A welding method for the corner weld of Q690qD bridge steel box bar

By adopting the single-sided double V-shaped groove welding method with blunt edge and the gas shielded welding combined process, the problem of poor weldability of Q690qD steel is solved, high-quality welding effect and deformation control are achieved, and the requirements of bridge steel box-type rods are met. Welding requirements.

CN114700595BActive Publication Date: 2024-10-15CHINA RAILWAY BAOJI BRIDGE YANGZHOU CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210481676.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-05
Publication Date
2024-10-15
Estimated Expiration
2042-05-05

AI Technical Summary

Technical Problem

Q690qD grade steel has poor weldability, stringent welding environment and process requirements, and welding deformation is difficult to control, affecting mechanical properties such as yield strength, tensile strength, and elongation.

Method used

The single-sided double V-shaped groove welding method with blunt edges is used, combined with the combined process of gas shielded welding and submerged arc automatic welding, and the welding temperature and heat input are controlled through the sequence of positioning welding, bottom welding, filling and cover welding, Reduce welding torsional deformation.

Benefits of technology

It effectively avoids the problem of weld penetration, ensures the quality and appearance of the weld, reduces welding deformation, and improves welding operability and quality control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114700595B_ABST
    Figure CN114700595B_ABST
Patent Text Reader

Abstract

The invention discloses a welding method for the corner weld of a Q690qD bridge steel box-type rod, comprising: symmetrically processing grooves on two long sides of a web, the groove shape is a single-sided double V-shaped groove with a blunt edge, and the blunt edge thickness of the single-sided double V-shaped groove is 2-6 mm; the angle of the upper V-shaped groove is 10-15°; the angle of the lower V-shaped groove is 45-55°; the depth of the lower V-shaped groove is 15-28 mm; the cover plate and the web are assembled into a box-type rod, and positioning welding is performed in the groove to connect the cover plate and the web together; the above-formed box-type rod is turned right by 90°, and two corner welds on one side of the box-type rod are welded; the above-formed box-type rod is turned right by 180° again, and then two corner welds on the other side of the box-type rod are welded. The method solves the manufacturing difficulties in the assembly and welding of the box-type rod, ensures the welding quality, and controls the welding deformation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of bridge manufacturing, and in particular relates to a welding method for the corner welds of a Q690qD bridge steel box-type rod. Background Art

[0002] Steel truss bridge is a structural form that hollows out a solid steel plate girder bridge according to certain rules. The overall structure is a beam stress-bearing mode. The main truss of the steel truss consists of an upper chord, a lower chord and a web, most of which are box-type members. The box-type design of the main truss member usually has a cover plate and a web plate thickness in the range of 30mm to 60mm. The corner welds between the cover plate and the web are mostly single-sided partial penetration welds, and the blunt edge of the corner weld groove is ≥2mm.

[0003] In recent years, with the vigorous development of bridge construction, steel truss bridges are pursuing lighter weight and larger spans while also promoting the development of high-performance steel for bridges. Steel with a yield strength of 690MPa has also emerged in the application of steel truss bridges. However, Q690qD grade steel has poor weldability compared to other low-strength grade bridge steels, and has more stringent requirements on welding environment and welding process. In addition, due to the particularity of Q690qD steel rolling process TMCP+tempering, the temperature of Q690qD steel for heat correction after welding deformation cannot exceed 600℃. Using higher temperature for heat correction will reduce the yield strength, tensile strength, elongation and other mechanical properties of steel to varying degrees.

[0004] Due to the weldability and thermal correction characteristics of Q690qD steel, Q690qD box-type rods need to control the welding heat input of the corner welds, reduce the welding filling amount, and use appropriate welding process methods to ensure welding quality and control welding deformation during factory manufacturing. Summary of the invention

[0005] In order to solve the above problems existing in the prior art, the present invention provides a welding method for the corner welds of Q690qD bridge steel box-type rods.

