Conjugated polymer based on thiophene[3,4-c]pyrrole-4,6-dione structure and preparation method and application thereof
Through conjugated polymers based on the thiophene [3,4-c]pyrrole-4,6-dione structure, the structural tonality and solubility problems of existing photocatalysts in photocatalytic water splitting for hydrogen production are achieved. An efficient and environmentally friendly photocatalytic water splitting method was developed to produce hydrogen, with a hydrogen production rate of 133.9 μmol.g-1.h-1.
Patent Information
- Application Number
- CN202210495901.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-09
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing organic photocatalysts have problems such as limited structural adjustability, complex equipment operation, and environmental pollution in the field of photocatalytic water splitting and hydrogen production. Moreover, most conjugated polymers are hydrophobic and difficult to dissolve.
A conjugated polymer based on the thiophene [3,4-c]pyrrole-4,6-dione structure is used to prepare a photocatalyst with good water solubility and suitable energy level of nanoparticles through C-H/C-H direct coupling reaction. Affinity polymer materials form aqueous solutions, solving dissolution problems and simplifying synthesis steps.
An efficient, simple, and environmentally friendly photocatalytic water splitting to produce hydrogen has been achieved. The nanoparticles have good dispersion in water, a wide visible light absorption range, and low production cost. They meet the energy requirements of photocatalytic hydrolysis for hydrogen production, and the hydrogen production rate reaches 133.9 μmol. g-1.h-1.
Smart Images

Figure CN114672003B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photocatalytic decomposition of water to produce hydrogen, and relates to a conjugated polymer based on a thiophene [3,4-c] pyrrole-4,6-dione structure, and a preparation method and application thereof. Background Art
[0002] Energy is an important material basis for the survival and development of human society. Due to the non-renewable and pollution problems of traditional energy (oil, coal, natural gas, etc.), it is particularly important to develop and utilize green energy. Solar energy is one of the important choices for sustainable energy supply in the future because of its inexhaustible, inexhaustible, widely distributed, clean and pollution-free characteristics. However, factors such as low solar energy flux density, great environmental impact on intensity, and inability to maintain constant energy supply make it difficult to develop and utilize it in a popularized manner. In order to solve these shortcomings of solar energy, developing new energy carriers to effectively collect solar energy is a feasible way, and hydrogen energy is an appropriate and effective energy carrier. According to the principle of hydrogen production, solar hydrogen production can be divided into solar thermal decomposition of water to produce hydrogen, solar photocatalytic decomposition of water to produce hydrogen, and solar biohydrogen production. Among them, solar photocatalytic hydrogen production has the advantages of simple equipment, simple operation, and no secondary pollution. It is a recyclable hydrogen production technology that has greatly attracted the attention of researchers. Compared with inorganic photocatalysts, which have poor response to visible light and limited tunability of energy gap, organic photocatalysts have great application potential in hydrogen production due to their designable structure, controllable molecular energy gap, adjustable light absorption and good photocatalytic activity. Conjugated polymer materials are widely used in solar cells, field effect transistors and other fields, but are rarely used in the field of photocatalytic hydrogen production. The preparation method of organic conjugated polymers is mainly obtained through traditional transition metal catalysis such as Suzuki coupling and Stille coupling reactions. This type of coupling reaction has many steps, harsh conditions, and difficult monomer purification. It produces stoichiometric metal organic reagent waste and causes environmental pollution. Importantly, most organic conjugated polymers are hydrophobic and need to be dissolved with the help of organic solvents.
[0003] Through searching, no patent publication documents related to the patent application of the present invention have been found. Summary of the invention
[0004] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a conjugated polymer based on a thiophene[3,4-c]pyrrole-4,6-dione structure and a preparation method and application thereof.
[0005] The technical solution adopted by the present invention to solve its technical problem is:
[0006] A conjugated polymer based on a thiophene[3,4-c]pyrrole-4,6-dione structure, wherein the chemical structure of the conjugated polymer is shown in formula (I):
[0007]
[0008] It is a thiophene[3,4-c]pyrrole-4,6-dione derivative monomer, referred to as monomer A;
[0009] Wherein, R1 is hydrogen, methyl, ethyl, octyl, decyl, hexadecyloxy, phenyl, p-octylphenyl or 2-hexyl-5-thienyl; n is 8-10000;
[0010] Wherein, monomer B is at least one of the following structural formulas:
[0011]
[0012] Wherein, Ar in formula (II) is one of the structural formulas of the B unit, or is at least one of the following structural formulas:
[0013]
[0014] Where X is O, N, S; Y is C, N, Si; R2-R 27 H, C1-C 30 Alkyl, C1-C 30 Alkyl substituent, C3-C 30 Cycloalkyl, C3-C 30 Cycloalkyl substituents, C1-C 30 Alkoxy, C1-C 30 Alkylthio, halogenated C1-C 30 Alkyl, halogenated C3-C 30 Cycloalkyl, halogenated C1-C 30 Alkoxy or halogenated C1-C 30alkylthio, and R1 and R2 are the same or different; the alkyl group is substituted or unsubstituted. When the alkyl group is substituted, the substituent is cycloalkyl, aryl, heteroaryl, heteroalicyclic, hydroxyl, aryloxy, mercapto, alkylthio, arylthio, cyano, halo, carbonyl, thiocarbonyl, O-carbamoyl, N-carbamoyl, O-thiocarbamoyl, N-thiocarbamoyl, C-acylamino, N-acylamino, S-sulfonylamino, N-sulfonylamino, C-carboxyl, O-carboxyl, thiocyanato, -NR'R" or amino including mono- and di-substituted amino groups and amino groups and protected derivatives; the cycloalkyl group is substituted or unsubstituted. When the cycloalkyl group is substituted, the substituent is cycloalkyl, aryl, heteroaryl, heteroalicyclic, hydroxy, aryloxy, mercapto, alkylthio, arylthio, cyano, halo, carbonyl, thiocarbonyl, O-carbamoyl, N-carbamoyl, O-thiocarbamoyl, N-thiocarbamoyl, C-acylamino, N-acylamino, S-sulfonylamino, N-sulfonylamino, C-carboxyl, O-carboxyl, thiocyanato, -NR'R" or amino including mono- and di-substituted amino groups and protected derivatives thereof.
