Polyether-modified polybutadiene and preparation method thereof
By reacting polybutadiene with epoxidation reagents and hydroxyl functional compounds, and then reacting with epoxy functional compounds, combined with acid catalysis and Zn/Co bimetallic catalysis, polybutadiene with pendant polyether chains was successfully prepared. , solving the complexity and structural limitations of the preparation methods in the prior art, and achieving polyether-modified polybutadiene with high purity and structural diversity.
Patent Information
- Application Number
- CN202080082791.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-23
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-11-23
AI Technical Summary
It is difficult to prepare linear polybutadiene with pendant polyether chains through a simple and direct alkoxylation reaction, especially when using epoxy-functional polybutadiene to prepare pendant hydroxyl-functional polybutadiene. There are structural limitations and process complexity issues, and a lack of widely available methods to alter the chemical composition of polyether-modified polybutadiene.
Polybutadiene is formed by reacting polybutadiene with an epoxidizing reagent to form epoxy-functional polybutadiene, which is then reacted with a hydroxyl-functional compound and further reacted with an epoxy-functional compound to form polyether-modified polybutadiene, using an acid Catalysis and Zn/Co double metal cyanide catalyst to achieve alkoxylation of pendant OH groups, controlling the chain length and monomer sequence of polyether groups.
The modification of linear polybutadiene directly alkoxylated at the comb position is achieved, with high purity and low residual epoxy groups. It can adjust the number and structure of polyether groups in a wide range and solve the existing problems. There are problems in the art with products containing incomplete functionalization and residual epoxy groups.
Smart Images

Figure FDA0004997027570000031 
Figure FDA0004997027570000032 
Figure FDA0004997027570000041
Abstract
Description
[0001] The present invention relates to a method for preparing polyether-modified polybutadiene and polyether-modified polybutadiene that can be prepared by the method, wherein the method comprises the following steps:
[0002] a) reacting at least one polybutadiene (A) with at least one epoxidizing agent (B) to obtain at least one epoxy-functional polybutadiene (C);
[0003] b) reacting the at least one epoxy-functional polybutadiene (C) with at least one hydroxy-functional compound (D) to obtain at least one hydroxy-functional polybutadiene (E);
[0004] c) reacting the at least one hydroxy-functional polybutadiene (E) with at least one epoxy-functional compound (F) to obtain at least one polyether-modified polybutadiene (G).
[0005] The polyether-modified polybutadienes according to the invention are thus obtainable by direct alkoxylation of pendant hydroxy-functional polybutadienes and have polyether groups in pendant (comb) positions.
[0006] Polybutadiene with pendant polyether groups is known and is prepared according to the prior art, for example, by reaction of reactive functionalized polybutadiene with polyethers. For example, Q. Gao et al. describe in Macromolecular Chemistry and Physics (2013), 214 (15), 1677-1687 an amphiphilic polymer comb structure prepared by grafting polyethylene glycol onto a polybutadiene backbone. According to JP 2011038003, polybutadiene functionalized with maleic anhydride units is reacted with amino-terminated polyethers. The result is a maleated polybutadiene with polyether groups in the comb position connected via amide or imide groups. In a similar process, according to J. Wang, Journal of Applied Polymer Science (2013), 128 (4), 2408-2413, polyethylene glycol is added to polybutadiene with a high proportion of 1,2-butadiene monomer units to form ester bonds. High molecular weight graft polymers with a comb structure are obtained by addition of epoxidized polybutadiene to OH-functional polyethers according to the method disclosed in JP 2002105209. According to Polymer International (1995), 38(3), 219-225, H. Decher et al. used addition of isocyanate-terminated polyethylene glycol to hydroxy-functional polybutadiene.
[0007] Also known are processes for preparing polyether-modified polybutadienes in which hydroxy-functional polybutadienes are reacted with epoxide compounds. For example, the prior art discloses the alkoxylation of OH-terminated polybutadienes.
[0008] For example, US 4994621 A describes the alkoxylation of hydroxy-terminated polybutadiene with ethylene oxide and propylene oxide in the presence of tetramethylammonium hydroxide. EP 2003156 A1 states that, due to structural reasons and the poor solubility of basic catalysts, base-catalyzed alkoxylation of OH-terminated polybutadiene is almost impossible, but rather double metal cyanide (DMC) catalysis is preferred. The use of OH-terminated polybutadiene in the alkoxylation leads only to polyether-polybutadiene-polyether triblock structures. According to EP 2003156 A1, this block structure is the reason for the poor miscibility with other reaction components in the preparation of polyurethanes.
[0009] In addition to the alkoxylation of hydroxyl-terminated polybutadiene, the alkoxylation of pendant hydroxyl-functional polybutadiene is also known. For example, Q. Gao et al. describe the preparation of pendant polyether-modified polybutadiene by alkoxylating pendant hydroxyl-functional polybutadiene with ethylene oxide in Macromolecular Chemistry and Physics (2013), 214 (15), 1677-1687. The pendant hydroxyl-functional polybutadiene used here is first prepared by epoxidation of polybutadiene, then reacting the epoxidized polybutadiene with a lithium-polybutadiene compound, and finally protonating the reaction product with methanolic HCl. This method produces polybutadiene with pendant polyether groups and pendant polybutadiene groups. Since there is always a polybutadiene group for each polyether group here, this method leads to a polyether-modified polybutadiene with a low HLB value (HLB ~ hydrophilic-lipophilic balance). In addition, the polyether-modified polybutadiene is branched in the polybutadiene part. Polyether-modified polybutadiene with a higher HLB value and / or an unbranched polybutadiene part cannot be prepared by this method. Another disadvantage of this method is the use of organometallic compounds (n-BuLi and lithium-polybutadiene), which place special demands on the process scheme due to their high sensitivity to air and moisture. This makes it difficult to implement the method industrially. To date, the prior art has not disclosed any method for preparing linear polybutadiene preferably with pendant polyether chains by a simple direct alkoxylation reaction of pendant hydroxyl-functional polybutadiene with alkylene oxide, wherein the pendant hydroxyl-functional polybutadiene is prepared from epoxy-functional polybutadiene without the use of organometallic compounds such as lithium-polybutadiene. In summary, it can be said that the prior art to date has not disclosed any method for preparing linear polybutadiene with polyether chains in comb-like positions by a simple direct alkoxylation reaction with alkylene oxide.
[0010] Chemical modification of polybutadiene by means of epoxidation and further reaction is known from the literature. The epoxide ring opening usually takes place by reaction with amines. JP 53117030 and DE 2943879 describe the addition of ethanolamine or diethanolamine, EP 351135 and DE 3305964 describe the reaction of epoxide groups with dimethylamine. DD 206286 discloses the addition of primary and secondary amines having 4 to 20 carbon atoms to epoxidized polybutadiene in polar solvents. Also known are polybutadienes modified with fatty acids. For example, DE 3442200 describes the addition of C6-C 22 The carboxylic acid is added to the epoxidized polybutadiene. No further alkoxylation of the reaction product is disclosed in these documents.
[0011] Amine-functional polybutadienes are not very suitable as starting compounds for the alkoxylation in the context of the present invention since they impart a generally undesirable basic character to the product, lead to discoloration or, for example, inhibit alkoxylation catalysts such as double metal cyanide.
[0012] According to the prior art, the addition of alcohols and water to epoxidized polybutadiene seems to be much more difficult than the addition of amines and carboxylic acids. Qing Gao et al. describe the addition of water catalyzed by trifluoromethanesulfonic acid to epoxidized polybutadiene in THF in J. Macromol. Sci., Part A: Pure and Applied Chemistry (2013), 50, 297-301. The purpose of WO 2016 / 142249 A1 is to prepare glassy polymers by adding water or alcohols having 1 to 4 carbon atoms to the epoxy groups of polybutadiene, and is limited to the preparation of OH-functional polybutadiene with a low molar mass of 300 to 2000 g / mol and a high content of 1,2-vinyl and 1,2-cyclovinyl double bonds of 50% to 80%.
[0013] Polybutadiene and modified polybutadienes are used in many cases as reactive components or formulation ingredients, for example to render the polymer hydrophobic or to make it flexible and to improve the mechanical properties. However, at present, the possible uses of alkoxylated polyether-modified polybutadienes are often limited due to the restriction to a few available triblock structures. To date, there has been no way to vary the chemical composition of polyether-modified polybutadienes over a wide range. Furthermore, there is no simple method for preparing such polymers.
[0014] It is an object of the present invention to overcome at least one of the disadvantages of the prior art.
[0015] A specific problem to be solved is to provide an improved process for preparing linear polybutadienes modified with polyether groups, preferably in comb-like (pendant) positions. The process should also make it possible to obtain linear polybutadienes preferably with pendant polyether groups very simply in terms of process technology and should be possible, for example, without the use of organolithium compounds. Polyether-modified polybutadienes should also be obtainable by direct alkoxylation of pendant hydroxy-functional polybutadienes. Another problem to be solved here is to provide improved pendant hydroxy-functional polybutadienes as precursors and chain starters for the alkoxylation in this process.
[0016] It has now been found that, surprisingly, this problem is solved by a process for preparing polyether-modified polybutadiene, which comprises the following steps:
[0017] a) reacting at least one polybutadiene (A) with at least one epoxidizing agent (B) to obtain at least one epoxy-functional polybutadiene (C);
[0018] b) reacting the at least one epoxy-functional polybutadiene (C) with at least one hydroxy-functional compound (D) to obtain at least one hydroxy-functional polybutadiene (E);
[0019] c) reacting the at least one hydroxy-functional polybutadiene (E) with at least one epoxy-functional compound (F) to obtain at least one polyether-modified polybutadiene (G).
[0020] It has further surprisingly been found that polybutadienes having a high proportion of 1,4 units and a low content of vinyl 1,2 units can, after epoxidation with hydrogen peroxide, readily react with OH-functional compounds under acid-catalyzed ring opening to give pendant OH-functional polybutadienes (polybutadiene alcohols) which can then be alkoxylated with alkylene oxides.
[0021] The problem solved by the invention is therefore solved by the subject matter of the independent claims. Advantageous configurations of the invention are specified in the dependent claims, the embodiments and the description.
[0022] The subject matter of the present invention is described by way of the following examples, but it is not intended to limit the present invention to these exemplary embodiments. In the case of the following specified ranges, general formulas or classes of compounds, these are intended not only to cover the corresponding ranges or groups of compounds explicitly mentioned, but also to cover all sub-ranges and sub-groups of compounds that can be obtained by excluding individual values (ranges) or compounds. In the case of citing documents in the context of this specification, their entire contents are intended to constitute part of the disclosure of the present invention.
[0023] Where average values are reported below, these are numerical average values unless otherwise stated. Where measured values, parameters or material properties determined by measurements are reported below, these are measured values, parameters or material properties measured at 25° C. and preferably at a pressure of 101 325 Pa (standard pressure), unless otherwise stated.
[0024] Where numerical ranges are reported hereinafter in the format “from X to Y”, where X and Y represent the limits of the numerical range, this is synonymous with the statement “from at least X up to and including Y” unless otherwise stated. Therefore, range descriptions include the range limits X and Y unless otherwise stated.
[0025] As long as a molecule / molecule fragment has one or more stereocenters or can be differentiated into isomers due to symmetry or due to other effects such as restricted rotation, all possible isomers are included in the present invention.
[0026] The following formulas (1) to (5) describe compounds or groups that are composed of repeating units (e.g., repeating fragments, blocks, or monomeric units) and that may have a molar mass distribution. The frequency of the repeating unit is reported by a subscript. The subscripts used in the formula should be regarded as statistical averages (numerical averages). The subscripts used and the value ranges of the reported subscripts should be regarded as the averages of the possible statistical distributions of the structures and / or mixtures thereof that actually exist. The various fragments or repeating units of the compounds described in the following formulas (1) to (5) may be statistically distributed. The statistical distribution is a block configuration with any desired number of blocks and with any desired order, or it may be subject to random distribution; they may also have an alternating configuration, or form a gradient on the chain in the presence of one chain; in particular, they may also form all mixed forms, in which groups with different distributions may optionally follow each other. The following formula includes all arrangements of repeating units. Thus, in the context of the present invention, where compounds such as polybutadiene (A), epoxy-functional polybutadiene (C), hydroxy-functional polybutadiene (E), polyether-modified polybutadiene (G) or polyether-modified polybutadiene (K) containing end-capped polyether groups are described (e.g., compounds that may have multiple instances of different units), these may appear in these compounds in a disordered manner (e.g., in a statistical distribution) or in an ordered manner. The number of units or the relative frequency in such compounds should be considered as the average value (numerical mean) of all corresponding compounds. As a result of the embodiments, specific embodiments may result in restrictions on the statistical distribution. For all regions not affected by such restrictions, the statistical distribution does not change.
