Urethane resin composition and leather sheet

By introducing anionic and nonionic groups into the urethane resin, combined with liquid polycarbonate polyol and nonionic emulsifier, the problem of difficult to balance the feel and stability of the urethane resin in water is solved. It achieves excellent hand feel and formulation stability, is suitable for resin impregnation of fiber substrates, and improves the heat resistance and hydrolysis resistance of the product.

CN114729182BActive Publication Date: 2024-10-18DIC CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202080074068.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-10
Publication Date
2024-10-18
Estimated Expiration
2040-09-10

AI Technical Summary

Technical Problem

The existing application of urethane resin in water is difficult to achieve both excellent hand feel and formulation stability, especially in the context of de-DMF, resulting in performance loss.

Method used

Use urethane resin with anionic and nonionic groups, combined with liquid polycarbonate polyol and nonionic emulsifier at room temperature, avoid using compounds with more than three hydroxyl groups, and optimize the molar ratio and molecular weight to Get excellent feel and formulation stability.

Benefits of technology

Under environmentally friendly conditions, the urethane resin composition has excellent feel and formulation stability, is suitable for impregnating resin for fiber substrates, and improves the heat resistance and hydrolysis resistance of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0003673371790000141
    Figure GDA0003673371790000141
  • Figure GDA0003673371790000142
    Figure GDA0003673371790000142
  • Figure GDA0003673371790000151
    Figure GDA0003673371790000151
Patent Text Reader

Abstract

The problem to be solved by the present invention is to provide a carbamate resin composition and a leather piece, wherein the carbamate resin composition has excellent hand feel and stability of the prepared liquid in a carbamate resin composition containing water. A carbamate resin composition contains a carbamate resin (A) having anionic groups and nonionic groups, a nonionic emulsifier (B) and water (C), wherein the carbamate resin (A) uses a polycarbonate polyol (a1) that is liquid at room temperature as a raw material, and does not use a compound (x2) having three or more hydroxyl groups as a raw material. In addition, the present invention provides a leather piece, characterized in that a coagulant of the carbamate resin composition is present in a fiber substrate. The carbamate resin (A) and the nonionic emulsifier (B) both preferably have oxyethylene groups and oxypropylene groups.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a urethane resin composition and a leather sheet. Background Art

[0002] Polyurethane resins are widely used in the manufacture of synthetic leather (including artificial leather) due to their good mechanical strength and hand feel. Among the above uses, solvent-based urethane resins containing N,N-dimethylformamide (DMF) have been the mainstream so far. However, against the background of DMF restrictions in Europe, the strengthening of volatile organic compounds (VOC) emission restrictions in China, and DMF restrictions by large clothing manufacturers, the de-DMFization of urethane resins used in each layer of synthetic leather is sought.

[0003] In order to cope with such environmental changes, urethane resin compositions in which urethane resin is dispersed in water have been widely studied (for example, see Patent Document 1). However, in existing products including the invention described in Patent Document 1, it is difficult to achieve both excellent hand feel and stability of the prepared solution.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2007-119749 Summary of the invention

[0007] Problems to be solved by the invention

[0008] The problem to be solved by the present invention is to provide a urethane resin composition having excellent texture and formulation stability among urethane resin compositions containing water.

[0009] Technical means of solving problems

[0010] The present invention provides a carbamate resin composition, which contains a carbamate resin (A) having anionic groups and nonionic groups, a nonionic emulsifier (B) and water (C), wherein the carbamate resin (A) uses a polycarbonate polyol (a1) that is liquid at room temperature as a raw material and does not use a compound (x2) having three or more hydroxyl groups as a raw material.

[0011] The present invention also provides a leather sheet comprising a fiber base material containing a coagulated product of the urethane resin composition.

[0012] Effects of the Invention

[0013] The urethane resin composition of the present invention contains water and is environmentally friendly. In addition, the urethane resin composition has excellent hand feel and stability of the prepared liquid. Therefore, the urethane resin composition can be particularly suitably used as a resin for impregnation of a fiber substrate. DETAILED DESCRIPTION

[0014] The urethane resin composition of the present invention contains a urethane resin (A) having an anionic group and a nonionic group, a nonionic emulsifier (B) and water (C), wherein the urethane resin (A) uses a polycarbonate polyol (a1) which is liquid at room temperature as a raw material and does not use a compound (x2) having three or more hydroxyl groups as a raw material.

[0015] In order to obtain an excellent hand feel, the urethane resin (A) used in the present invention must use a polycarbonate polyol (a1) that is liquid at room temperature. In the present invention, "liquid at room temperature" means that the polycarbonate polyol (a1) exhibits fluidity at 23°C and is liquid or viscous. As the polycarbonate polyol (a1), for example, a reaction product of a compound having two or more hydroxyl groups and carbonate and / or phosgene can be used.