[0015] Furthermore, the conjugated polymer is a linear organic conjugated polymer obtained by reacting a thiophene[3,4-c]pyrrole-4,6-dione derivative with different monomers B.
[0016] The preparation method of the conjugated polymer based on thiophene [3,4-c] pyrrole-4,6-dione structure as described above comprises the following steps:
[0017] ① Dissolve monomer A, monomer B, oxidant, base, palladium catalyst and additives in a solvent, heat and react under nitrogen protection, maintain the reaction system at 60-150°C, stir, and react for 12-72 hours.
[0018] ② After the reaction solution obtained in step ① is cooled to room temperature, it is added dropwise into methanol for precipitation, filtered to obtain a crude product, and the crude product is extracted with methanol and n-hexane Soxhlet in sequence, and then extracted with chloroform Soxhlet, the chloroform extract is collected, and after concentration, methanol is added for precipitation, the filter cake is obtained by suction filtration, and after vacuum drying, a polymer based on the thiophene [3,4-c] pyrrole-4,6-dione structure is obtained.
[0019] Further, the solvent is one or a mixture of toluene, xylene, 1,4-dioxane, o-xylene, tetrahydrofuran, N,N-dimethylacetamide, toluene and dimethyl sulfoxide;
[0020] The oxidant is one or a mixture of Ag2CO3 (silver carbonate), AgF (silver fluoride), AgOAc (silver acetate), Ag2O (silver oxide), Cu(OAc)2 (copper acetate), Cu(OTf)2 (copper trifluoromethanesulfonate), CuCl2 (copper chloride) and AgNO3 (silver nitrate);
[0021] The base is one or a mixture of Na2CO3 (sodium carbonate), K2CO3 (potassium carbonate), Cs2CO3 (cesium carbonate), NaHCO3 (sodium bicarbonate), NaOAc (sodium acetate), KOAc (potassium acetate), CsOAc (cesium acetate) and KF (potassium fluoride);
[0022] The additive is one or a mixture of PPh3 (triphenylphosphine), PCy3-HBF4 (tricyclohexylphosphine tetrafluoroborate), P(t-Bu)3 (tri-tert-butylphosphine), PivOH (pivalic acid), PCy3 (tricyclohexylphosphine), P(t-Bu)2MeHBF4 (di-tert-butylphosphine tetrafluoroborate), P(o-tolyl)3 (tri(o-tolyl)phosphine)), PCy3HBF4 (tricyclohexylphosphine tetrafluoroborate), TMEDA (tetramethylethylenediamine), HOAc (acetic acid) and P(2-MeOC6H4)3 (tri(o-methoxyphenyl)phosphine);
[0023] The palladium catalyst is Herrmann's Catalyst (trans-di-(m)-bis[2-(di-o-tolylphosphine)benzyl]acetate dipalladium (II)), Pd(dppf)Cl2 (dichloro(1,1'-di(diphenylphosphino)ferrocene)palladium), Pd(OAc)2 (palladium acetate), PdCl2 (palladium chloride), Pd2(dba)3 (tris(dibenzylidene dione) dipalladium), Pd(TFA)2 (palladium trifluoroacetate), PdCl2(PPh3)2 (bis(triphenylphosphine)palladium dichloride), Pd(OH) 2( Palladium hydroxide), Pd(PPh3)4 (tetrakis(triphenylphosphine)palladium) and Pd / C (palladium on carbon) or a mixture of some of them.
[0024] Furthermore, the ratio of monomer A, monomer B, palladium catalyst, additive, oxidant and base is 1:1:(0.05-0.2):(0.05-0.2):(1-4):(1-4) in terms of the amount of the substance; the reaction temperature is 60-150° C.;
[0025] The concentrations of the monomer A and the monomer B in the solvent are both 0.01-1 mol / L.
[0026] Furthermore, the crude product was subjected to Soxhlet extraction with methanol and n-hexane for 24 hours respectively; after concentration, methanol was added to settle for 24 hours; and dried in a vacuum drying oven at 60° C. for 12 hours.
[0027] A photocatalyst prepared by using the above-mentioned thiophene[3,4-c]pyrrole-4,6-dione structure-based conjugated polymer.
[0028] Further, the following steps are included:
[0029] Dissolve the thiophene[3,4-c]pyrrole-4,6-dione structure-based conjugated polymer and the amphiphilic polymer material in tetrahydrofuran to prepare a 1 mg / mL stock solution for later use;
[0030] The mother liquors are taken separately, mixed and diluted with tetrahydrofuran to the required concentration; the diluted mixed solution is ultrasonically dispersed, quickly poured into ultrapure water for ultrasonic vibration, and then an inert gas is introduced to remove the low-boiling point solvent in the solvent, and finally a nanoparticle aqueous solution is obtained, which is the photocatalyst.
