Optical laminate and display device
By adjusting the stress-strain curve characteristics of the adhesive layer, the problem of bubbles generated when the optical laminate is bent is solved and its bending durability is improved.
Patent Information
- Application Number
- CN202080079516.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-16
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-10-16
AI Technical Summary
When the optical laminate is bent, air bubbles are easily generated in the adhesive layer or between the adhesive layer and the connecting layer, causing floating or peeling between the layers, affecting the bending durability of the optical laminate.
By adjusting the stress-strain curve slope, stress relaxation rate, creep rate and deformation recovery rate of the first and second adhesive layers, the GL1' of the first adhesive layer and the GL2' of the second adhesive layer are ensured. Between 20≤GL1'≤150 and 20≤GL2'≤150, and satisfy GL1'
It effectively suppresses the generation of bubbles in and between the adhesive layers during bending, improves the static bending durability of the optical laminate, and ensures that no bubbles will float or peel within 24 hours.
Smart Images

Figure CN114730037B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an optical laminate and a display device. Background Art
[0002] Japanese Patent Application Publication No. 2018-027995 (Patent Document 1) describes a flexible image display device including a pressure-sensitive adhesive layer having excellent stress relaxation properties.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2018-027995 Summary of the invention
[0006] An optical laminate in which a plurality of layers are laminated with a pressure-sensitive adhesive layer interposed therebetween has a problem in that bubbles are easily generated in the pressure-sensitive adhesive layer or between the pressure-sensitive adhesive layer and a layer in contact with the pressure-sensitive adhesive layer when bent.
[0007] An object of the present invention is to provide an optical layered body that suppresses the generation of bubbles when bent, and a display device including the optical layered body.
[0008] The present invention provides the optical layered body and display device exemplified below.
[0009] [1] An optical laminate comprising, in this order, a front plate, a first pressure-sensitive adhesive layer, a polarizing plate, a second pressure-sensitive adhesive layer, and a back plate;
[0010] The slopes from the origin to the maximum stress value in the stress [Pa]-strain [%) curves of the first adhesive layer and the second adhesive layer are respectively defined as G L1 ' and G L2 ', the following equations (1) and (2) are satisfied:
[0011] 20≤G L1 '≤150 (1)
[0012] 20≤G L2 '≤150 (2).
[0013] [2] The optical layered body according to [1], further satisfying the following formula (3):
[0014] G L1 '<G L2 ' (3).
[0015] [3] The optical laminate according to [1] or [2], wherein the stress relaxation rate of the first pressure-sensitive adhesive layer satisfies the following formula (4) when σ1 is used:
[0016] 0.20≤σ1≤0.70 (4).
[0017] [4] The optical laminate according to [3], wherein the stress relaxation rate of the second pressure-sensitive adhesive layer satisfies the following formula (5) when σ2 is set:
[0018] σ1<σ2 (5).
[0019] [5] The optical layered body according to any one of [1] to [4], wherein the first pressure-sensitive adhesive layer satisfies the following formula (6) when the creep rate of the first pressure-sensitive adhesive layer is ε1 (%):
[0020] 1.5≤ε1≤20 (6).
[0021] [6] The optical laminate according to [5], wherein when the creep rate of the second adhesive layer is ε2〔%〕, the following formula (7) is satisfied:
[0022] ε1>ε2 (7).
[0023] [7] The optical laminate according to any one of [1] to [6], wherein the first pressure-sensitive adhesive layer satisfies the following formula (8) when the deformation recovery rate is R1 (%):
[0024] 2.5≤R1≤20 (8).
[0025] [8] The optical laminate according to [7], wherein the deformation recovery rate of the second pressure-sensitive adhesive layer is R2 (%), and satisfies the following formula (9):
[0026] R1<R2 (9).
[0027] [9] The optical layered body according to any one of [1] to [8], wherein the glass transition temperatures of the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer are respectively -70°C to -40°C.
[0028]
[10] A display device comprising the optical layered body according to any one of [1] to [9].
[0029]
[11] The display device according to
[10] , wherein the display device can be bent with the front panel side as the inner side.
[0030] According to the present invention, there are provided an optical layered body that suppresses generation of bubbles when bent, and a display device including the optical layered body. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic cross-sectional view showing an example of the optical layered body of the present invention.
[0032] Figure 2 This is a schematic diagram for explaining a method for measuring parameters using a dynamic mechanical analyzer.
[0033] Figure 3 This is a schematic diagram for explaining a static bending durability test. DETAILED DESCRIPTION
[0034] Hereinafter, the embodiments of the optical laminate of the present invention will be described with reference to the accompanying drawings, but the present invention is not limited to the following embodiments. In all the following drawings, in order to make each component easy to understand, the scale is appropriately adjusted and shown, and the scale of each component shown in the drawings is not necessarily consistent with the scale of the actual component.
[0035] <Optical laminate>
[0036] Figure 1 This is a schematic cross-sectional view of an optical layered body according to one embodiment of the present invention. Figure 1 The optical laminate 100 shown includes a front plate 101, a first pressure-sensitive adhesive layer 102, a polarizing plate 103, a second pressure-sensitive adhesive layer 104, and a rear plate 105 in this order. Hereinafter, the first pressure-sensitive adhesive layer 102 and the second pressure-sensitive adhesive layer 104 may be collectively referred to as pressure-sensitive adhesive layers.
[0037] The thickness of the optical layered body 100 varies depending on the function required for the optical layered body and the application of the optical layered body, and is not particularly limited, but is, for example, 30 to 3000 μm, preferably 50 to 2000 μm, and more preferably 70 to 1000 μm.
[0038] The top view shape of the optical stack 100 can be, for example, a square shape, preferably a square shape with long sides and short sides, and more preferably a rectangle. When the shape of the surface direction of the optical stack 100 is a rectangle, the length of the long side can be, for example, 10 mm to 1400 mm, preferably 50 mm to 600 mm. The length of the short side is, for example, 5 mm to 800 mm, preferably 30 mm to 500 mm, and more preferably 50 mm to 300 mm. Each layer constituting the optical stack 100 can be R-processed at the corners, or the ends can be notched, or the holes can be opened.
[0039] The optical laminate 100 can be used in, for example, a display device, etc. The display device is not particularly limited, and examples thereof include an organic electroluminescent (organic EL) display device, an inorganic electroluminescent (inorganic EL) display device, a liquid crystal display device, an electroluminescent display device, etc. The optical laminate 100 is suitable for a bendable display device.
[0040] [The slope from the origin to the maximum stress value G L ']
[0041] The slopes from the origin to the maximum stress value in the stress [Pa]-strain [%) curves of the first adhesive layer 102 and the second adhesive layer 104 are respectively defined as G L1 ' and G L2 ', the optical laminate 100 satisfies the following formula (1) and formula (2):
[0042] 20≤G L1 '≤150 (1)
[0043] 20≤G L2 '≤150 (2)
[0044] Preferably, the following formulas (1a) and (2a) are satisfied:
[0045] 25≤G L1 '≤95 (1a)
[0046] 25≤G L2 '≤95 (2a).
[0047] When the adhesive layer is subjected to a tensile test, a stress-strain curve can be drawn with strain as the horizontal axis and stress as the vertical axis. Generally, as the strain increases, the stress generated in the adhesive layer also increases, and the stress reaches its maximum value just before the cohesive failure of the adhesive layer. The slope G from the origin to the maximum stress value in the stress-strain curve of the adhesive layer is L 'It is expressed by (maximum stress value [Pa]) / (strain when stress reaches maximum [%). L 'It reflects not only the stress change when the adhesive layer undergoes elastic strain, but also the stress change until plastic strain occurs, and can be used as an indicator of the durability of the adhesive layer before cohesive failure. L When ' is larger, the stress generated by the adhesive layer relative to the strain is larger, and the cohesive force of the adhesive layer is excellent. L When ' is small, the stress generated by the adhesive layer relative to the strain is small, and the adhesive layer is easy to deform. L ' can be obtained according to the method described in the Example column described later.