[0027] Therefore, the present invention first provides a method for preparing one or more polyether-modified polybutadienes, the method comprising the following steps:
[0028] a) reacting at least one polybutadiene (A) with at least one epoxidizing agent (B) to obtain at least one epoxy-functional polybutadiene (C);
[0029] b) reacting the at least one epoxy-functional polybutadiene (C) with at least one hydroxy-functional compound (D) to obtain at least one hydroxy-functional polybutadiene (E);
[0030] c) reacting the at least one hydroxy-functional polybutadiene (E) with at least one epoxy-functional compound (F) to obtain at least one polyether-modified polybutadiene (G).
[0031] Preferably, the method according to the present invention further comprises at least one of the following optional steps:
[0032] d) reacting the at least one polyether-modified polybutadiene (G) with at least one capping agent (H) to obtain at least one polyether-modified polybutadiene (K) containing capped polyether groups;
[0033] e) lightening the color of the at least one polyether-modified polybutadiene (G) or (K).
[0034] The method is preferably further characterized by
[0035] In step a), >0 to 70%, preferably 1 to 50%, further preferably 2 to 40%, even further preferably 3 to 30%, particularly preferably 4 to 20%, of the double bonds of at least one polybutadiene (A) are epoxidized with the aid of performic acid prepared in situ from formic acid and H2O2;
[0036] In step b), one or more short-chain alcohols having 1 to 6 carbon atoms, in particular isobutanol, are added to the epoxy groups of at least one epoxy-functional polybutadiene (C) under ring opening, preferably using one or more acidic catalysts, in particular trifluoromethanesulfonic acid;
[0037] In step c), one or more epoxy-functional compounds (F) selected from alkylene oxides and optionally further epoxy-functional monomers are added to the pendant OH groups of the at least one hydroxy-functional polybutadiene (E) obtained in an alkoxylation reaction, preferably additionally using a Zn / Co double metal cyanide catalyst or a basic catalyst such as an amine, guanidine, amidine, alkali metal hydroxide or alkali metal alkoxide;
[0038] In step d), at least one polyether-modified polybutadiene (G) is optionally reacted with at least one blocking agent (H) selected from carboxylic acids, carboxylic anhydrides, halogenated hydrocarbons, isocyanates and carbonates to obtain at least one polyether-modified polybutadiene (K) containing blocked polyether groups;
[0039] In step e), the at least one polyether-modified polybutadiene (G) or (K) is lightened, optionally using activated carbon and / or hydrogen peroxide.
[0040] The process according to the invention makes it possible for the first time to modify linear polybutadienes by simple direct alkoxylation of pendant OH groups with polyether groups at comb positions. The chain length and monomer sequence in the polyether groups can be varied within wide ranges. The average number of polyether groups bonded to the polybutadiene can be adjusted in a controllable manner via the degree of epoxidation and hydroxyl functionalization and opens up a large structural diversity in hydroxyl-functional polybutadienes (E).
[0041] The grafting of polyethers known from the prior art onto polybutadiene is rarely quantitative in practice, and the reaction product generally contains free proportions of polyether and possibly unfunctionalized polybutadiene. The addition of the above-mentioned OH-functional polyethers via their OH groups onto the epoxidized polybutadiene is likewise generally incomplete, and the product contains residual unconverted epoxy groups. If the polyethers are used in excess, the residual content of epoxy groups can be reduced, but excess polyethers remain in the product since they cannot be removed by distillation.
[0042] The polybutadienes obtainable according to the invention having polyether groups in the comb-shaped positions are preferably substantially free of residual epoxy groups. The process products according to the invention are preferably substantially free of free polyether components. Preferably, substantially all of the polyethers are chemically linked to the polybutadiene via ether bonds. The process products according to the invention therefore differ significantly from the compounds known to date from the prior art due to their high purity.
[0043] A preferred configuration of step a) of the method according to the invention:
[0044] In step a) of the process according to the invention, at least one polybutadiene (A) is reacted with at least one epoxidizing agent (B) to obtain at least one epoxy-functional polybutadiene (C).
[0045] In this reaction, the double bonds of polybutadiene (A) are converted into epoxy groups. Various methods for epoxidizing polybutadiene (e.g., epoxidizing with percarboxylic acids and hydrogen peroxide) are known to those skilled in the art and are disclosed, for example, in CN101538338, JP 2004346310, DD 253627, and WO 2016 / 142249 A1. Performic acid is particularly suitable for preparing epoxy-functional polybutadiene (C) with a high proportion of 1,4 units and can be formed in situ from formic acid in the presence of hydrogen peroxide. Epoxidation is preferably carried out in a solvent such as toluene or chloroform, which is removed by distillation after the reaction and after washing off any peroxide residues.
[0046] Polybutadiene (A) is a polymer of 1,3-butadiene (buta-1,3-diene). The polymerization of 1,3-butadiene monomers is essentially achieved with 1,4 and / or 1,2 bonds. 1,4 bonds lead to so-called 1,4-trans units and / or 1,4-cis units, which are also collectively referred to as 1,4 units. 1,2 bonds lead to so-called 1,2 units. 1,2 units carry vinyl groups and are also referred to as vinyl 1,2 units. In the context of the present invention, 1,2 units are also referred to as "(X)", 1,4-trans units are referred to as "(Y)", and 1,4-cis units are referred to as "(Z)":
[0047]
[0048] The double bonds present in the unit are similarly referred to as 1,4-trans double bonds, 1,4-cis double bonds or 1,2 double bonds or 1,2 vinyl double bonds. 1,4-trans double bonds and 1,4-cis double bonds are also collectively referred to as 1,4 double bonds.
[0049] Polybutadiene (A) is therefore an unmodified polybutadiene. Polybutadiene (A) and methods for its preparation are known to those skilled in the art. It is preferably prepared by free radical, anionic or coordinated chain polymerization.
[0050] The free-radical chain polymerization is preferably carried out in the form of an emulsion polymerization. This leads to the statistical presence of the three units mentioned. At low reaction temperatures (about 5° C.), the proportion of vinyl groups decreases. Initiation is preferably carried out with potassium peroxodisulfate and iron salts or with hydrogen peroxide.
[0051] In the anionic chain polymerization, butyllithium is preferably used to initiate the chain polymerization. The polybutadiene (A) thus obtained contains about 40% of 1,4-cis units and 50% of 1,4-trans units.
[0052] In the case of coordination chain polymerization, preference is given to using Ziegler-Natta catalysts, in particular stereospecific Ziegler-Natta catalysts, which lead to polybutadienes (A) having a high proportion of 1,4-cis units.
[0053] The polymerization of 1,3-butadiene and also side reactions or other reactions, such as further reactions of the double bonds of the resulting 1,2 and 1,4 units of the polybutadiene, may also give rise to branched polybutadiene (A). However, the polybutadiene (A) used according to the invention is preferably linear, i.e. unbranched polybutadiene. The polybutadiene may also comprise small proportions of units other than 1,2 units, 1,4-trans units or 1,4-cis units. However, preferably, the mass proportion of the sum of 1,2 units, 1,4-trans units and 1,4-cis units, based on the total mass of the at least one polybutadiene (A), i.e. based on the total mass of all polybutadiene (A) used, is at least 80%, preferably at least 90%, in particular at least 99%.
[0054] For the process according to the invention, preference is given to using those polybutadienes (A) which have, based on the sum of 1,2 units and 1,4 units, 0 to 80% of 1,2 units and 20 to 100% of 1,4 units, preferably 0 to 30% of 1,2 units and 70 to 100% of 1,4 units, particularly preferably 0 to 10% of 1,2 units and 90 to 100% of 1,4 units, most preferably 0 to 5% of 1,2 units and 95 to 100% of 1,4 units.
[0055] Therefore, preferably, 0% to 80% of the double bonds of all polybutadiene (A) used are 1,2 vinyl double bonds and 20% to 100% are 1,4 double bonds, preferably 0% to 30% are 1,2 vinyl double bonds and 70% to 100% are 1,4 double bonds, particularly preferably 0% to 10% are 1,2 vinyl double bonds and 90% to 100% are 1,4 double bonds, most preferably 0% to 5% are 1,2 vinyl double bonds and 95% to 100% are 1,4 double bonds.
[0056] Therefore, for the inventive preparation of the product, preference is given to using polybutadiene (A) of formula (1)
[0057]
[0058] It has 0% to 80% 1,2 vinyl double bonds (subscript x) and 20% to 100% 1,4 double bonds (sum of subscripts y and z), preferably 0% to 30% 1,2 vinyl double bonds and 70% to 100% 1,4 double bonds, particularly preferably 0% to 10% 1,2 vinyl double bonds and 90% to 100% 1,4 double bonds, most preferably 0% to 5% 1,2 vinyl double bonds and 95% to 100% 1,4 double bonds. The ratio of 1,4-trans double bonds (subscript y) to 1,4-cis double bonds (subscript z) can be freely varied.
[0059] The subscripts x, y and z give the number of the corresponding butadiene units in the polybutadiene (A). The subscripts are numerical averages (number averages) over all polybutadiene polymers of the at least one polybutadiene (A).
[0060] The average molar mass and the polydispersity of the polybutadienes (A) of the formula (1) used can vary freely.
[0061] Preferably, the number average molar mass M of the at least one polybutadiene (A) is n It is 200 g / mol to 20000 g / mol, preferably 500 g / mol to 10000 g / mol, more preferably 700 g / mol to 5000 g / mol.
[0062] Alternatively, preferably, the number average molar mass M of at least one polybutadiene (A) is n It is 2100 g / mol to 20000 g / mol, more preferably 2200 g / mol to 10000 g / mol, most preferably 2300 g / mol to 5000 g / mol.
[0063] In the context of the present invention, the number-average molar mass M is preferably determined by gel permeation chromatography (EPC) as described in the examples. n , weight average molar mass M w and polydispersity (M w / M n ).
[0064] It is further preferred that the at least one polybutadiene (A) has a numerical average of 5 to 360, preferably 10 to 180, most preferably 15 to 90 units selected from 1,2 units, 1,4-cis units and 1,4-trans units.
[0065] Alternatively, preferably, at least one polybutadiene (A) has a numerical average of 35 to 360, preferably 40 to 180, most preferably 45 to 90 units selected from 1,2 units, 1,4-cis units and 1,4-trans units.
[0066] With further preference, the polybutadiene (A) used has a viscosity of 50 to 50,000 mPas, preferably 100 to 10 000 mPas, in particular 500 to 5000 mPas (determined in accordance with DIN EN ISO 3219:1994-10).
[0067] The polybutadiene used with particular preference is the commercially available BUTYROBUTENE from Evonik Industries AG / Evonik Operations GmbH. 110 and 130 products with the following typical indices:
[0068] 110: about 1% 1,2 vinyl double bonds, about 24% 1,4-trans double bonds, about 75% 1,4-cis double bonds, number average molar mass M n About 2600 g / mol, viscosity (20°C) 700-860 mPas (according to DIN EN ISO 3219:1994-10),
[0069] 130: about 1% 1,2 vinyl double bond, about 22% 1,4-trans double bond, about 77% 1,4-cis double bond, number average molar mass M n Approximately 4600 g / mol, viscosity (20° C.) 2700-3300 mPas (according to DIN EN ISO 3219:1994-10).
[0070] Polybutadienes which are particularly preferably used are also the products Lithene ultra AL and Lithene ActiV 50 available from Synthomer PLC, which have the following typical characteristic data:
[0071] Lithene ultra AL: about 40% 1,2-vinyl double bonds, about 60% 1,4 double bonds,
[0072] Lithene ActiV 50: about 70% 1,2 vinyl double bonds, about 30% 1,4 double bonds.