[0031] Furthermore, the amphiphilic polymer material includes PEG-PBLA (polyethylene glycol-polybenzyl aspartate), FA-PEG-PBLA (folic acid-polyethylene glycol-polybenzyl aspartate), FEG-PCL (polyethylene glycol-polycaprolactone), FEG-PLA (polyethylene glycol-polylactic acid), PEG-PLGA (polyethylene glycol-polylactic acid / glycolic acid copolymer), and DSPE-PEG (distearoyl phosphatidylethanolamine-polyethylene glycol).
[0032] The photocatalyst described above is used for photocatalytic decomposition of water to produce hydrogen.
[0033] The advantages and positive effects achieved by the present invention are:
[0034] 1. The thiophene [3,4-c] pyrrole-4,6-dione structure, i.e., monomer A, of the present invention has the characteristics of high symmetry, planar structure, and super strong ability to attract electrons. In the material, the charge in the molecule can be transferred, and the highest occupied orbital and the lowest unoccupied orbital energy levels of the polymer can be effectively adjusted. The conjugated polymer based on the thiophene [3,4-c] pyrrole-4,6-dione structure has a wide absorption spectrum, good thermal stability, and appropriate energy level, which meets the energy requirements of photocatalytic hydrolysis for hydrogen production. Its nanoparticles have good water solubility and high thermodynamic stability, and have a carbon dioxide content of 133.9 μmol.g at a concentration of 300 μg / mL. -1 .h -1 hydrogen production rate.
[0035] 2. The thiophene[3,4-c]pyrrole-4,6-dione structure conjugated polymer of the present invention is a linear organic conjugated polymer obtained by reacting a thiophene[3,4-c]pyrrole-4,6-dione derivative with different B structural units. The selected B structural units can form a planar structure with the thiophene[3,4-c]pyrrole-4,6-dione derivative, which is beneficial to the charge transfer in the catalyst during the photocatalytic decomposition of water to produce hydrogen.
[0036] 3. The preparation method of the present invention adopts CH / CH direct coupling, does not require pretreatment of raw materials, the raw materials are simple and easy to obtain, no end-capping treatment is required, the synthesis steps are simple, the production cost is low, there is no need to prepare monomers that have an impact on the environment such as metal tin compounds, borides or halides, and the post-treatment is simple.
[0037] 4. The present invention provides an efficient, simple and environmentally friendly method for preparing a conjugated polymer based on a thiophene [3,4-c] pyrrole-4,6-dione structure, and prepares nanoparticles thereof. The nanoparticles have good dispersibility in water and a wide visible light absorption range, solve the problem of organic solvent dissolution, and are suitable for application in the field of photocatalytic water decomposition and hydrogen production. The preparation method of the present invention has high atomic economy, low production cost and is environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 The electrochemical cyclic voltammetry curves of P6 and P15 in the present invention;
[0039] Figure 2 This is a graph of the hydrogen production rate of photocatalytic hydrolysis of Pdot6 and Pdot15 in the present invention. DETAILED DESCRIPTION
[0040] The embodiments of the present invention are described in detail below. It should be noted that the embodiments are descriptive rather than restrictive and cannot be used to limit the protection scope of the present invention.
[0041] The raw materials used in the present invention, unless otherwise specified, are conventional commercially available products; the methods used in the present invention, unless otherwise specified, are conventional methods in the art.
[0042] A conjugated polymer based on a thiophene[3,4-c]pyrrole-4,6-dione structure, wherein the chemical structure of the conjugated polymer is shown in formula (I):
[0043]
[0044] It is a thiophene[3,4-c]pyrrole-4,6-dione derivative monomer, referred to as monomer A;
[0045] Wherein, R1 is hydrogen, methyl, ethyl, octyl, decyl, hexadecyloxy, phenyl, p-octylphenyl or 2-hexyl-5-thienyl; n is 8-10000;
[0046] Wherein, monomer B is at least one of the following structural formulas:
[0047]
[0048] Wherein, Ar in formula (II) is one of the structural formulas of the B unit, or is at least one of the following structural formulas:
[0049]
[0050] Where X is O, N, S; Y is C, N, Si; R2-R 27 H, C1-C 30 Alkyl, C1-C 30 Alkyl substituent, C3-C 30 Cycloalkyl, C3-C 30 Cycloalkyl substituents, C1-C 30 Alkoxy, C1-C 30 Alkylthio, halogenated C1-C 30 Alkyl, halogenated C3-C 30 Cycloalkyl, halogenated C1-C 30 Alkoxy or halogenated C1-C 30 alkylthio, and R1 and R2 are the same or different; the alkyl group is substituted or unsubstituted. When the alkyl group is substituted, the substituent is cycloalkyl, aryl, heteroaryl, heteroalicyclic, hydroxyl, aryloxy, mercapto, alkylthio, arylthio, cyano, halo, carbonyl, thiocarbonyl, O-carbamoyl, N-carbamoyl, O-thiocarbamoyl, N-thiocarbamoyl, C-acylamino, N-acylamino, S-sulfonylamino, N-sulfonylamino, C-carboxyl, O-carboxyl, thiocyanato, -NR'R" or amino including mono- and di-substituted amino groups and amino groups and protected derivatives; the cycloalkyl group is substituted or unsubstituted. When the cycloalkyl group is substituted, the substituent is cycloalkyl, aryl, heteroaryl, heteroalicyclic, hydroxy, aryloxy, mercapto, alkylthio, arylthio, cyano, halo, carbonyl, thiocarbonyl, O-carbamoyl, N-carbamoyl, O-thiocarbamoyl, N-thiocarbamoyl, C-acylamino, N-acylamino, S-sulfonylamino, N-sulfonylamino, C-carboxyl, O-carboxyl, thiocyanato, -NR'R" or amino including mono- and di-substituted amino groups and protected derivatives thereof.