[0006] The technical problem to be solved by the present invention is achieved through the following technical solutions:

[0007] A method for welding corner welds of a Q690qD bridge steel box-shaped member, wherein the Q690qD bridge steel box-shaped member is composed of a cover plate and a web plate of the same material, and the welding method comprises the following steps:

[0008] S1: symmetrically processing grooves on the two long sides of the web, wherein the groove shape is a single-sided double V-shaped groove with a blunt edge, and the blunt edge thickness c of the single-sided double V-shaped groove is 2-6 mm; the angle of the upper V-shaped groove is 10-15°; the angle of the lower V-shaped groove is 45-55°; the depth h of the lower V-shaped groove is 15-28 mm;

[0009] S2: Then the cover plate is horizontally arranged and the web plate is vertically arranged to be assembled into a box-shaped rod, and the groove opening is made to face outward, and then positioning welding is performed in the groove to connect the cover plate and the web plate together;

[0010] S3: Flip the box-shaped bar formed in S2 to the right by 90°, and then weld the two corner welds on one side of the box-shaped bar. The welding process adopts gas shielded welding for base welding and submerged arc automatic welding for filling and capping welding, and the welding directions of the two corner welds are consistent;

[0011] S4: The box-shaped bar formed in S3 is turned rightward 180°, and then the two corner welds on the other side of the box-shaped bar are welded. The welding process uses gas shielded welding for base welding and submerged arc automatic welding for filling and covering welding, and the welding directions of the two corner welds are consistent.

[0012] Furthermore, in S2, the welding area is preheated before positioning welding, the preheating temperature is 75-250°C, and the weld is heated after welding, the heating temperature is 200-250°C, and the temperature is kept for more than 120 minutes, and then slowly cooled to room temperature.

[0013] Furthermore, in S3 and S4, the welding area is preheated before welding, the preheating temperature is 75-250°C, and the temperature between weld layers is maintained at 75-200°C during welding. After welding, the weld is heated to 200-250°C and kept warm for more than 120 minutes, and then slowly cooled to room temperature.

[0014] Furthermore, the base welding is performed using mixed gas protection, the welding wire is solid wire, the welding current is 180-220V, the welding voltage is 22-26V, the welding speed is 250-350mm / min, and the heat input is 0.54-1.10kJ / mm.

[0015] Furthermore, during the filling and capping welding, the welding current is 600-680A, the welding voltage is 30-34V, the welding speed is 360-460mm / min, and the heat input is 2.35-3.85kJ / mm.

[0016] Beneficial effects of the present invention:

[0017] 1. The present invention adopts a welding method combining mixed gas shielded welding and submerged arc automatic welding during welding, which can effectively avoid the problem of weld penetration when the assembly gap of the box-shaped corner weld is 0-3mm, and at the same time can ensure the fusion quality of the weld root and the appearance quality of the weld;

[0018] 2. The welding sequence adopted by the present invention can effectively reduce the welding torsional deformation of the box-type rod and reduce the difficulty of subsequent correction;

[0019] 3. This welding method is highly operable and can ensure the welding quality of box-shaped corner welds and control welding deformation.

[0020] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a structural schematic diagram of a box-type bar;

[0022] Figure 2 for Figure 1 A schematic diagram of the enlarged structure of part E in the middle;

[0023] FIG3( a ) is a schematic diagram of welding position 1;

[0024] FIG3( b ) is a schematic diagram of welding position 2. FIG.

[0025] Description of reference numerals:

[0026] 1-belly plate; 2-cover plate. DETAILED DESCRIPTION

[0027] The present invention is further described in detail below with reference to specific embodiments, but the embodiments of the present invention are not limited thereto.

[0028] Example 1

[0029] Please also see Figure 1 3, an embodiment of the present invention provides a welding method for a Q690qD bridge steel box-shaped corner weld, the Q690qD bridge steel box-shaped rod is composed of a web 1 on both sides and a cover plate 2 located on the upper and lower end surfaces of the web 1, the web 1 and the cover plate 2 are made of the same material, the thickness of the web 1 and the cover plate 2 are both 30 to 60 mm, and the corner weld between the cover plate 2 and the web 1 is a single-sided partial penetration weld, the welding method comprises the following steps:

[0030] S1: The two long sides of the web of the Q690qD bridge steel box-type member are symmetrically machined into grooves by mechanical equipment, wherein the groove shape is a single-sided double V-shaped groove with a blunt edge, wherein the blunt edge thickness c of the single-sided double V-shaped groove is 2 mm; the β angle of the upper V-shaped groove is 10°, and the setting of this angle can reduce the filling amount; the α angle of the lower V-shaped groove is 45°, and the depth h of the lower V-shaped groove is 15 mm, and the setting of this angle and depth can ensure the weld penetration and reduce the filling amount, thereby reducing the heat input and welding shrinkage deformation, thereby reducing the difficulty of subsequent thermal correction.