[0016] As the compound having two or more hydroxyl groups, for example, propylene glycol, butanediol, pentanediol, hexanediol, decanediol, caprolactone, cyclohexanedimethanol, 3-methyl-1,5-pentanediol, neopentyl glycol, isosorbide, etc. can be used. These compounds can be used alone or in combination of two or more. Among these, in terms of obtaining a more excellent feel, heat resistance and hydrolysis resistance, it is preferred to use a room temperature liquid type such as a combination of butanediol and hexanediol and / or a combination of pentanediol and hexanediol.

[0017] As the carbonate ester, for example, dimethyl carbonate, diethyl carbonate, diphenyl carbonate, ethylene carbonate, propylene carbonate, etc. These compounds may be used alone or in combination of two or more.

[0018] The number average molecular weight of the polycarbonate polyol (a1) is preferably in the range of 500 to 10,000, and more preferably in the range of 700 to 4,000, from the viewpoint of obtaining more excellent hand feel, heat resistance, and hydrolysis resistance. The number average molecular weight of the polycarbonate polyol (a1) refers to a value measured by gel permeation chromatography (GPC).

[0019] The urethane resin (A) used in the present invention does not use the compound (x2) having three or more hydroxyl groups as a raw material. When the compound (x2) is used, the urethane resin has a cross-linked structure, so the texture is impaired.

[0020] As the compound (x2), for example, trimethylolpropane, glycerol, etc. These compounds may be used alone or in combination of two or more.

[0021] The urethane resin (A) must have anionic groups and nonionic groups in order to achieve both excellent hand feel and stability of the prepared solution. The anionic groups and nonionic groups are provided by the compound (a2) having anionic groups and the compound (a3) ​​having nonionic groups, respectively.

[0022] As the compound (a2) having an anionic group, for example, compounds having a carboxyl group such as 2,2-dimethylol propionic acid, 2,2-dimethylol butanoic acid, 2,2-dimethylol butyric acid, and 2,2-dimethylol valeric acid; 3,4-diaminobutanesulfonic acid, 3,6-diamino-2-toluenesulfonic acid, 2,6-diaminobenzenesulfonic acid, N-(2-aminoethyl)-2-aminosulfonic acid, N-(2-aminoethyl)-2-aminoethylsulfonic acid, N-2-aminoethane-2-aminosulfonic acid, and N-(2-aminoethyl)-β-alanine; compounds having a sulfonyl group such as salts thereof, etc. These compounds may be used alone or in combination of two or more.

[0023] As the compound (a3) ​​having a nonionic group, for example, compounds having an oxyethylene structure and / or an oxypropylene group, such as polyethylene glycol, polyoxypropylene glycol, polyoxyethylene polyoxypropylene glycol, polyoxyethylene polyoxytetramethylene glycol, and polyethylene glycol monomethyl ether, can be used. These compounds can be used alone or in combination of two or more.

[0024] The nonionic group possessed by the urethane resin (A) used in the present invention preferably contains oxyethylene groups and oxypropylene groups in terms of obtaining a more excellent texture and a formulated liquid stability. In terms of obtaining a more excellent texture and a formulated liquid stability by incorporating these low-crystalline components into the main chain of the urethane resin (A), it is preferably introduced via a polyol containing oxyethylene groups and oxypropylene groups, and more preferably polyoxyethylene polyoxypropylene glycol.

[0025] The number average molecular weight of the polyoxyethylene polyoxypropylene glycol is preferably in the range of 500 to 10,000, and more preferably in the range of 1,000 to 4,000, in order to obtain a more excellent texture and stability of the prepared solution. The number average molecular weight of the polyoxyethylene polyoxypropylene glycol refers to a value measured by gel permeation chromatography (GPC).

[0026] The molar ratio (EO / PO) of the oxyethylene group (EO) to the oxypropylene group (PO) in the urethane resin (A) is preferably in the range of 20 / 80 to 90 / 10, more preferably in the range of 40 / 60 to 85 / 15, in order to obtain better texture and formulation stability.

[0027] The amount of the compound (a3) ​​having a nonionic group used is preferably in the range of 0.1% by mass to 20% by mass, more preferably in the range of 0.5% by mass to 15% by mass, in the raw materials constituting the urethane resin (A) in order to obtain better hydrolysis resistance, feel and formulation stability.

[0028] Specifically, for example, the urethane resin (A) may be a reaction product of a polyol including the polycarbonate polyol (a1), the compound having an anionic group (a2), the compound having a nonionic group (a3), and a polyisocyanate (a4).

[0029] As the polyol, in addition to using the polycarbonate polyol (a1), other polyols may be used in combination within the range that does not impair the effect of the present invention. As the other polyols, polycarbonate polyols, polyester polyols, polyether polyols, polyacrylic acid polyols, etc. that are solid at room temperature can be used. These polyols can be used alone or in combination of two or more. As the number average molecular weight of these polyols, for example, the range of 500 to 100,000 can be cited. The number average molecular weight of the polyol represents a value measured by gel permeation chromatography (GPC).