[0048] The optical laminate 100 satisfying formula (1) and formula (2) can suppress the generation of bubbles in the adhesive layer and between the adhesive layer and the layer connected to the adhesive layer even if it is kept in a bent state (hereinafter referred to as "static bending"). Here, suppressing the generation of bubbles during static bending means that no bubbles are generated within 24 hours even if the optical laminate is subjected to the static bending durability test described later. At this time, the generation of floating or peeling between the adhesive layer and the layer connected to the adhesive layer is also suppressed. The generation of bubbles can be judged by observation under an optical microscope.
[0049] In this specification, bending includes a bending form in which a curved surface is formed in the bending portion, and the curvature radius of the inner surface of the bending is not particularly limited. In addition, bending also includes bending in which the bending angle of the inner surface is greater than 0 degrees and less than 180 degrees, and folding in which the curvature radius of the inner surface is close to zero or the bending angle of the inner surface is 0 degrees.
[0050] G L 'The desired numerical range can be achieved by adjusting the type and amount of monomers of the base polymer contained in the adhesive composition used to form the adhesive layer; the type and amount of polymerization initiator, crosslinking agent and other additives; active energy rays, heat and other important factors that change the degree of crosslinking. For example, when the base polymer contained in the adhesive composition contains many long-chain alkyl (meth) acrylate monomers with more than 10 carbon atoms, G L 'There is a tendency to become smaller. For example, when the adhesive composition contains many polymerizable compounds, G L 'There is a tendency to get bigger.
[0051] The optical layered body 100 preferably satisfies the following formula (3):
[0052] G L1 '<G L2 ' (3)
[0053] When the optical stack 100 that satisfies formula (3) is statically bent with the front panel 101 on the inner side, the adhesive layer on the inner diameter side further alleviates the stress generated on the inner diameter side of the optical stack 100, so it is easy to bend. The generation of bubbles in the adhesive layer and between the adhesive layer and the layer connected to the adhesive layer is suppressed, which can improve the bending durability of the optical stack 100.
[0054] [Stress relaxation rate σ]
[0055] When the stress relaxation rate of the first pressure-sensitive adhesive layer 102 is σ1, the optical laminate 100 preferably satisfies the following formula (4):
[0056] 0.20≤σ1≤0.70 (4)
[0057] More preferably, the following formula (4a) is satisfied:
[0058] 0.20≤σ1≤0.55 (4a).
[0059] When the stress relaxation rate of the second pressure-sensitive adhesive layer 104 is σ2, the optical laminate 100 preferably satisfies the following formula (4′):
[0060] 0.20≤σ2≤0.70 (4')
[0061] More preferably, the following formula (4'a) is satisfied:
[0062] 0.20≤σ2≤0.55 (4'a).
[0063] The stress relaxation rate of the adhesive layer is represented by the ratio of the stress after the specified time when the adhesive layer is subjected to the tensile test to the stress generated just after the stretching. When the stress relaxation rate is small, the stress generated by the adhesive layer is easily relaxed. When the stress relaxation rate of the adhesive layer is within the above range, the optical laminate 100 is not easy to generate bubbles in the adhesive layer even if it is statically bent. In addition, the adhesion of the adhesive layer to the layer connected to the adhesive layer is also excellent, so the generation of bubbles between the adhesive layers is also suppressed. The stress relaxation rate can be obtained according to the method described in the embodiment column described later.
[0064] The optical layered body 100 preferably satisfies the following formula (5):
[0065] σ1<σ2 (5).
[0066] When the optical stack 100 satisfying formula (5) is statically bent with the front panel 101 on the inner side, the first adhesive layer 102 further alleviates the stress generated on the inner diameter side of the optical stack, so it is easy to bend, and the generation of bubbles in the adhesive layer and between the adhesive layer and the layer connected to the adhesive layer is easily suppressed.
[0067] [Creep rate ε]
[0068] When the creep rate of the first pressure-sensitive adhesive layer 102 is ε1〔%〕, the optical laminate 100 preferably satisfies the following formula (6):
[0069] 1.5≤ε1≤20 (6)
[0070] More preferably, the following formula (6a) is satisfied:
[0071] 3.0≤ε1≤10 (6a).
[0072] When the creep rate of the second pressure-sensitive adhesive layer 104 is ε2〔%〕, the optical laminate 100 preferably satisfies the following formula (6'):
[0073] 1.5≤ε2≤20 (6')
[0074] More preferably, the following formula (6'a) is satisfied:
[0075] 3.0≤ε2≤10 (6'a).
[0076] The creep rate of the adhesive layer is the maximum deformation rate when the adhesive layer is stretched for a certain time with a certain force. When the creep rate is large, the adhesive layer is easily deformed. When the creep rate of the adhesive layer is within the above range, it is not easy to generate bubbles in the adhesive layer even if the optical laminate 100 is statically bent. In addition, the adhesive layer and the layer connected to the adhesive layer are also excellent in adhesion, so the generation of bubbles between the layers is also suppressed. The creep rate can be obtained according to the method described in the embodiment column described later.
[0077] The optical layered body 100 preferably satisfies the following formula (7):
[0078] ε1>ε2 (7).
[0079] When the optical stack 100 satisfying formula (7) is statically bent with the front panel 101 on the inner side, the first adhesive layer 102 further alleviates the stress generated on the inner diameter side of the optical stack, so it is easy to bend, and the generation of bubbles in the adhesive layer and between the adhesive layer and the layer connected to the adhesive layer is easily suppressed.
[0080] [Deformation recovery rate R]
[0081] When the deformation recovery rate of the first pressure-sensitive adhesive layer 102 is defined as R1 (%), the optical laminate 100 preferably satisfies the following formula (8):
[0082] 2.5≤R1≤20 (8)
[0083] More preferably, the following formula (8a) is satisfied:
[0084] 3.0≤R1≤10 (8a).
[0085] When the deformation recovery rate of the second pressure-sensitive adhesive layer 104 is defined as R2 (%), the optical laminate 100 preferably satisfies the following formula (8'):
[0086] 2.5≤R2≤20 (8')
[0087] More preferably, the following formula (8'a) is satisfied:
[0088] 3.0≤R2≤10 (8'a).
[0089] The deformation recovery rate of the adhesive layer represents the ratio of the adhesive layer to shrink after a specified time from the removal of the load in the tensile test of the adhesive layer. When the deformation recovery rate is large, the shrinkage of the adhesive layer after stretching is excellent. When the deformation recovery rate of the adhesive layer is within the above range, it is not easy to generate bubbles in the adhesive layer even if the optical laminate 100 is statically bent. In addition, the adhesion between the adhesive layer and the layer connected to the adhesive layer is also excellent, so the generation of bubbles between the layers is also suppressed. The deformation recovery rate can be obtained according to the method described in the embodiment column described later.
[0090] The optical layered body 100 preferably satisfies the following formula (9):
[0091] R1<R2 (9).
[0092] When the optical stack 100 satisfying formula (9) is statically bent with the front panel 101 on the inner side, the second adhesive layer 104 further alleviates the stress generated on the outer diameter side of the optical stack 100, so it is easy to bend, and the generation of bubbles in the adhesive layer and between the adhesive layer and the layer connected to the adhesive layer is easily suppressed.