[0031] By processing the groove with mechanical equipment, the processing quality of the groove can be improved and the adverse effects of poor groove forming on the assembly gap and welding quality of the weld can be avoided.

[0032] S2: Then the cover plate is arranged horizontally and the web plate is arranged vertically to assemble into a box-shaped rod, such as Figure 1 As shown, the groove is opened outward, and then positioning welding is performed in the groove of the box-shaped corner weld to connect the cover plate and the web plate together. Specifically, 80% Ar + 20% CO2 mixed gas shielded welding is used for positioning welding, wherein the model of the solid welding wire is SM-110 and the diameter of the welding wire is 1.2 mm.

[0033] Before positioning welding, preheat the welding area to 75°C. After welding, heat the weld to 200°C and keep it warm for 120 minutes. Then cover the weld with insulation cotton and slowly cool it to room temperature to prevent the weld from cracking due to excessive cooling.

[0034] S3: The box-shaped bar formed in S2 is flipped to the right by 90°. Specifically, the position after flipping is shown in FIG3(a). Then, two corner welds A and B on one side of the box-shaped bar are welded. The welding process adopts gas shielded welding for base welding and submerged arc automatic welding for filling and covering welding, and the welding directions of the two corner welds are consistent.

[0035] Specifically, the base welds of weld A and weld B in Figure 3(a) are welded by 80% Ar+20% CO2 mixed gas shielded welding, and the filling and cap welds of weld A and weld B are welded by submerged arc automatic welding. The welding wire model is XY-S80Q, and the welding wire diameter is 4 mm; the flux model is XY-AF85QNH; weld A and weld B can be welded simultaneously or at different times, but the welding direction must be consistent, so that the deformation of the entire box-type rod is uniform, reducing the difficulty of thermal correction.

[0036] In addition, the welding area needs to be preheated before welding, and the preheating temperature is 75°C. During the welding process, the temperature between the weld layers is maintained at 75°C. After welding, the weld is heated to 200°C and kept warm for 120 minutes. The weld is then covered with insulation cotton and slowly cooled to room temperature to prevent the weld from cooling too quickly and causing cracks.

[0037] S4: After the welding of welds A and B is completed, the box-shaped bar formed by S3 is flipped 180° to the right to the position shown in Figure 3(b), and then the two corner welds C and D on the other side of the box-shaped bar are welded. The welding process uses gas shielded welding for base welding and submerged arc automatic welding for filling and covering welding, and the welding directions of the two corner welds are consistent.

[0038] Specifically, the base welds of weld C and weld D in Figure 3(b) are welded by 80% Ar + 20% CO2 mixed gas shielded welding, and the filling and cap welds of weld C and weld D are welded by submerged arc automatic welding. The welding wire model is XY-S80Q and the welding wire diameter is 4 mm; the flux model is XY-AF85QNH; weld C and weld D can be welded simultaneously or at different times, but the welding method must be consistent with that of weld A and weld B.

[0039] In addition, the welding area needs to be preheated before welding, and the preheating temperature is 75°C. During the welding process, the temperature between the weld layers is maintained at 75°C. After welding, the weld is heated to 200°C and kept warm for 120 minutes. The weld is then covered with insulation cotton and slowly cooled to room temperature to prevent the weld from cooling too quickly and causing cracks.

[0040] Specifically, when welding the base welds of welds A, B, C, and D, the welding current is 180A, the welding voltage is 22V, the welding speed is 250mm / min, and the heat input is 0.54kJ / mm; when welding the filling and cover welds of welds A, B, C, and D, the welding current is 600A, the welding voltage is 30V, the welding speed is 360mm / min, and the heat input is 2.35kJ / mm.