[0073] The degree of epoxidation is determined quantitatively, for example, with the aid of 13 C NMR spectroscopy or epoxy number titration (determination of the epoxy equivalent in accordance with DIN EN ISO 3001:1999) and can be adjusted in a controlled and reproducible manner via the process conditions, in particular via the relationship between the amount of hydrogen peroxide used and the amount of double bonds in the initial charge of polybutadiene.
[0074] Preferably, in step a) of the process according to the invention, >0% to 70%, preferably 1% to 50%, further preferably 2% to 40%, even further preferably 3% to 30%, particularly preferably 4% to 20% of all double bonds of the at least one polybutadiene (A) are epoxidized.
[0075] In principle, epoxidizing agents (B) which can be used are all epoxidizing agents known to the person skilled in the art. Preferably, the epoxidizing agent (B) is selected from peroxycarboxylic acids (percarboxylic acids, peracids), preferably from meta-chloroperbenzoic acid, peracetic acid (peracetic acid) and peroxyformic acid (performic acid), in particular peroxyformic acid (performic acid). The peroxycarboxylic acid is preferably formed in situ from the corresponding carboxylic acid and hydrogen peroxide.
[0076] With particular preference, the at least one epoxidation agent (B) comprises performic acid which is preferably formed in situ from formic acid and hydrogen peroxide.
[0077] The epoxidation of the at least one polybutadiene (A) occurs preferentially at the 1,4 double bonds in a statistical distribution on the polybutadiene chain. The epoxidation of the 1,2 double bonds can also occur and likewise occurs in a statistical distribution at these bonds on the polybutadiene chain. However, the epoxidation of the 1,2 double bonds is less favored than the epoxidation of the 1,4 double bonds. The reaction product therefore contains epoxy-functional polybutadiene polymers whose degrees of epoxidation differ from one another. Therefore, all stated degrees of epoxidation should be regarded as average values.
[0078] It is further preferred that during the process according to the invention, stabilizers or antioxidants are used to stabilize the reactants, intermediates and products in order to avoid undesired polymerization of double bonds. Suitable for this purpose are, for example, sterically hindered phenols known to the person skilled in the art, which can be used, for example 20. 1010(BASF), 1076 (BASF) and 1135 (BASF) is commercially available. It is further preferred to carry out the entire preparation process under an inert atmosphere, for example under nitrogen. The unmodified reactants (i.e. at least one polybutadiene (A)) and the polyether-modified end products according to the invention (i.e. at least one polyether-modified polybutadiene (G) or (K)) should also preferably be stored in a manner that excludes air as much as possible.
[0079] A preferred configuration of step b) of the method according to the invention:
[0080] In step b) of the process according to the invention, the at least one epoxy-functional polybutadiene (C) is reacted with at least one hydroxy-functional compound (D) to obtain at least one hydroxy-functional polybutadiene (E).
[0081] In this reaction, the addition of at least one hydroxy-functional compound (D) to at least one epoxy-functional polybutadiene (C) takes place (addition reaction). Thus, the reaction takes place so that one or more covalent bonds are formed between at least one hydroxy-functional compound (D) and at least one epoxy-functional polybutadiene (C). The reaction preferably comprises (at least in an idealized form) a reaction step in which at least one hydroxyl group of at least one hydroxy-functional compound (D) carries out a nucleophilic attack on at least one epoxy group of at least one epoxy-functional polybutadiene (C) with the ring opening of at least one epoxy group.
[0082] In principle, in the context of the method according to the invention, all compounds having at least one hydroxyl group can be added to the epoxy group of polybutadiene. Hydroxy-functional compounds (D) can be selected from, for example, alcohols, carboxylic acids and water. Preferably, at least one hydroxy-functional compound (D) is selected from monofunctional alcohols having 1 to 6 carbon atoms, further preferably selected from monofunctional alcohols having 2 to 4 carbon atoms, more preferably selected from ethanol, 1-propanol, isopropanol, 1-butanol, 2-butanol and isobutanol. Any desired mixture of these alcohols can also be used here. However, it is particularly preferred that the hydroxy-functional compound (D) used is not methanol. Another suitable hydroxy-functional compound (D) is water. Water can be used alone or in combination with one or more other hydroxy-functional compounds (D). For example, a mixture of alcohol and water or a mixture of carboxylic acid and water can be used in step b). Therefore, it is not necessary to dry at least one hydroxy-functional compound (D), such as an alcohol or a carboxylic acid, and make it free of water.
[0083] The molar ratio of OH groups of the hydroxyl-functional compound (D) to the epoxy groups of the epoxy-functional polybutadiene (C) can vary within wide ranges. However, based on the stoichiometric ratio of hydroxyl groups to epoxy groups of the epoxy-functional polybutadiene (C), the hydroxyl-functional compound (D) is preferably used in a stoichiometric excess in order to achieve a quantitative conversion of all epoxy groups. Preferably, therefore, in step b), the total number of hydroxyl groups in all hydroxyl-functional compounds (D): the total number of epoxy groups in all epoxy-functional polybutadiene (C) is >1:1 to 50:1, further preferably 2:1 to 35:1, even further preferably 3:1 to 30:1, particularly preferably 3:1 to 25:1. Excess compound (D) can be removed after the reaction (for example by distillation) and, if desired, can be reused.
[0084] In a preferred embodiment, the reaction is carried out in the presence of at least one acidic catalyst. The catalyst is optionally uniformly dissolved in the reaction mixture or unevenly distributed therein in solid form, such as a sulfonic acid ion exchanger. In the context of the present invention, preferred catalysts are such as sulfuric acid, sulfonic acid and trifluoroacetic acid, more preferably trifluoromethanesulfonic acid. Therefore preferably, in step b), an acid, more preferably sulfuric acid, sulfonic acid and / or trifluoroacetic acid, particularly preferably trifluoromethanesulfonic acid, is used as the catalyst.
[0085] The type and amount of acid used are selected so as to achieve very rapid and quantitative addition of the at least one hydroxy-functional compound (D) onto the epoxy groups of the at least one epoxy-functional polybutadiene (C). Preference is given to using trifluoromethanesulfonic acid in a concentration of 1 ppmw to 1000 ppmw (ppmw = ppm by mass), more preferably in a concentration of 50 ppmw to 300 ppmw, based on the reaction mixture.
[0086] The reaction of at least one epoxy-functional polybutadiene (C) with at least one hydroxy-functional compound (D) in the presence of an acidic catalyst is preferably carried out in a temperature range of 20° C. to 120° C. and is limited at the upper end by the boiling point of the hydroxy-functional compound (D) or, when a plurality of hydroxy-functional compounds (D) are used, by the boiling point of the most volatile hydroxy-functional compound (D). The reaction is preferably carried out at 50° C. to 90° C. The components are stirred for several hours until the epoxide groups are converted as completely as possible. The analysis of the epoxide groups can be carried out by NMR spectroscopy or by known epoxy value titration methods (as described in the examples). Preferably, the reaction conditions in step b) are selected so that more than 97% of the epoxide groups produced in step a) are converted under ring opening. Particularly preferably, epoxide groups are no longer detected in the product from step b), i.e. in the at least one hydroxy-functional polybutadiene (E).
[0087] After the reaction, the acidic reaction mixture is neutralized. For this purpose, in principle any alkaline neutralizing agent can be added. Preferably, sodium bicarbonate in solid form or in aqueous solution is used for neutralization. Any excess hydroxy-functional compound (D) and any water are preferably removed by distillation, and the precipitated salt is filtered off if necessary. Preferably, aqueous sodium bicarbonate solution is used here, because a light-colored product is obtained thereby.
[0088] Each epoxy group in the epoxy-functional polybutadiene (C) generates a repeating unit of the formula (2a), (2b) or (2c) after ring opening by the hydroxy-functional compound (D) of the formula A-OH:
[0089]
[0090] A is preferably a monovalent organic radical which may also carry additional hydroxyl groups, or a hydrogen radical. For example, if a monofunctional fatty alcohol having 1 to 6 carbon atoms is used as the hydroxy-functional compound (D), then A is an alkyl radical having 1 to 6 carbon atoms. In the case of water as the hydroxy-functional compound (D), A is a hydrogen radical, i.e. A═H. If, for example, a carboxylic acid is used as the hydroxy-functional compound (D), then A is an acyl radical. Thus, each converted epoxy group produces at least one pendant OH group. If, as in the case of water, A═H, then each converted epoxy group produces exactly two pendant OH groups. In all other cases, i.e. A≠H, each converted epoxy group produces exactly one pendant OH group.
[0091] In the case of polybutadienes (A) having a predominant proportion of 1,4 units, which are preferred according to the invention, those of the formula (2a) predominate among the repeating units of the formulae (2a), (2b) and (2c).
[0092] Preferably, the at least one hydroxy-functional polybutadiene (E) has 20% to 100%, preferably 70% to 100%, further preferably 90% to 100%, particularly preferably 95% to 100%, of repeating units of the formula (2a), based on the sum of repeating units of the formulae (2a), (2b) and (2c).
[0093] It is further preferred that the proportion of repeating units of the formulae (2a), (2b) and (2c) together, based on the total number of all repeating units of the at least one hydroxy-functional polybutadiene (E), is >0% to 70%, preferably 1% to 50%, further preferably 2% to 40%, even further preferably 3% to 30%, particularly preferably 4% to 20%. It is correspondingly preferred that the degree of hydroxylation is >0% to 70%, preferably 1% to 50%, further preferably 2% to 40%, even further preferably 3% to 30%, particularly preferably 4% to 20%. After the conversion in step b), the degree of hydroxylation of the hydroxy-functional polybutadiene (E) corresponds to the degree of epoxidation of the corresponding epoxy-functional polybutadiene (C).
[0094] A preferred configuration of step c) of the method according to the invention:
[0095] In step c) of the process according to the invention, the at least one hydroxy-functional polybutadiene (E) is reacted with at least one epoxy-functional compound (F) to obtain at least one polyether-modified polybutadiene (G).
[0096] The at least one hydroxy-functional polybutadiene (E) from step b) is used in step c) as a starting compound for reaction with at least one epoxy-functional compound (F). At least one epoxy-functional compound (F) (hereinafter also referred to as "monomer" or "epoxy monomer" or "epoxide") is added to the OH groups of at least one hydroxy-functional polybutadiene (E) in a polyaddition reaction under ring opening and preferably in the presence of a suitable catalyst. This leads to the formation of a polybutadiene according to the invention having polyether chains in comb-like (pendant) positions, i.e. to at least one polyether-modified polybutadiene (G). The polyether-modified polybutadiene (G) is preferably a linear polybutadiene with pendant (side) modification with polyether groups. Therefore, preferably, the polyether-modified polybutadiene (G) has a linear polybutadiene backbone and pendant polyether groups.
[0097] The reaction in step c) is preferably an alkoxylation reaction, ie the polyaddition of alkylene oxides onto at least one hydroxy-functional polybutadiene (E). However, the reaction in step c) can also be carried out using glycidyl compounds instead of or in addition to the alkylene oxides.
[0098] Thus, preferably, the at least one epoxy-functional compound used in step c) is selected from alkylene oxides, preferably from alkylene oxides having 2 to 18 carbon atoms, further preferably from alkylene oxides having 2 to 8 carbon atoms, particularly preferably from ethylene oxide, propylene oxide, 1-butylene oxide, cis-2-butylene oxide, trans-2-butylene oxide, 1,1-dimethylethylene oxide (isobutylene oxide) and styrene oxide; and / or the at least one epoxy-functional compound used in step c) is selected from glycidyl compounds, preferably from monofunctional glycidyl compounds, more preferably from phenyl glycidyl ether, o-cresyl glycidyl ether, tert-butylphenyl glycidyl ether, allyl glycidyl ether, butyl glycidyl ether, 2-ethylhexyl glycidyl ether, C 12 / C 14 Fatty alcohol glycidyl ether and C 13 / C 15 Fatty alcohol glycidyl ether.
[0099] The monomers can be added individually in pure form, alternatingly and continuously in any metering sequence, or simultaneously in mixed form. The sequence of the monomer units in the resulting polyether chain is thus in block distribution or random distribution or gradient distribution in the final product.