[0093] The stress relaxation rate, creep rate and deformation recovery rate of the adhesive layer can be achieved within the desired numerical range by adjusting the type and amount of monomers of the base polymer contained in the adhesive composition used to constitute the adhesive layer; the type and amount of polymerization initiator, cross-linking agent and other additives; active energy rays, heat and other important factors that change the degree of cross-linking, etc.
[0094] [Glass transition temperature]
[0095] In the optical laminate 100, the glass transition temperatures of the first adhesive layer and the second adhesive layer are preferably -70°C to -40°C, respectively. When the glass transition temperature of the adhesive layer is -40°C or less, the flexibility of the adhesive layer is good, so the optical laminate 100 can be easily bent. When the glass transition temperature of the adhesive layer is lower than -70°C, the cohesive force of the adhesive layer becomes low, and the adhesive force under the durable condition is reduced. The glass transition temperature of the adhesive layer can be measured according to the method described in the column of the examples described later.
[0096] The glass transition temperature of the adhesive layer can be adjusted to the desired range by adjusting the type and amount of monomers constituting the base polymer contained in the adhesive composition; the type and amount of polymerization initiators, crosslinking agents and other additives; active energy rays, heat and other important factors that change the degree of crosslinking. In order to make the glass transition temperature of the adhesive layer below -40°C, the base polymer contained in the adhesive composition is preferably mixed with an acrylic monomer having a glass transition temperature of below -40°C, preferably below -45°C, and more preferably below -50°C as a homopolymer. As such a monomer, for example, n-butyl acrylate (T g :-55℃)、n-octyl acrylate(T g :-65℃)、2-ethylhexyl acrylate(T g :-58℃)、2-ethylhexyl acrylate(T g :-70℃)、propylene isononyl ester (T g :-58℃)、Isodecyl acrylate(T g:-60℃)、Isodecyl methacrylate (T g :-41℃)、n-lauryl methacrylate (T g :-65℃)、Tridecyl acrylate (T g :-55℃)、Tridecyl methacrylate (T g : -40°C), preferably n-butyl acrylate and 2-ethylhexyl acrylate. These monomers may be used alone or in combination of two or more.
[0097] The base polymer contained in the adhesive composition preferably contains 80% by mass or more, more preferably 85% by mass or more, and further preferably 95% by mass or more of a monomer having a glass transition temperature of -40°C or less as a homopolymer. In addition, the base polymer contained in the adhesive composition preferably contains 99.9% by mass or less, more preferably 99.5% by mass or less, and further preferably 99% by mass or less of a monomer having a glass transition temperature of -40°C or less as a homopolymer. When the content of the monomer having a glass transition temperature of -40°C or less as a homopolymer is within such a range, the glass transition temperature of the adhesive layer is likely to fall within the above range.
[0098] In order to easily set the glass transition temperature of the adhesive layer within the above range, the base polymer contained in the adhesive composition preferably contains as little monomer as a homopolymer having a glass transition temperature exceeding 0°C as possible, and the upper limit of such monomer is preferably 15% by mass or less, more preferably 10% by mass or less, and further preferably 5% by mass or less.
[0099] [Front panel]
[0100] As long as the front panel 101 is a plate-like body that can transmit light, the material and thickness are not limited. The front panel can be composed of only one layer, or it can be composed of more than two layers. As the front panel 101, a plate-like body made of resin (such as a resin plate, a resin sheet, a resin film, etc.), a plate-like body made of glass (such as a glass plate, a glass film, etc.) can be cited. The front panel can also be a laminate of a plate-like body made of resin and a plate-like body made of glass. The front panel 101 can constitute the outermost surface of the display device.
[0101] The thickness of the front panel 101 may be, for example, 10 μm to 300 μm, preferably 20 μm to 200 μm, and more preferably 30 μm to 100 μm. In the present invention, the thickness of each layer constituting the optical layered body 100 can be measured by the thickness measuring method described in the examples below.
[0102] When the front panel 101 is a plate-like body made of resin, the plate-like body made of resin is not limited as long as it is a plate-like body that can transmit light. As the resin constituting the plate-like body made of resin, for example, triacetyl cellulose, acetyl cellulose butyrate, ethylene-vinyl acetate copolymer, propionyl cellulose, butyryl cellulose, acetyl propionyl cellulose, polyester, polystyrene, polyamide, polyetherimide, poly(methyl)acrylic acid, polyimide, polyether sulfone, polysulfone, polyethylene, polypropylene, polymethylpentene, polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, polyvinyl acetal, polyether ketone, polyether ether ketone, polyether sulfone, polymethyl methacrylate, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polycarbonate, polyamide-imide and other macromolecules can be cited. These macromolecules can be used alone or in combination of two or more. From the viewpoint of improving strength and transparency, the resin plate-like body is preferably a resin film formed of a polymer such as polyimide, polyamide, or polyamideimide.
[0103] From the viewpoint of improving hardness, the front panel 101 can be a resin film with a hard coating. The hard coating can be formed on one side of the resin film or on both sides. The hardness and scratch resistance can be improved by providing a hard coating. The hard coating is, for example, a cured layer of an ultraviolet curable resin. As ultraviolet curable resins, for example, acrylic resins, silicone resins, polyester resins, polyurethane resins, amide resins, epoxy resins, etc. can be cited. In order to improve the hardness, the hard coating can also include additives. The additives are not particularly limited, and inorganic particles, organic particles or mixtures thereof can be cited. When the two sides of the resin film have hard coatings, the composition and thickness of each hard coating can be the same as or different from each other.
[0104] When the front panel 101 is a glass plate, it is preferable to use tempered glass for display. The thickness of the glass plate may be, for example, 10 μm to 1000 μm, or 20 μm to 500 μm. The use of a glass plate can provide the front panel 101 with excellent mechanical strength and surface hardness.
[0105] When the optical laminate 100 is used in a display device, the front panel 101 not only has the function of protecting the front surface (screen) of the display device (function as a window film), but also has the function of a touch sensor, a blue light cutoff function, a viewing angle adjustment function, etc.
[0106] [First adhesive layer]
[0107] The first adhesive layer 102 is interposed between the front panel 101 and the polarizing plate 103 to bond them together. The first adhesive layer 102 may be a single layer or may be composed of two or more layers, but is preferably a single layer.
[0108] The first adhesive layer 102 may be composed of an adhesive composition having a (meth) acrylic resin, a rubber resin, a polyurethane resin, an ester resin, a silicone resin, or a polyvinyl ether resin as a main component (base polymer). As the adhesive composition constituting the first adhesive layer 102, an adhesive composition having a (meth) acrylic resin having excellent transparency, weather resistance, heat resistance, etc. as a base polymer is suitable. The adhesive composition may be an active energy ray curable type or a thermosetting type.
[0109] As the (meth)acrylic resin used in the adhesive composition, a polymer or copolymer using one or more of (meth)acrylic acid esters such as butyl (meth)acrylate, ethyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate as monomers is appropriately used. It is preferred to copolymerize a polar monomer with the base polymer. As polar monomers, monomers having carboxyl groups, hydroxyl groups, amide groups, amino groups, epoxy groups, etc., such as (meth)acrylic acid compounds, 2-hydroxypropyl (meth)acrylate compounds, hydroxyethyl (meth)acrylate compounds, (meth)acrylamide compounds, N,N-dimethylaminoethyl (meth)acrylate compounds, and glycidyl (meth)acrylate compounds can be cited. As a monomer constituting the (meth)acrylic resin, a photoreactive compound having a benzoyl group can also be used, and the compound described as Chemical Formula 1 in Korean Patent Publication No. 10-2019-0005427 can be exemplified. Such a photoreactive compound can improve durability by inducing additional crosslinking due to activation by additional photocuring.
