is, the full battery constructed with solid electrolyte after mechanical polishing cannot cycle normally.
[0058] Example 2
[0059] A three-dimensional composite negative electrode was constructed by soaking carbon cloth (CC) in a 0.1M nitrate solution. Ultrasonication for 10 minutes during the soaking process could also improve the lithium affinity of the carbon cloth. The lithium metal was heated to 200°C and the three-dimensional composite electrode was immersed in molten lithium. The molten lithium could be automatically adsorbed into the carbon cloth. The composite negative electrode material was obtained by soaking for 40 seconds.
[0060] LNO-CC / / LE / / LNO-CC and Li / / LE / / Li symmetric lithium batteries were assembled using carbon cloth and pure lithium sheets as electrodes, respectively, using ester electrolytes without any additives, and their cycle stability was evaluated.
[0061] The results are as follows Figure 6 As shown, the resulting LNO-CC / / LE / / LNO-CC symmetric cell can be used at 1 mA cm -2 (1mAh cm -2 ) for 500 hours under stable cycling conditions. In contrast, the symmetrical battery constructed with pure lithium sheets has a large overpotential fluctuation and short circuits after 80 hours of cycling.
[0062] Example 3
[0063] The CNT film was immersed in a 0.1M nitrate solution to construct a three-dimensional composite negative electrode. No ultrasound was used during the immersion process, which could also improve the lithium affinity of the CNT film. The lithium metal was heated to 200°C and the three-dimensional composite electrode was immersed. The molten lithium could be automatically adsorbed into the interior of the CNT film. After immersion for 5 minutes, a composite negative electrode material was obtained.
[0064] LNO-CNT / / LE / / NCM811 and Li / / LE / / NCM811 full lithium batteries were assembled using CNT membrane and pure lithium sheet as electrodes, ester electrolyte and high-load NCM811 cathode, and their cycle stability was evaluated.
[0065] The obtained LNO-CNT / / LE / / NCM811 full battery can be stably cycled for 100 cycles at 1C with a capacity retention rate of 30%. In a comparative experiment, the capacity retention rate of the full battery constructed with pure lithium sheets was only 4% after 100 cycles at 1C.
[0066] like Figure 7 As shown in the figure, the obtained LNO-CNT / / LE / / NCM811 full battery can be stably cycled for 100 cycles at 1C with a capacity retention rate of 30%. In contrast, the capacity retention rate of the full battery constructed with pure lithium sheets is only 4% after 100 cycles at 1C.
[0067] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A composite lithium metal negative electrode material, comprising a skeleton material and a Li 3 N, LiNO x and metallic lithium; The skeleton material is a three-dimensional porous copper film and / or a three-dimensional porous aluminum film; The preparation method of the composite lithium metal negative electrode material, The following steps are involved: A) mixing the framework material with a nitrate solution and drying to obtain an additive material; B) mixing the additive material with molten metal lithium and obtaining a composite lithium metal negative electrode material after cooling; the mass of the additive material accounts for 1 to 4.5% of the mass of the metal lithium.
2. The method for preparing the composite lithium metal negative electrode material according to claim 1, The following steps are involved: A) mixing the framework material with a nitrate solution and drying to obtain an additive material; B) mixing the additive material with molten metal lithium, and obtaining a composite lithium metal negative electrode material after cooling.
3. The preparation method according to claim 2, It is characterized in that The nitrate includes one or more of aluminum nitrate, magnesium nitrate, lithium nitrate, zinc nitrate, copper nitrate, silver nitrate, nickel nitrate, tin nitrate, bismuth nitrate, antimony nitrate and iron nitrate.
4. The preparation method according to claim 3, It is characterized in that In the step A), the mass ratio of nitrate to framework material is 1:(10-30).
5. The preparation method according to claim 2, It is characterized in that The concentration of the nitrate solution is 0.05-0.2 mol / L.
6. The preparation method according to claim 2, It is characterized in that The framework material and the nitrate solution are mixed under ultrasonic conditions; the ultrasonic time is 10 to 60 minutes.
7. A lithium metal battery comprising the composite lithium metal negative electrode material according to claim 1.
8. The lithium metal battery according to claim 7, It is characterized in that The lithium metal battery is one or more of a liquid metal lithium battery, a liquid lithium-sulfur battery, a liquid lithium-air battery, an all-solid-state metal lithium battery, an all-solid-state lithium ion battery and an all-solid-state lithium-sulfur battery.
Citation Information
Cited By
Modification method of negative electrode of lithium metal battery
CN120767294A