[0100] By means of the process according to the invention, pendant polyether chains are built up on polybutadiene which can be prepared in a controlled and reproducible manner with regard to structure and molar mass.
[0101] The sequence of the monomer units can be varied via the order of addition within wide ranges.
[0102] The molar mass of the pendant polyether groups can be varied within wide ranges by the process according to the invention and can be specifically and reproducibly controlled via the molar ratio of added monomers to OH groups of the at least one initial charge of hydroxy-functional polybutadiene (E) from step b).
[0103] The polyether-modified polybutadienes (G) prepared according to the invention are preferably characterized in that they contain B groups bonded to the polybutadiene backbone via ether groups according to formulae (3a), (3b) and (3c)
[0104]
[0105] As described above for step b), the A group in formulae (3a), (3b) and (3c) is derived from the compound A-OH, i.e. the hydroxy-functional compound (D) used in step b). As also described above, two cases should be distinguished in step b), i.e. A≠H or A=H. In the first case, i.e. when A≠H, the A group in formulae (3a), (3b) and (3c) is identical to the A group in formulae (2a), (2b) and (2c). In the second case, i.e. when A=H, the A group in formulae (3a), (3b) and (3c) is in each case independently H or a B group. For example, if a monofunctional fatty alcohol having 1 to 6 carbon atoms is used as the hydroxy-functional compound (D), A is an alkyl group having 1 to 6 carbon atoms. For example, if a carboxylic acid is used as the hydroxy-functional compound (D), A is an acyl group. However, if water is used as hydroxy-functional compound (D), then in the case of reaction with one or more epoxy-functional compounds (F), A in formulae (3a), (3b) and (3c) is a B group; in the case of no reaction, A remains hydrogen. Thus, each pendant hydroxyl group converted produces exactly one pendant -OB group. The B group is in turn formed from one or more monomers, preferably from a plurality of monomers, of the at least one epoxy-functional compound (F) used.
[0106] In the context of the present invention, it is possible in principle to use all alkoxylation catalysts known to the person skilled in the art, for example basic catalysts such as alkali metal hydroxides, alkali metal alkoxides, amines, guanidines, amidines, phosphorus compounds such as triphenylphosphine, and further acidic and Lewis-acidic catalysts such as SnCl4, SnCl2, SnF2, BF3 and BF3 complexes, and double metal cyanide (DMC) catalysts.
[0107] Before the epoxide is fed, i.e. before the addition of at least one epoxy-functional compound (F) used, the reactor partially filled with the starter and the catalyst is rendered inert, for example with nitrogen. This is achieved, for example, by repeated alternating evacuation and nitrogen supply. It is advantageous to evacuate the reactor to less than 200 mbar after the last nitrogen injection. It is therefore preferred to add the first amount of epoxy monomer to the evacuated reactor. The monomer is metered in while stirring and optionally cooling to remove the released reaction heat and to maintain the preselected reaction temperature. The starter used is at least one hydroxy-functional polybutadiene (E), or a polyether-modified polybutadiene (G) that has been prepared by the process of the invention can be used as a starter, as further described below.
[0108] DMC Catalysis
[0109] Preference is given to using zinc / cobalt DMC catalysts, especially those containing zinc hexacyanocobaltate(III). Preference is given to using the DMC catalysts described in US Pat. No. 5,158,922, US 20030119663, WO 01 / 80994. The catalysts may be amorphous or crystalline.
[0110] Preferably, the catalyst concentration is preferably from >0 ppmw to 1000 ppmw, preferably from >0 ppmw to 700 ppmw, more preferably from 10 ppmw to 500 ppmw, based on the total mass of the product formed.
[0111] The catalyst is preferably metered into the reactor only once. The catalyst should preferably be clean, dry and free of basic impurities that could inhibit the DMC catalyst. The amount of catalyst should preferably be set to provide sufficient catalytic activity for the process. The catalyst can be metered in solid form or in the form of a catalyst suspension. If a suspension is used, OH-functional starters are particularly suitable as suspension media.
[0112] To start the DMC-catalyzed reaction, it may be advantageous to first activate the catalyst with a portion of at least one epoxy-functional compound (F), preferably selected from alkylene oxides, especially propylene oxide, and / or ethylene oxide. After the alkoxylation reaction has started, the continuous addition of monomers can be started.
[0113] In the case of the DMC-catalyzed reaction in step c), the reaction temperature is preferably 60 to 200°C, more preferably 90 to 160°C, and more preferably 100 to 140°C.
[0114] In the case of a DMC-catalyzed reaction in step c), the internal reactor pressure is preferably from 0.02 bar to 100 bar, further preferably from 0.05 bar to 20 bar, more preferably from 0.1 bar to 10 bar (absolute).
[0115] More preferably, the DMC catalytic reaction in step c) is carried out at a temperature of 100° C. to 140° C. and a pressure of 0.1 bar to 10 bar.
[0116] The reaction can be carried out in a suitable solvent, for example, for the purpose of reducing viscosity. After the epoxide addition is completed, it is preferably followed by a further reaction for a period of time to complete the conversion. Further reaction can be carried out, for example, by a continuous reaction under the reaction conditions (i.e., maintaining, for example, temperature) without adding reactants. The DMC catalyst is usually retained in the reaction mixture.
[0117] After the conversion is complete, unreacted epoxide and any other volatile components can be removed by vacuum distillation, steam or gas stripping or other deodorization methods. The final product is filtered at <100°C to remove any turbid material.
[0118] Base Catalysis
[0119] In addition to the DMC catalyst, it is also possible according to the invention to use a basic catalyst in step c). Particularly suitable are alkali metal alkoxides, such as sodium methoxide and potassium methoxide, which are added in solid form or in the form of their methanolic solutions. Furthermore, it is possible to use all alkali metal hydroxides, in particular sodium hydroxide and potassium hydroxide, for example in solid form or in the form of aqueous or alcoholic solutions. Furthermore, it is also possible according to the invention to use basic nitrogen compounds, preferably amines, guanidines and amidines, more preferably tertiary amines such as trimethylamine and triethylamine.
[0120] Preference is given to using basic catalysts in a concentration of >0 to 100 mol %, preferably >0 to 50 mol %, more preferably 3 to 40 mol %, based on the amount of OH groups in the starter.
[0121] The reaction temperature in the case of the base-catalyzed reaction in step c) is preferably 80 to 200°C, further preferably 90 to 160°C, more preferably 100 to 160°C.
[0122] The internal reactor pressure in the case of the base-catalyzed reaction in step c) is preferably from 0.2 bar to 100 bar, further preferably from 0.5 bar to 20 bar, more preferably from 1 bar to 10 bar (absolute).
[0123] More preferably, the base-catalyzed reaction in step c) is carried out at a temperature of 100 to 160°C and a pressure of 1 to 10 bar.
[0124] The reaction may optionally be carried out in a suitable solvent. After the epoxide addition is complete, it is preferably followed by a further reaction for a period of time to complete the conversion. The further reaction may be carried out, for example, by a continuous reaction under reaction conditions without the addition of reactants. After the conversion is complete, unreacted epoxide and any other volatile components may be removed by vacuum distillation, steam or gas stripping or other deodorization methods. Volatile catalysts such as amines are removed here.
[0125] To neutralize the alkaline crude product, an acid such as phosphoric acid or sulfuric acid or a carboxylic acid such as acetic acid and lactic acid is added. Preference is given to using aqueous phosphoric acid and lactic acid. The amount of the respective acid used is determined by the amount of alkaline catalyst used beforehand. The alkaline polybutadiene with pendant polyether groups is stirred in the presence of an acid, preferably at 40° C. to 95° C., and then distilled to dryness in a vacuum distillation at <100 mbar and 80° C. to 130° C. The neutralized product is finally filtered, preferably at <100° C., to remove precipitated salts.
[0126] Preferably, the end product according to the invention has a water content of <0.2% (reported as mass fraction based on the total mass of the end product) and an acid number of <0.5 mg KOH / g and is virtually free of phosphates.
[0127] Products as starting materials
[0128] It is not always possible to achieve the desired molar mass of the end product in a single reaction step, especially in the alkoxylation step. In particular, when long polyether side chains are the target and / or the starter from step b) has a high OH functionality, large amounts of epoxy monomers need to be added. The reactor geometry sometimes does not allow this. The polyether-modified polybutadiene (G) prepared according to the invention by step c) carries OH groups at the end of each of its pendant polyether groups and is therefore suitable as a starter for the construction of higher molecular weight conversion products. In the context of the present invention, they are precursors and starting compounds for the synthesis of polybutadienes with longer polyether groups. Therefore, at least one epoxy-functional compound (F) can be converted in step c) in a plurality of constituent steps.
[0129] According to the invention, the alkoxylation level of the product prepared in step c) by means of DMC catalysis can be increased by fresh addition of epoxy monomers by DMC catalysis or by using one of the above-mentioned basic catalysts or acidic catalysts. Optionally, further DMC catalysts can be added, for example, to increase the reaction rate in the chain extension.
[0130] The products prepared under base catalysis from step c) can be alkoxylated to higher molar masses under alkaline or acidic conditions or by DMC catalysis. In step c), neutralization is advantageously omitted if the aim is to react the basic precursors with the monomers further under base catalysis. Additional basic catalysts can optionally be added, for example, in order to increase the reaction rate in the chain extension.
[0131] Optional step d)
[0132] In an optional further step d), the at least one polyether-modified polybutadiene (G) is reacted with at least one capping agent (H) to obtain at least one polyether-modified polybutadiene (K) containing capped polyether groups.
[0133] This further converts the B groups of the polyether-modified polybutadiene (G) having hydroxyl groups at the terminal positions to produce ester, ether, carbamate and / or carbonate groups at the terminal positions. The end-capping of polyethers is known to those skilled in the art, for example esterification with carboxylic acids and carboxylic anhydrides, especially acetylation with acetic anhydride; etherification with halogenated hydrocarbons, especially methylation with methyl chloride by the Williamson ether synthesis principle; carbamateization by reaction of OH groups with isocyanates, especially with monoisocyanates such as octadecyl isocyanate; and carbonation by reaction with dimethyl carbonate and diethyl carbonate.
[0134] Optional step e)
[0135] In an optional step e), the at least one polyether-modified polybutadiene (G) or (K) is lightened in color.
[0136] If the optional step e) follows the optional step d), the color of the at least one polyether-modified polybutadiene (K) containing end-capped polyether groups is lightened. If, on the other hand, the optional step d) is omitted, the optional step e) follows step c) of the process according to the invention and the color of the at least one polyether-modified polybutadiene (G) is lightened. For example, the color lightening can be achieved by adding activated carbon, preferably activated carbon in a suitable solvent, or by treatment with hydrogen peroxide. The color lightening can preferably be achieved via the Gardner color number (determined in accordance with DIN EN ISO 4630). Preferably, the Gardner color number of the polyether-modified polybutadiene (G) or (K) is reduced by at least 1, preferably by at least 2, as a result of the color lightening. Particular preference is given to polyether-modified polybutadienes (G) or (K) having a Gardner color number of not more than 3, in particular not more than 2.5.
[0137] Reactor
[0138] The reactor used for the method according to the invention can in principle be any suitable reactor type that allows controlled reaction and any heat release therein. The reaction scheme can be continuous, semi-continuous or batchwise in a manner known from chemical engineering, and can be flexibly matched with available production equipment. Except conventional stirred tank reactor, a jet loop reactor with gas phase and internal heat exchanger tubes as described in WO 01 / 062826 can also be used. In addition, no gas phase loop reactor can be used.
[0139] Polyether modified polybutadiene
[0140] The invention further provides polybutadienes modified with polyether groups in the comb-like (pendant) positions, as can be prepared by the process according to the invention.
[0141] The present invention therefore further provides polyether-modified polybutadienes (G) or (K) obtainable by the process according to the invention.
[0142] The polyether-modified polybutadiene (G) or (K) is preferably a linear polybutadiene having a pendant (side) modification with a polyether group. Therefore, it is preferred that the polyether-modified polybutadiene (G) or (K) has a linear polybutadiene backbone and pendant polyether groups.
