Aluminum alloy material and manufacturing method thereof
By forming a titanium and zirconium compound film on the surface of the aluminum alloy material and controlling the current density of the electrode polarization curve, the problem of easy deterioration of the aluminum alloy material at the bonding interface is solved, and the bonding durability is significantly improved.
Patent Information
- Application Number
- CN202080082571.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-04-21
- Filing Date
- 2020-09-24
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-09-24
AI Technical Summary
Existing aluminum alloy materials are prone to deterioration at the bonding interface, resulting in insufficient bonding durability, especially under tensile stress and corrosive environments.
By performing specific chemical formation treatment on the surface of the aluminum alloy material to form a film containing titanium and zirconium compounds, and performing acid etching and chemical formation treatment under specific electrochemical conditions, the current density in the electrode polarization curve is controlled to reach 10 μA/cm2. The electrode potential is in the range of -1350mV ~ -1150mV to suppress cathode activity and interface degradation.
Significantly improves the bonding durability of aluminum alloy materials and other materials, prevents interface degradation caused by load tensile stress and corrosion, and extends the service life of the bonding.
Smart Images

Figure CN114746579B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an aluminum alloy material and a manufacturing method thereof. Background Art
[0002] In the past, in order to improve the surface properties of aluminum alloy materials, aluminum alloy materials subjected to various surface treatment methods have been proposed. Patent document 1 (Japanese Patent Publication No. 2014-62277) discloses an aluminum alloy plate having an aluminum alloy substrate and an aluminum oxide film formed on the surface of the aluminum alloy substrate, wherein the aluminum oxide film contains at least one additive element having a PB ratio (Pilling-Bedworth ratio) of 1.00 or more, 0.01 to 10 atomic % of zirconium, and 0.1 atomic % or more and less than 10 atomic % of magnesium.
[0003] Patent document 2 (Japanese Patent Publication No. 2015-206117) discloses a surface-treated aluminum alloy plate, which comprises an aluminum alloy plate containing magnesium and an oxide film formed on the surface of the aluminum alloy plate. The plate is subjected to chemical conversion treatment (Japanese: chemical conversion treatment) during use. The thickness of the oxide film is 1 to 30 nm, the magnesium concentration is 1 to 20 atomic%, the zirconium concentration is 0.2 to 10 atomic%, and the halogen concentration and phosphorus concentration are less than 0.1 atomic%, respectively.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2014-62277
[0007] Patent Document 2: Japanese Patent Application Publication No. 2015-206117 Summary of the invention
[0008] Problems to be solved by the invention
[0009] Although aluminum alloy materials subjected to various surface treatments have been proposed in the past, aluminum alloy materials with controlled surface electrochemical activity have not been fully studied. The inventors of the present invention have repeatedly conducted intensive research to solve the above-mentioned problems, and found that an aluminum alloy material with reduced surface electrochemical activity can be obtained by subjecting the surface of the substrate to a specific surface treatment. In addition, it was found that the interface between the aluminum alloy material and other materials is not prone to deterioration, and the bonding durability between the aluminum alloy material and other materials is improved, thus completing the present invention. That is, the purpose of the present invention is to provide an aluminum alloy material with excellent bonding durability with other materials and a method for manufacturing the same.
[0010] Means for solving problems
[0011] In order to solve the above-mentioned problems, the present invention has the following embodiments.
[0012] [1] An aluminum alloy material comprising: a substrate composed of an aluminum alloy; and a chemical conversion treatment film on a surface of the substrate, wherein:
[0013] In a 5 wt % NaCl static aqueous solution at 25°C and pH 5.5, the aluminum alloy material was measured with a silver-silver chloride electrode in saturated KCl as a reference electrode and a scanning speed of 20 mV / min. In the obtained cathodic polarization curve, the absolute value of the current density reached 10 μA / cm 2 The electrode potential is -1350mV~-1150mV.
[0014] [2] The aluminum alloy material according to [1] above, wherein:
[0015] The substrate is composed of an aluminum alloy containing 0.3 to 5.0 wt % of Mg.
[0016] [3] The aluminum alloy material according to [1] or [2] above, wherein:
[0017] The chemical conversion film contains a titanium compound and a zirconium compound.
[0018] The titanium compound is at least one of titanium oxide and titanium hydroxide,
[0019] The zirconium compound is at least one of zirconium oxide and zirconium hydroxide,
[0020] The total amount of the titanium compound and the zirconium compound in the chemical conversion film is 2 to 29 mg / m 2 .
[0021] [4] A method for manufacturing an aluminum alloy material, wherein the aluminum alloy material is measured in a 5 wt% NaCl static aqueous solution at 25°C and pH 5.5 using a silver-silver chloride electrode in saturated KCl as a reference electrode and at a scanning speed of 20 mV / min, and in the resulting cathode polarization curve, the absolute value of the current density reaches 10 μA / cm 2 The electrode potential is -1350mV to -1150mV, and the manufacturing method has the following characteristics:
[0022] A step of acid-etching a substrate made of an aluminum alloy containing Mg; and
[0023] a step of performing a chemical conversion treatment on the surface of the acid-etched substrate to form a chemical conversion treatment film,
[0024] The etching amount of the substrate in the acid etching step [E: (mg / m 2)] relative to the Mg amount [M (wt%)] in the substrate, satisfies the relationship of 10M≤E≤200M.
[0025] [5] According to the method for manufacturing an aluminum alloy material described in [4] above, in the step of forming the chemical conversion treatment film, a treatment solution containing a titanium fluoride compound and a zirconium fluoride compound is used, and the chemical conversion treatment is carried out in a manner such that the total mass concentration of the titanium fluoride compound and the zirconium fluoride compound in the treatment solution [C (ppm, converted to the amount of metal elements)] and the treatment time [t (seconds)] satisfy 50≤C×t≤1500.