[0041] Example 2

[0042] Please also see Figure 1 3, an embodiment of the present invention provides a welding method for a Q690qD bridge steel box-shaped corner weld, the Q690qD bridge steel box-shaped rod is composed of a web 1 on both sides and a cover plate 2 located on the upper and lower end surfaces of the web 1, the web 1 and the cover plate 2 are made of the same material, the thickness of the web 1 and the cover plate 2 are both 30 to 60 mm, and the corner weld between the cover plate 2 and the web 1 is a single-sided partial penetration weld, the welding method comprises the following steps:

[0043] S1: The two long sides of the web of the Q690qD bridge steel box-type member are symmetrically machined into grooves by mechanical equipment, wherein the groove shape is a single-sided double V-shaped groove with a blunt edge, wherein the blunt edge thickness c of the single-sided double V-shaped groove is 4 mm; the β angle of the upper V-shaped groove is 13°, and the setting of this angle can reduce the filling amount; the α angle of the lower V-shaped groove is 50°, and the depth h of the lower V-shaped groove is 22 mm. The setting of this angle and depth can ensure the weld penetration and reduce the filling amount, thereby reducing the heat input and welding shrinkage deformation, thereby reducing the difficulty of subsequent thermal correction.

[0044] By processing the groove with mechanical equipment, the processing quality of the groove can be improved and the adverse effects of poor groove forming on the assembly gap and welding quality of the weld can be avoided.

[0045] S2: Then the cover plate is arranged horizontally and the web plate is arranged vertically to assemble into a box-shaped rod, such as Figure 1 As shown, the groove is opened outward, and then positioning welding is performed in the groove of the box-shaped corner weld to connect the cover plate and the web plate together. Specifically, 80% Ar + 20% CO2 mixed gas shielded welding is used for positioning welding, wherein the model of the solid welding wire is SM-110 and the diameter of the welding wire is 1.2 mm.

[0046] Before positioning welding, the welding area is preheated to 163°C. After welding, the weld is heated to 225°C and kept warm for 150 minutes. The weld is then covered with insulation cotton and slowly cooled to room temperature to prevent the weld from cooling too quickly and causing cracks.

[0047] S3: The box-shaped bar formed in S2 is flipped to the right by 90°. Specifically, the position after flipping is shown in FIG3(a). Then, two corner welds A and B on one side of the box-shaped bar are welded. The welding process adopts gas shielded welding for base welding and submerged arc automatic welding for filling and covering welding, and the welding directions of the two corner welds are consistent.

[0048] Specifically, the base welds of weld A and weld B in Figure 3(a) are welded by 80% Ar+20% CO2 mixed gas shielded welding, and the filling and cap welds of weld A and weld B are welded by submerged arc automatic welding. The welding wire model is XY-S80Q, and the welding wire diameter is 4 mm; the flux model is XY-AF85QNH; weld A and weld B can be welded simultaneously or at different times, but the welding direction must be consistent, so that the deformation of the entire box-type rod is uniform, reducing the difficulty of thermal correction.

[0049] In addition, the welding area needs to be preheated before welding, and the preheating temperature is 163°C. During the welding process, the temperature between the weld layers is maintained at 138°C. After welding, the weld is heated to 225°C and kept warm for 150 minutes. The weld is then covered with insulation cotton and slowly cooled to room temperature to prevent the weld from cooling too quickly and causing cracks.

[0050] S4: After the welding of welds A and B is completed, the box-shaped bar formed by S3 is flipped 180° to the right to the position shown in Figure 3(b), and then the two corner welds C and D on the other side of the box-shaped bar are welded. The welding process uses gas shielded welding for base welding and submerged arc automatic welding for filling and covering welding, and the welding directions of the two corner welds are consistent.

[0051] Specifically, the base welds of weld C and weld D in Figure 3(b) are welded by 80% Ar + 20% CO2 mixed gas shielded welding, and the filling and cap welds of weld C and weld D are welded by submerged arc automatic welding. The welding wire model is XY-S80Q and the welding wire diameter is 4 mm; the flux model is XY-AF85QNH; weld C and weld D can be welded simultaneously or at different times, but the welding method must be consistent with that of weld A and weld B.

[0052] In addition, the welding area needs to be preheated before welding, and the preheating temperature is 163°C. During the welding process, the temperature between the weld layers is maintained at 138°C. After welding, the weld is heated to 225°C and kept warm for 150 minutes. The weld is then covered with insulation cotton and slowly cooled to room temperature to prevent the weld from cooling too quickly and causing cracks.