[0143] The present invention likewise further provides a polyether-modified polybutadiene (G) or (K) which is preferably obtainable by the process according to the invention, characterised in that the polyether-modified polybutadiene (G) or (K) comprises repeating units selected from the following divalent groups:
[0144]
[0145] in
[0146] A is independently at each occurrence a monovalent organic radical or a hydrogen radical,
[0147] is preferably independently selected at each occurrence from monovalent hydrocarbon radicals having 1 to 6 carbon atoms,
[0148] More preferably, each occurrence is independently selected from alkyl groups having 1 to 4 carbon atoms;
[0149] B is independently selected at each occurrence from a group of formula (4a)
[0150]
[0151] Preferably, each occurrence is independently selected from the group consisting of
[0152]
[0153] More preferably, each occurrence is independently selected from the group consisting of
[0154]
[0155] R 1 is independently selected at each occurrence from monovalent hydrocarbon groups having 1 to 16 carbon atoms,
[0156] is preferably independently in each case an alkyl radical having 1 to 16 carbon atoms or a phenyl radical,
[0157] More preferably independently at each occurrence is methyl, ethyl or phenyl;
[0158] R 2 The formula is -CH2-OR 3 Groups;
[0159] R 3 is independently selected at each occurrence from a monovalent hydrocarbon radical having 3 to 18 carbon atoms;
[0160] Preferably, independently in each case, allyl, butyl, an alkyl group having 8 to 15 carbon atoms, or a phenyl group which may be substituted by a monovalent radical selected from a hydrocarbon group having 1 to 4 carbon atoms;
[0161] More preferably tert-butylphenyl or o-tolyl;
[0162] R 4 is independently in each case a monovalent organic radical having 1 to 18 carbon atoms or hydrogen, preferably hydrogen;
[0163] and
[0164] m, n, o, p and q are each independently 0 to 300, preferably 0 to 200, more preferably 0 to 100, provided that the sum of m, n, o, p and q is greater than 1, preferably greater than 5, more preferably greater than 10;
[0165] Every permutation of repeating units (U), (V), (W), (X), (Y) and (Z) as well as every permutation of repeating units in a B group is included.
[0166] R 1 , R 2 , R 3 and R 4 The radicals may each independently be linear or branched, saturated or unsaturated, aliphatic or aromatic, and substituted or unsubstituted.
[0167] Common symbols (In formula (4a), R = R 1 or R 2 , or in formula (4b) and (4c), R=CH3) Unit or formula , but the preferred expression is unit.
[0168] Common symbols in formula (4a) Expression Unit or formula but preferably represents unit.
[0169] More preferably, R 4 The radicals are independently selected in each case from monovalent hydrocarbon radicals having 1 to 18 carbon atoms, acyl radicals -C(=O)R 5 , carbamate group -C(=O)NH-R6 , carbonate group -C(=O)OR 7 and hydrogen; R 4 Further preferably, each occurrence is independently selected from alkyl having 1 to 18 carbon atoms, alkylene having 1 to 18 carbon atoms, acyl-C(═O)R 5 , carbamate group C(=O)NH-R 6 , carbonate group -C(=O)OR 7 and hydrogen; more preferably, R 4 It's hydrogen.
[0170] R 5 In each case it is independently an alkyl or alkenyl group having 1 to 18 carbon atoms, preferably having 1 to 10 carbon atoms, more preferably methyl.
[0171] R 6 In each case independently it is an alkyl or aryl group having 1 to 18 carbon atoms, preferably having 6 to 18 carbon atoms.
[0172] R 7 Independently in each case is an alkyl radical having 1 to 18 carbon atoms, preferably having 1 or 2 carbon atoms.
[0173] It is preferred here that the sum of all repeating units (U), (V) and (W) in the at least one polyether-modified polybutadiene (G) or (K) divided by the sum of all repeating units (U), (V), (W), (X), (Y) and (Z) is >0% to 70%, preferably 1% to 50%, further preferably 2% to 40%, even further preferably 3% to 30%, particularly preferably 4% to 20%.
[0174] This means that >0 to 70%, preferably 1 to 50%, further preferably 2 to 40%, even further preferably 3 to 30%, particularly preferably 4 to 20%, of the repeating units (U), (V), (W), (X), (Y) and (Z) are polyether-modified.
[0175] Preferably, the polyether-modified polybutadiene (G) or (K) is a polybutadiene of formula (5) modified with pendant polyether groups,
[0176]
[0177] The proportion of the polyether-modified repeating units represented by formula (5) is >0% to 70%, preferably 1% to 50%, further preferably 2% to 40%, even further preferably 3% to 30%, and particularly preferably 4% to 20%, based on the sum of all repeating units represented by formula (5), wherein the proportion is calculated as [(d+e+f) / (a+b+c+d+e+f)]*100%.
[0178] Repeating units with subscripts a, b, c, d, e and f are distributed over the polybutadiene chain in an arbitrary statistical manner. Therefore, all subscripts reported should be considered as average values.
[0179] The number average molar mass M of the polybutadiene component of the polyether-modified polybutadiene (G) or (K) n , weight average molar mass M w The polybutadiene component is understood to mean the component of the polyether-modified polybutadiene (G) or (K) from the polybutadiene (A) used in the process. In formula (5), the polybutadiene component of the polyether-modified polybutadiene (G) or (K) is understood to mean the component of the polymer obtained by subtracting the AO and BO groups from the polyether-modified polybutadiene (G) or (K).
[0180] Preferably, the number average molar mass M of the polybutadiene component of the polyether-modified polybutadiene (G) or (K) is n It is 200 g / mol to 20000 g / mol, preferably 500 g / mol to 10000 g / mol, more preferably 700 g / mol to 5000 g / mol.
[0181] Alternatively, preferably, the number average molar mass M of the polybutadiene component of the polyether-modified polybutadiene (G) or (K) is n It is 2100 g / mol to 20000 g / mol, preferably 2200 g / mol to 10000 g / mol, more preferably 2300 g / mol to 5000 g / mol.
[0182] The number average molar mass M of the polybutadiene component n Here it is defined as the number average molar mass M of the base polybutadiene (A) n .
[0183] Further preferably, the polyether-modified polybutadiene (G) or (K) has a numerical average number of repeating units of 5 to 360, more preferably 10 to 180, most preferably 15 to 90, wherein the repeating units are selected from (U), (V), (W), (X), (Y) and (Z).
[0184] Alternatively, preferably, the polyether-modified polybutadiene (G) or (K) has a numerical average number of repeating units of 35 to 360, more preferably 40 to 180, most preferably 45 to 90, wherein the repeating units are selected from (U), (V), (W), (X), (Y) and (Z).
[0185] Further preferably, the polyether-modified polybutadiene (G) or (K) is characterized in that 0 to 80%, preferably 0 to 30%, particularly preferably 0 to 10%, most preferably 0 to 5%, of the double bonds present are 1,2 vinyl double bonds and 20 to 100%, preferably 70 to 100%, particularly preferably 90 to 100%, most preferably 95 to 100% of the double bonds present are 1,4 double bonds.
[0186] Therefore, compounds of the formula (5) are preferred in the context of the present invention, based on the total number of repeat units containing double bonds (sum of a+b+c), having 0% to 80% of 1,2 vinyl double bonds (subscript a) and 20% to 100% of 1,4 double bonds (sum of subscripts b and c), preferably having 0% to 30% of 1,2 vinyl double bonds and 70% to 100% of 1,4 double bonds, particularly preferably having 0% to 10% of 1,2 vinyl double bonds and 90% to 100% of 1,4 double bonds, most preferably 0% to 5% of 1,2 vinyl double bonds and 95% to 100% of 1,4 double bonds. The ratio of 1,4-trans double bonds (subscript b) to 1,4-cis double bonds (subscript c) can be freely varied.
[0187] Particular preference is given to compounds of the formula (5) which have >95% of repeating units with the subscript d, based on the sum of repeating units d+e+f. The ratio of repeating units e and f to one another can vary freely.
[0188] Very particular preference is given to the polybutadienes from Evonik Industries AG / Evonik Operations GmbH and Lithene ultra AL described above. 110 and 130 and those polyether-modified polybutadienes (G) or (K) such as Lithene ActiV 50 from Synthomer PLC.
[0189] The molar mass and polydispersity of the B groups can vary freely. However, preferably, the average molar mass of the B groups is from 100 g / mol to 20 000 g / mol, preferably from 200 g / mol to 15 000 g / mol, more preferably from 400 g / mol to 10 000 g / mol. The average molar mass of the B groups can be calculated based on the number of OH groups of the hydroxy-functional polybutadiene (E) used, from the starting weight of the monomers used. Thus, for example, if 40 g of ethylene oxide is used and the amount of the hydroxy-functional polybutadiene (E) used has 0.05 mol of OH groups, the average molar mass of the B groups is 800 g / mol.
[0190] Depending on the composition and molar mass, the polyether-modified polybutadiene (G) or (K) is liquid, pasty or solid.
[0191] The number average molar mass M of the polyether-modified polybutadiene (G) or (K) n It is preferably 1000 to 6000 g / mol, further preferably 1500 to 5000 g / mol, particularly preferably 2000 to 4000 g / mol.
[0192] Their polydispersities are variable within a wide range. According to the GPC method relative to PPG standards, the polydispersity of at least one polyether-modified polybutadiene (G) or (K) is preferably M w / M n =1.5 to 10, more preferably 2 to 9, more preferably 3 to 8.
[0193] The following examples describe the invention by way of illustration and are not intended to limit the invention, the scope of application of which is clear from the entire description and claims to the embodiments cited in the examples. Example:
[0194] General approach:
[0195] Gel Permeation Chromatography (GPC):
[0196] GPC measurement was performed under the following measurement conditions to determine the polydispersity (M w / M n ), weight average molar mass (M w ) and number average molar mass (M n ): Column assembly (length 65 cm), temperature 30°C, THF as mobile phase, flow rate 1 ml / min, sample concentration 10 g / l, RI detector, evaluation against polypropylene glycol standards.
[0197] Determination of 1,4-cis, 1,4-trans and 1,2 unit content in polybutadiene:
[0198] You can use 1 The content of 1,4-cis, 1,4-trans and 1,2 units is determined by H NMR spectroscopy. This method is familiar to those skilled in the art.
[0199] Determination of epoxy group content (epoxy content, epoxidation level) in polybutadiene:
[0200] With the help of 13C NMR spectroscopy determines the content of epoxy groups. A Bruker Avance 400 NMR spectrometer was used. For this purpose, the samples were dissolved in deuterated chloroform. The epoxy content is defined as the proportion of epoxidized butadiene units in mol %, based on the totality of all repeating units present in the sample. This corresponds to the number of epoxy groups in the epoxidized polybutadiene divided by the number of double bonds in the polybutadiene used.
[0201] Determination of acid value:
[0202] The acid value is determined by titration in accordance with DIN EN ISO 2114.
[0203] Determination of color lightening:
[0204] The lightening of the color is determined by the change in the Gardner color number (determined in accordance with DIN ISO 4630).
[0205] Synthesis Example:
[0206] Step a), Preparation of epoxidized polybutadiene
[0207] Embodiment A1:
[0208] Using polybutadiene ( 110) Preparation of epoxidized polybutadiene. According to the prior art, 1600 g of 110 and 86.4 g of concentrated formic acid in 4000 g of chloroform. Subsequently, 320 g of a 30% H2O2 solution (30% by weight of H2O2 based on the total mass of the aqueous solution) was slowly added dropwise, and the solution was heated to 50°C for 7 hours. After the reaction was completed, the mixture was cooled to room temperature, the organic phase was removed and washed four times with distilled water. Excess chloroform and residual water were distilled off. 1556 g of product was obtained, which was mixed with 1000 ppm of 1135 Mix and store under nitrogen.
[0209] pass 13 C NMR evaluation gave an epoxidation level of about 8.9% of the double bonds.
[0210] M w =4669 g / mol; M n =1931 g / mol; M w / M n =2.4.