[0110] The adhesive composition may only contain the above-mentioned base polymer, but usually further contains a crosslinking agent. Examples of the crosslinking agent include metal ions having a valence of more than two and forming a carboxylic acid metal salt with a carboxyl group, polyamine compounds forming an amide bond with a carboxyl group, polyepoxide compounds or polyols forming an ester bond with a carboxyl group, and polyisocyanate compounds forming an amide bond with a carboxyl group. The crosslinking agent is preferably a polyisocyanate compound.
[0111] The active energy ray-curable adhesive composition has the property of being cured by being irradiated with active energy rays such as ultraviolet rays and electron beams, and has the property of being able to have adhesiveness and be closely attached to a covering such as a film before being irradiated with active energy rays, and being able to be cured by irradiation with active energy rays to adjust the adhesion. The active energy ray-curable adhesive composition is preferably an ultraviolet curable type. In addition to the base polymer and the crosslinking agent, the active energy ray-curable adhesive composition further contains an active energy ray polymerizable compound. It may also contain a photopolymerization initiator, a photosensitizer, etc. as needed.
[0112] Examples of active energy ray polymerizable compounds include (meth)acrylic acid compounds such as (meth)acrylic acid ester monomers having at least one (meth)acrylic acid ester group in the molecule; (meth)acrylic acid ester oligomers having at least two (meth)acrylic acid ester groups in the molecule obtained by reacting two or more functional group-containing compounds; and (meth)acrylic acid compounds such as (meth)acrylic acid ester oligomers having at least two (meth)acrylic acid ester groups in the molecule. The adhesive composition may contain 0.1 parts by mass or more of the active energy ray polymerizable compound relative to 100 parts by mass of the solid content of the adhesive composition, and may contain 10 parts by mass or less, 5 parts by mass or less, or 2 parts by mass or less of the active energy ray polymerizable compound.
[0113] Examples of the photopolymerization initiator include benzophenone, benzyl dimethyl ketal, and 1-hydroxycyclohexanone. The photopolymerization initiator may include one or more types. When the adhesive composition includes the photopolymerization initiator, the total content thereof may be, for example, 0.01 to 3.0 parts by mass relative to 100 parts by mass of the solid content of the adhesive composition.
[0114] The adhesive composition may contain additives such as microparticles, beads (resin beads, glass beads, etc.), glass fibers, resins other than base polymers, adhesion-imparting agents, fillers (metal powder, other inorganic powders, etc.), antioxidants, ultraviolet absorbers, dyes, pigments, colorants, defoaming agents, corrosion inhibitors, photopolymerization initiators, etc., for imparting light scattering properties.
[0115] The first adhesive layer 102 can be formed by applying an organic solvent dilution of the above-mentioned adhesive composition on a substrate and drying it. The first adhesive layer 102 can also be formed using an adhesive sheet, which is formed using an adhesive composition. When an active energy ray-curable adhesive composition is used, the formed adhesive layer can be irradiated with active energy rays to form an adhesive layer having a desired degree of curing.
[0116] The thickness of the first adhesive layer 102 is not particularly limited, and is, for example, preferably 1 μm to 100 μm, more preferably 3 μm to 50 μm, and may be 20 μm or more.
[0117] From the viewpoint of improving the cohesive force of the first adhesive layer 102, when the first adhesive layer 102 is made into a reference adhesive layer with a thickness of 150 μm, the shear modulus at a temperature of 25° C. is preferably 0.01 MPa or more, more preferably 0.02 MPa or more, preferably 0.50 MPa or less, more preferably 0.10 MPa or less, and may also be 0.08 MPa or less. When the shear modulus of the first adhesive layer 102 is within this range, the optical laminate 100 is not prone to cohesive failure even if it is bent, and it is also not easy to generate bubbles. The shear modulus can be adjusted by changing the type and content of the monomers constituting the base polymer contained in the adhesive composition, additives, crosslinking degree, etc.
[0118] [Polarizing plate]
[0119] The polarizer 103 may be, for example, a linear polarizer, a circular polarizer, an elliptical polarizer, etc. The circular polarizer includes a linear polarizer and a phase difference layer. The circular polarizer can absorb external light reflected in the image display device, and thus can provide the optical laminate 100 with a function as an antireflection film.
[0120] The thickness of the polarizing plate 103 is usually 5 μm or more, and may be 20 μm or more, 25 μm or more, or 30 μm or more. The thickness of the polarizing plate 103 is preferably 80 μm or less, and more preferably 60 μm or less.
[0121] (Linear polarizer)
[0122] The linear polarizer has the function of selectively transmitting linear polarized light in a certain direction of non-polarized light such as natural light. The linear polarizer can be provided with a stretched film or stretched layer adsorbed with a dichroic pigment, a solidified product containing a polymerizable liquid crystal compound and a dichroic pigment, and a liquid crystal layer in which the dichroic pigment is dispersed and oriented in the solidified product of the polymerizable liquid crystal compound, etc. as a polarizer layer. A dichroic pigment refers to a pigment having a property that the absorbance in the long axis direction of the molecule is different from the absorbance in the short axis direction. Compared with a stretched film or stretched layer adsorbed with a dichroic pigment, a linear polarizer using a liquid crystal layer as a polarizer layer has no restrictions on the bending direction, and is therefore preferred.
[0123] (Polarizer layer as a stretched film or stretched layer having a dichroic dye adsorbed thereon)
[0124] The polarizer layer of a stretched film having a dichroic dye adsorbed thereon can generally be manufactured through the following steps, namely, a step of uniaxially stretching a polyvinyl alcohol resin film, a step of dyeing the polyvinyl alcohol resin film with a dichroic dye such as iodine to adsorb the dichroic dye, a step of treating the polyvinyl alcohol resin film having the dichroic dye adsorbed thereon with an aqueous boric acid solution, and a step of washing the film with water after the treatment with the aqueous boric acid solution.
[0125] The thickness of the polarizer layer is usually 30 μm or less, preferably 18 μm or less, and more preferably 15 μm or less. Reducing the thickness of the polarizer layer is advantageous for thinning the polarizing plate 103. The thickness of the polarizer layer is usually 1 μm or more, for example, 5 μm or more.
[0126] The polyvinyl alcohol resin is obtained by saponifying a polyvinyl acetate resin. As the polyvinyl acetate resin, in addition to polyvinyl acetate which is a homopolymer of vinyl acetate, copolymers of vinyl acetate and other monomers copolymerizable therewith can also be used. Examples of other monomers copolymerizable with vinyl acetate include unsaturated carboxylic acid compounds, olefin compounds, vinyl ether compounds, unsaturated sulfone compounds, and (meth)acrylamide compounds having an ammonium group.
[0127] The saponification degree of the polyvinyl alcohol resin is usually about 85 mol% to 100 mol%, preferably 98 mol% or more. The polyvinyl alcohol resin may be modified, and polyvinyl formal, polyvinyl acetal, etc. modified with aldehydes may also be used. The degree of polymerization of the polyvinyl alcohol resin is usually 1000 to 10000, preferably 1500 to 5000.
[0128] The polarizer layer as a stretching layer adsorbed with a dichroic pigment can usually be manufactured via the following steps, that is, a step of applying a coating liquid containing the above-mentioned polyvinyl alcohol resin to a substrate film, a step of uniaxially stretching the obtained laminated film, a step of dyeing the polyvinyl alcohol resin layer of the laminated film after uniaxial stretching with a dichroic pigment so that the dichroic pigment is adsorbed to make the polarizer layer, a step of treating the film adsorbed with the dichroic pigment with an aqueous boric acid solution, and a step of washing with water after the treatment based on the aqueous boric acid solution. The substrate film used to form the polarizer layer can also be used as a protective layer for the polarizer layer. The substrate film can also be peeled off and removed from the polarizer layer as needed. The material and thickness of the substrate film can be the same as the material and thickness of the thermoplastic resin film described later.