[0030] The polyol may be used together with a chain extender having a number average molecular weight preferably in the range of 50 to 450, if necessary. The number average molecular weight of the chain extender refers to a value calculated from a chemical structural formula.

[0031] As the chain extender, there can be used: a chain extender having a hydroxyl group, such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 1,3-propylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, hexamethylene glycol, sucrose, methylene glycol, glycerol, sorbitol, bisphenol A, 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ether, etc.; a chain extender having an amino group, such as ethylenediamine, 1,2-propylenediamine, 1,6-hexamethylenediamine, piperazine, 2,5-dimethylpiperazine, isophoronediamine, 1,2-cyclohexanediamine, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, 4,4'-dicyclohexylmethanediamine, 3,3'-dimethyl-4,4'-dicyclohexylmethanediamine, hydrazine, etc. These chain extenders can be used alone or in combination of two or more. Among these, the chain extender having an amino group is preferred because more excellent hydrolysis resistance and light resistance can be obtained.

[0032] As the polyisocyanate (a4), for example, aromatic polyisocyanates such as phenylene diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, naphthalene diisocyanate, polymethylene polyphenyl polyisocyanate, and carbodiimidized diphenylmethane polyisocyanate can be used; aliphatic or alicyclic polyisocyanates such as hexamethylene diisocyanate, lysine diisocyanate, dimer acid diisocyanate, cyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, xylene diisocyanate, tetramethylxylene diisocyanate, and norbornene diisocyanate can be used. These polyisocyanates can be used alone or in combination of two or more. Among these, in terms of obtaining a more excellent light resistance, preferably aliphatic polyisocyanates and / or alicyclic polyisocyanates, more preferably alicyclic polyisocyanates.

[0033] Examples of the method for producing the urethane resin (A) include a method of charging the raw materials together and reacting them, etc. Examples of the method for producing the urethane resin (A) include a method of performing the reaction at a temperature of 50° C. to 100° C. for 3 to 10 hours.

[0034] When the carbamate resin (A) is produced, it is preferred to inactivate the isocyanate groups remaining in the carbamate resin (A). When the isocyanate groups are inactivated, it is preferred to use an alcohol having a hydroxyl group such as methanol. When the alcohol is used, the amount used is preferably in the range of 0.001 to 10 parts by mass relative to 100 parts by mass of the carbamate resin (A).

[0035] In addition, an organic solvent may be used when producing the urethane resin (A). As the organic solvent, for example, ketone compounds such as acetone and methyl ethyl ketone; ether compounds such as tetrahydrofuran and dioxane; acetate compounds such as ethyl acetate and butyl acetate; nitrile compounds such as acetonitrile; amide compounds such as dimethylformamide and N-methylpyrrolidone, etc. can be used. These organic solvents may be used alone or in combination of two or more. Furthermore, the organic solvent is preferably removed by distillation or the like.

[0036] The acid value of the urethane resin (A) is preferably in the range of 0.1 mgKOH / g to 15 mgKOH / g, and more preferably in the range of 1 mgKOH / g to 8 mgKOH / g, in order to obtain more excellent hydrolysis resistance, softness and hand feel. The acid value of the urethane resin (A) can be adjusted by the amount of the compound (a2) having an anionic group, and the determination method thereof is described in the Examples described below.

[0037] The weight average molecular weight of the urethane resin (A) is preferably in the range of 50,000 to 700,000, and more preferably in the range of 100,000 to 500,000, in order to obtain more excellent hydrolysis resistance, light resistance, and heat resistance. The weight average molecular weight of the urethane resin (A) refers to a value measured by gel permeation chromatography (GPC) under the following conditions.

[0038] The nonionic emulsifier (B) is an essential component in order to obtain excellent texture and stability of the prepared liquid.

[0039] As the nonionic emulsifier (B), for example, emulsifiers having oxyethylene groups such as polyoxyethylene nonylphenyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene distyrenated phenyl ether, polyoxyethylene lauryl ether, polyoxyethylene oleyl ether, polyoxyethylene stearyl ether, and polyoxyethylene sorbitan tetraoleate; emulsifiers having oxyethylene groups and oxypropylene groups such as polyoxyethylene polyoxypropylene copolymers, etc. These nonionic emulsifiers may be used alone or in combination of two or more.

[0040] Among these, it is preferred to use an emulsifier having an oxyethylene group and an oxypropylene group in terms of obtaining a more excellent feel and stability of the formulated liquid. The average number of moles of the oxyethylene group added is preferably in the range of 5 to 100, and more preferably in the range of 10 to 50. The average number of moles of the oxypropylene group added is preferably in the range of 5 to 50, and more preferably in the range of 10 to 40.