[0051] Preferably, the conjugated polymer is a linear organic conjugated polymer obtained by reacting a thiophene[3,4-c]pyrrole-4,6-dione derivative with different monomers B.
[0052] The preparation method of the conjugated polymer based on thiophene [3,4-c] pyrrole-4,6-dione structure as described above comprises the following steps:
[0053] ① Dissolve monomer A, monomer B, oxidant, base, palladium catalyst and additives in a solvent, heat and react under nitrogen protection, maintain the reaction system at 60-150°C, stir, and react for 12-72 hours.
[0054] ② After the reaction solution obtained in step ① is cooled to room temperature, it is added dropwise into methanol for precipitation, filtered to obtain a crude product, and the crude product is extracted with methanol and n-hexane Soxhlet in sequence, and then extracted with chloroform Soxhlet, the chloroform extract is collected, and after concentration, methanol is added for precipitation, the filter cake is obtained by suction filtration, and after vacuum drying, a polymer based on the thiophene [3,4-c] pyrrole-4,6-dione structure is obtained.
[0055] Preferably, the solvent is one or a mixture of toluene, xylene, 1,4-dioxane, o-xylene, tetrahydrofuran, N,N-dimethylacetamide, toluene and dimethyl sulfoxide;
[0056] The oxidant is one or a mixture of Ag2CO3 (silver carbonate), AgF (silver fluoride), AgOAc (silver acetate), Ag2O (silver oxide), Cu(OAc)2 (copper acetate), Cu(OTf)2 (copper trifluoromethanesulfonate), CuCl2 / (copper chloride) and AgNO3 (silver nitrate);
[0057] The base is one or a mixture of Na2CO3 (sodium carbonate), K2CO3 (potassium carbonate), Cs2CO3 (cesium carbonate), NaHCO3 (sodium bicarbonate), NaOAc (sodium acetate), KOAc (potassium acetate), CsOAc (cesium acetate) and KF (potassium fluoride);
[0058] The additives are PPh3 (triphenylphosphine), PCy3-HBF4 (tricyclohexylphosphine tetrafluoroborate), P(t-Bu)3 tri-tert-butylphosphine, PivOH (pivalic acid), PCy3 (tricyclohexylphosphine), P(t-Bu)2MeHBF4 (di-tert-butylphosphine tetrafluoroborate), P(o-tolyl)3 (tri(o-toluene)phosphine)), PCy3HBF 4( tricyclohexylphosphine tetrafluoroborate), TMEDA (tetramethylethylenediamine), HOAc (acetic acid) and P(2-MeOC6H4)3 (tri(o-methoxyphenyl)phosphine) or a mixture of several thereof;
[0059] The palladium catalyst is Herrmann's Catalyst (trans-di-(m)-bis[2-(di-o-tolylphosphine)benzyl]acetate dipalladium (II)), Pd(dppf)Cl2 (dichloro(1,1'-bis(diphenylphosphino)ferrocene)palladium), Pd(OAc)2 (palladium acetate), PdCl 2( (palladium chloride), Pd2(dba)3(tris(dibenzylidenedione)dipalladium), Pd(TFA)2(palladium trifluoroacetate), PdCl2(PPh3)2(bis(triphenylphosphine)palladium dichloride), Pd(OH)2(palladium hydroxide), Pd(PPh3)4(tetrakis(triphenylphosphine)palladium) and Pd / C (palladium on carbon) or a mixture of any of the above.
[0060] Preferably, the ratio of monomer A, monomer B, palladium catalyst, additive, oxidant and base is 1:1:(0.05-0.2):(0.05-0.2):(1-4):(1-4) in terms of the amount of the substance; the reaction temperature is 60-150° C.;
[0061] The concentrations of the monomer A and the monomer B in the solvent are both 0.01-1 mol / L.
[0062] Preferably, the crude product is subjected to Soxhlet extraction with methanol and n-hexane for 24 hours respectively; after concentration, methanol is added to settle for 24 hours; and drying is carried out in a vacuum drying oven at 60° C. for 12 hours.
[0063] A photocatalyst prepared by using the above-mentioned thiophene[3,4-c]pyrrole-4,6-dione structure-based conjugated polymer.
[0064] Preferably, the method comprises the following steps:
[0065] Dissolve the thiophene[3,4-c]pyrrole-4,6-dione structure-based conjugated polymer and the amphiphilic polymer material in tetrahydrofuran to prepare a 1 mg / mL stock solution for later use;
[0066] The mother liquors are taken separately, mixed and diluted with tetrahydrofuran to the required concentration; the diluted mixed solution is ultrasonically dispersed, quickly poured into ultrapure water for ultrasonic vibration, and then an inert gas is introduced to remove the low-boiling point solvent in the solvent, and finally a nanoparticle aqueous solution is obtained, which is the photocatalyst.
[0067] Preferably, the amphiphilic polymer material includes PEG-PBLA (polyethylene glycol-polybenzyl aspartate), FA-PEG-PBLA (folic acid-polyethylene glycol-polybenzyl aspartate), FEG-PCL (polyethylene glycol-polycaprolactone), FEG-PLA (polyethylene glycol-polylactic acid), PEG-PLGA (polyethylene glycol-polylactic acid / glycolic acid copolymer), and DSPE-PEG (distearoyl phosphatidylethanolamine-polyethylene glycol).