[0129] The polarizer layer of the stretched film or stretched layer adsorbed with the dichroic dye can be used directly as a linear polarizer, or a protective layer can be formed on one or both sides thereof and used as a linear polarizer. As the protective layer, a thermoplastic resin film described later can be used. The thickness of the obtained linear polarizer is preferably 2 μm to 40 μm.
[0130] Examples of thermoplastic resin films include cyclic polyolefin resin films; cellulose acetate resin films composed of resins such as triacetyl cellulose and diacetyl cellulose; polyester resin films composed of resins such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate; polycarbonate resin films; (meth) acrylic resin films; polypropylene resin films, and other films known in the art. The polarizer layer and the protective layer may be laminated via a laminating layer described later.
[0131] From the viewpoint of thinning, the thickness of the thermoplastic resin film is usually 100 μm or less, preferably 80 μm or less, more preferably 60 μm or less, further preferably 40 μm or less, further preferably 30 μm or less, and is usually 5 μm or more, preferably 10 μm or more.
[0132] A hard coating layer may also be formed on the thermoplastic resin film. The hard coating layer may be formed on one surface of the thermoplastic resin film or may be formed on both surfaces. By providing the hard coating layer, a thermoplastic resin film having improved hardness and scratch resistance may be produced. The hard coating layer may be formed in the same manner as the hard coating layer formed on the above-mentioned resin film.
[0133] (Polarizer layer as liquid crystal layer)
[0134] The polymerizable liquid crystal compound used to form the liquid crystal layer is a compound having a polymerizable reaction group and exhibiting liquid crystal properties. The polymerizable reaction group is a group that participates in the polymerization reaction, preferably a photopolymerizable reaction group. The photopolymerizable reaction group refers to a group that can participate in the polymerization reaction through active free radicals, acids, etc. generated by a photopolymerization initiator. As photopolymerizable functional groups, vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, acryloyloxy, methacryloyloxy, oxirane, oxetane, etc. can be cited. Among them, acryloyloxy, methacryloyloxy, vinyloxy, oxirane and oxetane are preferred, and acryloyloxy is more preferred. The type of polymerizable liquid crystal compound is not particularly limited, and rod-shaped liquid crystal compounds, disc-shaped liquid crystal compounds and mixtures thereof can be used. The liquid crystal properties of the polymerizable liquid crystal compound can be thermotropic liquid crystal or lyotropic liquid crystal, and as a phase sequence structure, it can be a nematic liquid crystal or a smectic liquid crystal.
[0135] The dichroic dye used in the polarizer layer of the liquid crystal layer preferably has a maximum absorption wavelength (λMAX) in the range of 300 to 700 nm. Examples of such dichroic dyes include acridine dyes, The present invention can be used for the preparation of the present invention. ...
[0136] The polarizer layer as a liquid crystal layer can be formed by, for example, applying a composition for forming a polarizer layer comprising a polymerizable liquid crystal compound and a dichroic pigment on an orientation film formed on a substrate film, polymerizing and curing the polymerizable liquid crystal compound. It is also possible to form a coating film by applying a composition for forming a polarizer layer on a substrate film, and stretching the coating film together with the substrate film to form a polarizer layer. The substrate film used to form the polarizer layer can also be used as a protective layer for the polarizer layer. The material and thickness of the substrate film are the same as those of the above-mentioned thermoplastic resin film.
[0137] As a composition for forming a polarizer layer comprising a polymerizable liquid crystal compound and a dichroic pigment and a method for manufacturing a polarizer layer using the composition, the technical schemes described in Japanese Patent Publication No. 2013-37353, Japanese Patent Publication No. 2013-33249, Japanese Patent Publication No. 2017-83843, etc. can be exemplified. In addition to the polymerizable liquid crystal compound and the dichroic pigment, the composition for forming a polarizer layer may further include additives such as a solvent, a polymerization initiator, a crosslinking agent, a leveling agent, an antioxidant, a plasticizer, and a sensitizer. These components can be used only one type, or two or more types can be used in combination.
[0138] The polymerization initiator that the composition for forming the polarizer layer may contain is a compound that can initiate the polymerization reaction of the polymerizable liquid crystal compound. In terms of being able to initiate the polymerization reaction under lower temperature conditions, a photopolymerization initiator is preferred. Specifically, a photopolymerization initiator that can generate active free radicals or acids by the action of light can be cited, wherein a photopolymerization initiator that generates free radicals by the action of light is preferred. The content of the polymerization initiator is preferably 1 to 10 parts by mass, more preferably 3 to 8 parts by mass, relative to the total amount of 100 parts by weight of the polymerizable liquid crystal compound. Within this range, the reaction of the polymerizable group is fully carried out, and it is easy to stabilize the orientation state of the liquid crystal compound.
[0139] The thickness of the polarizer layer as the liquid crystal layer is usually 10 μm or less, preferably 0.5 μm to 8 μm, and more preferably 1 μm to 5 μm.
[0140] The polarizer layer as the liquid crystal layer can be used as a linear polarizer without peeling off the substrate film, or the substrate film can be peeled off from the polarizer layer and removed as a linear polarizer. The polarizer layer as the liquid crystal layer can also be used as a linear polarizer by forming a protective layer on one or both sides thereof. As the protective layer, the above-mentioned thermoplastic resin film can be used.
[0141] The polarizer layer as the liquid crystal layer may have a cover layer on one or both sides of the polarizer layer for the purpose of protecting the polarizer layer. The cover layer may be formed, for example, by coating the polarizer layer with a material (composition) for forming the cover layer. As the material constituting the cover layer, for example, photocurable resins, water-soluble polymers, etc. may be cited. As the material constituting the cover layer, (meth) acrylic resins, polyvinyl alcohol resins, etc. may be used.
[0142] The polarizing plate 103 is arranged such that the linear polarizing plate is on the first adhesive layer 102 side relative to the retardation layer. The outermost layer constituting the polarizing plate 103 and in contact with the first adhesive layer 102 is preferably a base film, a protective layer or an overcoat layer included in the linear polarizing plate.
[0143] (Phase difference layer)
[0144] The phase difference layer can be 1 layer or more than 2 layers. The phase difference layer can have a cover layer for protecting its surface, a substrate film for supporting the phase difference layer, etc. The phase difference layer includes a λ / 4 layer, and can further include at least one of a λ / 2 layer or a positive C layer. When the phase difference layer includes a λ / 2 layer, the λ / 2 layer and the λ / 4 layer are stacked in sequence from the linear polarizer side. When the phase difference layer includes a positive C layer, the λ / 4 layer and the positive C layer can be stacked in sequence from the linear polarizer side, or the positive C layer and the λ / 4 layer can be stacked in sequence from the linear polarizer side. The thickness of the phase difference layer is, for example, 0.1 μm to 10 μm, preferably 0.5 μm to 8 μm, and more preferably 1 μm to 6 μm.
[0145] The phase difference layer may be formed of a resin film exemplified as a material for the protective layer, or may be formed of a layer cured by a polymerizable liquid crystal compound. The phase difference layer may further include an alignment film. The phase difference layer may have a laminating layer for laminating the λ / 4 layer to the λ / 2 layer and the positive C layer.
[0146] When the polymerizable liquid crystal compound is cured to form a phase difference layer, the phase difference layer can be formed by applying a composition containing a polymerizable liquid crystal compound to a substrate film and curing it. An orientation film can be formed between the substrate film and the coating layer. The material and thickness of the substrate film can be the same as the material and thickness of the thermoplastic resin film. When the phase difference layer is formed by curing the polymerizable liquid crystal compound, the phase difference layer can be assembled in an optical laminate in the form of an orientation film and a substrate film. The phase difference layer can be bonded to the linear polarizer via a bonding layer.