[0053] Specifically, when welding the base welds of welds A, B, C, and D, the welding current is 200A, the welding voltage is 24V, the welding speed is 300mm / min, and the heat input is 0.82kJ / mm; when welding the filling and cover welds of welds A, B, C, and D, the welding current is 640A, the welding voltage is 32V, the welding speed is 410mm / min, and the heat input is 3.10kJ / mm.

[0054] Example 3

[0055] Please also see Figure 1 3, an embodiment of the present invention provides a welding method for a Q690qD bridge steel box-shaped corner weld, the Q690qD bridge steel box-shaped rod is composed of a web 1 on both sides and a cover plate 2 located on the upper end surface of the web 1, the web 1 and the cover plate 2 are made of the same material, the thickness of the web 1 and the cover plate 2 are both 30 to 60 mm, and the corner weld between the cover plate 2 and the web 1 is a single-sided partial penetration weld, the welding method comprises the following steps:

[0056] S1: The two long sides of the web of the Q690qD bridge steel box-type member are symmetrically machined into grooves by mechanical equipment, wherein the groove shape is a single-sided double V-shaped groove with a blunt edge, wherein the blunt edge thickness c of the single-sided double V-shaped groove is 6 mm; the β angle of the upper V-shaped groove is 15°, and the setting of this angle can reduce the filling amount; the α angle of the lower V-shaped groove is 55°, and the depth h of the lower V-shaped groove is 28 mm, and the setting of this angle and depth can ensure the weld penetration and reduce the filling amount, thereby reducing the heat input and welding shrinkage deformation, thereby reducing the difficulty of subsequent thermal correction.

[0057] By processing the groove with mechanical equipment, the processing quality of the groove can be improved and the adverse effects of poor groove forming on the assembly gap and welding quality of the weld can be avoided.

[0058] S2: Then the cover plate is arranged horizontally and the web plate is arranged vertically to assemble into a box-shaped rod, such as Figure 1 As shown, the groove is opened outward, and then positioning welding is performed in the groove of the box-shaped corner weld to connect the cover plate and the web plate together. Specifically, 80% Ar + 20% CO2 mixed gas shielded welding is used for positioning welding, wherein the model of the solid welding wire is SM-110 and the diameter of the welding wire is 1.2 mm.

[0059] Before positioning welding, preheat the welding area to 250℃. After welding, heat the weld to 250℃ and keep it warm for 180min. Then cover the weld with insulation cotton and slowly cool it to room temperature to prevent the weld from cracking due to too fast cooling speed.

[0060] S3: The box-shaped bar formed in S2 is flipped to the right by 90°. Specifically, the position after flipping is shown in FIG3(a). Then, two corner welds A and B on one side of the box-shaped bar are welded. The welding process adopts gas shielded welding for base welding and submerged arc automatic welding for filling and covering welding, and the welding directions of the two corner welds are consistent.

[0061] Specifically, the base welds of weld A and weld B in Figure 3(a) are welded by 80% Ar+20% CO2 mixed gas shielded welding, and the filling and cap welds of weld A and weld B are welded by submerged arc automatic welding. The welding wire model is XY-S80Q, and the welding wire diameter is 4 mm; the flux model is XY-AF85QNH; weld A and weld B can be welded simultaneously or at different times, but the welding direction must be consistent, so that the deformation of the entire box-type rod is uniform, reducing the difficulty of thermal correction.

[0062] In addition, the welding area needs to be preheated before welding, and the preheating temperature is 250℃. During the welding process, the temperature between the weld layers is maintained at 200℃. After welding, the weld is heated to 250℃ and kept warm for 180 minutes. Then, the weld is covered with insulation cotton and slowly cooled to room temperature to prevent the weld from cooling too quickly and causing cracks.

[0063] S4: After the welding of welds A and B is completed, the box-shaped bar formed by S3 is flipped 180° to the right to the position shown in Figure 3(b), and then the two corner welds C and D on the other side of the box-shaped bar are welded. The welding process uses gas shielded welding for base welding and submerged arc automatic welding for filling and covering welding, and the welding directions of the two corner welds are consistent.