[0211] Embodiment A2:
[0212] By the method described in Example A1, a 2L four-necked flask was initially charged with 200 g of 110 and 6.5 g of concentrated formic acid in 200 g of chloroform, and 24 g of a 30% H2O2 solution (30% by weight of H2O2 based on the total mass of the aqueous solution) were added. After 7 hours at 50°C, phase separation, washing with distilled water and subsequent distillation, 191 g of the obtained product were obtained. 13 The epoxidation level of double bonds by C NMR analysis was about 6.7% of the epoxidized polybutadiene.
[0213] M w =4624 g / mol; M n =2022 g / mol; M w / M n =2.3.
[0214] Embodiment A3:
[0215] By the method described in Example A1, a 2L four-necked flask was initially charged with 200 g of 110 and 19.5 g of concentrated formic acid in 200 g of chloroform, and 72 g of a 30% H2O2 solution (30% by weight of H2O2 based on the total mass of the aqueous solution) were added. After 7 hours at 50°C, phase separation, washing with distilled water and subsequent distillation, 196 g of the obtained product were obtained. 13 The epoxidation level of double bonds by C NMR analysis was about 16.2% of the epoxidized polybutadiene.
[0216] M w =4943 g / mol; M n =2083 g / mol; M w / M n =2.4.
[0217] Embodiment A4:
[0218] By the method described in Example A1, a 2L four-necked flask was initially charged with 200 g of 110 and 24.2 g of concentrated formic acid in 200 g of chloroform, and 89.3 g of a 30% H2O2 solution (30% by weight of H2O2 based on the total mass of the aqueous solution) were added. After 7 hours at 50°C, phase separation, washing with distilled water and subsequent distillation, 204 g of the obtained product were obtained. 13 The epoxidation level of double bonds by C NMR analysis was about 21.0% of the epoxidized polybutadiene.
[0219] M w =4843 g / mol; M n =2025 g / mol; M w / Mn =2.4.
[0220] Embodiment A5:
[0221] By the method described in Example A1, a 2L four-necked flask was initially charged with 200 g of 110 and 10.8 g of concentrated formic acid in 200 g of toluene, and 40 g of a 30% H2O2 solution (30% by weight of H2O2 based on the total mass of the aqueous solution) were added. After 10 hours at 50° C., phase separation, washing with saturated NaHCO3 solution and subsequent distillation, 172 g of the obtained product were obtained. 13 The epoxidation level of double bonds by C NMR analysis was about 7.6% of the epoxidized polybutadiene.
[0222] M w =4634 g / mol; M n =2020 g / mol; M w / M n =2.3.
[0223] Embodiment A6:
[0224] By the method described in Example A1, a 20 L reactor was initially charged with 2000 g of polybutadiene ( 130) and 191 g of concentrated formic acid in 5000 g of chloroform, and 710 g of a 30% H2O2 solution (30% by weight of H2O2 based on the total mass of the aqueous solution) were added. After 7 hours at 50°C, phase separation, washing with distilled water and subsequent distillation, 1980 g of the obtained product were obtained. 13 The epoxidation level of double bonds by C NMR analysis was about 14.6% of the epoxidized polybutadiene.
[0225] M w =15 333 g / mol; M n =3455 g / mol; M w / M n =4.4.
[0226] Embodiment A7:
[0227] By the method described in Example A1, 800 g of 110 and 43.2 g of concentrated formic acid in 800 g of chloroform, and 160 g of a 30% H2O2 solution (30% by weight of H2O2 based on the total mass of the aqueous solution) were added. After 5 hours at 50°C, phase separation, washing with distilled water and subsequent distillation, 755 g of the obtained product were obtained. 13The epoxidation level of double bonds by C NMR analysis was about 8.7% of the epoxidized polybutadiene.
[0228] M w =4593 g / mol; M n =1975 g / mol; M w / M n =2.3.
[0229] Embodiment A8:
[0230] By the method described in Example A1, a 2L four-necked flask was initially charged with 200 g of polybutadiene of formula (1) having the structure x=40%, y+z=60% (Lithene ultra AL) and 122 g of concentrated formic acid in 200 g of chloroform, and 299 g of a 30% H2O2 solution (30% by weight of H2O2 based on the total mass of the aqueous solution) was added. After 7 hours at 50°C, phase separation, washing with distilled water and subsequent distillation, 218 g of the obtained product was obtained. 13 The epoxidation level of double bonds by C NMR analysis was about 60% of the epoxidized polybutadiene.
[0231] M w =1670 g / mol; M n =832 g / mol; M w / M n =2.0.
[0232] Embodiment A9:
[0233] By the method described in Example A1, a 2L four-necked flask was initially charged with 200 g of polybutadiene of formula (1) having the structure x=70%, y+z=30% (Lithene ActiV 50) and 61 g of concentrated formic acid in 200 g of chloroform, and 151 g of a 30% H2O2 solution (30% by weight of H2O2 based on the total mass of the aqueous solution) was added. After 6 hours at 50°C, phase separation, washing with distilled water and subsequent distillation, 205 g of the obtained product was obtained. 13 The epoxidation level of double bonds by C NMR analysis was about 30% of the epoxidized polybutadiene.
[0234] M w =1821 g / mol; M n =1045 g / mol; M w / M n =1.7.
[0235] Step b), Preparation of OH-functional polybutadiene
[0236] Embodiment B1:
[0237] A hydroxylated polybutadiene having a hydroxylation level of about 21% was prepared using the epoxidized polybutadiene prepared in Example A4. The hydroxylation level here is the number of OH groups of the OH-functional polybutadiene divided by the number of double bonds in the polybutadiene used in step a). For preparation, a 100 ml four-necked flask under a nitrogen atmosphere was initially charged with 18 g of epoxidized polybutadiene in 45 g of n-propanol, and 80 ppmw (based on the mass of the epoxidized polybutadiene) of trifluoromethanesulfonic acid (1% solution) dissolved in n-propanol was added while stirring. The mixture was then heated to 70° C. and stirred at this temperature for 8 hours. The reaction mixture became transparent during the reaction. After the reaction was completed, the mixture was cooled to room temperature and the solution was neutralized by adding 0.8 mg of solid NaHCO3 and then filtered. Excess alcohol was distilled off under reduced pressure. The alcohol recovered by distillation can be reused in subsequent synthesis. 16.9 g of a light brown product was obtained, which was mixed with 1000 ppm of 1135 Mix and store under nitrogen.
[0238] pass 13 Evaluation of C NMR showed complete conversion of all epoxy groups, which gave a hydroxylation level of approximately 21%.
[0239] M w =14 463 g / mol; M n =2789 g / mol; M w / M n =5.2.
[0240] Embodiment B2:
[0241] To prepare a hydroxylated polybutadiene having a hydroxylation level of about 8.9%, 20 g of the epoxidized polybutadiene prepared in Example A1 were initially charged to 45 g of n-propanol by the method described in Example B1 and 80 ppmw (based on the mass of the epoxidized polybutadiene) of trifluoromethanesulfonic acid (1% solution) dissolved in n-propanol were added while stirring. After stirring at 70° C. for 7 hours, the reaction mixture was neutralized at room temperature (RT) with 0.9 mg of solid NaHCO and filtered, and the excess alcohol was distilled off under reduced pressure. 18 g of a light brown product were obtained, which were mixed with 1000 ppm of 1135 Mix and store under nitrogen.
[0242] pass 13 Evaluation of C NMR showed complete conversion of all epoxy groups, which gave a hydroxylation level of approximately 8.9%.
[0243] M w =28 138 g / mol; M n=2534 g / mol; M w / M n =11.1.
[0244] Embodiment B3:
[0245] To prepare a hydroxylated polybutadiene with a hydroxylation level of about 21%, 18 g of the epoxidized polybutadiene prepared in Example A4 were initially charged to 45 g of isopropanol by the method described in Example B1 and 80 ppmw (based on the mass of the epoxidized polybutadiene) of trifluoromethanesulfonic acid (1% solution) dissolved in isopropanol were added while stirring. After stirring at 70° C. for 7 hours, the reaction mixture was neutralized at RT with 0.8 mg of solid NaHCO and filtered, and the excess alcohol was distilled off under reduced pressure. 16.4 g of a light brown product were obtained, which were mixed with 1000 ppm of 1135 Mix and store under nitrogen.
[0246] pass 13 Evaluation of C NMR showed complete conversion of all epoxy groups, which gave a hydroxylation level of approximately 21%.
[0247] M w =14 012 g / mol; M n =2534 g / mol; M w / M n =5.5.
[0248] Embodiment B4:
[0249] To prepare a hydroxylated polybutadiene with a hydroxylation level of about 21%, 54 g of the epoxidized polybutadiene prepared in Example A4 were initially charged to 135 g of isobutanol by the method described in Example B1 and 80 ppmw (based on the mass of the epoxidized polybutadiene) of trifluoromethanesulfonic acid (1% solution) dissolved in isobutanol were added while stirring. After stirring at 70° C. for 5 hours, the reaction mixture was neutralized at RT with 2.4 mg of solid NaHCO and filtered, and the excess alcohol was distilled off under reduced pressure. 50 g of a light brown product were obtained, which were mixed with 1000 ppm of 1135 Mix and store under nitrogen.
[0250] pass 13 Evaluation of C NMR showed complete conversion of all epoxy groups, which gave a hydroxylation level of approximately 21%.
[0251] M w =11 357 g / mol; M n =2690 g / mol; M w / M n=4.2.
[0252] Embodiment B5:
[0253] To prepare a hydroxylated polybutadiene having a hydroxylation level of about 8.9%, a 20 L reactor was initially charged with 1500 g of the epoxidized polybutadiene prepared in Example A1 in 3150 g of isobutanol (which was recovered by distillation in Example B6) by the method described in Example B1, and 80 ppmw (based on the mass of the epoxidized polybutadiene) of trifluoromethanesulfonic acid (1% solution) dissolved in isobutanol was added while stirring. After stirring at 70° C. for 5 hours, the reaction mixture was neutralized at RT with 67.5 mg of solid NaHCO3 and filtered, and the excess alcohol was distilled off under reduced pressure. 1380 g of a light brown product was obtained, which was mixed with 1000 ppm of 1135 Mix and store under nitrogen.
[0254] pass 13 Evaluation of C NMR showed complete conversion of all epoxy groups, which gave a hydroxylation level of approximately 8.9%.
[0255] M w =8597 g / mol; M n =2306 g / mol; M w / M n =3.7.
[0256] Embodiment B6:
[0257] To prepare a hydroxylated polybutadiene having a hydroxylation level of about 14.6%, a 20 L reactor was initially charged with 1600 g of the epoxidized polybutadiene prepared in Example A6 in 4500 g of isobutanol by the method described in Example B1 and 80 ppmw (based on the mass of the epoxidized polybutadiene) of trifluoromethanesulfonic acid (1% solution) dissolved in isobutanol was added while stirring. After stirring at 70° C. for 10 hours, the reaction mixture was neutralized at RT with 72 mg of solid NaHCO and filtered, and the excess alcohol was distilled off under reduced pressure. 1470 g of a light brown product was obtained, which was mixed with 1000 ppm of 1135 Mix and store under nitrogen.
[0258] pass 13 Evaluation of C NMR showed complete conversion of all epoxy groups, which gave a hydroxylation level of approximately 14.6%.
[0259] M w =51 674 g / mol; M n =4081 g / mol; M w / Mn =12.7.
[0260] Embodiment B7:
[0261] To prepare a hydroxylated polybutadiene having a hydroxylation level of about 8.7%, a 2 L reactor was initially charged with 720 g of the epoxidized polybutadiene prepared in Example A7 in 720 g of isobutanol, and 80 ppmw (based on the mass of the epoxidized polybutadiene) of trifluoromethanesulfonic acid (1% solution) dissolved in isobutanol was added while stirring. After stirring at 70° C. for 7 hours, the reaction mixture was mixed at room temperature with 10 ml of a saturated aqueous NaHCO solution and chloroform to clarify the mixture. After stirring for 1.5 hours, the mixture was filtered and excess water, alcohol and chloroform were distilled off under reduced pressure. 742 g of a pale yellow product was obtained, which was mixed with 1000 ppm of 1135 Mix and store under nitrogen.
[0262] pass 13 Evaluation of C NMR showed complete conversion of all epoxy groups, which resulted in a hydroxylation level of approximately 8.7%.