[0026] Effects of the Invention
[0027] An aluminum alloy material having excellent bonding durability with other materials and a method for producing the same can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a diagram showing a plate-shaped aluminum alloy material used for measuring a cathode polarization curve.
[0029] Figure 2 This is a graph showing the cathode polarization curve of the aluminum alloy material of Example 2. DETAILED DESCRIPTION
[0030] 1. Aluminum alloy material
[0031] The aluminum alloy material of the present invention comprises: a substrate composed of an aluminum alloy; and a chemical conversion treatment film on the surface of the substrate. In addition, in a cathode polarization curve obtained by measuring the aluminum alloy material in a 5 wt % NaCl static aqueous solution at 25° C. and pH 5.5 with a silver-silver chloride electrode in saturated KCl as a reference electrode and at a scanning speed of 20 mV / min, the absolute value of the current density reaches 10 μA / cm 2 The electrode potential is -1350mV~-1150mV.
[0032] For example, in the case of bonding aluminum alloy materials to other parts via adhesives (other materials), if the interface between the aluminum alloy material and the adhesive is subjected to tensile stress during use, the deterioration of the bonding interface between the aluminum alloy material and the adhesive (interface degradation) will be aggravated. The cause of interface degradation is that moisture and salt penetrate from the bonding end surface and cause corrosion of the aluminum alloy material, or the infiltrated moisture and the aluminum alloy material react to cause the growth of surface oxide film. In addition to the gradual penetration of moisture from the bonding interface, water vapor permeates through the adhesive and also causes moisture penetration. Furthermore, in the actual use environment of the adhesive, the bonding part is always in a state of being loaded with tensile stress and is also exposed to a corrosive environment. That is, the mechanical degradation that causes the bonding interface to crack physically and the chemical degradation caused by the penetration of moisture and salt into the bonding interface are superimposed and occur simultaneously, forming a harsh degradation environment that exceeds the previous assumption. As a result, in the previous surface treatment method, the bonding durability in such a harsh environment is insufficient.
[0033] In this regard, the aluminum alloy material of the present invention controls the electrochemical properties of the surface to an appropriate range, thereby being able to suppress the degradation of the interface between the aluminum alloy material and the adhesive due to load tensile stress and corrosion, and being able to suppress the degradation caused by the penetration of moisture, salt, etc. The electrochemical properties of the surface of the aluminum alloy material can be measured by measuring the polarization curve. For the aluminum alloy material of the present invention, in the cathode polarization curve, the absolute value of the current density reaches 10μA / cm 2 The electrode potential is -1350mV to -1150mV. In addition, the aluminum alloy material of the present invention has the characteristics of the cathodic polarization curve as described above even when constituting an interface with a material other than an adhesive, and thus can suppress interface degradation caused by load tensile stress, corrosion, penetration of moisture and salt, etc.
[0034] The principle of the electrochemical properties of the aluminum alloy material surface affecting interface degradation is as follows. On the surface of the aluminum alloy, there is a dense natural oxide film with a thickness of about several nanometers, which is generated by reaction with air and water. The natural oxide film is an insulating film with high protectiveness, so it can ensure the corrosion resistance of the aluminum alloy. However, the natural oxide film has defects, which become the starting point of corrosion. When the aluminum alloy corrodes, the following anodic reaction and cathodic reaction occur simultaneously.
[0035] (Anode reaction) Al→Al 3+ +3e -
[0036] (Cathode reaction)O 2 +2H 2 O+4e - →4OH-
[0037] 2H + +2e - →H 2
[0038] This is because, in order to meet the condition of electrical neutrality, it is necessary to consume the electrons generated by the anodic reaction, i.e., the ionization (dissolution) of metallic aluminum, in the cathodic reaction (reduction reaction of dissolved oxygen or hydrogen ions). As mentioned above, the defects existing in the natural oxide film on the surface of the aluminum alloy act as active sites for generating these anodic and cathodic reactions. However, in the defects of these films, the substances that function as sites for the cathode reaction are limited to crystalline precipitates with high potential existing on the surface of the aluminum alloy. That is, the corrosion rate of the aluminum alloy depends on the activity of the cathode reaction on the surface (cathode activity). In addition, the surface of the aluminum alloy continuously reacts with water to grow the surface oxide film, and the principle is the same as described above. Therefore, in order to effectively suppress the degradation of the bonding interface, it is effective to properly control the electrochemical properties of the aluminum alloy surface, especially the cathode activity.
[0039] When the cathode activity on the surface of the aluminum alloy is high, corrosion reaction is easily generated on the surface of the aluminum alloy, and the degradation of the bonding interface is aggravated. Therefore, a chemical conversion treatment film is formed on the surface of the aluminum alloy by chemical conversion treatment, so that the cathode activity of the surface can be appropriately reduced, and the degradation of the bonding interface can be suppressed. However, in the case where a thick film is unnecessarily formed on the surface of the aluminum alloy due to excessive chemical conversion treatment, although the cathode activity of the surface is greatly reduced, it is easy to produce the degradation of the chemical conversion treatment film itself, the destruction and peeling in the chemical conversion treatment film, resulting in a decrease in bonding durability. Therefore, in the present invention, the degradation of the bonding interface and the decrease in bonding durability can be suppressed by appropriately adjusting the electrochemical properties of the aluminum alloy surface. Here, the electrochemical properties of the aluminum alloy surface can be evaluated by measuring the polarization curve.