[0041] As for the cloud point of the nonionic emulsifier (B), in terms of rapidly (sharp) solidifying when heated while maintaining excellent stability of the formulated liquid and obtaining a softer feel, it is preferably in the range of 40°C to 80°C, and more preferably in the range of 50°C to 80°C. Furthermore, the cloud point of the nonionic emulsifier (B) is determined according to the following method in accordance with the book (New-Introduction to Surfactants, written by Takehiko Fujimoto, Sanyo Chemical Industries, Ltd., 1992). That is, a 5% by mass aqueous solution of the nonionic emulsifier is kept at a constant temperature for 30 minutes, and it is observed whether the nonionic emulsifier is insoluble in the solution. When the temperature rises, the temperature at which the nonionic emulsifier begins to become insoluble is set as the cloud point.

[0042] The amount of the nonionic emulsifier (B) is preferably in the range of 0.1% by mass to 10% by mass, more preferably in the range of 1% by mass to 6% by mass, relative to 100 parts by mass of the urethane resin (A) (solid content), in order to obtain a more excellent feel and stability of the prepared solution.

[0043] As the water (C), for example, ion exchange water, distilled water, etc. can be used. These waters can be used alone or in combination of two or more. As the content of the water (C), for example, the range of 30% by mass to 90% by mass in the urethane resin composition can be cited.

[0044] The urethane resin composition of the present invention contains the urethane resin (A), the nonionic emulsifier (B), and the water (C) as essential components, but other additives may be used as necessary.

[0045] As the other additives, for example, coagulants, urethanization catalysts, neutralizers, silane coupling agents, tackifiers, fillers, thixotropy imparting agents, adhesion imparting agents, waxes, heat stabilizers, light resistance stabilizers, fluorescent whitening agents, foaming agents, pigments, dyes, conductivity imparting agents, antistatic agents, moisture permeability enhancers, water repellents, oil repellents, hollow foams, flame retardants, water absorbents, moisture absorbents, deodorants, foam stabilizers, anti-caking agents, anti-hydrolysis agents, etc. These additives can be used alone or in combination of two or more.

[0046] As described above, the urethane resin composition of the present invention contains water and is environmentally friendly. In addition, the urethane resin composition has excellent hand feel and stability of the prepared liquid. Therefore, the urethane resin composition can be particularly suitably used as a resin for impregnation of a fiber substrate.

[0047] Next, the leather piece of the present invention will be described.

[0048] The leather sheet includes a coagulated product of the urethane resin composition in a fiber base material.

[0049] As the fiber substrate, for example, polyester fiber, polyethylene fiber, nylon fiber, acrylic fiber, polyurethane fiber, acetate fiber, rayon fiber, polylactic acid fiber, cotton, linen, silk, wool, glass fiber, carbon fiber, nonwoven fabrics, woven fabrics, knitted fabrics, etc. formed by blended fibers thereof, etc. can be used.

[0050] Examples of a method for producing the leather sheet include a method of impregnating the fiber base material with the urethane resin composition and then coagulating the urethane resin.

[0051] Examples of a method for impregnating the fiber base with the urethane resin aqueous dispersion include a method of directly immersing the fiber base in a tank storing the urethane resin aqueous dispersion and squeezing the fiber base using a mangle or the like.

[0052] Next, as a method for coagulating the urethane resin (A), for example, there can be mentioned a heat-sensitive coagulation method of heating the fiber base material impregnated with the urethane resin to 50° C. to 130° C., a method of treating with saturated steam (0 MPa to 0.6 MPa) at 100° C. or higher, or superheated steam at 160° C. to 190° C., etc. Thereafter, drying at 80° C. to 180° C. may be performed as necessary.

[0053] The leather sheet can be used for shoes, bags, clothing, furniture components such as chairs and sofas, automotive interior materials such as car seats and steering wheels, moisture-permeable and waterproof materials, artificial leather, abrasive materials, and core materials for felt pens.

[0054] An intermediate layer, an adhesive layer, a surface layer, a surface treatment layer, etc. may be laminated on the leather sheet as necessary.

[0055] Example

[0056] Hereinafter, the present invention will be described in more detail using examples.

[0057] [Example 1]

[0058] Under a nitrogen stream, 400 parts by mass of a room temperature liquid polycarbonate polyol ("Duranol T5652" manufactured by Asahi Kasei Corporation, number average molecular weight: 2,000, hereinafter referred to as "liquid PC (1)"), 6.6 parts by mass of dimethylol propionic acid (hereinafter referred to as "DMPA"), 32 parts by mass of polyoxyethylene polyoxypropylene glycol (number average molecular weight: 1,750, EO / PO = 50 / 50, hereinafter referred to as "EOPO (1)"), and 543 parts by mass of methyl ethyl ketone were added to a four-necked flask equipped with a stirrer, a reflux cooling tube, a thermometer, and a nitrogen blowing tube. After uniform mixing, 105 parts by mass of dicyclohexylmethane diisocyanate (hereinafter referred to as "H12MDI") were added, and then 0.1 parts by mass of bismuth octylate was added, and the mixture was reacted at 70°C for about 1 hour to obtain a methyl ethyl ketone solution of a urethane polymer. Next, 5.3 parts by mass of triethylamine and 16 parts by mass of an emulsifier of polyoxyethylene polyoxypropylene glycol (average number of moles of oxyethylene groups added: 25, average number of moles of oxypropylene groups added: 30, cloud point: 58° C., hereinafter referred to as “EOPO emulsifier (1)”) were added to the methyl ethyl ketone solution of the urethane polymer obtained by the above method and mixed, and then 846 parts by mass of ion exchange water and 20 parts by mass of isophorone diamine were added. The methyl ethyl ketone was then distilled off under reduced pressure to obtain a urethane resin composition (X-1) containing a urethane resin (A-1) (acid value of urethane resin (A-1): 5 mgKOH / g, weight average molecular weight: 240,000).