[0263] M w =8674 g / mol; M n =2459 g / mol; M w / M n =3.5.
[0264] Embodiment B8:
[0265] To prepare a hydroxylated polybutadiene with a hydroxylation level of about 60%, 200 g of the epoxidized polybutadiene prepared in Example A8 were initially charged to 500 g of isobutanol by the method described in Example B1 and 80 ppmw (based on the mass of the epoxidized polybutadiene) of trifluoromethanesulfonic acid (1% solution) dissolved in isobutanol were added while stirring. After stirring at 70° C. for 6 hours, the reaction mixture was neutralized at RT with 9.0 mg of solid NaHCO and filtered, and the excess alcohol was distilled off under reduced pressure. 318 g of a light brown product were obtained, which was mixed with 1000 ppm of 1135 Mix and store under nitrogen.
[0266] pass 13 Evaluation of C NMR showed complete conversion of all epoxy groups, which resulted in a hydroxylation level of approximately 60%.
[0267] M w =3140 g / mol; M n =1264 g / mol; M w / Mn =2.5.
[0268] Embodiment B9:
[0269] To prepare a hydroxylated polybutadiene with a hydroxylation level of about 30%, 150 g of the epoxidized polybutadiene prepared in Example A9 were initially charged to 375 g of isobutanol by the method described in Example B1 and 80 ppmw (based on the mass of the epoxidized polybutadiene) of trifluoromethanesulfonic acid (1% solution) dissolved in isobutanol were added while stirring. After stirring at 70° C. for 7 hours, the reaction mixture was neutralized at RT with 6.8 mg of solid NaHCO and filtered, and the excess alcohol was distilled off under reduced pressure. 192 g of a light brown product were obtained, which were mixed with 1000 ppm of 1135 Mix and store under nitrogen.
[0270] pass 13 Evaluation of C NMR showed complete conversion of all epoxy groups, which resulted in a hydroxylation level of approximately 30%.
[0271] M w =2972 g / mol; M n =1100 g / mol; M w / M n =2.7.
[0272] Step c), Alkoxylation of OH-functional polybutadiene
[0273] Alkoxylation using DMC catalysts:
[0274] Example C1:
[0275] A 3-liter autoclave was initially charged with 335 g of the hydroxylated polybutadiene prepared in Example B5 and 0.45 g of zinc hexacyanocobaltate DMC catalyst under nitrogen and heated to 130° C. with stirring. The reactor was evacuated to an internal pressure of 30 mbar in order to remove any volatile components present by distillation. The DMC catalyst was activated by feeding a portion of 41.0 g of propylene oxide. 15 minutes after the start of the reaction (pressure drop in the reactor), a further 144.3 g of propylene oxide were metered in continuously while cooling at 130° C. and a maximum reactor internal pressure of 0.6 bar (absolute) within 1 hour. The reaction was continued at 130° C. for 30 minutes and then degassed. Volatile components such as residual propylene oxide were distilled off under reduced pressure. The product was cooled to below 80° C. and a portion of 165.5 g was discharged. The medium-viscous and orange-colored turbid alkoxylated polybutadiene was mixed with 1000 ppm of 1135 Mix and store under nitrogen.
[0276] Mw =14 310 g / mol; M n =2698 g / mol; M w / M n =5.3.
[0277] The remaining amount in the reactor was heated again to 130°C and 126.4 g of propylene oxide were then added continuously. After the addition was complete and the reaction was continued for 30 minutes, the mixture was degassed again and another 171.3 g of product sample was taken. The medium viscous and orange turbid alkoxylated polybutadiene was mixed with 1000 ppm of 1135 Mix and store under nitrogen.
[0278] M w =13 450 g / mol; M n =3139 g / mol; M w / M n =4.3.
[0279] The remaining amount in the reactor was heated again to 130° C., and then 81.0 g of propylene oxide were added continuously. After the addition was complete and the reaction was continued for 30 minutes, the mixture was degassed again and 391.3 g of the entire reactor content was discharged. The medium-viscous and orange-colored turbid alkoxylated polybutadiene was mixed with 1000 ppm of 1135 Mix and store under nitrogen.
[0280] M w =15 430 g / mol; M n =3723 g / mol; M w / M n =4.1.
[0281] Example C2:
[0282] A 3-liter autoclave was initially charged with 211 g of the hydroxylated polybutadiene prepared in Example B5 and 0.26 g of zinc hexacyanocobaltate DMC catalyst under nitrogen and heated to 130° C. with stirring. The reactor was evacuated to an internal pressure of 30 mbar to remove any volatile components present by distillation. The DMC catalyst was activated by feeding a portion of 28.0 g of an equimolar mixture of propylene oxide and ethylene oxide. 20 minutes after the start of the reaction (pressure drop in the reactor), a further 74.3 g of the EO / PO mixture was metered in continuously while cooling at 130° C. and a maximum reactor internal pressure of 0.6 bar (absolute) within 40 minutes. The reaction was continued at 130° C. for 30 minutes and then degassed. Volatile components such as residual propylene oxide and ethylene oxide were distilled off under reduced pressure. The product was cooled to below 80° C. and a portion of 54 g was discharged. The medium-viscous and orange-colored turbid alkoxylated polybutadiene was mixed with 1000 ppm of 1135 Mix and store under nitrogen.
[0283] M w =13 690 g / mol; M n =2547 g / mol; M w / M n =5.4.
[0284] The remaining amount in the reactor was heated again to 130°C and then 84.7 g of an equimolar mixture of propylene oxide and ethylene oxide were added continuously. After the addition was complete and the reaction was continued for 30 minutes, the mixture was degassed again and another 73.1 g product sample was taken. The medium viscous and orange turbid alkoxylated polybutadiene was mixed with 1000 ppm of 1135 Mix and store under nitrogen.
[0285] M w =13 110 g / mol; M n =2868 g / mol; M w / M n =4.6.
[0286] The remaining amount in the reactor was heated again to 130° C., and then 66.7 g of an equimolar mixture of propylene oxide and ethylene oxide were added continuously. After the addition was complete and the reaction was continued for 30 minutes, the mixture was degassed again and 337.6 g of the entire reactor content was discharged. The medium viscous and orange turbid alkoxylated polybutadiene was mixed with 1000 ppm of 1135 Mix and store under nitrogen.
[0287] M w =15 190 g / mol; M n =3845 g / mol; Mw / M n =4.0.
[0288] Alkoxylation with basic catalysts:
[0289] Example C3:
[0290] A 3-liter autoclave was initially charged with 196.1 g of the hydroxylated polybutadiene prepared in Example B5 and 11.1 g of a 30% sodium methoxide solution (30% by weight of a sodium methoxide solution in methanol, based on the total mass of the solution) under nitrogen, and the mixture was stirred at 50° C. for 1 hour. Subsequently, the mixture was heated to 115° C. while stirring, and the reactor was evacuated to an internal pressure of 30 mbar to distill off excess methanol and other volatile components present. 324 g of propylene oxide were continuously metered in, while cooling at 115° C. and a maximum reactor internal pressure of 3.5 bar (absolute) over a period of 6 hours. The reaction was continued at 115° C. for 30 minutes, followed by degassing. Volatile components such as residual propylene oxide were distilled off under reduced pressure. The product was cooled to below 80° C. A portion of 51 g was discharged, and this medium-viscous and orange-colored transparent alkoxylated polybutadiene was neutralized with lactic acid to an acid number of 0.1 mg KOH / g and 1000 ppm of 1135 Mix and store under nitrogen.
[0291] M w =18 690 g / mol; M n =2888 g / mol; M w / M n =6.5.
[0292] The remaining amount in the reactor was heated to 115°C again, and then 216 g of propylene oxide was added continuously. After the addition was completed and the reaction was continued for 30 minutes, the mixture was degassed again, cooled to 95°C, neutralized with 30% H3PO4 (30% by weight of H3PO4 aqueous solution based on the total mass of the solution), and mixed with 1000 ppm of 1135. The water was removed by vacuum distillation and the precipitated salts were filtered off. 675 g of a transparent product with an acid value of 0.1 mg KOH / g was isolated and stored under nitrogen.
[0293] M w =22 850 g / mol; M n =3160 g / mol; M w / M n =7.2.
[0294] Example C4:
[0295] A 3-liter autoclave was initially charged with 197.3 g of the hydroxylated polybutadiene prepared in Example B5 and 11.2 g of a 30% sodium methoxide solution (30% by weight of a sodium methoxide solution in methanol, based on the total mass of the solution) under nitrogen, and the mixture was stirred at 50° C. for 1 hour. Subsequently, the mixture was heated to 115° C. while stirring, and the reactor was evacuated to an internal pressure of 30 mbar to distill off excess methanol and other volatile components present. 82.5 g of ethylene oxide were continuously metered in, while cooling at 115° C. and a maximum reactor internal pressure of 3.5 bar (absolute) within 45 minutes. The reaction was continued at 115° C. for 30 minutes, followed by degassing. Volatile components such as residual ethylene oxide were distilled off under reduced pressure. The product was cooled to below 80° C. and a portion of 49.7 g was discharged. The orange, transparent alkoxylated polybutadiene, which was solid at room temperature, was neutralized with lactic acid to an acid number of 0.1 mg KOH / g and with 1000 ppm of 1135 Mix and store under nitrogen.
[0296] M w =16 100 g / mol; M n =2945 g / mol; M w / M n =5.5.
[0297] The remaining amount in the reactor was heated again to 115° C., and then 68 g of ethylene oxide were added continuously. After the addition was complete and the reaction was continued for 30 minutes, the mixture was degassed again and cooled to 95° C. A portion of 59 g was discharged and this orange, transparent alkoxylated polybutadiene, which was solid at room temperature, was neutralized with lactic acid to an acid value of 0.1 mg KOH / g and 1000 ppm of 1135 Mix and store under nitrogen.
[0298] M w =17 410 g / mol; M n =3413 g / mol; M w / M n =5.1.
[0299] The remaining amount in the reactor was heated again to 115° C., and then 54.4 g of ethylene oxide were added continuously. After the addition was complete and the reaction was continued for 30 minutes, the mixture was degassed again and cooled to 95° C. 280 g of the remaining product were discharged, and this orange, transparent alkoxylated polybutadiene, which was solid at room temperature, was neutralized with lactic acid to an acid value of 0.1 mg KOH / g and 1000 ppm of 1135 Mix and store under nitrogen.
[0300] M w =19 000 g / mol; Mn =3874 g / mol; M w / M n =4.9.
[0301] Example C5:
[0302] A 3-liter autoclave was initially charged with 194 g of the hydroxylated polybutadiene prepared in Example B5 and 11.0 g of a 30% sodium methoxide solution (30% by weight of a sodium methoxide solution in methanol, based on the total mass of the solution) under nitrogen, and the mixture was stirred at 50° C. for 1 hour. Subsequently, the mixture was heated to 115° C. while stirring, and the reactor was evacuated to an internal pressure of 30 mbar in order to distill off excess methanol and other volatile components present. 94.5 g of ethylene oxide and 53.4 g of propylene oxide were metered in continuously in the form of a mixture simultaneously, while cooling at 115° C. and a maximum reactor internal pressure of 3.5 bar (absolute) over a period of 5.5 hours. The reaction was continued at 115° C. for 30 minutes, followed by degassing. Volatile components such as residual alkylene oxides were distilled off under reduced pressure. The product was cooled to below 80° C. and a portion of 31.3 g was discharged. The orange transparent alkoxylated polybutadiene which is liquid at room temperature is neutralized with lactic acid to an acid value of 0.1 mg KOH / g and 1000 ppm 1135 Mix and store under nitrogen.
[0303] M w =16 230 g / mol; M n =2810 g / mol; M w / M n =5.8.
[0304] The remaining amount in the reactor was heated again to 115° C., and then 85.9 g of ethylene oxide and 48.5 g of propylene oxide were added simultaneously and continuously in the form of a mixture. After the addition was complete and the reaction was continued for 30 minutes, the mixture was degassed again and cooled to 95° C. A portion of 34.3 g was discharged and this orange, transparent alkoxylated polybutadiene, which was liquid at room temperature, was neutralized with lactic acid to an acid value of 0.1 mg KOH / g and 1000 ppm of 1135 Mix and store under nitrogen.