[0040] In the cathode polarization curve of the aluminum alloy material of the present invention, the absolute value of the current density reaches 10 μA / cm 2 The electrode potential is -1350mV to -1150mV. In the cathode polarization curve of the aluminum alloy material of the present invention, when the absolute value of the current density reaches 10μA / cm 2 When the electrode potential is higher than -1150 mV, the cathode activity on the aluminum alloy surface is not sufficiently suppressed, thereby reducing the bonding durability. In addition, unless otherwise specified, the electrode potential referred to in this specification refers to the value measured using a silver-silver chloride electrode (SSE) in saturated KCl at 25°C as the reference electrode. In addition, in the cathode polarization curve of the aluminum alloy material of the present invention, when the absolute value of the current density reaches 10 μA / cm 2When the electrode potential is lower than -1350mV, the thickness of the formed chemical treatment film exceeds the required level, resulting in a decrease in the bonding durability. Therefore, the electrode potential is preferably -1330mV to -1175mV, and more preferably -1310mV to -1200mV. In the cathode polarization curve, the absolute value of the current density reaches 10μA / cm 2 The electrode potential is within the above range, so that the aluminum alloy material can have better bonding durability. In addition, by appropriately treating the substrate composed of the aluminum alloy, the electrochemical properties of the surface can be controlled, and the absolute value of the current density in the cathode polarization curve can reach 10μA / cm 2 Specifically, as the surface treatment, by appropriately controlling various conditions of acid etching, chemical conversion treatment, and treatments accompanying these surface treatments as needed, the electrochemical properties of the aluminum alloy material surface can be optimized.
[0041] The cathode polarization curve of the aluminum alloy material of the present invention is measured as follows. First, prepare an open container in an atmosphere at a temperature of 25°C, inject 300ml of a 5% by mass NaCl aqueous solution at 25°C and pH 5.5 into the container and let it stand. In addition, at this time, the pH of the NaCl aqueous solution can be adjusted to pH 5.5 using NaOH or HCl. The container used for the measurement has a depth that enables the test piece to be fully immersed, as long as the aspect ratio (the ratio of the bottom diameter to the height) is not an extreme value, and is not particularly limited. As an example, a beaker with a volume of 500mL is appropriate. Figure 1 is a diagram showing a plate-shaped aluminum alloy material used for measuring a cathode polarization curve. Figure 1 A represents the surface graph, Figure 1 B indicates the back view. Figure 1As shown, the aluminum alloy to be measured is cut into a 5cm×2cm plate-shaped test piece by a shearing machine. A test piece without damage or dirt is selected. At a position about 5mm away from one end in the length direction of the plate-shaped test piece 10, 1cm×1cm is exposed as a measuring surface (the measuring surface is set at only one location on the surface of the test piece), and the remaining part is covered with a silicone resin to define an evaluation area 11. At this time, one end 12 in the length direction of the test piece on the opposite side of the evaluation area part 11 is exposed about 5mm in advance, and the measurement terminal is connected. Next, the test piece and the electrode plate (platinum electrode) are immersed in the NaCl aqueous solution and left to stand for 30 minutes. At this time, about half of the length direction of the test piece is immersed below the liquid surface. At this time, the contact part with the measurement terminal is not wetted, and the measurement surface is immersed to more than 1cm below the water surface. The platinum electrode is not particularly limited as long as it is an electrode used for conventional dynamic potential polarization measurement. As an example, the following method can be cited: a platinum wire with a diameter of 0.7 mm and a length of 120 mm is used, and it is immersed more than 5 cm below the liquid surface during measurement. In addition, degassing and stirring are not performed during the measurement. In addition, a silver-silver chloride electrode (HS-205C, manufactured by East Asia DKK Co., Ltd.) in saturated KCl at 25°C is used as a reference electrode, and a polarization curve is obtained by three-electrode measurement. 30 minutes after the test piece begins to be immersed, a constant potential meter (SDPS-511U, manufactured by Shrinks Co., Ltd.) is used to scan the potential in a decreasing direction from the natural potential of the test piece to measure the cathode polarization curve. At this time, the potential scanning rate is set to 20 mV / minute. Moreover, the absolute value of the current density reaches 10 μA / cm 2 Here, the absolute value of the current density is 10 μA / cm 2 This means that the positive and negative signs of the measured current value are removed and the cathode current density reaches 10μA / cm 2 For example, in a measuring device that uses a negative sign to represent cathode current, the measured value of cathode current density is expressed as -10 μA / cm 2 , so the minus sign is removed and expressed as 10 μA / cm 2 In addition, the evaluation area 11 of the test piece is accurately measured, and the current density is calculated by dividing the measured current by the actual evaluation area 11. Preferably, the above measurement is performed on three different test pieces and the average value is selected. In addition, when the current density reaches 10 μA / cm 2 When the current density reaches 10μA / cm 2 Therefore, polarization must be performed until it can be confirmed that the current density exceeds 10 μA / cm 2 The potential is preferably measured to below -1600 mV.
[0042] Hereinafter, each component constituting the aluminum alloy material according to one embodiment will be described.
[0043] (Base material)
[0044] The substrate is not particularly limited as long as it is composed of an aluminum alloy, and can be a substrate composed of a 1000 series aluminum alloy (pure aluminum alloy), a 2000 series aluminum alloy (Al-Cu-Mg series aluminum alloy), a 3000 series aluminum alloy (Al-Mn series aluminum alloy), a 4000 series aluminum alloy (Al-Si series aluminum alloy), a 5000 series aluminum alloy (Al-Mg series aluminum alloy), a 6000 series aluminum alloy (Al-Mg-Si series alloy), and a 7000 series alloy (Al-Zn-Mg series aluminum alloy). From the viewpoint of the strength and corrosion resistance of the substrate composed of an aluminum alloy, an aluminum alloy containing 0.3 to 5.0 weight % of Mg is preferably used.