[0147] [Second adhesive layer]
[0148] The second adhesive layer 104 is interposed between the polarizing plate 103 and the back plate 105 to bond them together. The second adhesive layer 104 may be composed of a single layer or two or more layers, but is preferably composed of a single layer.
[0149] The composition and compounding ingredients of the adhesive composition constituting the second adhesive layer 104, the type of the adhesive composition (whether it is active energy ray-curable, thermosetting, etc.), additives that can be blended in the adhesive composition, the method for preparing the second adhesive layer, the thickness of the second adhesive layer, etc. are the same as those shown in the description of the first adhesive layer 102 mentioned above.
[0150] The second adhesive layer 104 may be the same as or different from the first adhesive layer 102 in terms of the composition and ingredients of the adhesive composition, thickness, and the like.
[0151] From the viewpoint of improving the cohesive force of the second adhesive layer 104, when the second adhesive layer 104 is a reference adhesive layer with a thickness of 150 μm, the shear modulus at a temperature of 25° C. is preferably 0.01 MPa or more, more preferably 0.02 MPa or more, preferably 0.50 MPa or less, more preferably 0.10 MPa or less, and may also be 0.08 MPa or less. When the shear modulus of the second adhesive layer 104 is within this range, the optical laminate 100 is not prone to cohesive failure even if it is bent, and it is not easy to generate bubbles. The shear modulus can be adjusted by changing the type and content of the monomers constituting the base polymer contained in the adhesive composition, additives, crosslinking degree, etc.
[0152] [Lamination layer]
[0153] The optical laminate 100 may include a laminating layer for joining two layers. The laminating layer is a layer composed of an adhesive or a bonding agent. The adhesive used as the material of the laminating layer may use the same adhesive composition as the adhesive composition constituting the first adhesive layer 102. The laminating layer may also use other adhesives, such as (meth) acrylic adhesives, styrene adhesives, silicone adhesives, rubber adhesives, polyurethane adhesives, polyester adhesives, epoxy copolymer adhesives, etc., which are different from the adhesive constituting the first adhesive layer 102.
[0154] For the adhesive as the material of the laminating layer, for example, one or more of water-based adhesives, active energy ray-cured adhesives, etc. can be combined to form. As water-based adhesives, for example, polyvinyl alcohol resin aqueous solutions, water-based two-component polyurethane emulsion adhesives, etc. can be cited. Active energy ray-cured adhesives are adhesives that are cured by irradiating active energy rays such as ultraviolet rays, for example, adhesives containing polymerizable compounds and photopolymerization initiators, adhesives containing photoreactive resins, adhesives containing binder resins and photoreactive crosslinking agents, etc. can be cited. As the above-mentioned polymerizable compounds, photopolymerizable monomers such as photocurable epoxy monomers, photocurable acrylic monomers, photocurable urethane monomers, and oligomers from these monomers can be cited. As the above-mentioned photopolymerization initiator, compounds containing active species such as neutral free radicals, anionic free radicals, and cationic free radicals that are generated by irradiating active energy rays such as ultraviolet rays can be cited.
[0155] The thickness of the bonding layer may be, for example, 1 μm or more, preferably 1 μm to 25 μm, more preferably 2 μm to 15 μm, and further preferably 2.5 μm to 5 μm.
[0156] The two opposing surfaces to be bonded via the bonding layer may be subjected to corona treatment, plasma treatment, flame treatment, etc. in advance, or may have a primer layer or the like.
[0157] [Back panel]
[0158] As the rear plate 105 , a plate-like body that can transmit light, a component used in a general display device, or the like can be used.
[0159] The thickness of rear plate 105 may be, for example, 5 μm to 2000 μm, preferably 10 μm to 1000 μm, and more preferably 15 μm to 500 μm.
[0160] The plate-like body used in rear plate 105 may be composed of only one layer or may be composed of two or more layers, and the structure exemplified for the plate-like body described in connection with front plate 101 may be used.
[0161] As components used in a general display device used in the back panel 105, for example, a touch sensor panel, an organic EL display element, etc. As the stacking order of the components in the display device, for example, a window film / circular polarizing plate / touch sensor panel / organic EL display element, a window film / touch sensor panel / circular polarizing plate / organic EL display element, etc. can be mentioned.
[0162] (Touch sensor panel)
[0163] The touch sensor panel is not limited as long as it is a panel with a sensor (i.e., a touch sensor) that can detect the touched position. The detection method of the touch sensor is not limited, and examples thereof include touch sensor panels such as a resistive film method, an electrostatic capacitance coupling method, an optical sensor method, an ultrasonic method, an electromagnetic induction coupling method, and a surface elastic wave method. Due to the low cost, it is preferred to use a touch sensor panel of a resistive film method or an electrostatic capacitance coupling method.
[0164] As an example of a touch sensor of a resistive film type, there can be cited a component consisting of a pair of substrates arranged facing each other, an insulating spacer sandwiched between the pair of substrates, a transparent conductive film provided as a resistive film on the inner front surface of each substrate, and a touch position detection circuit. In an image display device provided with a touch sensor of a resistive film type, when the surface of the front panel is touched, the opposing resistive films are short-circuited and current flows through the resistive films. The touch position detection circuit detects the change in voltage at this time, thereby detecting the touched position.
[0165] As an example of a capacitive coupling touch sensor, there is a component consisting of a substrate, a transparent electrode for position detection provided on the entire surface of the substrate, and a touch position detection circuit. In an image display device provided with a capacitive coupling touch sensor, when the surface of the front panel is touched, the transparent electrode is grounded at the touched point via the electrostatic capacitance of the human body. The touch position detection circuit detects the grounding of the transparent electrode, thereby detecting the touched position.
[0166] The thickness of the touch sensor panel may be, for example, 5 μm to 2000 μm, preferably 5 μm to 100 μm, more preferably 5 μm to 50 μm, and may be 5 μm to 20 μm.
[0167] The touch sensor panel may be a component having a touch sensor pattern formed on a substrate film. Examples of the substrate film may be the same as those in the description of the thermoplastic resin film. In addition, the touch sensor panel may be transferred from the substrate film to the covering via the adhesive layer. That is, the touch sensor panel may not have a substrate film. The thickness of the touch sensor pattern may be, for example, 1 μm to 20 μm.
[0168] [Method for producing optical layered body]
[0169] The optical laminate 100 can be manufactured by a method comprising the following steps, that is, a step of laminating the layers constituting the optical laminate 100 to each other via an adhesive layer. When the layers are laminated to each other via an adhesive layer and a laminating layer, in order to adjust the adhesion, it is preferred that one or both sides of the laminating surface are subjected to surface activation treatments such as corona treatment. The conditions of the corona treatment can be appropriately set, and the conditions can be different on one side and the other side of the laminating surface.
[0170] <Display device>
[0171] The display device of the present invention includes the above-mentioned optical laminate 100. The display device is not particularly limited, and for example, an image display device such as an organic EL display device, an inorganic EL display device, a liquid crystal display device, and an electroluminescent display device can be cited. A touch sensor can be further laminated in the optical laminate, and the display device can have a touch panel function. The display device including the optical laminate of the present invention exhibits excellent durability in static bending and can be used as a flexible display that can be bent or rolled.
[0172] In the display device, the optical laminate 100 is arranged on the viewing side of the display element of the display device with the front panel 101 facing outward (the side opposite to the display element side, ie, the viewing side). The display device can be bent with the front panel 101 side facing inward.