[0068] The photocatalyst described above is used for photocatalytic decomposition of water to produce hydrogen.
[0069] Specifically, the relevant preparation and detection examples are as follows:
[0070] The general process of the reaction is as follows: a thiophene [3,4-c] pyrrole-4,6-dione derivative (monomer A), monomer B, a palladium catalyst, an oxidant, a base, an additive, and a solvent are added to a reaction vessel. Under nitrogen protection, the reaction system is maintained at 60 to 150° C. and reacted for 12 to 72 hours to obtain a crude polymer product.
[0071]
[0072] A monomer
[0073] When the structure of monomer A is The structure of monomer B is
[0074] Example 1: When X=O, R2=R3=H
[0075] Monomer A (1 eq), monomer B (1 eq), silver carbonate (8 eq), potassium acetate (8 eq), herrmann's catalyst (0.01 eq) and di(tert-butyl)phosphine methyl tetrafluoroborate (0.04 eq) were dissolved in 4 mL of N,N-dimethylacetamide, stirred at 60°C, and reacted for 72 hours. After the reaction solution was cooled, it was poured into methanol and filtered to obtain a crude product. The crude product was Soxhlet extracted with methanol and n-hexane for 24 hours, and finally Soxhlet extracted with chloroform until the extract in the Soxhlet extraction tube was colorless. The extraction was stopped, the chloroform extract was collected, concentrated to 2 mL, and dripped into 60 mL of methanol for sedimentation. After sedimentation for 24 hours, the filter cake was dried in a vacuum drying oven at 60°C for 12 hours to obtain polymer P1 (yield: 56.4%, M n =2.00 KDa, PDI =1.30).
[0076] Example 2: When X=S, R2=R3=H
[0077] Monomer A (1 eq), monomer B (1 eq), silver carbonate (4 eq), potassium acetate (4 eq), tetrakis(triphenylphosphine)palladium (0.01 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.02 eq) were dissolved in 1 mL of N,N-dimethylacetamide solvent, stirred at 120°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P2 (yield: 88.4%, M n =27.00 KDa, PDI =1.80).
[0078] Example 3: When X=S, R2=H, R3=CH3
[0079] Monomer A (1 eq), monomer B (1 eq), silver carbonate (4 eq), potassium acetate (4 eq), tetrakis(triphenylphosphine)palladium (0.01 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.02 eq) were dissolved in 1 mL of N,N-dimethylacetamide solvent, stirred at 80°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P3 (yield: 69.08%, Mn=22.00 KDa, PDI=1.40).
[0080] Example 4: When X=S, R2=H, R3=C8H 17 hour
[0081] Monomer A (1 eq), monomer B (1 eq), silver carbonate (6 eq), potassium acetate (6 eq), tetrakis(triphenylphosphine)palladium (0.01 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.03 eq) were dissolved in 1.5 mL of N,N-dimethylacetamide solvent, stirred at 150°C, and reacted for 12 hours. The post-treatment was the same as in Example 1 to obtain polymer P4 (yield: 55.5%, Mn=26.00 KDa, PDI=1.50).
[0082] When the structure of monomer A is The structure of monomer B is
[0083] Embodiment 5:
[0084] Monomer A (0.01 eq), monomer B (0.01 eq), silver carbonate (0.04 eq), potassium acetate (0.04 eq), tetrakis(triphenylphosphine)palladium (0.0001 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.0002 eq) were dissolved in 1 mL of N,N-dimethylacetamide solvent, stirred at 80°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P5 (yield: 63.16%, Mn=19.00 KDa, PDI=1.80).
[0085] When the structure of monomer A is The structure of monomer B is
[0086] Example 6: When Y=C, R4=R5=C8H 17 hour
[0087] Monomer A (1 eq), monomer B (1 eq), silver carbonate (1 eq), potassium acetate (1 eq), dichloro[1,1,-bis(diphenylphosphino)ferrocene]palladium (0.005 eq) and di(tert-butyl)phosphinomethyl tetrafluoroborate (0.005 eq) were dissolved in 1 mL of N,N-dimethylacetamide solvent, stirred at 80°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P6 (yield: 66.17%, Mn=25.00 KDa, PDI=1.60).
[0088] Example 7: When Y=N, R4=C8H 17 , R5=no time
[0089] Monomer A (1 eq), monomer B (1 eq), silver carbonate (4 eq), potassium acetate (4 eq), palladium acetate (0.001 eq) and di(tert-butyl)phosphine methyl tetrafluoroborate (0.08 eq) were dissolved in 1 mL of N,N-dimethylacetamide solvent, stirred at 90°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P7 (yield: 65%, Mn=22.00 KDa, PDI=1.60).
[0090] Example 8: When Y=Si, R4=R5=C8H 17 hour
[0091] Monomer A (1 eq), monomer B (1 eq), silver carbonate (4 eq), potassium acetate (4 eq), palladium chloride (0.01 eq) and di(tert-butyl)phosphine methyl tetrafluoroborate (0.05 eq) were dissolved in 1 mL of N,N-dimethylacetamide solvent, stirred at 80°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P8 (yield: 66.17%, Mn=26.0 KDa, PDI=1.80). When the structure of monomer A is The structure of monomer B is
[0092] Example 9: When R6=R7=H
[0093] Monomer A (1 eq), monomer B (1 eq), silver carbonate (4 eq), potassium acetate (4 eq), tetrakis(triphenylphosphine)palladium (0.001 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.02 eq) were dissolved in 1 mL of N,N-dimethylacetamide solvent, stirred at 100°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P9 (yield: 59.3%, Mn=25.00 KDa, PDI=1.60).