[0045] (Chemical treatment film)
[0046] The chemical conversion film is a film obtained by subjecting the surface of the substrate to a chemical conversion treatment described below. The chemical conversion film preferably contains an inorganic compound, and more preferably contains a titanium compound and a zirconium compound. The titanium compound is preferably at least one of titanium oxide and titanium hydroxide, and the zirconium compound is preferably at least one of zirconium oxide and zirconium hydroxide. In addition, when the chemical conversion film contains a titanium compound and a zirconium compound, the total amount of the titanium compound and the zirconium compound in the chemical conversion film is converted into a metal element amount, preferably 2 to 29 mg / m 2 , more preferably 3 to 27 mg / m 2 , more preferably 4 to 20 mg / m 2 When the total amount of the titanium compound and the zirconium compound is within the above range, the aluminum alloy material can have excellent bonding durability. In addition, the amount of each titanium compound and zirconium compound converted into metal element amount is preferably at least 1 mg / m 2 , more preferably at least 1.5 mg / m 2 In addition, the above "converted to metal element amount" means per 1m 2 The amount of Ti and Zr in the chemical conversion film. The film thickness of the chemical conversion film is preferably less than 50 nm, more preferably less than 30 nm, and further preferably 1 nm to 20 nm. 2The total amount of Ti and Zr in the chemical conversion film can be measured by drawing a calibration curve based on a reference plate with a known film amount and using a fluorescent X-ray analyzer (XRF). In addition, the film thickness of the chemical conversion film can be measured using GD-OES (Glow Discharge Optical Emission Spectroscopy). When the value when the luminous intensity of aluminum fully reaches the main body (substrate) is used as the reference, the sputtering depth at the moment when 50% of the reference value is reached is set as the film thickness.
[0047] 2. Manufacturing method of aluminum alloy materials
[0048] According to the manufacturing method of the aluminum alloy material of the present invention, the aluminum alloy material is manufactured as follows: in a 5wt% NaCl static aqueous solution at 25°C and pH 5.5, a silver-silver chloride electrode in saturated KCl is used as a reference electrode, and the aluminum alloy material is measured at a scanning speed of 20mV / min. In the obtained cathode polarization curve, the absolute value of the current density reaches 10μA / cm 2 The electrode potential is -1350mV to -1150mV. The manufacturing method comprises: a step of acid etching a substrate composed of an aluminum alloy containing Mg; and a step of performing a chemical conversion treatment on the surface of the substrate after acid etching to form a chemical conversion treatment film. In addition, the etching amount of the substrate in the acid etching step [E: (mg / m 2 )] Acid etching is performed in a manner that satisfies the relationship of 10M≤E≤200M relative to the Mg content [M (wt%)] in the substrate. Regarding the aluminum alloy material manufactured by the manufacturing method of the aluminum alloy material of the present invention, in the cathode polarization curve, the absolute value of the current density reaches 10μA / cm 2The electrode potential becomes -1350mV to -1150mV. Therefore, the interface between the aluminum alloy material and the adhesive can be suppressed from deteriorating due to tensile stress and corrosion, and can be suppressed from deteriorating due to the penetration of moisture, salt, etc. In addition, the aluminum alloy material of the present invention has the characteristics of the cathodic polarization curve as described above even when constituting an interface with a material other than an adhesive, so that the interface degradation caused by tensile stress, corrosion, penetration of moisture and salt, etc. can be suppressed. In addition, the above-mentioned E is 10M or more, so that the surface of the substrate after acid etching becomes clean, and a chemical conversion treatment film that is well in close contact with the surface of the substrate can be formed. On the other hand, if E exceeds 200M and increases excessively, the surface unevenness caused by etching and dirt (microparticles of insoluble substances produced by the acid remaining after etching) affect the bonding durability. This is because the dirt enters the inside of the surface unevenness and cannot be easily removed, thereby affecting the adhesion with the adhesive. Therefore, when E is 200M or less, unnecessary increase of surface irregularities and excessive generation of dirt can be suppressed, and the bonding durability between the aluminum alloy material and other materials can be improved. Hereinafter, each step of the method for producing the aluminum alloy material of the present invention will be described in detail.
[0049] (Rolling and heat treatment)
[0050] In one example, after the aluminum alloy is formed into an ingot according to a common method, homogenization treatment, hot rolling, cold rolling, intermediate annealing, cold rolling, or homogenization treatment, hot rolling, cold rolling are sequentially performed, and the aluminum alloy plate rolled to the final plate thickness is used as a substrate. Next, the aluminum alloy plate rolled to the final plate thickness is subjected to heat treatment. At this time, if the heat treatment is performed in the atmosphere, magnesium, which is an easily oxidizable element in the aluminum alloy, diffuses on the surface and combines with oxygen, forming a layer containing a large amount of magnesium oxide on the surface of the aluminum alloy plate.
[0051] (Degreasing process)
[0052] Before the acid etching process, a degreasing process can be arbitrarily performed. The purpose is to remove rolling oil, processing oil, lubricating oil, etc. attached to the surface of the aluminum alloy plate in the process before pickling. The solution used in the cleaning process is not particularly limited, but an alkaline cleaning agent, a surfactant or a mixture thereof, or an organic solvent can be appropriately used, followed by a water washing process. In the case where there is little oil attached to the surface of the aluminum alloy plate, the cleaning process can also be omitted. In addition, when the degreasing process is implemented, if an alkaline degreasing agent is used, a certain amount of dissolution of the base aluminum alloy occurs. If the amount of substrate dissolved in the cleaning process increases excessively, sometimes a large amount of dirt adheres to the surface of the plate and affects the subsequent processes. Therefore, when the degreasing process is performed, the amount of aluminum alloy dissolved is preferably set to 50 mg / m 2 Below, more preferably 40 mg / m 2In addition, in etching using an alkali, substances with low solubility in alkali, such as magnesium oxide, on the surface of the aluminum alloy plate cannot be removed, and therefore, the acid etching step cannot be replaced by alkali etching.