[0173] The display device of the present invention can be used as portable devices such as smart phones and tablets, televisions, digital photo frames, electronic billboards, detectors, instruments, office equipment, medical instruments, computer equipment, etc.
[0174] Example
[0175] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited thereto.
[0176] [Adhesive layer]
[0177] A 1 L reactor with nitrogen reflux and equipped with a cooling device for easy temperature control was charged with a monomer mixture consisting of 2-ethylhexyl acrylate (2-EHA), n-butyl acrylate (n-BA), N-(2-hydroxyethyl)acrylamide (HEAA), isodecyl acrylate (IDA), behenyl acrylate (BHA), and compound I shown in Table 1. After nitrogen reflux for 1 hour to remove oxygen, the solution was maintained at 60°C.
[0178] After the monomer mixture was uniformly mixed, a photopolymerization initiator, benzyl dimethyl ketal (I-651) and 1-hydroxycyclohexyl phenyl ketone (I-184) were added in the amounts shown in Table 1. The mixture was irradiated with a UV lamp (10 mW) while stirring to produce acrylic polymers A1 to A6.
[0179] [Table 1]
[0180]
[0181]
[0182] The obtained acrylic polymers A1 to A6, isodecyl acrylate (IDA), N-(2-hydroxyethyl)acrylamide (HEAA), and benzophenone (BPO) were mixed in the amounts shown in Table 2 to prepare adhesive compositions B1 to B9.
[0183] [Table 2]
[0184]
[0185] Adhesive compositions B1 to B9 were applied to a release film A (polyethylene terephthalate film, 38 μm thick) coated with a silicone release agent in a 25 μm thick manner. A release film B (polyethylene terephthalate film, 38 μm thick) was bonded thereto and UV irradiated to produce an adhesive sheet consisting of release film A / adhesive layer / release film B. The UV irradiation conditions were a cumulative light dose of 400 mJ / cm 2 , illumination 1.8mW / cm 2 (UVV reference).
[0186] The sources of the compounds used are as follows.
[0187] 2-EHA: Tokyo Chemical Industry Co., Ltd., Japan
[0188] n-BA: Tokyo Chemical Industry Co., Ltd., Japan
[0189] HEAA: Tokyo Chemical Industry Co., Ltd., Japan
[0190] IDA: Miwon specialty chemical, South Korea
[0191] BHA: Tokyo Chemical Industry Co., Ltd., Japan
[0192] I-651: BASF, Germany
[0193] I-184: BASF, Germany
[0194] BPO: Tokyo Chemical Industry Co., Ltd., Japan
[0195] [Front panel]
[0196] A film having a hard coat layer formed on one surface of a resin film was prepared as the front panel 101. The resin film was a 40 μm thick polyimide resin film. The hard coat layer was a 10 μm thick layer formed of a composition containing a dendrimer having a multifunctional acrylic group at the end.
[0197] [Circular polarizing plate]
[0198] A circular polarizer was prepared as the polarizer 103. A linear polarizer having a triacetyl cellulose (TAC) film (KC2UA, manufactured by Konica Minolta Co., Ltd., thickness 25 μm), an orientation film, a linear polarizer layer, and a cover layer in this order was prepared. The linear polarizer layer was formed using a composition containing a polymerizable liquid crystal compound and a dichroic pigment, and had a thickness of 2 μm. The cover layer was a polyvinyl alcohol resin layer, and had a thickness of 1.0 μm.
[0199] A phase difference laminate is laminated on the cover layer side of the linear polarizer via an adhesive layer to obtain a circular polarizer. The phase difference laminate has a λ / 4 phase difference layer, an adhesive layer, and a positive C layer in order from the linear polarizer side. The λ / 4 phase difference layer is a cured layer of a polymerizable liquid crystal compound and has a thickness of 3 μm. The thickness of the adhesive layer is 5 μm. The positive C layer is a cured layer of a polymerizable liquid crystal compound and has a thickness of 3 μm.
[0200] [Back panel]
[0201] A touch sensor having a touch sensor pattern layer, an adhesive layer, and a base layer laminated in this order was prepared as the back panel 105. The touch sensor pattern layer included an ITO layer as a transparent conductive layer and a cured layer of an acrylic resin composition as a separation layer, and had a thickness of 7 μm.
[0202] The adhesive layer was provided on the release layer side of the touch sensor pattern layer and had a thickness of 3 μm. A cyclic olefin resin (COP) film (ZF-14, manufactured by Zeon Co., Ltd., thickness 23 μm) was used as the base material layer.
[0203] [Production of optical laminate]
[0204] As shown in Table 3, an adhesive sheet composed of the adhesive composition shown in Table 2 was used as the first adhesive layer 102, and the side of the front panel 101 without the hard coat layer was bonded to the TAC film side of the polarizer 103. In addition, as shown in Table 3, an adhesive sheet composed of the adhesive composition shown in Table 2 was used as the second adhesive layer 104, and the phase difference layer side of the circular polarizer was bonded to the touch sensor pattern layer side of the touch sensor to produce Figure 1 The optical laminate 100 of the layer structure shown (Examples 1 to 4 and Comparative Examples 1 and 2). The front panel, circular polarizer, touch sensor and adhesive layer were subjected to double-sided corona treatment before bonding. The corona treatment was performed using TEC-4AX (manufactured by Ushio Electric Co., Ltd.). The slope G from the origin to the maximum stress of the adhesive layer was measured according to the following method: L ', stress relaxation rate σ, creep rate ε, deformation recovery rate R, glass transition temperature T g , shear elastic modulus, and static bending durability of the optical laminate 100. The results are shown in Table 3.
[0205] [Table 3]
[0206]
[0207] <Thickness of layer>
[0208] The measurement was performed using a contact-type film thickness measuring device (“MS-5C” manufactured by Nikon Corporation). The polarizer layer and the alignment film were measured using a laser microscope (“OLS3000” manufactured by Olympus Corporation).
[0209] <The slope G from the origin to the maximum stress value L '>
[0210] The slope from the origin to the maximum stress value was measured using a dynamic mechanical analyzer (DMA, Q-800, manufactured by TA Instruments). Figure 2 As shown, a test piece is prepared by joining the ends of two polycarbonate (PC) rods 501 to each other via an adhesive layer. The shape of the adhesive layer 502 is 6mm×10mm×25μm in width×length×thickness, and the shape of the PC rod 501 is 6mm×20mm×1mm in width×length×thickness. The bonding area between the adhesive layer 502 and the PC rod 501 is 6mm×10mm in width×length. A clamp is installed in an area of 5mm in length at both ends of the PC rod 501 of the test piece, and one of the clamps is fixed. The other clamp is stretched at a speed of 100μm / min. at a temperature of 25°C to produce a stress [Pa]-strain [%] curve. In the obtained stress-strain curve, the slope from the origin to the maximum stress is calculated.
[0211] <Stress relaxation rate σ>
[0212] A dynamic mechanical analyzer (DMA, Q-800, manufactured by TA Instruments) was used to measure the stress relaxation rate (Stress Relaxation) of the adhesive layer. The test piece was the same as the test piece used in the determination of the slope from the origin to the maximum stress value. A clamp was installed in the 5mm length area at both ends of the PC rod 501 of the test piece, and one of the clamps was fixed. The other clamp was stretched continuously for 300 seconds in an environment of a temperature of 25°C to maintain a strain of 25%, and the stress was measured.
[0213] Stress relaxation rate = stress after 300 seconds [MPa] / stress after 7.0 seconds [MPa]
[0214] <Creep rate ε>
[0215] Use a dynamic mechanical analyzer (DMA, Q-800, manufactured by TA Instruments) to measure the creep rate (Creep) of the adhesive layer. The test piece is the same as the test piece used in the determination of the slope from the origin to the maximum stress value. Install a clamp in the 5mm length area at both ends of the PC rod 501 of the test piece, and fix one of the clamps. Continue to stretch the other clamp with a stress of 1MPa, and measure the strain (%) value after 1200 seconds.