[0094] When the structure of monomer A is The structure of monomer B is
[0095] Example 10: When R8=R9=H
[0096] Monomer A (1 eq), monomer B (1 eq), silver carbonate (4 eq), potassium acetate (4 eq), tetrakis(triphenylphosphine)palladium (0.01 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.02 eq) were dissolved in 1 mL of N,N-dimethylacetamide solvent, stirred at 80°C, and reacted for 36 hours. The post-treatment was the same as in Example 1 to obtain polymer P10 (yield: 65.3%, Mn=22.00 KDa, PDI=1.80).
[0097] When the structure of monomer A is The structure of monomer B is
[0098] Example 11: When R 10 =R 11 =H
[0099] Monomer A (1 eq), monomer B (1 eq), silver carbonate (4 eq), potassium acetate (4 eq), tetrakis(triphenylphosphine)palladium:dichloro[1,1,-bis(diphenylphosphino)ferrocene]palladium=1:1 (0.01 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.02 eq) were dissolved in 1 mL of N,N-dimethylacetamide solvent, stirred at 80°C, and reacted for 24 hours. Post-treatment was the same as in Example 1 to obtain polymer P11 (yield: 63.3%, Mn=19.00 KDa, PDI=1.90).
[0100] When the structure of monomer A is The structure of monomer B is
[0101] Embodiment 12:
[0102] Monomer A (1 eq), monomer B (1 eq), silver carbonate (4 eq), potassium acetate (4 eq), tetrakis(triphenylphosphine)palladium:herrmann's catalyst = 1:2 (0.01 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.02 eq) were dissolved in 1 mL of N,N-dimethylacetamide solvent, stirred at 80°C, and reacted for 24 hours. Post-treatment was the same as in Example 1 to obtain polymer P12 (yield: 40.3%, Mn = 15.00 KDa, PDI = 1.90).
[0103] When the structure of monomer A is The structure of monomer B is
[0104] Example 13: When R 12 =R 13 =OC8H 17 ,hour
[0105] Monomer A (1 eq), monomer B (1 eq), silver carbonate (4 eq), potassium acetate (4 eq), tetrakis(triphenylphosphine)palladium / herrmann's catalyst (m / m=1:1) (0.01 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.02 eq) were dissolved in 1 mL of N,N-dimethylacetamide solvent, stirred at 80°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P13 (yield: 24.8%, Mn=27.00 KDa, PDI=1.50).
[0106] When the structure of monomer A is The structure of monomer B is
[0107] Example 14: When m=0, R 14 =R 15 =H
[0108] Monomer A (1 eq), monomer B (1 eq), potassium carbonate (4 eq), copper acetate (4 eq), tetrakis(triphenylphosphine)palladium (0.01 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.02 eq) were dissolved in 1 mL of N,N-dimethylacetamide solvent, stirred at 80°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P14 (yield: 59.3%, Mn=9.00 KDa, PDI=1.60).
[0109] Example 15: When m=0, R 14 =R 15 =C8H 17 ,hour
[0110] Monomer A (1 eq), monomer B (1 eq), potassium carbonate (8 eq), copper acetate (1 eq), tetrakis(triphenylphosphine)palladium (0.01 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.02 eq) were dissolved in 1 mL of N,N-dimethylacetamide solvent, stirred at 80°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P15 (yield: 47.3%, Mn=18.00, PDI=1.20).
[0111] Example 16: When m=1, R 14 =R 15 =C8H 17 , Ar=thiophene
[0112] Monomer A (1 eq), monomer B (1 eq), potassium carbonate (1 eq), potassium acetate (8 eq), tetrakis(triphenylphosphine)palladium (0.01 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.02 eq) were dissolved in 1 mL of N,N-dimethylacetamide solvent, stirred at 80°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P16 (yield: 56.83%, Mn=30.00 KDa, PDI=1.90).