[0053] (Acid etching process)
[0054] In the acid etching step, the substrate composed of the aluminum alloy containing Mg is subjected to acid etching. The conditions for the acid etching are as long as the etching amount of the substrate [E: (mg / m 2)] It is sufficient that the condition of the relationship of 10M≤E≤200M is satisfied relative to the Mg amount [M (wt%)] in the substrate before acid etching, and there is no particular limitation. By performing acid etching under the condition of satisfying the relationship of 10M≤E≤200M, the fragile layer existing on the surface of the aluminum alloy substrate can be removed and the bonding durability can be improved. The fragile layer is a mixture of substances such as the surface deterioration layer produced in mechanical processing such as the rolling process and aluminum oxide and magnesium oxide grown on the surface of the aluminum alloy in the heat treatment process. If bonding is performed in a state where these fragile layers remain, the bonding durability decreases. For aluminum alloys containing a large amount of magnesium as an easily oxidizable element, magnesium oxide is easily generated in the heat treatment process, and the fragile layer tends to be formed thick. Therefore, in order to optimize the etching amount according to the magnesium alloy content of the substrate, E / M is set to 10 to 200. E / M is preferably 20 to 150, and more preferably 30 to 100. In addition, M is preferably 0.3 to 5.0wt%, more preferably 1.0 to 5.0wt%, and further preferably 2.0 to 5.0wt%. The amount of Mg in the substrate before etching can be measured by the emission spectrophotometry method specified in H 1305:2005, but any method that can obtain the same degree of accuracy will do. In addition, in the case of a purchased manufactured substrate, the amount of Mg can also be calculated from the Mg content disclosed in the substrate. Regarding the etching amount E of the substrate, a test piece obtained by cutting the substrate into an appropriate size can be used to measure the dry mass before and after etching, and the difference in the measurement results (mass before etching - mass after etching) is divided by the area of the test piece and converted into a value per unit area for calculation. The size of the test piece at this time can be arbitrary, but if the area is small, the change in weight is also reduced, which affects the measurement accuracy. Therefore, it is necessary to consider the accuracy of the balance used for weighing and set the area of the test piece to an appropriate size. As an etching solution for acid etching, nitric acid, sulfuric acid, hydrofluoric acid, phosphoric acid, or an acid as a mixed solution thereof can be used. The etching solution can arbitrarily contain an etching aid (oxidant), a surfactant, a chelating agent, etc. The acid concentration in the etching solution (in the case of a mixed solution, the total concentration of each acid solution) is preferably 0.01% by weight to 30% by weight, more preferably 0.03% by weight to 25% by weight, and further preferably 0.05% by weight to 20% by weight. The temperature of the etching solution is preferably 30 to 90°C, more preferably 40 to 90°C, and further preferably 45 to 90°C. The etching time is preferably 1 second to 30 seconds, more preferably 1 to 25 seconds, and further preferably 1 to 20 seconds. It is preferred to perform a water washing process after the acid etching process. In the water washing process, it is preferred to use water with a conductivity of 500mS / m or less at a temperature of 20°C. If water with high conductivity is used, various ions contained in the water are sometimes adsorbed on the surface of the aluminum alloy and become the main reason for the decrease in bonding durability. The water temperature in the water washing process is preferably 30°C to 90°C, more preferably 40°C to 85°C, and further preferably 45°C to 80°C.This is because the solubility of most substances in water with high temperature increases, so it is effective for cleaning the surface of the etched aluminum alloy substrate. When the water temperature of the water washing is high, the cleaning effect increases, but sometimes it leads to an increase in energy costs. If the water temperature of the water washing exceeds 90°C, sometimes the aluminum alloy substrate reacts with water to form a hydrated oxide film of aluminum on the surface. In addition, if the time of the water washing process is too long, sometimes the aluminum surface gradually reacts with the water washing water to form aluminum oxide. If it is too short, sometimes it is impossible to fully remove the treatment liquid attached to the surface. Therefore, the time of the water washing process is preferably 0.5 seconds to 30 seconds, and more preferably 1 second to 20 seconds.
[0055] (Step of forming a chemical conversion film)
[0056] In the process of forming a chemical treatment film, the surface of the substrate after acid etching is subjected to chemical treatment to form a chemical treatment film. There are multiple sites of cathode reaction on the surface after the acid etching process, and the bonding durability can be improved by forming an appropriate chemical treatment film. The chemical treatment film can be formed by the electrochemical reaction of the ions dissolved in the treatment solution and the aluminum alloy surface, so it is preferably an inorganic chemical treatment film. This is because the site of the cathode reaction present on the surface of the aluminum alloy substrate also plays a role as a site that is easy to form a film during the formation process of the chemical treatment film. Therefore, in the case of forming a chemical treatment film by the electrochemical reaction of the aluminum alloy with the ions dissolved in the solution, the cathode reaction site on the aluminum alloy surface can be efficiently covered. In addition, even in the inorganic chemical treatment film, it is particularly preferred to contain both titanium and zirconium. This is because the oxide or hydroxide of titanium and the oxide or hydroxide of zirconium formed as the chemical treatment film are chemically stable, and it is difficult to cause chemical changes even in a degraded environment, which is effective for preventing the bonding durability from decreasing. In addition, when a chemical conversion film is formed on the surface of an aluminum alloy substrate, as described above, the film is gradually formed from the cathode reaction site on the surface, so the electrochemical properties of the aluminum alloy surface are constantly changing during the process. Therefore, by adding elements with different solubility and electrode potential in the solution, namely titanium and zirconium, to the treatment solution, it is possible to widely cope with the aluminum alloy surface that is constantly changing during the formation of the chemical conversion film, and the surface of the aluminum alloy can be effectively and optimally covered with the chemical conversion film.