[0059] [Example 2]

[0060] Under a nitrogen stream, 400 parts by mass of a room temperature liquid polycarbonate polyol ("Duranol GE502" manufactured by Asahi Kasei Corporation, number average molecular weight: 2,000, hereinafter referred to as "liquid PC (2)"), 6.6 parts by mass of DMPA, 32 parts by mass of EOPO (1), and 543 parts by mass of methyl ethyl ketone were added to a four-necked flask equipped with a stirrer, a reflux cooling tube, a thermometer, and a nitrogen blowing tube. After uniform mixing, 105 parts by mass of H12MDI was added, followed by 0.1 parts by mass of bismuth octylate, and the mixture was reacted at 70°C for about 1 hour to obtain a methyl ethyl ketone solution of a carbamate polymer. Next, 5.3 parts by mass of triethylamine and 16 parts by mass of EOPO emulsifier (1) were added to the methyl ethyl ketone solution of the urethane polymer obtained by the above method and mixed, and then 846 parts by mass of ion exchange water and 20 parts by mass of isophorone diamine were added. Then, the methyl ethyl ketone was distilled off under reduced pressure to obtain a urethane resin composition (X-2) containing a urethane resin (A-2) (acid value of the urethane resin (A-2): 5 mgKOH / g, weight average molecular weight: 280,000).

[0061] [Example 3]

[0062] Under a nitrogen flow, 400 parts by mass of liquid PC (1), 6.6 parts by mass of DMPA, 32 parts by mass of polyoxyethylene polyoxypropylene glycol (number average molecular weight: 1,400, EO / PO=75 / 25, hereinafter referred to as "EOPO (2)") and 544 parts by mass of methyl ethyl ketone were added to a four-necked flask including a stirrer, a reflux cooling tube, a thermometer and a nitrogen blowing tube. After uniform mixing, 107 parts by mass of H12MDI was added, followed by 0.1 parts by mass of bismuth octylate, and the mixture was reacted at 70°C for about 1 hour to obtain a methyl ethyl ketone solution of a carbamate polymer. Next, 5.4 parts by mass of triethylamine and 16 parts by mass of EOPO emulsifier (1) were added to the methyl ethyl ketone solution of the urethane polymer obtained by the above method and mixed, and then 850 parts by mass of ion exchange water and 21 parts by mass of isophorone diamine were added. The methyl ethyl ketone was then distilled off under reduced pressure to obtain a urethane resin composition (X-3) containing a urethane resin (A-3) (acid value of the urethane resin (A-3): 5 mgKOH / g, weight average molecular weight: 260,000).

[0063] [Example 4]

[0064] Under a nitrogen flow, 400 parts by mass of liquid PC (1), 6.4 parts by mass of DMPA, 32 parts by mass of polyoxyethylene polyoxypropylene glycol (number average molecular weight: 3,000, EO / PO=75 / 25, hereinafter referred to as "EOPO (3)") and 540 parts by mass of methyl ethyl ketone were added to a four-necked flask including a stirrer, a reflux cooling tube, a thermometer and a nitrogen blowing tube. After uniform mixing, 102 parts by mass of H12MDI was added, followed by 0.1 parts by mass of bismuth octylate, and the mixture was reacted at 70°C for about 1 hour to obtain a methyl ethyl ketone solution of a carbamate polymer. Next, 5.2 parts by mass of triethylamine and 16 parts by mass of EOPO emulsifier (1) were added to the methyl ethyl ketone solution of the urethane polymer obtained by the above method and mixed, and then 850 parts by mass of ion exchange water and 20 parts by mass of isophorone diamine were added. The methyl ethyl ketone was then distilled off under reduced pressure to obtain a urethane resin composition (X-4) containing a urethane resin (A-4) (acid value of the urethane resin (A-4): 5 mgKOH / g, weight average molecular weight: 300,000).