[0113] Example 17: When m=1, R 14 =R 15 =C8H 17 , Ar=benzene
[0114] Monomer A (1 eq), monomer B (1 eq), potassium carbonate (8 eq), copper acetate (4 eq), tetrakis(triphenylphosphine)palladium (0.01 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.02 eq) were dissolved in 1 mL of N,N-dimethylacetamide solvent, stirred at 80°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P17 (yield: 58.83%, Mn=29.00 KDa, PDI=1.90)
[0115] Example 18: When m=1, R 14 =R 15 =C8H 17 , R 16 =R 17 =H
[0116] Monomer A (1 eq), monomer B (1 eq), silver carbonate (4 eq), potassium acetate (4 eq), tetrakis(triphenylphosphine)palladium (0.01 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.02 eq) were dissolved in 1 mL of xylene solvent, stirred at 80°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P18 (yield: 58.83%, Mn=26.00 KDa, PDI=1.90)
[0117] Example 19: When m=1, R 14 =R 15 =C8H 17 , R 18 =H
[0118] Monomer A (1 eq), monomer B (1 eq), silver carbonate (4 eq), potassium acetate (4 eq), tetrakis(triphenylphosphine)palladium (0.01 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.02 eq) were dissolved in 1 mL of toluene solvent, stirred at 80°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P19 (yield: 61.32%, Mn=25.263 KDa, PDI=2.00)
[0119] Example 20: When m=1, R 14 =R 15 =C8H 17 , R 19 =R 20 =H
[0120] Monomer A (1 eq), monomer B (1 eq), silver carbonate (4 eq), potassium acetate (4 eq), tetrakis(triphenylphosphine)palladium (0.01 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.02 eq) were dissolved in 1 mL of tetrahydrofuran solvent, stirred at 80°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P20 (yield: 59.8%, Mn=22.00 KDa, PDI=1.70)
[0121] Example 21: When m=1, R 14 =R 15 =C8H 17 , R 21 =H
[0122] Monomer A (1 eq), monomer B (1 eq), silver carbonate (4 eq), potassium acetate (4 eq), tetrakis(triphenylphosphine)palladium (0.01 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.02 eq) were dissolved in 1 mL of a mixed solvent of N,N-dimethylacetamide / xylene (v:v=1:1), stirred at 80°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P21 (yield: 48.5%, Mn=20.00 KDa, PDI=1.90)
[0123] Example 22: When m=1, R 14 =R 15 =C8H 17 , R 22 =R 23 =H
[0124] Monomer A (1 eq), monomer B (1 eq), silver carbonate (8 eq), potassium acetate (8 eq), tetrakis(triphenylphosphine)palladium (0.02 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.04 eq) were dissolved in 2 mL of a mixed solvent of N,N-dimethylacetamide / xylene (v:v=1:1), stirred at 80°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P22 (yield: 68.1%, Mn=29.00 KDa, PDI=1.20)
[0125] Example 23: When m=1, R 14 =R 15 =C8H 17 , Y=N,R 24 =C8H 17 , R 25 = No time
[0126] Monomer A (1 eq), monomer B (1 eq), silver carbonate (4 eq), potassium acetate (4 eq), tetrakis(triphenylphosphine)palladium (0.01 eq) and triphenylphosphine (0.02 eq) were dissolved in 1 mL of a mixed solvent of N,N-dimethylacetamide / xylene (v:v=1:1), stirred at 80°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P23 (yield: 50.9%, Mn=20.00 KDa, PDI=1.70)
[0127] Example 24: When m=1, R 14 =R 15 =C8H 17 , X=Y,R 24 =R 25 =C8H 17 hour
[0128] Monomer A (1 eq), monomer B (1 eq), silver carbonate (4 eq), potassium acetate (4 eq), tetrakis(triphenylphosphine)palladium (0.01 eq) and tricyclohexylphosphine tetrafluoroborate (0.02 eq) were dissolved in 1 mL of a mixed solvent of N,N-dimethylacetamide / xylene (v:v=1:1), stirred at 80°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P24 (yield: 49.1%, Mn=18.00 KDa, PDI=1.80)
[0129] Example 25: When m=1, R 14 =R 15 =C8H 17 , Y=Si,R 24 =R 25 =C8H 17 hour
[0130] Monomer A (1 eq), monomer B (1 eq), silver carbonate (4 eq), potassium acetate (4 eq), tetrakis(triphenylphosphine)palladium (0.01 eq) and tricyclohexylphosphine (0.02 eq) were dissolved in 1 mL of a mixed solvent of N,N-dimethylacetamide / xylene (v:v=1:1), stirred at 80°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P25 (yield: 49.1%, Mn=19.00 KDa, PDI=1.60)
[0131] Example 26: When m=1, R 14 =R 15 =H, hour
[0132] Monomer A (1 eq), monomer B (1 eq), silver carbonate (4 eq), potassium acetate (4 eq), tetrakis(triphenylphosphine)palladium (0.01 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.02 eq) were dissolved in 1 mL of a mixed solvent of N,N-dimethylacetamide / xylene (v:v=1:1), stirred at 80°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P26 (yield: 43.4%, Mn=10.00 KDa, PDI=1.80).
[0133] Example 27: When m=1, R 14 =R 15 =C8H 17 , R 26 =R 27 =H
[0134] Monomer A (1 eq), monomer B (1 eq), silver carbonate: copper acetate = 1:1 (4 eq), potassium acetate (4 eq), tetrakis(triphenylphosphine) palladium (0.01 eq) and di(tert-butyl)phosphinemethyl tetrafluoroborate (0.02 eq) were dissolved in 1 mL of a mixed solvent of N,N-dimethylacetamide / xylene (v:v = 1:1), stirred at 80°C, and reacted for 48 hours. Post-treatment was the same as in Example 1 to obtain polymer P27 (yield: 42.5%, Mn = 9.00 KDa, PDI = 2.00)
[0135] Example 28: Select the polymer P6 and the amphiphilic polymer PEG-PBLA (polyethylene glycol-polyaspartic acid benzyl ester) in Example 6 and dissolve them in tetrahydrofuran to prepare a 1 mg / mL solution for use. Take 5 mL of P6 mother liquor and 1 mL of PEG-PBLA mother liquor from the above-mentioned standby solutions and dissolve them in 50 mL of tetrahydrofuran. After ultrasonicating the above solution for 15 minutes, add it dropwise to 50 mL of ultrapure water, ultrasonicate it again for 15 minutes to make it completely dispersed, and then slowly pass nitrogen to remove tetrahydrofuran, and finally obtain a 100 μg / mL Pdot6 nanoparticle aqueous solution. Except for the different sampling concentrations, the preparation methods of 300 μg / mL and 500 μg / mL nanoparticle aqueous solutions are the same.