[0057] In addition, preferably, between the washing process in the acid etching process and the process of forming the chemical treatment film, drying and blowing are not carried out, and the aluminum alloy surface is kept wetted by the washing water. This is because it is possible to prevent the various oxides on the aluminum alloy surface removed in the acid etching process from contacting with the air and growing thicker again. However, if in a state of long-term contact with the washing water, various oxides begin to grow on the aluminum alloy surface. Therefore, it is preferred that the process of forming the chemical treatment film is started within 30 seconds after the washing process in the acid etching process ends, more preferably within 10 seconds, and further preferably within 5 seconds. In addition, it is most preferably within 2 seconds.
[0058] In the process of forming the chemical conversion film, preferably, the chemical conversion treatment is carried out using a treatment solution containing a titanium hydride compound and a zirconium fluoride compound so that the total mass concentration [C (ppm, converted to the amount of metal elements)] of the titanium fluoride compound and the zirconium fluoride compound in the treatment solution and the treatment time [t (seconds)] satisfy 50≤C×t≤1500. When C×t is within the above range, an optimal chemical conversion film can be formed on the surface of the aluminum alloy after the acid etching process. Examples of the titanium fluoride compound include 6-fluorotitanic acid (H 2 TiF 6 ) and its salts (especially potassium salt, sodium salt, ammonium salt) etc. As zirconium fluoride compounds, 6-fluorozirconic acid (H 2 ZF 6) and its salts (especially potassium salt, sodium salt, ammonium salt), etc. Preferably 50≤C×t≤1500, more preferably 80≤C×t≤1400, and further preferably 100≤C×t≤1300. When C×t is less than 50, it is sometimes impossible to fully form a chemical conversion treatment film on the surface of the aluminum alloy. In addition, when C×t exceeds 1500, the chemical conversion treatment film is sometimes formed too thick, resulting in a decrease in adhesion durability. The total mass concentration C (converted to the amount of metal elements) of the titanium fluoride compound and the zirconium fluoride compound in the treatment liquid is preferably 20 to 400 ppm, more preferably 30 to 350 ppm, and further preferably 40 to 300 ppm. The time t is preferably 0.5 to 30 seconds, more preferably 1 to 25 seconds, and further preferably 1.5 seconds to 20 seconds. The mass concentration of the titanium fluoride compound in the treatment liquid is preferably 10 to 400 ppm, more preferably 15 to 300 ppm, and further preferably 20 to 200 ppm in terms of metal elements. The mass concentration of the zirconium fluoride compound in the treatment liquid is preferably 10 to 400 ppm, more preferably 15 to 300 ppm, and further preferably 20 to 200 ppm. The temperature of the treatment liquid is preferably 30 to 80° C., more preferably 35 to 70° C., and further preferably 40 to 65° C. If the concentration of the titanium fluoride compound and the zirconium fluoride compound in the treatment liquid, the treatment time, and the treatment temperature are within the above ranges, and further [C (ppm, converted to the amount of metal element)] and the treatment time [t (seconds)] are within the above ranges, the chemical conversion treatment film on the surface of the aluminum alloy can be most appropriately attached.
[0059] In addition, as the treatment area of the aluminum alloy substrate increases, the Al ions dissolved from the substrate in the treatment solution for chemical treatment gradually increase. If the Al ions increase, it becomes the main reason for hindering the formation of the chemical treatment film. The Al ion concentration in the treatment solution does not affect the formation of the chemical treatment film until it reaches about 800ppm. The Al ion concentration in the treatment solution is preferably below 600ppm, more preferably below 500ppm.
[0060] In one example, a water washing process is performed immediately after the process of forming a chemical conversion treatment film. As a result, the treatment liquid remaining on the surface can be quickly removed, and the thickness of the chemical conversion treatment film can be appropriately adjusted by controlling the reaction time between the substrate surface and the treatment liquid. Furthermore, it is possible to prevent the components of the treatment liquid from remaining on the surface of the chemical conversion treatment film. If the components of the treatment liquid remain on the surface of the chemical conversion treatment film, it will cause a decrease in the adhesion durability and discoloration of the substrate surface. The time from the process of forming the chemical conversion treatment film to the water washing process is preferably within 2 seconds, more preferably within 1 second. The conductivity of the water used in the water washing process is preferably less than 100mS / m at a temperature of 20°C, and more preferably less than 50mS / m. If water with high conductivity is used, various ions contained in the water remain on the substrate surface and cause a decrease in the adhesion durability and discoloration of the substrate surface. In addition, for the determination of conductivity, for example, an AC two-pole method can be used.
[0061] The washing process after the process of forming the chemical treatment film affects the final quality of the substrate surface, so it is preferred to set multiple washing processes of more than two stages. In the case where the washing process after the process of forming the chemical treatment film is set multiple times, it is preferably set to within 2 seconds, more preferably within 1 second. In addition, preferably, the conductivity of the water in the washing process performed thereafter is the same or lower than the conductivity of the water used in the initial washing process after the process of forming the chemical treatment film. Thus, the components in the chemical treatment solution that cannot be completely removed in the first washing process can be fully removed. If the washing process time is too long, sometimes the surface of the aluminum alloy substrate gradually reacts with the washing water to form aluminum oxide, but if the washing process time is too short, the cleaning effect cannot be fully obtained. Therefore, the total value of the time of the washing process performed after the process of forming the chemical treatment film is preferably 0.5 seconds to 30 seconds, more preferably 1 second to 20 seconds. In addition, when the water temperature is high, the solubility of most substances in water increases. Therefore, when the water temperature in the water washing process after the process of forming the chemical treatment film is high, the cleaning effect is improved. If the water temperature in the water washing process exceeds 90°C, it sometimes leads to an increase in energy costs. In addition, it sometimes causes a hydration reaction between the aluminum alloy substrate and water to form a hydrated oxide film of aluminum on the surface of the substrate. Therefore, the water temperature in at least the initial water washing process after the process of forming the chemical treatment film is preferably 30°C to 90°C, more preferably 40°C to 85°C, and further preferably 50°C to 85°C. The water temperature in the subsequent water washing process only needs to be in the range of 10°C to 90°C. Preferably, hot air drying is performed after the water washing process to remove water droplets remaining on the surface of the aluminum alloy substrate.