[0065] [Example 5]

[0066] Under a nitrogen flow, 400 parts by mass of liquid PC (1), 6.6 parts by mass of DMPA, 32 parts by mass of EOPO (1) and 544 parts by mass of methyl ethyl ketone were added to a four-necked flask including a stirrer, a reflux cooling tube, a thermometer and a nitrogen blowing tube. After uniform mixing, 105 parts by mass of H12MDI was added, followed by 0.1 parts by mass of bismuth octylate, and the mixture was reacted at 70° C. for about 1 hour to obtain a methyl ethyl ketone solution of a carbamate polymer. Next, 5.3 parts by mass of triethylamine and 16 parts by mass of an emulsifier of polyoxyethylene polyoxypropylene glycol (average number of moles of oxyethylene group added: 20, average number of moles of oxypropylene group added: 20, cloud point: 70°C, hereinafter referred to as "EOPO emulsifier (2)") were added to the methyl ethyl ketone solution of the urethane polymer obtained by the above method and mixed, and then 846 parts by mass of ion exchange water and 20 parts by mass of isophorone diamine were added. The methyl ethyl ketone was then distilled off under reduced pressure to obtain a urethane resin composition (X-5) containing a urethane resin (A-5) (acid value of urethane resin (A-5): 5 mgKOH / g, weight average molecular weight: 250,000).

[0067] [Example 6]

[0068] Under a nitrogen flow, 400 parts by mass of liquid PC (1), 6.4 parts by mass of DMPA, 32 parts by mass of EOPO (1) and 535 parts by mass of methyl ethyl ketone were added to a four-necked flask equipped with a stirrer, a reflux cooling tube, a thermometer and a nitrogen blowing tube. After uniform mixing, 52 parts by mass of H12MDI and 44 parts by mass of isophorone diisocyanate (hereinafter referred to as "IPDI") were added, followed by 0.1 parts by mass of bismuth octylate. The mixture was reacted at 70° C. for about 1 hour to obtain a methyl ethyl ketone solution of a carbamate polymer. Next, 5.2 parts by mass of triethylamine and 16 parts by mass of EOPO emulsifier (1) were added to the methyl ethyl ketone solution of the urethane polymer obtained by the above method and mixed, and then 833 parts by mass of ion exchange water and 20 parts by mass of isophorone diamine were added. Then, the methyl ethyl ketone was distilled off under reduced pressure to obtain a urethane resin composition (X-6) containing a urethane resin (A-6) (acid value of the urethane resin (A-6): 5 mgKOH / g, weight average molecular weight: 180,000).

[0069] [Comparative Example 1]

[0070] In Example 1, except that a room temperature solid polycarbonate polyol ("ETERNACOLL UH-200" manufactured by Ube Industries, Ltd., number average molecular weight: 2,000, hereinafter referred to as "solid PC") was used instead of liquid PC (1), the same procedure as in Example 1 was carried out to obtain a urethane resin composition (XR-1) containing a urethane resin (AR-1).

[0071] [Comparative Example 2]

[0072] Under a nitrogen flow, 400 parts by mass of liquid PC (1), 6.6 parts by mass of DMPA, 32 parts by mass of EOPO (1), 4 parts by mass of trimethylolpropane (hereinafter referred to as "TMP") and 565 parts by mass of methyl ethyl ketone were added to a four-necked flask including a stirrer, a reflux cooling tube, a thermometer and a nitrogen blowing tube. After uniform mixing, 122 parts by mass of H12MDI was added, followed by 0.1 parts by mass of bismuth octylate, and the mixture was reacted at 70° C. for about 1 hour to obtain a methyl ethyl ketone solution of a carbamate polymer. Next, 5.3 parts by mass of triethylamine and 16 parts by mass of EOPO emulsifier (1) were added to the methyl ethyl ketone solution of the urethane polymer obtained by the above method and mixed, and then 883 parts by mass of ion exchange water and 24 parts by mass of isophorone diamine were added. The methyl ethyl ketone was then distilled off under reduced pressure to obtain a urethane resin composition (XR-2) containing a urethane resin (AR-2) (acid value of the urethane resin (AR-2): 5 mgKOH / g, weight average molecular weight: 290,000).

[0073] [Comparative Example 3]

[0074] Under nitrogen flow, 400 parts by mass of liquid PC (1), 32 parts by mass of EOPO (1), and 518 parts by mass of methyl ethyl ketone were added to a four-necked flask equipped with a stirrer, a reflux cooling tube, a thermometer, and a nitrogen blowing tube. After uniform mixing, 86 parts by mass of H12MDI were added, followed by 0.1 parts by mass of bismuth octylate, and the mixture was reacted at 70°C for about 1 hour to obtain a methyl ethyl ketone solution of a urethane polymer. Subsequently, 16 parts by mass of EOPO emulsifier (1) was added to the methyl ethyl ketone solution of a urethane polymer obtained by the above method, and the mixture was mixed. Then, 802 parts by mass of ion exchange water and 17 parts by mass of isophorone diamine were added, and the methyl ethyl ketone was distilled off under reduced pressure to obtain a urethane resin composition (XR-3) containing a urethane resin (AR-3) (acid value of urethane resin (AR-3): 0 mgKOH / g, weight average molecular weight: 280,000).