[0136] Example 29: Select polymer P15 in Example 15 and amphiphilic polymer FEG-PLA (polyethylene glycol-polylactic acid) to prepare 100 μg / mL Pdot15 nanoparticle aqueous solution, and the operation steps are the same as Example 28.
[0137] Example 30: Electrochemical band gap measurement of polymers using electrochemical cyclic voltammetry. The polymer synthesized in some examples was dissolved in chloroform, and then the solution was dripped onto a platinum sheet of a working electrode, and a 0.1 mol / L tetrabutylammonium hexafluorophosphate anhydrous acetonitrile solution was used as the electrolyte solution; a three-electrode system was formed with a glassy carbon electrode as the working electrode, a saturated calomel electrode as the reference electrode, and a platinum wire as the auxiliary electrode. Ferrocene / ferrocene salt was used as an internal standard to measure the electrochemical properties of the polymer. The HOMO and LUMO energy levels of the polymer were calculated according to the following formula:
[0138] HOMO=-e(E ox onset +4.8)(eV)
[0139] LUMO=-e(E red onset +4.8)(eV)
[0140] Where E ox onset and E red onset are the initial oxidation and reduction potentials of the polymers, respectively. The electrochemical band gaps corresponding to the polymers synthesized in the above embodiments are calculated by the above formulas as shown in Table 1
[0141] Table 1 Electrochemical band gaps of the polymers described in some examples
[0142]
[0143] The conjugated polymers in the above examples were subjected to electrochemical tests as shown in Table 1. The results show that the band gaps of the polymers prepared in the present invention all meet the band gap requirement of greater than 1.8 eV required for photocatalytic decomposition of water to produce hydrogen.
[0144] Example 31: Take 50 mL of the polymer nanoparticle solution of Examples 28 to 29, add 50 mL of ascorbic acid solution (0.2 mol / L), adjust the pH to about 4 with 0.1 mol / L NaOH, ultrasonicate for 15 minutes, and use the Perfil Labsolar 6A all-glass automatic online trace gas analysis system for testing under full spectrum irradiation for 7 hours to obtain the hydrogen production rate results.
[0145] Table 2 Hydrogen production rate (μmol.g -1 .h -1 )result
[0146]
[0147] As can be seen from Table 2, at different concentrations, Example 28 has the highest hydrogen production rate at 300 μg / mL, followed by 100 μg / mL, and finally 500 μg / mL; Example 29 has the highest hydrogen production rate at 100 μg / mL, reaching 44.14 μmol.g -1 .h -1 .
[0148] By comparing Examples 28 and 29, it was found that the hydrogen production rate of Example 28 was greater than that of Example 29, which indicates that the increase in the planarity of the conjugated polymer is beneficial to improving the hydrogen production rate.
[0149] Figure 1 The electrochemical cyclic voltammetry curves of P6 and P15 in Example 30 are shown in FIG. Figure 1 E ox onset and E red onset According to the formula, the HOMO of P6 is -0.82eV, LUMO is 1.67eV, and the electrochemical band gap is 2.49eV. The HOMO of P15 is -0.95eV, LUMO is 1.3eV, and the electrochemical band gap is 2.45eV. The energy level band gap can meet the photon energy required for exciton excitation.
[0150] Figure 2 Figure 31 shows the rate of hydrogen production from photocatalytic hydrolysis of Pdot6 and Pdot15 in Example 31. Figure 2 It can be seen that the conjugated polymer has certain photocatalytic water hydrogen production performance.
[0151] Although the embodiments of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments.
Claims
1. A photocatalyst prepared by using a conjugated polymer based on a thiophene[3,4-c]pyrrole-4,6-dione structure, wherein the conjugated polymer based on a thiophene[3,4-c]pyrrole-4,6-dione structure is polymer P6 or polymer P15; The chemical structure of the polymer P6 is shown in formula (I): n is 8-10000, It is a thiophene[3,4-c]pyrrole-4,6-dione derivative monomer, referred to as monomer A, and the structure of monomer A is The structure of monomer B is Y=C,R4=R5=C8H 17 ; The chemical structure of the polymer P15 is shown in formula (I): n is 8-10000, It is a thiophene[3,4-c]pyrrole-4,6-dione derivative monomer, referred to as monomer A, and the structure of monomer A is The structure of monomer B is m=0,R 14 =R 15 =C8H 17 ; The preparation method thereof comprises the following steps: Dissolve the thiophene[3,4-c]pyrrole-4,6-dione structure-based conjugated polymer and the amphiphilic polymer material in tetrahydrofuran to prepare a 1 mg / mL stock solution for later use; The mother liquors are taken separately, mixed and diluted with tetrahydrofuran to the required concentration; the diluted mixed solution is ultrasonically dispersed, quickly poured into ultrapure water for ultrasonic vibration, and then an inert gas is introduced to remove the low-boiling point solvent in the solvent, and finally a nanoparticle aqueous solution is obtained, which is the photocatalyst.
2. The photocatalyst according to claim 1, characterized in that: The amphiphilic polymer material includes polyethylene glycol-polyaspartic acid benzyl ester, folic acid-polyethylene glycol-polyaspartic acid benzyl ester, polyethylene glycol-polycaprolactone, polyethylene glycol-polylactic acid, polyethylene glycol-polylactic acid / glycolic acid copolymer, and distearoyl phosphatidylethanolamine-polyethylene glycol.
3. Use of the photocatalyst as claimed in claim 1 in photocatalytic water decomposition to produce hydrogen.