[0062] (Processing methods for each process)
[0063] Regarding the above-mentioned degreasing process, acid etching process, chemical conversion treatment film forming process, and water washing process accompanying each process, a method of spraying treatment liquid on the surface of the aluminum alloy and a method of passing the aluminum alloy through a treatment tank filled with treatment liquid (immersion method) are appropriately adopted.
[0064] (How to use aluminum alloy materials)
[0065] After the aluminum alloy material of the present invention is provided with an adhesive layer on the surface of the chemical conversion treatment film, it can be further bonded with other aluminum alloy materials and used as a component for automobiles, construction machinery, and conveyors. The aluminum alloy material of the present invention has excellent bonding durability relative to other materials, and therefore, it can be firmly bonded to other aluminum alloy materials via an adhesive, and can maintain bonding strength for a long time. As adhesives, epoxy resins, acrylic resins, polyurethane resins, etc. can be cited, and thermosetting epoxy resins are preferably used. The thickness of the adhesive layer provided on the surface of the chemical conversion treatment film is not particularly limited, but is preferably 10 to 5000 μm, more preferably 20 to 3000 μm, and further preferably 30 to 1000 μm.
[0066] Example
[0067] Hereinafter, the present invention will be described in detail based on the examples. In addition, the present invention is not limited to the examples shown below, and the structure thereof can be appropriately changed within the scope not impairing the gist of the present invention.
[0068] (Examples 1 to 8)
[0069] A substrate having a thickness of 1 mm and a size of 7 cm×15 cm as shown in Table 1 below was prepared, and acid etching was performed on the substrate under the following conditions. Examples 1 to 3 were acid-etched for 6 seconds using an etching solution of 60°C, 0.5 mass % sulfuric acid + 0.05 mass % hydrofluoric acid under the conditions shown in Table 1. Similarly, Examples 4 to 7 were acid-etched for 4 seconds using an etching solution of 60°C, 0.5 mass % sulfuric acid + 0.05 mass % hydrofluoric acid under the conditions shown in Table 1. In addition, Example 8 was acid-etched for 4 seconds using an etching solution of 80°C, 10 mass % sulfuric acid under the conditions shown in Table 1. After acid etching, the substrate was washed with ion-exchanged water having an electrical conductivity of 0.2 mS / m at 20°C and a temperature of 70°C. Next, a chemical conversion treatment was immediately performed under the conditions of temperature, composition, and treatment time shown in Table 1, thereby obtaining an aluminum alloy material having a substrate and a chemical conversion treatment film with the film amount shown in Table 1. In addition, the titanium fluoride compound and the zirconium fluoride compound used in Examples 1 to 8 are hexafluorotitanic acid and hexafluorozirconic acid, respectively. Immediately after the chemical conversion treatment, the substrate was washed with ion-exchanged water at 70°C with an electrical conductivity of 0.2 mS / m at 20°C, and then washed with ion-exchanged water at room temperature (specifically 20°C) with an electrical conductivity of 0.1 mS / m at 20°C, and then dried by spraying hot air at 50°C. In addition, the electrical conductivity of water was measured using the "Portable Conductivity Meter ES-71" manufactured by Horiba, Ltd.
[0070] (Comparative Examples 1-2)
[0071] In Comparative Example 1, a substrate of the same size as the substrate used in the example shown in Table 1 below was prepared, and the substrate was acid-etched for 4 seconds using an etching solution of a component of 10 mass % sulfuric acid at 80°C under the conditions shown in Table 1, and the substrate was washed with ion-exchanged water at 70°C with an electrical conductivity of 0.2 mS / m at 20°C, thereby obtaining an aluminum alloy substrate. In addition, no chemical conversion treatment was performed in Comparative Example 1. In Comparative Example 2, acid etching was performed for 1 second using an etching solution of a component of 10 mass % sulfuric acid at 50°C under the conditions shown in Table 1, and the substrate was washed with ion-exchanged water at 70°C with an electrical conductivity of 0.2 mS / m at 20°C after the acid etching, and then, the chemical conversion treatment was immediately performed under the conditions shown in Table 1, thereby obtaining an aluminum alloy material having a substrate and a chemical conversion treatment film of the film amount shown in Table 1. In addition, the titanium fluoride compound and the zirconium fluoride compound used in Comparative Example 2 were hexafluorotitanic acid and hexafluorozirconic acid, respectively. After the chemical conversion treatment, the substrate is immediately washed with ion-exchanged water at 70°C with an electrical conductivity of 0.2 mS / m at 20°C, and then washed with ion-exchanged water at room temperature (specifically 20°C) with an electrical conductivity of 0.1 mS / m at 20°C, and then dried by spraying hot air at 50°C.
[0072]
Table 1
[0073]
[0074] The cathode polarization curve of the aluminum alloy material of each example obtained in the above manner was measured by the above method. Figure 2 This is a graph showing the cathode polarization curve of the aluminum alloy material of Example 2 measured in the above manner.