[0064] Specifically, the base welds of weld C and weld D in Figure 3(b) are welded by 80% Ar + 20% CO2 mixed gas shielded welding, and the filling and cap welds of weld C and weld D are welded by submerged arc automatic welding. The welding wire model is XY-S80Q and the welding wire diameter is 4 mm; the flux model is XY-AF85QNH; weld C and weld D can be welded simultaneously or at different times, but the welding method must be consistent with that of weld A and weld B.

[0065] In addition, the welding area needs to be preheated before welding, and the preheating temperature is 250℃. During the welding process, the temperature between the weld layers is maintained at 200℃. After welding, the weld is heated to 250℃ and kept warm for 180 minutes. Then, the weld is covered with insulation cotton and slowly cooled to room temperature to prevent the weld from cooling too quickly and causing cracks.

[0066] Specifically, when welding the base welds of welds A, B, C, and D, the welding current is 220A, the welding voltage is 26V, the welding speed is 350mm / min, and the heat input is 1.10kJ / mm; when welding the filling and cover welds of welds A, B, C, and D, the welding current is 680A, the welding voltage is 34V, the welding speed is 460mm / min, and the heat input is 3.85kJ / mm.

[0067] Practice has proved that the welding method of the present invention solves the manufacturing problems in the assembly and welding of box-type members composed of the upper chord, lower chord and web members of the steel truss by setting reasonable groove types, welding sequences, welding processes and other measures, ensures welding quality, controls welding deformation, and can fully meet the welding quality requirements of the project. At the same time, it has extremely high practical and promotion value, and can play a good reference role in the subsequent manufacture of similar steel trusses.

[0068] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. A welding method for the corner weld of a Q690qD bridge steel box-type member, wherein the Q690qD bridge steel box-type member is composed of a cover plate and a web plate of the same material, and the corner weld between the cover plate and the web plate is a single-sided partial penetration weld, characterized in that: The welding method comprises the following steps: S1: The grooves are symmetrically processed on the two long sides of the web, wherein the groove shape is a single-sided double V-shaped groove with a blunt edge, and the blunt edge thickness c of the single-sided double V-shaped groove is 2-6 mm; the angle β of the upper V-shaped groove is 10-15°; the angle α of the lower V-shaped groove is 45-55°; the depth h of the lower V-shaped groove is 15-28 mm; S2: Then the cover plate is horizontally arranged and the web plate is vertically arranged to be assembled into a box-shaped rod, and the groove opening is made to face outward, and then positioning welding is performed in the groove to connect the cover plate and the web plate together; S3: Flip the box-shaped bar formed in S2 to the right by 90°, and then weld the two corner welds on one side of the box-shaped bar. The welding process adopts gas shielded welding for base welding and submerged arc automatic welding for filling and capping welding, and the welding directions of the two corner welds are consistent; S4: The box-shaped bar formed in S3 is turned rightward 180°, and then the two corner welds on the other side of the box-shaped bar are welded. The welding process uses gas shielded welding for base welding and submerged arc automatic welding for filling and capping welding, and the welding directions of the two corner welds are consistent; The base welding is protected by 80% Ar + 20% CO2 mixed gas, the welding wire is solid wire, the welding current is 180-220V, the welding voltage is 22-26V, the welding speed is 250-350mm / min, and the heat input is 0.54-1.10kJ / mm; During the filling and capping welding, the welding current is 600-680A, the welding voltage is 30-34V, the welding speed is 360-460mm / min, and the heat input is 2.35-3.85kJ / mm.

2. The welding method for the corner weld of Q690qD bridge steel box bar according to claim 1 is characterized in that: In S2, the welding area is preheated before positioning welding, the preheating temperature is 75-250°C, and the weld is heated after welding, the heating temperature is 200-250°C, and the temperature is kept for more than 120 minutes, and then slowly cooled to room temperature.

3. The welding method for the corner weld of Q690qD bridge steel box bar according to claim 1 is characterized in that: In S3 and S4, the welding area is preheated before welding, the preheating temperature is 75-250°C, and the temperature between weld layers is maintained at 75-200°C during welding. After welding, the weld is heated to 200-250°C and kept warm for more than 120 minutes, and then slowly cooled to room temperature.