[0075] [Comparative Example 4]

[0076] Under nitrogen flow, 400 parts by mass of liquid PC (1), 6.6 parts by mass of DMPA, and 504 parts by mass of methyl ethyl ketone were added to a four-necked flask equipped with a stirrer, a reflux cooling tube, a thermometer, and a nitrogen blowing tube. After uniform mixing, 98 parts by mass of H12MDI were added, followed by 0.1 parts by mass of bismuth octylate, and the mixture was reacted at 70°C for about 1 hour to obtain a methyl ethyl ketone solution of a urethane polymer. Subsequently, 6 parts by mass of triethylamine and 16 parts by mass of EOPO emulsifier (1) were added to the methyl ethyl ketone solution of the urethane polymer obtained by the above method, and the mixture was mixed. Then, 785 parts by mass of ion exchange water and 19 parts by mass of isophorone diamine were added, and the methyl ethyl ketone was distilled off under reduced pressure to obtain a urethane resin composition (XR-4) containing a urethane resin (AR-4) (acid value of urethane resin (AR-4): 5 mgKOH / g, weight average molecular weight: 310,000).

[0077] [Comparative Example 5]

[0078] In Example 1, a urethane resin composition (XR-5) containing a urethane resin (AR-5) was obtained in the same manner as in Example 1 except that the EOPO emulsifier (1) was not used.

[0079] [Method for measuring number average molecular weight and weight average molecular weight]

[0080] The number average molecular weight of the polyol and the weight average molecular weight of the urethane resin used in the examples and comparative examples are values ​​measured by gel permeation chromatography (GPC) under the following conditions.

[0081] Measuring device: High-speed GPC device ("HLC-8220GPC" manufactured by Tosoh Corporation)

[0082] Column: The following columns manufactured by Tosoh Corporation were connected in series and used.

[0083] "TSKgel G5000" (7.8mm I.D. × 30cm) × 1 piece

[0084] "TSKgel G4000" (7.8mm I.D. × 30cm) × 1 piece

[0085] "TSKgel G3000" (7.8mm I.D. × 30cm) × 1 piece

[0086] "TSKgel G2000" (7.8mm I.D. × 30cm) × 1 piece

[0087] Detector: RI (differential refractometer)

[0088] Column temperature: 40℃

[0089] Eluent: tetrahydrofuran (THF)

[0090] Flow rate: 1.0mL / min

[0091] Injection volume: 100 μL (sample concentration is 0.4 mass% tetrahydrofuran solution)

[0092] Standard sample: The following standard polystyrene was used to prepare a standard curve.

[0093] (Standard Polystyrene)

[0094] "TSKgel Standard Polystyrene A-500" manufactured by Tosoh Corporation

[0095] "TSKgel Standard Polystyrene A-1000" manufactured by Tosoh Corporation

[0096] "TSKgel Standard Polystyrene A-2500" manufactured by Tosoh Corporation

[0097] "TSKgel Standard Polystyrene A-5000" manufactured by Tosoh Corporation

[0098] "TSKgel Standard Polystyrene F-1" manufactured by Tosoh Corporation

[0099] "TSKgel Standard Polystyrene F-2" manufactured by Tosoh Corporation

[0100] "TSKgel Standard Polystyrene F-4" manufactured by Tosoh Corporation

[0101] "TSKgel Standard Polystyrene F-10" manufactured by Tosoh Corporation

[0102] "TSKgel Standard Polystyrene F-20" manufactured by Tosoh Corporation

[0103] "TSKgel Standard Polystyrene F-40" manufactured by Tosoh Corporation

[0104] "TSKgel Standard Polystyrene F-80" manufactured by Tosoh Corporation

[0105] "TSKgel Standard Polystyrene F-128" manufactured by Tosoh Corporation

[0106] "TSKgel Standard Polystyrene F-288" manufactured by Tosoh Corporation

[0107] "TSKgel Standard Polystyrene F-550" manufactured by Tosoh Corporation

[0108] [Method for measuring the acid value of urethane resin (A)]

[0109] The urethane resin composition obtained in the examples and comparative examples was dried, and 0.05 g to 0.5 g of the dried and solidified resin particles were weighed into a 300 mL conical flask. Then, about 80 mL of a mixed solvent having a mass ratio of tetrahydrofuran to ion exchange water [tetrahydrofuran / ion exchange water] of 80 / 20 was added to obtain a mixed solution.

[0110] Next, after mixing the phenolphthalein indicator in the mixed solution, titration is performed using a pre-calibrated 0.1 mol / L potassium hydroxide aqueous solution. The acid value (mgKOH / g) of the anionic urethane resin (X) is calculated based on the amount of the potassium hydroxide aqueous solution used in the titration and the following calculation formula (1).