[0216] Creep rate (%) = strain after 1200 seconds (%)
[0217] <Deformation recovery rate R>
[0218] A dynamic mechanical analyzer (DMA, Q-800, manufactured by TA Instruments) was used to measure the deformation recovery rate (Recovery) of the adhesive layer. The test piece is the same as the test piece used in the determination of the slope from the origin to the maximum stress value. A clamp is installed in the area of 5 mm in length at both ends of the PC rod 501 of the test piece, and one of the clamps is fixed. The other clamp is stretched and the strain of 25% is maintained for 300 seconds. After 300 seconds, the load is removed, and the strain is measured after 5 seconds (after 305 seconds).
[0219] Deformation recovery rate (%) = strain after 300 seconds (= 25%) - strain after 305 seconds (%)
[0220] <Glass transition temperature T g >
[0221] After the adhesive was dried at 100° C. for 1 hour, the glass transition temperature (T g ).
[0222] <Shear elastic modulus>
[0223] The shear modulus was measured using a viscoelasticity measuring device (MCR-301, Anton Paar). The adhesive sheet was made 20 mm wide by 20 mm long, the release film was peeled off, and multiple sheets were stacked in a thickness of 150 μm. After the laminated adhesive layer was bonded to the glass plate, it was measured in a temperature range of -20°C to 100°C in a state bonded to the measurement chip at a frequency of 1.0 Hz, a deformation of 1%, and a heating rate of 5°C / min, and the shear modulus value at 25°C was confirmed.
[0224] <Static bending durability test>
[0225] Figure 3The method of the static bending durability test (mandrel bending test) is shown in FIG. First, the optical stack 100 is cut into test pieces of 1 cm×10 cm. The optical stack 100 is placed on a test plate 504 with the front panel 101 side facing upward, and an iron rod 503 (5 mm in diameter) is placed on it. Figure 3 (A) in the figure). The iron rod 503 is wound around the iron rod 503 and the front panel 101 is folded and fixed by hand ( Figure 3 (B) in the figure.
[0226] The static bending durability was evaluated as follows based on the period during which bubbles were not generated between the polarizing plate 103 and the first and second adhesive layers 102 and 104 or within the first and second adhesive layers 102 and 104. The generation of bubbles was determined by observation under an optical microscope.
[0227] A: No bubbles were generated after 72 hours.
[0228] B: Bubbles were generated within more than 48 hours and within 72 hours.
[0229] C: Bubbles were generated within more than 24 hours and within 48 hours.
[0230] D: Bubbles are generated within 24 hours.
[0231] Explanation of symbols
[0232] 100 optical laminate, 101 front panel, 102 first adhesive layer, 103 polarizing plate, 104 second adhesive layer, 105 back panel, 501 polycarbonate rod, 502 adhesive layer, 503 iron rod, 504 test plate.
Claims
1. An optical laminate comprising, in order, a front plate, a first adhesive layer, a polarizing plate, a second adhesive layer and a back plate, The slopes from the origin to the maximum stress value in the stress-strain curves of the first adhesive layer and the second adhesive layer are respectively defined as G L1 ' and G L2 ', the following equations (1), (2) and (3) are satisfied: 20≤G L1 '≤150 (1) 20≤G L2 '≤150 (2) G L1 '<G L2 ' (3) in, The unit of stress is Pa and the unit of strain is %.
2. The optical layered body according to claim 1, wherein: When the stress relaxation rate of the first adhesive layer is σ1, the following formula (4) is satisfied: 0.20≤σ1≤0.70 (4).
3. The optical laminate according to claim 2, wherein: When the stress relaxation rate of the second adhesive layer is set to σ2, the following formula (5) is satisfied: σ1<σ2 (5).
4. The optical layered body according to any one of claims 1 to 3, wherein When the creep rate of the first adhesive layer is ε1, the following formula (6) is satisfied: 1.5≤ε1≤20 (6) The unit of creep rate is %.
5. The optical layered body according to claim 4, wherein: When the creep rate of the second adhesive layer is set to ε2, the following formula (7) is satisfied: ε1>ε2 (7) The unit of creep rate is %.
6. The optical layered body according to any one of claims 1 to 3 and 5, wherein When the deformation recovery rate of the first adhesive layer is defined as R1, the following formula (8) is satisfied: 2.5≤R1≤20 (8) The unit of deformation recovery rate is %.
7. The optical layered body according to claim 6, wherein: When the deformation recovery rate of the second adhesive layer is defined as R2, the following formula (9) is satisfied: R1<R2 (9) The unit of deformation recovery rate is %.
8. The optical layered body according to any one of claims 1 to 3, 5 and 7, wherein The glass transition temperatures of the first adhesive layer and the second adhesive layer are respectively -70°C to -40°C.
9. An optical laminate comprising, in order, a front plate, a first adhesive layer, a polarizing plate, a second adhesive layer, and a back plate, The slopes from the origin to the maximum stress value in the stress-strain curves of the first adhesive layer and the second adhesive layer are respectively defined as G L1 ' and G L2 ', the following equations (1) and (2) are satisfied: 20≤G L1 '≤150 (1) 20≤G L2 '≤150 (2) in, The unit of stress is Pa, and the unit of strain is %. When the stress relaxation rate of the first adhesive layer is σ1 and the stress relaxation rate of the second adhesive layer is σ2, the following equations (4) and (5) are satisfied: 0.20≤σ1≤0.70 (4) σ1<σ2 (5).
10. An optical laminate comprising, in order, a front plate, a first adhesive layer, a polarizing plate, a second adhesive layer, and a back plate, The slopes from the origin to the maximum stress value in the stress-strain curves of the first adhesive layer and the second adhesive layer are respectively defined as G L1 ' and G L2 ', the following equations (1) and (2) are satisfied: 20≤G L1 '≤150 (1) 20≤G L2 '≤150 (2) in, The unit of stress is Pa, and the unit of strain is %. When the creep rate of the first adhesive layer is ε1 and the creep rate of the second adhesive layer is ε2, the following equations (6) and (7) are satisfied: 1.5≤ε1≤20 (6) ε1>ε2 (7) The unit of creep rate is %.
11. An optical laminate comprising, in order, a front plate, a first adhesive layer, a polarizing plate, a second adhesive layer, and a back plate, The slopes from the origin to the maximum stress value in the stress-strain curves of the first adhesive layer and the second adhesive layer are respectively defined as G L1 ' and G L2 ', the following equations (1) and (2) are satisfied: 20≤G L1 '≤150 (1) 20≤G L2 '≤150 (2) in, The unit of stress is Pa, and the unit of strain is %. When the deformation recovery rate of the first adhesive layer is set to R1 and the deformation recovery rate of the second adhesive layer is set to R2, the following equations (8) and (9) are satisfied: 2.5≤R1≤20 (8) R1<R2 (9) The unit of deformation recovery rate is %. 12 . A display device comprising the optical layered body according to claim 1 .
13. The display device according to claim 12, wherein: The bending can be performed with the front panel side as the inner side.
Citation Information
Patent Citations
Polarization element, circularly polarizing plate and method of manufacturing those
JP2013033249A
Polarizer and method for manufacturing the same
JP2013037353A
Polarizing plate
JP2017083843A
Adhesive composition for flexible image display device, adhesive layer for flexible image display device, laminate for flexible image display device, and flexible image display device
JP2018027995A
Adhesive composition and adhesive sheet prepared from the same
KR1020190005427A