[0305] M w =19 160 g / mol; M n =3014 g / mol; M w / M n =6.4.
[0306] The remaining amount in the reactor was heated again to 115°C, and then 79.3 g of ethylene oxide and 44.9 g of propylene oxide were added simultaneously and continuously in the form of a mixture. After the addition was complete and the reaction was continued for 30 minutes, the mixture was degassed again, cooled to 95°C, neutralized with 30% H3PO4, and mixed with 1000 ppm of 1135. The water was removed by vacuum distillation and the precipitated salts were filtered off. 522 g of a transparent product with an acid value of 0.1 mg KOH / g was isolated and stored under nitrogen.
[0307] M w =24 030 g / mol; M n =3251 g / mol; M w / M n =7.4.
[0308] Example C6:
[0309] Under nitrogen, 208 g of the hydroxylated polybutadiene prepared in Example B5 and 4.6 g of solid potassium methoxide are charged into a 3-liter autoclave and stirred at 50° C. for 1 hour. Subsequently, the mixture is heated to 115° C. while stirring, and the reactor is evacuated to an internal pressure of 30 mbar to distill off the volatile components present. 115 g of propylene oxide are continuously metered in, while cooling at 115° C. and a maximum reactor internal pressure of 3.0 bar (absolute) within 2 hours. The reaction is continued at 115° C. for 30 minutes and then degassed. Volatile components such as residual propylene oxide are distilled off under reduced pressure. The product is cooled to below 80° C., neutralized with lactic acid to an acid number of 0.1 mg KOH / g and mixed with 1000 ppm of 1135 mixing. 315 g of a brown, transparent alkoxylated polybutadiene which is liquid at room temperature is obtained and stored under nitrogen.
[0310] M w =14 350 g / mol; M n =2657 g / mol; M w / M n =5.4.
[0311] Example C7:
[0312] A 3 l autoclave was initially charged with 400 g of the hydroxylated polybutadiene prepared in Example B7 and 20.3 g of a 30% sodium methoxide solution (30% by weight of a sodium methoxide solution in methanol, based on the total mass of the solution) under nitrogen, and the mixture was stirred at 50° C. for 1 hour. The mixture was subsequently heated to 115° C. while stirring and the reactor was evacuated to an internal pressure of 30 mbar in order to remove the excess methanol and other volatile components present by distillation. Subsequently, 488 g of propylene oxide were metered in continuously while cooling at 115° C. and a maximum reactor internal pressure of 3.5 bar (absolute) over a period of 6 hours. Upon completion of the addition and after a further reaction time of 30 minutes, the mixture was degassed again, cooled to 95° C., neutralized with 30% H3PO4 (30% by weight of an aqueous H3PO4 solution, based on the total mass of the solution) and reacted with 1000 ppm of 1135. The water was removed by vacuum distillation and the precipitated salt was filtered off. 826 g of a reddish brown transparent product with an acid value of 0.1 mg KOH / g was isolated and stored under nitrogen.
[0313] M w =14 672 g / mol; M n =2740 g / mol; M w / M n =5.4.
[0314] Example C8:
[0315] A 3 l autoclave was initially charged with 250 g of the hydroxylated polybutadiene prepared in Example B8 and 49.7 g of a 30% sodium methoxide solution (30% by weight of a sodium methoxide solution in methanol, based on the total mass of the solution) under nitrogen, and the mixture was stirred at 50° C. for 1 hour. The mixture was subsequently heated to 115° C. while stirring and the reactor was evacuated to an internal pressure of 30 mbar in order to remove the excess methanol and other volatile components present by distillation. Subsequently, 1202 g of propylene oxide were metered in continuously while cooling at 115° C. and a maximum reactor internal pressure of 3.5 bar (absolute) over a period of 10 hours. Upon completion of the addition and after a further reaction time of 30 minutes, the mixture was degassed again, cooled to 95° C., neutralized with 30% H3PO4 (30% by weight of an aqueous H3PO4 solution, based on the total mass of the solution) and reacted with 1000 ppm of 1135 were mixed. Water was removed by vacuum distillation and the precipitated salts were filtered off. 1365 g of a transparent product with an acid value of 0.1 mg KOH / g was isolated and stored under nitrogen.
[0316] M w =11 072 g / mol; M n =2460 g / mol; M w / M n=4.5.
[0317] Example C9:
[0318] A 3 l autoclave was initially charged with 150 g of the hydroxylated polybutadiene prepared in Example B9 and 20.0 g of a 30% sodium methoxide solution (30% by weight of a sodium methoxide solution in methanol, based on the total mass of the solution) under nitrogen, and the mixture was stirred at 50° C. for 1 hour. The mixture was subsequently heated to 115° C. while stirring and the reactor was evacuated to an internal pressure of 30 mbar in order to remove the excess methanol and other volatile components present by distillation. Subsequently, 484 g of propylene oxide were metered in continuously while cooling at 115° C. and a maximum reactor internal pressure of 3.5 bar (absolute) over a period of 6 hours. Upon completion of the addition and after a further reaction time of 30 minutes, the mixture was degassed again, cooled to 95° C., neutralized with 30% H3PO4 (30% by weight of an aqueous H3PO4 solution, based on the total mass of the solution) and reacted with 1000 ppm of 1135. The water was removed by vacuum distillation and the precipitated salts were filtered off. 599 g of a transparent product with an acid value of 0.1 mg KOH / g was isolated and stored under nitrogen.
[0319] M w =8914 g / mol; M n =2073 g / mol; M w / M n =4.3.
[0320] Step e), post-processing for lightening of color
[0321] Lighten the color by adding activated carbon
[0322] Embodiment E1:
[0323] In a 100 ml single-necked flask, 20 g of the alkoxylated polybutadiene prepared in Example C7 (Gardner color number: 4.3) were mixed with 10 ml of chloroform and 1 g of activated carbon (Norit SX 1). After stirring at room temperature for 2 hours, the activated carbon was filtered off and the excess solvent was removed under reduced pressure. 19 g of light-colored alkoxylated polybutadiene were isolated.
[0324] Gardner color number: 2.1.
[0325] Lighten the color by adding hydrogen peroxide:
[0326] Embodiment E2:
[0327] In a 100 ml single-necked flask with a reflux condenser, 20 g of the alkoxylated polybutadiene prepared in Example C7 (Gardner color number: 4.3) were equilibrated to 60° C. and mixed with 5% by weight of a 30% hydrogen peroxide solution (30% by weight of H O based on the total mass of the aqueous solution). The mixture was stirred at 80° C. for 2 hours, and then water and excess hydrogen peroxide were distilled off under full vacuum. 20 g of a light-colored product (Gardner color number: 1.8) were isolated.
Claims
1. A method for preparing one or more polyether-modified polybutadienes, comprising the steps of: a) reacting at least one polybutadiene (A) with at least one epoxidizing agent (B) to obtain at least one epoxy-functional polybutadiene (C); b) reacting the at least one epoxy-functional polybutadiene (C) with at least one hydroxy-functional compound (D) to obtain at least one hydroxy-functional polybutadiene (E); c) reacting the at least one hydroxy-functional polybutadiene (E) with at least one epoxy-functional compound (F) to obtain at least one polyether-modified polybutadiene (G), The hydroxy-functional compound (D) is selected from monofunctional alcohols having 1 to 6 carbon atoms, carboxylic acids and water, The reaction in step b) is an addition reaction of at least one hydroxy-functional compound (D) onto at least one epoxy-functional polybutadiene (C).
2. The method according to claim 1, further comprising the steps of: d) reacting the at least one polyether-modified polybutadiene (G) with at least one capping agent (H) to obtain at least one polyether-modified polybutadiene (K) containing capped polyether groups.
3. The method according to claim 1 or 2, further comprising the following steps: e) lightening the color of the at least one polyether-modified polybutadiene (G) or (K).
4. The method according to claim 1 or 2, characterized in that: 0% to 80% of the double bonds of all polybutadienes (A) used are 1,2 vinyl double bonds and 20% to 100% are 1,4 double bonds.
5. The method according to claim 1 or 2, characterized in that: The number average molar mass M of the at least one polybutadiene (A) is n 200 g / mol to 20000 g / mol.
6. The method according to claim 1 or 2, characterized in that: From >0% to 70% of the double bonds of the at least one polybutadiene (A) are epoxidized.
7. The method according to claim 1 or 2, characterized in that: The at least one epoxidation agent (B) comprises performic acid.
8. The method according to claim 1 or 2, characterized in that: The at least one hydroxy-functional compound (D) is chosen from monofunctional alcohols having 2 to 4 carbon atoms.
9. The method according to claim 1 or 2, characterized in that: In step b), the total number of hydroxyl groups in all the hydroxyl-functional compounds (D): the total number of epoxy groups in all the epoxy-functional polybutadienes (C) is >1:1 to 50:
1.
10. The method according to claim 1 or 2, characterized in that: In step b), an acid is used as catalyst.
11. The method according to claim 1 or 2, characterized in that: The at least one epoxy-functional compound used in step c) is selected from: a. an alkylene oxide having 2 to 18 carbon atoms, and / or b. Glycidyl compounds.
12. The method according to claim 1 or 2, characterized in that: In step c) an alkoxylation catalyst is used.
13. Polyether-modified polybutadiene (G) obtainable by the process according to claim 1 or any one of claims 3 to 12.
14. Polyether-modified polybutadiene (K), obtainable by the process according to any one of claims 2 to 12.
15. The polyether-modified polybutadiene (G) according to claim 13 or the polyether-modified polybutadiene (K) according to claim 14, characterized in that: The polyether-modified polybutadiene (G) or (K) comprises repeating units selected from the following divalent groups: in A is independently at each occurrence a monovalent organic group or a hydrogen group; B is independently selected at each occurrence from a group of formula (4a) R 1 is independently selected at each occurrence from a monovalent hydrocarbon radical having 1 to 16 carbon atoms; R 2 The formula is -CH2-OR 3 Groups; R 3 is independently selected at each occurrence from a monovalent hydrocarbon radical having 3 to 18 carbon atoms; R 4 is independently at each occurrence a monovalent organic group having 1 to 18 carbon atoms or hydrogen; and m, n, o, p and q are each independently 0 to 300, provided that the sum of m, n, o, p and q is greater than 1; Every permutation of repeating units (U), (V), (W), (X), (Y) and (Z) as well as every permutation of repeating units in a B group is included.
16. The polyether-modified polybutadiene according to claim 15, characterized in that: The sum of all repeating units (U), (V) and (W) divided by the sum of all repeating units (U), (V), (W), (X), (Y) and (Z) is >0% to 70%.
17. The polyether-modified polybutadiene (G) according to claim 15, characterized in that The polybutadiene has the formula (5) Wherein, based on the sum of all repeating units represented by formula (5), the proportion of the polyether-modified repeating units represented by formula (5) is >0% to 70%, wherein the proportion is calculated as [(d+e+f) / (a+b+c+d+e+f)]*100%.
18. The polyether-modified polybutadiene according to claim 13 or 14, characterized in that: Number average molar mass M of the polybutadiene part n 200 g / mol to 20000 g / mol.
19. The polyether-modified polybutadiene according to claim 13 or 14, characterized in that: 0% to 80% of the double bonds present are 1,4 double bonds.
20. The polyether-modified polybutadiene according to claim 15, characterized in that: The average molar mass of the B group is 100 g / mol to 20000 g / mol.
21. The polyether-modified polybutadiene according to claim 17, characterized in that: The average molar mass of the B group is 100 g / mol to 20000 g / mol.
Citation Information
Patent Citations
short-circuit proof, MEDIUM VOLTAGE STABILIZED DUAL CURRENT SUPPLY
DD206286A1
PROCESS FOR PRODUCTION OF POLYBUTADIENE EPOXIDES
DD253627A1
Coating composition for electrodeposition by cathode precipitation
DE2943879A1
USE OF CATIONIC POLYMERS AS ANTISTATIC ADDITIVES TO HAIR TREATMENT PRODUCTS
DE3305964A1
Aqueous dispersion of cationic crosslinked resin particles and its usage
EP0351135A2