[0111] In the calculation formula A = (B × f × 5.611) / S (1), A is the solid acid value of the resin (mgKOH / g), B is the amount of 0.1 mol / L potassium hydroxide aqueous solution used for titration (mL), f is the factor of 0.1 mol / L potassium hydroxide aqueous solution, S is the mass of the resin particles (g), and 5.611 is the formula weight of potassium hydroxide (56.11 / 10).

[0112] [Evaluation method of prepared liquid stability]

[0113] The urethane resin compositions obtained in the examples and comparative examples were diluted with water to a solid content of 20% by mass, and 1 part by mass of sodium chloride was added to 100 parts by mass of the prepared solution to obtain a prepared solution. The prepared solution was allowed to stand at 40° C. for 1 week and evaluated as follows.

[0114] “A”: No change in appearance.

[0115] "B": A slight amount of precipitate was observed.

[0116] "C": A large amount of precipitate was confirmed.

[0117] [Method for producing impregnated nonwoven fabric]

[0118] The urethane resin compositions obtained in the examples and comparative examples were diluted with water so that the solid content was 20% by mass, and 1 part by mass of sodium chloride was added to 100 parts by mass of the prepared solution to obtain a prepared solution. The prepared solution was impregnated into a polyester fiber containing 200 g / m 2 The nonwoven fabric was squeezed by a roller so that the pickup rate (pickup) was 100%. Then, it was left to stand in saturated steam at 100°C for 2 minutes and dried in a dryer at 100°C for 20 minutes to prepare an impregnated nonwoven fabric (leather sheet).

[0119] [Evaluation method of hand feel]

[0120] The obtained impregnated nonwoven fabric was evaluated by touch as follows.

[0121] "A": Soft and supple.

[0122] "B": has a little softness.

[0123] "C": Poor softness.

[0124] [Evaluation method of light resistance]

[0125] The obtained impregnated nonwoven fabric was irradiated with 110 MJ of light under the conditions of 89° C. and 50% humidity using a xenon fade meter (“SX75P” manufactured by Gas Test Instruments Co., Ltd.) and evaluated visually as follows.

[0126] “A”: No change in appearance.

[0127] "B": Slight yellowing occurs.

[0128] "C": intense yellowing occurs.

[0129] [Evaluation method of hydrolysis resistance]

[0130] The obtained impregnated nonwoven fabric was cured under moist heat conditions of 70° C. and 95% humidity for 5 weeks and evaluated by visual inspection as follows.

[0131] “A”: No change in appearance.

[0132] "B": The appearance has a gloss change.

[0133] "C": Glossiness changes and stickiness occurs in the appearance.

[0134] [Table 1]

[0135]

[0136] [Table 2]

[0137]

[0138] [Table 3]

[0139]

[0140] It was found that the prepared liquids of Examples 1 to 6, which are the urethane resin compositions of the present invention, are excellent in stability, feel, light resistance, and hydrolysis resistance.

[0141] On the other hand, Comparative Example 1 is a form in which a room temperature solid polycarbonate polyol was used instead of the polycarbonate polyol (a1), and the texture was poor.

[0142] Comparative Example 2 is a form using trimethylolpropane having three hydroxyl groups as a raw material, and the texture is poor.

[0143] Comparative Example 3 is a form using a urethane resin having no anionic group, and the stability of the prepared solution is poor.

[0144] Comparative Example 4 is a form using a urethane resin having no nonionic group, and the texture and the stability of the prepared solution are poor.

[0145] Comparative Example 5 is a form in which the nonionic emulsifier (B) is not used, and the texture and the stability of the prepared liquid are poor.

Claims

1. A urethane resin composition, characterized in that The invention comprises: a urethane resin (A) having an anionic group and a nonionic group, a nonionic emulsifier (B) and water (C), wherein the urethane resin (A) is made of a polycarbonate polyol (a1) which is liquid at room temperature and does not contain a compound (x2) having three or more hydroxyl groups as a raw material, The nonionic groups in the urethane resin (A) include oxyethylene groups and oxypropylene groups. The molar ratio EO / PO of the oxyethylene group and the oxypropylene group in the urethane resin (A) is in the range of 20 / 80 to 90 / 10.

2. The urethane resin composition according to claim 1, wherein The oxyethylene group and the oxypropylene group are derived from a polyol having an oxyethylene group and an oxypropylene group.

3. The urethane resin composition according to claim 1 or 2, wherein The nonionic emulsifier (B) has an oxyethylene group and an oxypropylene group.

4. A leather piece, characterized in that: A coagulant of the urethane resin composition according to any one of claims 1 to 3 is present in a fiber base material.

Citation Information

Patent Citations

  • Aqueous polyurethane resin dispersion composition for surface skin layer of fibrous laminate material, method for producing fibrous laminate material and synthetic leather

    JP2007119749A

  • Sheet-like article

    CN105745375A