[0075] As a bonding evaluation, the aluminum alloy materials obtained in each example were evaluated by the method based on the modified APGE test described in the Japanese Patent Gazette No. 2018-527467, and the bonding fracture cycle Cy was measured. The detailed order of the modified APGE test is as follows. Two test pieces with a length of 52.5 mm and a width of 25 mm were bonded using an epoxy adhesive so that the bonding length reached 12.5 mm and the bonding thickness reached 0.2 mm. In addition, in order to prevent the test piece with a plate thickness of 1 mm from deforming during the test, the same type of plate was pre-pasted with the same adhesive. Next, for the 6 pairs of test pieces made in the above order, they were connected at their respective ends using stainless steel bolts. In addition, in order to prevent dissimilar metal contact corrosion caused by contact between the test piece and the stainless steel bolt, insulation was implemented by winding a sealing tape around the bolt and other appropriate methods. Maintain a state in which a tensile stress of 2400N is always applied to both ends of the 6 pairs of connections. Furthermore, the connection body in a state of being stressed is immersed in a 5 mass % NaCl aqueous solution for 15 minutes, taken out at room temperature of 25°C and allowed to dry naturally within 105 minutes, and placed in a constant temperature and humidity chamber at 50°C and relative humidity set to 90% RH for 22 hours. According to this method, the durability in a very harsh bonding interface degradation environment where tensile stress and corrosive environment are superimposed can be evaluated. In addition, the time from the time when a tensile stress of 2400N is applied to the time when the 22 hours of maintenance in the constant temperature and humidity chamber ends is set as one cycle for statistics, and one cycle of the test is performed within one day on a working day. In addition, the state of keeping the connection body in the constant temperature and humidity chamber for 48 hours on a rest day is not counted as a test cycle. The joining condition of the sample is confirmed at the beginning of the next cycle. If a break is found in the bonding part of any one of the 6 pairs of connected test pieces, the number of cycles at that moment is set as the first break (the break of the first pair). In addition, even if the test piece is found to be broken during the period from when the stress of 2400N is loaded until it is placed in the constant temperature and humidity chamber, the number of cycles at that moment is set as the first fracture. The broken test piece is removed, a single plate of the same size as a pair of test pieces is inserted and fastened to the other test pieces with bolts, and stress is applied again to restart the test cycle. In addition, in the case where the bonding parts of multiple test pieces are broken at the same time, the same number of cycles is counted for each test piece. For example, when there is no fracture at the end of 18 cycles, and 2 pairs of the 6 pairs of test pieces are broken at the beginning of the 20th cycle, 20 cycles are set for the first fracture and the second fracture, respectively, and the next fracture becomes the third fracture. This sequence is repeated until the 4th fracture (the moment of any 4 pairs of fractures among the 6 pairs of connected test pieces) and the test is continued.Then, the average value of the number of cycles from the first fracture to the fourth fracture was calculated (rounded to the first decimal place) and set to Cy. The case where Cy<18 was evaluated as "×", the case where 18≤Cy<20 was evaluated as "0", and the case where 20≤Cy was evaluated as "□". The above measurement results are shown in Table 2 below.
[0076]
Table 2
[0077]
[0078] According to Table 2, the bonding evaluations in Examples 1 to 8 were “0” or “◎”, while the bonding evaluations in Comparative Examples 1 to 2 were “×”. This shows that the aluminum alloy material of the present invention has excellent bonding durability.
Claims
1. An aluminum alloy material comprising: a substrate composed of an aluminum alloy; and a chemical conversion treatment film on the surface of the substrate, wherein: In a 5 wt % NaCl static aqueous solution at 25°C and pH 5.5, the aluminum alloy material was measured with a silver-silver chloride electrode in saturated KCl as a reference electrode and a scanning speed of 20 mV / min. In the obtained cathodic polarization curve, the absolute value of the current density reached 10 μA / cm 2 The electrode potential is -1350mV~-1150mV, The chemical conversion film contains a titanium compound and a zirconium compound. The titanium compound is at least one of titanium oxide and titanium hydroxide, The zirconium compound is at least one of zirconium oxide and zirconium hydroxide.
2. The aluminum alloy material according to claim 1, wherein: The substrate is composed of an aluminum alloy containing 0.3 to 5.0 wt % of Mg.
3. The aluminum alloy material according to claim 1 or 2, wherein: The total amount of the titanium compound and the zirconium compound in the chemical conversion film is 2 to 29 mg / m 2 .
4. A method for manufacturing an aluminum alloy material, wherein: In a 5 wt % NaCl static aqueous solution at 25°C and pH 5.5, the aluminum alloy material was measured at a scanning rate of 20 mV / min using a silver-silver chloride electrode in saturated KCl as a reference electrode. In the obtained cathodic polarization curve, the absolute value of the current density reached 10 μA / cm 2 The electrode potential is -1350mV to -1150mV, and the manufacturing method has the following steps: A step of acid etching a substrate composed of an aluminum alloy containing Mg; a step of performing a chemical conversion treatment on the surface of the acid-etched substrate to form a chemical conversion treatment film; and The water washing step is carried out immediately after the step of forming the chemical conversion treatment film. The etching amount E of the substrate in the acid etching process satisfies the relationship of 10M≤E≤200M relative to the Mg amount M in the substrate, where the unit of E is mg / m 2 , the unit of M is wt%, In the process of forming the chemical conversion treatment film, a treatment solution containing a titanium fluoride compound and a zirconium fluoride compound is used to carry out chemical conversion treatment in a manner such that the total mass concentration C of the titanium fluoride compound and the zirconium fluoride compound in the treatment solution and the treatment time t satisfy 50≤C×t≤1500, wherein the unit of C is ppm and converted into the amount of metal element, and the unit of t is second.
5. The method for producing an aluminum alloy material according to claim 4, wherein: The time from the step of forming the chemical conversion treatment film to the step of washing with water is within 2 seconds.
6. The method for producing an aluminum alloy material according to claim 4 or 5, wherein: The water washing step is performed multiple times in two or more stages.
Citation Information
Patent Citations
Aluminum alloy sheet, joined body and automotive member using the same
JP2014062277A
Surface-treated aluminum alloy sheet
JP2015206117A
Method for pretreating an aluminum surface with a composition containing zirconium and molybdenum
JP2018527467A
Chromium-free passivation surface treatment process of aluminium material
CN102321881A
Aluminum alloy composition, aluminum extrusion tube and fin material with improved corrosion durability comprising same, and heat exchanger constructed of same
CN105637107A